Aqueous coating composition

A water-based paint with a graft copolymer of polyorganosiloxane addresses antifouling and film-forming issues by reducing tan δ at seawater temperatures, enhancing film strength and antifouling properties in marine environments.

JP2024143794APending Publication Date: 2024-10-11KANEKA CORP

Patent Information

Application Number
JP2023056677
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional water-based paints lack sufficient antifouling properties and film-forming capabilities, particularly in marine environments, necessitating improvements in coating films to reduce loss tangent (tan δ) at seawater temperatures.

Method used

A water-based paint formulation incorporating a graft copolymer composed of polyorganosiloxane with specific structural units, including a first graft portion without a chain transfer agent and a second graft portion with a chain transfer agent, enhancing film-forming properties and reducing tan δ at seawater temperatures.

Benefits of technology

The formulation provides a coating film with excellent antifouling properties and improved film-forming capabilities, offering superior performance in marine applications by maintaining a low loss tangent (tan δ) and reducing blister formation when immersed in water.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143794000001
    Figure 2024143794000001
Patent Text Reader

Abstract

To provide an aqueous coating composition having excellent film-forming properties and capable of providing a coating film having a low loss tangent (tanδ) under seawater temperature.SOLUTION: There is provided an aqueous coating composition which comprises a graft copolymer (A) containing a non-crosslinked polyorganosiloxane containing a specific structural unit and a graft moiety, wherein the graft moiety includes a first graft moiety and a second graft moiety, each of which has a specific structure.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a water-based paint. [Background technology]

[0002] Various paints (e.g., antifouling paints) have been developed. Currently, the mainstream of paints is solvent-based paints, but in recent years, from the viewpoints of environmental conservation and safety and hygiene, there has been a rapid shift to water-based paints. Examples of water-based paints include the technologies described in Patent Documents 1 and 2. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-260883 A [Patent Document 2] JP 2007-191531 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the above-mentioned conventional techniques are insufficient from the viewpoint of the antifouling property of the coating film, and there is room for further improvement. In addition, it is preferable that the coating material has excellent film-forming properties.

[0005] One embodiment of the present invention has been made in consideration of the above problems, and its object is to provide a new water-based paint that has excellent film-forming properties and can provide a coating film with a small loss tangent (tan δ) at seawater temperature. [Means for solving the problem]

[0006] The present inventors conducted extensive research to solve the above problems and have now completed the present invention.

[0007] That is, one embodiment of the present invention includes the following configuration. [1] A polymerizable composition comprising a graft copolymer (A), the graft copolymer (A) comprising a polyorganosiloxane and a graft portion graft-bonded to the polyorganosiloxane, the polyorganosiloxane comprising (a) a structural unit U1 derived from a monomer containing (a-1) one or more hydrolyzable silyl groups and (a-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule, and (b) being non-crosslinked, the graft portion comprising a first graft portion and a second graft portion, the first graft portion being the second graft portion contains (a) a structural unit U2 derived from a monomer containing (a-1) one or more hydrolyzable silyl groups and (a-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule, and does not contain (b) a structural unit U3 derived from a monomer containing (b-1) one or more hydrolyzable silyl groups and (b-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule. [2] The water-based paint according to [1], wherein the graft portion contains 7.0% by weight to 20.0% by weight of the structural unit U2 relative to 100% by weight of the graft portion. [3] The water-based paint according to [1] or [2], wherein the glass transition temperature of the graft portion is 25°C or higher. [4] The water-based coating material according to any one of [1] to [3], wherein the polyorganosiloxane contains 0.001 wt % to 10.0 wt % of the structural unit U1 relative to 100 wt % of the polyorganosiloxane. [5] The water-based paint according to any one of [1] to [4], wherein the graft portion further contains a constitutional unit derived from a reactive emulsifier. [6] The water-based paint according to [5], wherein the graft portion contains 0.1 wt % to 20.0 wt % of a constituent unit derived from the reactive emulsifier, relative to 100 wt % of the graft portion. [7] The water-based coating material according to any one of [1] to [6], wherein the polyorganosiloxane has a volume average particle size of 0.03 μm to 50.00 μm. [8] The water-based coating material according to any one of [1] to [7], wherein the polyorganosiloxane accounts for 55% by weight to 90% by weight of 100% by weight of the graft copolymer (A). [9] The water-based coating material according to any one of [1] to [8], further comprising a polymer (B), the polymer (B) comprising a structural unit derived from one or more monomers selected from the group consisting of an aromatic vinyl monomer, a vinyl cyan monomer, and a (meth)acrylate monomer.

[10] The water-based paint according to any one of [1] to [9], further comprising an antifouling agent.

[11] The water-based paint according to [9], wherein the polymer (B) accounts for 5.0% by weight or more of the total of the graft copolymer (A) and the polymer (B) being 100% by weight.

[12] A method for producing an aqueous coating film, comprising a step of applying the aqueous coating material according to any one of [1] to

[11] to an underwater structure.

[13] A method for producing a polyorganosiloxane, comprising: a step 1 of polymerizing a monomer mixture for forming a polyorganosiloxane, the monomer mixture including (a) an organosiloxane, and (b) (b-1) a monomer M1 having one or more hydrolyzable silyl groups in the molecule, and (b-2) one or more ethylenically unsaturated groups and / or mercapto groups, to obtain a polyorganosiloxane; and a step 2 of polymerizing a monomer mixture for forming a graft portion in the presence of the polyorganosiloxane obtained in the step 1, wherein in the step 1, the total amount of a polyfunctional alkoxysilane compound and a polyfunctional monomer is 0.50% by weight or less in 100% by weight of the monomer mixture for forming a polyorganosiloxane, and in the step 2, and step 2b of polymerizing a monomer mixture for forming a second graft portion, wherein in step 2a, the monomer mixture for forming the first graft portion contains (a) a monomer M2 derived from a monomer containing (a-1) one or more hydrolyzable silyl groups in the molecule and (a-2) one or more ethylenically unsaturated groups and / or mercapto groups, and does not contain (b) a chain transfer agent, and in step 2b, the monomer mixture for forming the second graft portion contains (a) a chain transfer agent, and does not contain (b) a monomer M3 containing (b-1) one or more hydrolyzable silyl groups in the molecule and (b-2) one or more ethylenically unsaturated groups and / or mercapto groups. Effect of the Invention

[0008] According to one embodiment of the present invention, it is possible to provide a water-based paint having excellent film-forming properties and capable of providing a coating film having a small loss tangent (tan δ) at seawater temperature. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims. In addition, embodiments or examples obtained by combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment. All academic documents and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more (including A and greater than A) and B or less (including B and smaller than B)".

[0010] In this specification, a "structural unit derived from an X monomer" contained in a polymer, copolymer, or resin may be referred to as an "X unit".

[0011] 1. Technical Concept of One Embodiment of the Present Invention It is common to apply antifouling paints to underwater structures. Currently, solvent-based paints are the mainstream of such paints, but from the viewpoints of environmental conservation and safety and health, there is a rapid shift to water-based paints.

[0012] Known examples of water-based antifouling coating compositions include those described in Patent Document 2. Also, known examples of water-based coating materials include those described in Patent Document 1.

[0013] However, in the techniques described in any of the documents, there is still room for improvement in terms of the antifouling properties required for an antifouling paint. Note that Patent Document 1 does not particularly mention the antifouling properties of the water-based coating material.

[0014] Conventionally, it has been believed that the antifouling properties of a silicone-based antifouling paint can be improved by increasing the elasticity of the paint film. The present inventor has conducted intensive research to provide a water-based paint that can provide a paint film with better antifouling properties than conventional paints. In the process, the present inventor has hypothesized that not only the elasticity of the paint film but also its viscosity can affect the antifouling properties, and that the antifouling properties of the paint film can be improved by reducing the loss tangent (tan δ), which is one of the indicators of the balance between elasticity and viscosity. Based on this hypothesis, the present inventor has conducted intensive research with the aim of providing a water-based paint that can provide a paint film with a small loss tangent (tan δ) at seawater temperature. As a result, the present inventor has independently discovered a novel finding that the higher the glass transition temperature of the graft portion, the lower the loss tangent (tan δ) of the paint film at seawater temperature.

[0015] Water-based paints are also required to have film-forming properties. The present inventor then conducted intensive research with the aim of providing a water-based paint with excellent film-forming properties. As a result, the present inventor independently discovered a new finding that the use of a chain transfer agent in the polymerization of the graft portion can result in a water-based paint with excellent film-forming properties. Although the reason for this is unclear, it is speculated that the use of a chain transfer agent in the polymerization of the graft portion produces a polymer that has the same composition as the graft portion and is not graft-bonded to the polyorganosiloxane, and that such a polymer improves the film-forming properties of the water-based paint. Note that the embodiment of the present invention is not limited to such a speculation.

[0016] As a result of the above-mentioned investigation, the present inventors produced a graft copolymer in which a graft part with a high glass transition temperature was formed using a chain transfer agent, and evaluated the film-forming property of the water-based paint obtained using the graft copolymer. As a result, it was surprising that the water-based paint obtained in this way had poor film-forming property, even though a chain transfer agent was used to form the graft part. Therefore, the present inventors have further conducted intensive research with the aim of providing a water-based paint having excellent film-forming properties and capable of providing a coating film having a small loss tangent (tan δ) at seawater temperature. As a result, the present inventors have surprisingly and independently found that a water-based paint having excellent film-forming properties and capable of providing a coating film having a low loss tangent (tan δ) at seawater temperature can be provided by using the following composition, and have completed the present invention: A water-based paint comprising a graft copolymer (A), (i) the graft copolymer (A) comprises a polyorganosiloxane and a graft portion grafted to the polyorganosiloxane; (ii) the polyorganosiloxane contains a specific structural unit U1 and is non-crosslinked; (iii) the graft portion comprises a first graft portion and a second graft portion; (iv) the first graft portion contains a specific structural unit U2 and does not contain a structural unit derived from a chain transfer agent; (v) The water-based paint has a second graft portion that contains a structural unit derived from a chain transfer agent and does not contain the specific structural unit U3.

[0017] [2. Water-based paint] An aqueous coating material according to one embodiment of the present invention comprises a graft copolymer (A), the graft copolymer (A) comprises a polyorganosiloxane and a graft portion graft-bonded to the polyorganosiloxane, the polyorganosiloxane (a) comprises a structural unit U1 derived from a monomer containing (a-1) one or more hydrolyzable silyl groups and (a-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule, and (b) is non-crosslinked, the graft portion comprises a first graft portion and a second graft portion, The first graft portion (a) comprises a structural unit U2 derived from a monomer containing (a-1) one or more hydrolyzable silyl groups and (a-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule, and does not comprise a structural unit derived from (b) a chain transfer agent, and the second graft portion (a) comprises a structural unit derived from a chain transfer agent, and does not comprise a structural unit U3 derived from a monomer containing (b-1) one or more hydrolyzable silyl groups and (b-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule.

[0018] In this specification, "the water-based paint according to one embodiment of the present invention" may also be referred to as "the present water-based paint".

[0019] Since the present water-based paint has the above-mentioned constitution, it has the advantage of being able to provide a coating film with excellent film-forming properties and a small loss tangent (tan δ) at seawater temperature. A coating film with a small loss tangent (tan δ) at seawater temperature is considered to have excellent antifouling properties at seawater temperature (e.g., antifouling properties against aquatic organisms). Therefore, the present water-based paint can be suitably used as an antifouling paint for underwater structures. A method for measuring the loss tangent (tan δ) of a coating film of a water-based paint in one embodiment of the present invention will be described in detail in the examples below.

[0020] In other words, another embodiment of the present invention includes a graft copolymer (A), the graft copolymer (A) includes a polyorganosiloxane and a graft portion grafted to the polyorganosiloxane, the polyorganosiloxane includes (a) (a-1) one or more hydrolyzable silyl groups in the molecule, and (a-2) one or more ethylenically unsaturated groups and / or mercapto groups, and includes a structural unit U1 derived from a monomer having such a monomer, and (b) is non-crosslinked, the graft portion includes a first graft portion and a second graft portion, and the first graft portion includes a second graft portion and a third graft portion. (a) comprises a structural unit U2 derived from a monomer containing (a-1) one or more hydrolyzable silyl groups and (a-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule, and does not comprise a structural unit derived from (b) a chain transfer agent, and the second graft portion comprises (a) a structural unit derived from a chain transfer agent, and does not comprise a structural unit U3 derived from a monomer containing (b) (b-1) one or more hydrolyzable silyl groups and (b-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule.

[0021] (2-1. Graft Copolymer (A)) The graft copolymer (A) contains a polyorganosiloxane and a graft portion graft-bonded to the polyorganosiloxane.

[0022] (2-1-1. Polyorganosiloxane) The polyorganosiloxane includes (i) an organosiloxane-based unit and (ii) a structural unit U1 derived from a monomer containing, in the molecule, (ii-a) one or more hydrolyzable silyl groups and (ii-b) one or more ethylenically unsaturated groups and / or mercapto groups.

[0023] The inclusion of polyorganosiloxane in the graft copolymer (A) allows the water-based paint to provide a coating film with excellent water repellency. The water repellency of a coating film can be correlated with the contact angle of the coating film. Therefore, the water repellency of a coating film can be evaluated by the contact angle of the coating film. It can also be said that the inclusion of polyorganosiloxane in the graft copolymer (A) allows the water-based paint to provide a coating film with a large contact angle. In addition, the inclusion of polyorganosiloxane in the graft copolymer (A) allows the coating film provided by the water-based paint to have sufficient heat resistance and excellent impact resistance at low temperatures.

[0024] (Organosiloxane unit) The organosiloxane-based units are not particularly limited, but examples thereof include (a) alkyl or aryl di-substituted silyloxy units such as dimethylsilyloxy units, diethylsilyloxy units, methylphenylsilyloxy units, diphenylsilyloxy units, and dimethylsilyloxy-diphenylsilyloxy units, and (b) alkyl or aryl mono-substituted silyloxy units such as organohydrogensilyloxy units in which a portion of the alkyl in the side chain is substituted with a hydrogen atom. The polyorganosiloxane may contain only one type of the above-mentioned organosiloxane-based units, or may contain two or more types in combination.

[0025] Since the resulting water-based coating material can provide a coating film with excellent heat resistance, the polyorganosiloxane preferably contains organosiloxane-based units in an amount of 50 mol% or more, more preferably 60 mol% or more, even more preferably 70 mol% or more, even more preferably 80 mol% or more, even more preferably 90 mol% or more, and particularly preferably 95 mol% or more, out of 100 mol% of all structural units contained in the polyorganosiloxane.

[0026] Since the obtained water-based paint can provide a coating film with better heat resistance, the polyorganosiloxane preferably contains 50 mol% or more of one or more structural units selected from the group consisting of dimethylsilyloxy unit, methylphenylsilyloxy unit and dimethylsilyloxy-diphenylsilyloxy unit, more preferably 60 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, even more preferably 90 mol% or more, and particularly preferably 95 mol% or more of the total structural units contained in the polyorganosiloxane (100 mol%). The raw material of the dimethylsilyloxy unit is easier to obtain and cheaper than other organosiloxane monomers. Therefore, from the viewpoint of availability and economy, the polyorganosiloxane preferably contains 50 mol% or more of dimethylsilyloxy units, more preferably 60 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, even more preferably 90 mol% or more, and particularly preferably 95 mol% or more, of 100 mol% of all structural units contained in the polyorganosiloxane.

[0027] (Unit U1) In preparing polyorganosiloxane, a monomer M1 containing (a) one or more hydrolyzable silyl groups and (b) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule is used as a raw material to obtain a polyorganosiloxane containing a structural unit U1.

[0028] The hydrolyzable silyl group contained in the monomer M1 used in one embodiment of the present invention is not particularly limited.

[0029] Examples of the hydrolyzable silyl group include a halogenosilyl group, an acyloxysilyl group, an amidosilyl group, an aminosilyl group, an alkenyloxysilyl group, an aminoxysilyl group, an oximesilyl group, an alkoxysilyl group, a thioalkoxysilyl group, and a silanol group.

[0030] The hydrolyzable silyl group of the monomer M1 is preferably an alkoxysilyl group because of its high polymerization reactivity and ease of handling. When the monomer M1 contains two or more hydrolyzable silyl groups in the molecule, the multiple hydrolyzable silyl groups may be the same or different from each other.

[0031] The ethylenically unsaturated group contained in the monomer M1 used in one embodiment of the present invention is not particularly limited.

[0032] Examples of the ethylenically unsaturated group include a vinyl group, an acryloyl group, and a methacryloyl group.

[0033] From the viewpoint of reactivity during the formation of the first graft portion and the formation of the second graft portion, the ethylenically unsaturated group of the monomer M1 is preferably one or more selected from the group consisting of an acryloyl group and a methacryloyl group. When the monomer M1 contains two or more ethylenically unsaturated groups in the molecule, the multiple ethylenically unsaturated groups may be the same or different from each other. The "time of forming the first graft portion" and the "time of forming the second graft portion" can also be referred to as "time of polymerization of the monomer mixture for forming the first graft portion" and "time of polymerization of the monomer mixture for forming the second graft portion", respectively.

[0034] Specific examples of the monomer M1 include, for example, (a) vinyl silanes such as vinylmethyldimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, and tetramethyltetravinylcyclotetrasiloxane, (b) β-methacryloyloxyethyldimethoxymethylsilane, 3-(meth)acryloyloxypropyltrimethoxysilane, 3-(meth)acryloyloxypropyldimethoxymethylsilane, 3-(meth)acryloyloxypropylmethoxydimethylsilane, 3-(meth)acryloyloxypropyltriethoxysilane, 3-(meth)acryloyloxypropyldiethoxymethylsilane, 3-(meth)acryloyloxypropyl Examples of the silane include (meth)acryloyloxyalkylsilanes such as diethoxyethylsilane, 3-(meth)acryloyloxypropylethoxydimethylsilane, 3-(meth)acryloyloxypropylethoxydiethylsilane, and δ-(meth)acryloyloxybutyldiethoxymethylsilane; and (c) mercaptoalkylsilanes such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyldimethoxymethylsilane, 3-mercaptopropylmethoxymethidylsilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropyldiethoxymethylsilane, and 3-mercaptopropyldiethoxyethylsilane. Specific examples of the monomer M1 include p-vinylphenylmethyldimethoxysilane, 2-(m-vinylphenyl)ethylmethyldimethoxysilane, 1-(m-vinylphenyl)methyldimethylisopropoxysilane, 2-(p-vinylphenyl)ethylmethyldimethoxysilane, 3-(p-vinylphenoxy)propylmethyldiethoxysilane, 3-(p-vinylbenzoyloxy)propylmethyldimethoxysilane, 1-(o-vinylphenyl)-1,1,2-trimethyl-2,2-dimethoxydisilane, 1-(p-vinylphenyl)-1,1-diphenyl-3-ethyl-3,3-diethoxydisiloxane, m-vinylphenyl-[3-(triethoxysilyl)propyl]diphenylsilane, and [3-(p-isopropenylbenzoylamino)propyl]phenyldipropoxysilane. These monomers M1 may be used alone or in combination of two or more.

[0035] Examples of the monomer M1 include β-methacryloyloxyethyl dimethoxymethyl silane, 3-(meth)acryloyloxypropyl trimethoxy silane, 3-(meth)acryloyloxypropyl dimethoxy methyl silane, 3-(meth)acryloyloxypropyl methoxy dimethyl silane, 3-(meth)acryloyloxypropyl triethoxy silane, 3-(meth)acryloyloxypropyl diethoxy methyl silane, 3-(meth)acryloyloxypropyl diethoxy ethyl silane, 3- At least one selected from the group consisting of (meth)acryloyloxypropylethoxydimethylsilane, 3-(meth)acryloyloxypropylethoxydiethylsilane, and δ-(meth)acryloyloxybutyldiethoxymethylsilane, is preferred, and at least one selected from the group consisting of 3-(meth)acryloyloxypropyltrimethoxysilane and 3-(meth)acryloyloxypropyldimethoxymethylsilane is more preferred. This configuration has the advantage that the polymerization of the first graft portion forming monomer mixture and the second graft forming monomer mixture in the presence of polyorganosiloxane can be efficiently carried out. As a result, it has the advantage that a graft copolymer (A) with a high graft rate can be obtained.

[0036] The polyorganosiloxane preferably contains 0.001% by weight to 10.0% by weight of the structural unit U1 in 100% by weight of the polyorganosiloxane, more preferably 0.001% by weight to 5.0% by weight, even more preferably 0.01% by weight to 5.0% by weight, even more preferably 1.0% by weight to 5.0% by weight, and particularly preferably 1.0% by weight to 3.0% by weight. This configuration has the advantage that the polymerization of the first graft portion forming monomer mixture and the second graft forming monomer mixture in the presence of the polyorganosiloxane can be efficiently carried out. As a result, it has the advantage that a graft copolymer (A) with a high graft rate can be obtained.

[0037] (Cross-linked structure of polyorganosiloxane) By using a polyfunctional alkoxysilane compound and / or a polyfunctional monomer during the preparation of polyorganosiloxane, a crosslinked structure can be introduced into the polyorganosiloxane. Therefore, the polyfunctional alkoxysilane compound and the polyfunctional monomer can be said to be crosslinking agents in the polyorganosiloxane. In one embodiment of the present invention, the polyorganosiloxane is non-crosslinked. Here, "the polyorganosiloxane is non-crosslinked" means that the total amount of the polyfunctional alkoxysilane compound and the polyfunctional monomer used during the preparation of the polyorganosiloxane is 0.50% by weight or less in 100% by weight of the monomer mixture for forming the polyorganosiloxane. In other words, in one embodiment of the present invention, the polyorganosiloxane is substantially non-crosslinked. The total amount of the polyfunctional alkoxysilane compound and the polyfunctional monomer used in preparing the polyorganosiloxane is preferably 0.50% by weight or less, more preferably 0.20% by weight or less, even more preferably 0.10% by weight or less, and particularly preferably 0.01% by weight or less, based on 100% by weight of the monomer mixture for forming the polyorganosiloxane.

[0038] Examples of polyfunctional alkoxysilane compounds include tetramethoxysilane, tetraethoxysilane (TEOS), tetraisopropoxysilane, tetrabutoxysilane, tetraoctylsilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, methyltriisopropoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, and dimethyldimethoxysilane.

[0039] A polyfunctional monomer can be said to be a monomer having two or more radically polymerizable reactive groups in the same molecule. The radically polymerizable reactive group is, for example, a carbon-carbon double bond. Examples of polyfunctional monomers include (meth)acrylates having an ethylenically unsaturated double bond, such as allyl alkyl (meth)acrylates and allyloxy alkyl (meth)acrylates, and do not include butadiene. Examples of monomers having two (meth)acrylic groups include ethylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, butane diol di(meth)acrylate, hexane diol di(meth)acrylate, cyclohexane dimethanol di(meth)acrylate, and polyethylene glycol di(meth)acrylates. Examples of the polyethylene glycol di(meth)acrylates include triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, and polyethylene glycol (600) di(meth)acrylate. Examples of monomers having three (meth)acrylic groups include alkoxylated trimethylolpropane tri(meth)acrylates, glycerol propoxy tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate. Examples of the alkoxylated trimethylolpropane tri(meth)acrylates include trimethylolpropane tri(meth)acrylate and trimethylolpropane triethoxy tri(meth)acrylate. Further, examples of monomers having four (meth)acrylic groups include pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, etc. Further, examples of monomers having five (meth)acrylic groups include dipentaerythritol penta(meth)acrylate, etc. Further, examples of monomers having six (meth)acrylic groups include ditrimethylolpropane hexa(meth)acrylate, etc.Polyfunctional monomers also include diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, divinylbenzene, and the like.

[0040] In this specification, monomers containing (1) one or more hydrolyzable silyl groups and (2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule, such as monomer M1, monomer M2, and monomer M3, are not included in the term "polyfunctional monomer."

[0041] (Volume average particle size of polyorganosiloxane) The volume average particle diameter of the polyorganosiloxane is preferably 0.03 μm to 50.00 μm, more preferably 0.05 μm to 10.00 μm, more preferably 0.08 μm to 2.00 μm, even more preferably 0.10 μm to 1.00 μm, even more preferably 0.10 μm to 0.80 μm, and particularly preferably 0.10 μm to 0.50 μm. When the volume average particle diameter of the polyorganosiloxane is (a) 0.03 μm or more, polyorganosiloxane having a desired volume average particle diameter can be stably obtained, and when it is (b) 50.00 μm or less, the obtained water-based paint has excellent film-forming properties. The volume average particle diameter of the polyorganosiloxane can be measured using a dynamic light scattering particle size distribution measuring device or the like using an aqueous latex containing polyorganosiloxane as a sample. The method for measuring the volume average particle size of the polyorganosiloxane will be described in detail in the following Examples.

[0042] (2-1-2. Core part) The graft copolymer (A) includes a polyorganosiloxane and a graft portion grafted to the polyorganosiloxane. In the graft copolymer (A), the graft portion can cover at least a part of the polyorganosiloxane, or can cover the entire polyorganosiloxane. At least a part of the graft portion is preferably present on the outermost side of the graft copolymer (A). Therefore, the polyorganosiloxane can be said to be the core portion of the graft copolymer (A). In other words, the graft copolymer (A) includes a core portion including a polyorganosiloxane and a graft portion grafted to the core portion.

[0043] The core part may be composed of only one type of polyorganosiloxane having the same composition of the structural units (type and content ratio), or may be composed of two or more types of polyorganosiloxane having different compositions of the structural units (type and content ratio). In addition to one or more types of polyorganosiloxane, the core part may contain one or more types of other rubber.

[0044] Examples of other rubbers include (a) natural rubber, (b) diene rubbers containing 50% by weight or more of structural units derived from diene monomers in 100% by weight of rubber, and (c) (meth)acrylate rubbers containing 50% by weight or more of structural units derived from (meth)acrylate monomers in 100% by weight of rubber, etc. In this specification, (meth)acrylate means acrylate and / or methacrylate.

[0045] The core part preferably contains 55 parts by weight to 100 parts by weight of polyorganosiloxane in 100 parts by weight of the core part, more preferably contains 60 parts by weight to 100 parts by weight, more preferably contains more than 60 parts by weight and less than 100 parts by weight, more preferably contains 62 parts by weight to 100 parts by weight, more preferably contains 65 parts by weight to 100 parts by weight, more preferably contains 70 parts by weight to 100 parts by weight, more preferably contains 75 parts by weight to 100 parts by weight, more preferably contains 80 parts by weight to 100 parts by weight, more preferably contains 85 parts by weight to 100 parts by weight, even more preferably contains 90 parts by weight to 100 parts by weight, and particularly preferably contains 95 parts by weight to 100 parts by weight. According to this configuration, the water-based paint has the advantage of being able to provide a smaller loss tangent (tan δ) at seawater temperature. The core part may contain 100 parts by weight of polyorganosiloxane per 100 parts by weight of the core part, that is, the core part may be composed only of polyorganosiloxane.

[0046] (Volume average particle size of core part) The volume average particle diameter of the core part is preferably 0.03 μm to 50.00 μm, more preferably 0.05 μm to 10.00 μm, more preferably 0.08 μm to 2.00 μm, even more preferably 0.10 μm to 1.00 μm, even more preferably 0.10 μm to 0.80 μm, and particularly preferably 0.10 μm to 0.50 μm. When the volume average particle diameter of the core part is (a) 0.03 μm or more, the core part having the desired volume average particle diameter can be stably obtained, and when it is (b) 50.00 μm or less, the obtained water-based paint has excellent film-forming properties. The volume average particle diameter of the core part can be measured by the same method as the volume average particle diameter of polyorganosiloxane using a dynamic light scattering type particle size distribution measuring device or the like, using the aqueous latex containing the core part as a sample.

[0047] (2-1-3. Graft part) The graft portion is (i) grafted to the polyorganosiloxane, and (ii) includes a first graft portion and a second graft portion. At least a part of the graft portion may be grafted to the polyorganosiloxane, and not all of the graft portion may be grafted to the polyorganosiloxane.

[0048] In the graft copolymer (A), (a) a first graft portion may be formed on the outside of the polyorganosiloxane, and a second graft portion may be formed on the outside of the first graft portion, or (b) a second graft portion may be formed on the outside of the polyorganosiloxane, and the first graft portion may be formed on the outside of the second graft portion.

[0049] In this specification, "a first graft portion is formed on the outside of the polyorganosiloxane" means that the first graft portion is formed after the formation of the polyorganosiloxane. In this specification, "a second graft portion is formed on the outside of the first graft portion" means that the second graft portion is formed after the formation of the first graft portion.

[0050] In the graft copolymer (A), the first graft portion is formed on the outside of the polyorganosiloxane, and the second graft portion is formed on the outside of the first graft portion (hereinafter also referred to as "Case C"). In Case C, the first graft portion may cover at least a part of the polyorganosiloxane, or may cover the entire polyorganosiloxane. In other words, in Case C, at least a part of the first graft portion may be present on the outside of the polyorganosiloxane. In Case C, the entire first graft portion may be present on the outside of the polyorganosiloxane. In Case C, the second graft portion may cover at least a part of the first graft portion, or may cover the entire first graft portion. In other words, in Case C, at least a part of the second graft portion may be present on the outside of the first graft portion. In Case C, the entire second graft portion may be present on the outside of the first graft portion. In case C, at least a portion of the first graft portion may be grafted to the polyorganosiloxane.

[0051] In this specification, "the second graft portion is formed on the outside of the polyorganosiloxane" means that the second graft portion is formed after the formation of the polyorganosiloxane. In this specification, "the first graft portion is formed on the outside of the second graft portion" means that the first graft portion is formed after the formation of the second graft portion.

[0052] In the graft copolymer (A), the second graft portion is formed on the outside of the polyorganosiloxane, and the first graft portion is formed on the outside of the second graft portion (hereinafter also referred to as "Case D"). In Case D, the second graft portion may cover at least a part of the polyorganosiloxane, or may cover the entire polyorganosiloxane. In other words, in Case D, at least a part of the second graft portion may be present on the outside of the polyorganosiloxane. In Case D, the entire second graft portion may be present on the outside of the polyorganosiloxane. In Case D, the first graft portion may cover at least a part of the second graft portion, or may cover the entire second graft portion. In other words, in Case D, at least a part of the first graft portion may be present on the outside of the second graft portion. In Case D, the entire first graft portion may be present on the outside of the second graft portion. In case D, at least a portion of the second graft portion may be grafted to the polyorganosiloxane.

[0053] Since water-based paints have the advantage of being superior in film-forming properties and capable of providing coating films with smaller loss tangents (tan δ) at seawater temperatures, it is preferred that in the graft copolymer (A), a first graft portion is formed on the outside of the (a) polyorganosiloxane, and a second graft portion is formed on the outside of the first graft portion.

[0054] The number of the first graft portion and the second graft portion included in the graft portion is not particularly limited. For example, the first graft portion may be formed on the outside of the polyorganosiloxane, the second graft portion may be formed on the outside of the first graft portion, and the first graft portion may be further formed on the outside of the second graft portion.

[0055] The graft portion may include a graft portion other than the first graft portion and the second graft portion. The "graft portion other than the first graft portion and the second graft portion" may be referred to as the "other graft portion." When the graft portion includes the other graft portion, it is preferable that the other graft portion is formed outside the first graft portion, and the second graft portion is formed outside the other graft portion. In other words, it is preferable that the graft portion formed after the formation of the core portion is the first graft portion, and it is preferable that the graft portion formed last is the second graft portion.

[0056] (First graft part) The first graft portion contains (a) a structural unit U2 derived from a monomer containing (a-1) one or more hydrolyzable silyl groups and (a-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule, and does not contain (b) a structural unit derived from a chain transfer agent.

[0057] In the graft copolymer (A), the first graft portion preferably covers at least a part of the polyorganosiloxane or covers the entire polyorganosiloxane, in other words, the first graft portion is preferably graft-bonded to the polyorganosiloxane.

[0058] (Unit U2) When preparing the first graft portion, a monomer M2 containing (a) one or more hydrolyzable silyl groups and (b) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule is used as a raw material, whereby the first graft portion containing the structural unit U2 can be obtained.

[0059] The first graft portion contains the structural unit U2, which has the advantage that the occurrence of blisters when a coating film obtained from a water-based paint is immersed in water is reduced or eliminated.

[0060] The "structural unit derived from a monomer containing (1) one or more hydrolyzable silyl groups in the molecule and (2) one or more ethylenically unsaturated groups and / or mercapto groups" contained in the polyorganosiloxane and the "structural unit derived from a monomer containing (1) one or more hydrolyzable silyl groups in the molecule and (2) one or more ethylenically unsaturated groups and / or mercapto groups" contained in the first graft portion may be the same or different. In order to clarify this, for convenience, in this specification, the "structural unit derived from a monomer containing (1) one or more hydrolyzable silyl groups in the molecule and (2) one or more ethylenically unsaturated groups and / or mercapto groups" contained in the polyorganosiloxane and the first graft portion are referred to as "structural unit U1" and "structural unit U2", respectively.

[0061] The hydrolyzable silyl group contained in the monomer M2, the ethylenically unsaturated group contained in the monomer M2, and specific examples of the monomer M2 are the same as those explained above in the section (structural unit U2), and therefore the explanation is hereby incorporated by reference and will not be repeated here.

[0062] The hydrolyzable silyl group contained in the monomer M2 is not particularly limited. The hydrolyzable silyl group of the monomer M2 is preferably an alkoxysilyl group, because (a) it is highly crosslinkable (vinyl polymerization reactive), (b) it is easy to handle, (c) it is inexpensive, and (d) it reduces or eliminates the occurrence of blisters when a coating film obtained from a water-based paint is immersed in water. When the monomer M2 contains two or more hydrolyzable silyl groups in the molecule, the multiple hydrolyzable silyl groups may be the same or different from each other.

[0063] The ethylenically unsaturated group of the monomer M2 is preferably one or more selected from the group consisting of an acryloyl group and a methacryloyl group, because (a) it is highly crosslinkable (vinyl polymerization reactive), (b) it is easy to handle, (c) it is inexpensive, (d) the water-based paint can provide a coating film with a lower loss tangent (tan δ), and (e) when the coating film obtained from the water-based paint is immersed in water, the occurrence of blisters is reduced or eliminated. When the monomer M2 contains two or more ethylenically unsaturated groups in the molecule, the multiple ethylenically unsaturated groups may be the same or different from each other. The term "at the time of forming the first graft portion" can also be said to be "at the time of polymerization of the monomer mixture for forming the first graft portion".

[0064] The monomer M2 is not particularly limited. The monomer M2 is preferably a (meth)acryloyloxyalkylsilane, and more preferably a (meth)acryloyloxyalkylsilane, such as β-methacryloyloxyethyldimethoxymethylsilane, 3-(meth)acryloyloxypropyltrimethoxysilane, 3-(meth)acryloyloxypropyldimethoxymethyl ... More preferred is one or more selected from the group consisting of ethylsilane, 3-(meth)acryloyloxypropyl methoxydimethylsilane, 3-(meth)acryloyloxypropyl triethoxysilane, 3-(meth)acryloyloxypropyl diethoxymethylsilane, 3-(meth)acryloyloxypropyl diethoxyethylsilane, 3-(meth)acryloyloxypropyl ethoxydimethylsilane, 3-(meth)acryloyloxypropyl ethoxydiethylsilane, and δ-(meth)acryloyloxybutyl diethoxymethylsilane.

[0065] The first graft portion preferably contains 1.0 wt % to 80.0 wt %, more preferably 1.0 wt % to 75.0 wt %, more preferably 1.0 wt % to 70.0 wt %, more preferably 1.0 wt % to 65.0 wt %, more preferably 1.0 wt % to 60.0 wt %, more preferably 1.0 wt % to 55.0 wt %, more preferably 1.0 wt % to 50.0 wt %, and more preferably 1.0 wt % to 45.0 wt % of the structural unit U2, based on 100 wt % of the first graft portion. Preferably, the water-based paint contains 1.0% by weight to 40.0% by weight, more preferably 2.0% by weight to 38.0% by weight, more preferably 3.0% by weight to 35.0% by weight, more preferably 4.0% by weight to 33.0% by weight, more preferably 5.0% by weight to 30.0% by weight, more preferably 5.5% by weight to 28.0% by weight, more preferably 6.0% by weight to 25.0% by weight, even more preferably 6.5% by weight to 23.0% by weight, and particularly preferably 7.0% by weight to 20.0% by weight. This configuration has the advantages that (a) the water-based paint can provide a coating film with a lower loss tangent (tan δ), and (b) the generation of blisters when the coating film obtained from the water-based paint is immersed in water is further reduced or eliminated.

[0066] The graft portion preferably contains 0.5 wt% to 80.0 wt%, more preferably 1.0 wt% to 75.0 wt%, more preferably 1.2 wt% to 70.0 wt%, more preferably 1.5 wt% to 65.0 wt%, more preferably 1.7 wt% to 60.0 wt%, more preferably 2.0 wt% to 55.0 wt%, more preferably 2.2 wt% to 50.0 wt%, and more preferably 2.5 wt% to 45.0 wt%, of the structural unit U2, based on 100 wt% of the graft portion; It is more preferable that the composition contains 2.7% by weight to 40.0% by weight, more preferably 3.0% by weight to 38.0% by weight, more preferably 3.5% by weight to 35.0% by weight, more preferably 4.0% by weight to 33.0% by weight, more preferably 5.0% by weight to 30.0% by weight, more preferably 5.5% by weight to 28.0% by weight, more preferably 6.0% by weight to 25.0% by weight, even more preferably 6.5% by weight to 23.0% by weight, and particularly preferably 7.0% by weight to 20.0% by weight. This configuration has the advantages that (a) the water-based paint can provide a coating film with a lower loss tangent (tan δ), and (b) the generation of blisters when the coating film obtained from the water-based paint is immersed in water is further reduced or eliminated.

[0067] The first graft portion does not contain a structural unit derived from a chain transfer agent. In this specification, "the first graft portion does not contain a structural unit derived from a chain transfer agent" means that the content of the structural unit derived from the chain transfer agent in the first graft portion is 0.01% by weight or less in 100% by weight of the first graft portion. Since the first graft portion does not contain a structural unit derived from a chain transfer agent, the polymer has the same structure as the first graft portion (i.e., a polymer containing the structural unit U2), and the amount of polymer that is not grafted to any polymer (e.g., polyorganosiloxane) is zero or very small. As a result, it has the advantage of excellent film-forming properties.

[0068] The first graft portion may contain a structural unit other than the structural unit U2. The structural unit other than the structural unit U2 is not particularly limited. The first graft portion preferably contains, as a structural unit other than the structural unit U2, a structural unit derived from one or more monomers selected from the group consisting of an aromatic vinyl monomer, a vinyl cyan monomer, and a (meth)acrylate monomer. According to this configuration, the first graft portion can have the function of solidifying the substantially non-crosslinked polyorganosiloxane. Therefore, according to this configuration, the obtained water-based paint has excellent film-forming properties, and the coating film of the water-based paint has excellent strength.

[0069] Specific examples of aromatic vinyl monomers include styrene, α-methylstyrene, p-methylstyrene, and divinylbenzene.

[0070] Specific examples of vinyl cyanide monomers include acrylonitrile and methacrylonitrile.

[0071] Specific examples of the (meth)acrylate monomer include: (a) alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; (b) aromatic ring-containing (meth)acrylates such as phenoxyethyl (meth)acrylate and benzyl (meth)acrylate; (c) 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate; (d) glycidyl (meth)acrylates such as glycidyl (meth)acrylate and glycidyl alkyl (meth)acrylate; (e) alkoxyalkyl (meth)acrylates; (f) allyl alkyl (meth)acrylates such as allyl (meth)acrylate and allyl alkyl (meth)acrylate; (g) polyfunctional (meth)acrylates such as monoethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, etc.

[0072] From the viewpoint of reactivity during the formation of the first graft portion, the (meth)acrylate monomer is preferably at least one selected from the group consisting of methyl acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate. In addition, by mixing at least one selected from the group consisting of methyl acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate, which have a relatively low glass transition temperature of the homopolymer, with methyl methacrylate, which have a relatively high glass transition temperature of the homopolymer, to prepare a monomer mixture for forming the first graft portion, the glass transition temperature of the resulting first graft portion can be adjusted to a desired temperature.

[0073] The first graft portion may contain only one type of structural unit derived from one or more monomers selected from the group consisting of aromatic vinyl monomers, vinyl cyan monomers, and (meth)acrylate monomers, or may contain a combination of two or more types of structural units.

[0074] The first graft portion preferably contains 60% by weight to 99% by weight of the constituent units derived from the aromatic vinyl monomer, the constituent units derived from the vinyl cyan monomer, and the constituent units derived from the (meth)acrylate monomer in total, more preferably 62% by weight to 98% by weight, even more preferably 65% ​​by weight to 97% by weight, particularly preferably 68% by weight to 96% by weight, and most preferably 70% by weight to 95% by weight, in 100% by weight of the first graft portion. This configuration has the advantage that the resulting water-based paint has excellent film-forming properties.

[0075] From the viewpoint of achieving both the film-forming properties of the water-based paint and the reactivity during the formation of the first graft portion, it is preferable that the first graft portion contains a structural unit derived from a (meth)acrylate monomer, and it is more preferable that the first graft portion contains a structural unit derived from methyl methacrylate and a structural unit derived from butyl methacrylate.

[0076] The first graft portion preferably contains 60% to 99% by weight of structural units derived from a (meth)acrylate monomer, more preferably 62% to 98% by weight, even more preferably 65% ​​to 97% by weight, particularly preferably 68% to 96% by weight, and most preferably 70% to 95% by weight, based on 100% by weight of the first graft portion. This configuration has the advantage of excellent reactivity during the formation of the first graft portion.

[0077] The first graft portion preferably contains 60% by weight to 99% by weight of structural units derived from methyl methacrylate and structural units derived from butyl methacrylate in total, more preferably 62% by weight to 98% by weight, even more preferably 65% ​​by weight to 97% by weight, particularly preferably 68% by weight to 96% by weight, and most preferably 70% by weight to 95% by weight, based on 100% by weight of the first graft portion. This configuration has the advantage of being more excellent in reactivity when forming the first graft portion.

[0078] (Second graft part) The second graft portion (a) contains a structural unit derived from a chain transfer agent, and does not contain (b) a structural unit U3 derived from a monomer containing (b-1) one or more hydrolyzable silyl groups and (b-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule.

[0079] (Structural unit derived from chain transfer agent) The use of a chain transfer agent as a raw material in the preparation of the second graft portion has the advantage of being able to provide a water-based paint with superior film-forming properties. When a chain transfer agent is used as a raw material in the preparation of the second graft portion, the result is a second graft portion containing a structural unit derived from the chain transfer agent.

[0080] The chain transfer agent is not particularly limited, and known chain transfer agents such as t-dodecyl mercaptan, n-dodecyl mercaptan, normal octyl mercaptan, and 2-ethylhexyl thioglycolate can be used.

[0081] The second graft portion preferably contains 0.01% by weight to 5.0% by weight of structural units derived from a chain transfer agent, more preferably 0.05% by weight to 3.0% by weight, even more preferably 0.10% by weight to 2.0% by weight, even more preferably 0.15% by weight to 1.0% by weight, and particularly preferably 0.18% by weight to 0.80% by weight, based on 100% by weight of the second graft portion. This configuration has the advantage of being able to provide a water-based paint with excellent film-forming properties.

[0082] The second graft portion does not include a structural unit derived from a monomer containing (1) one or more hydrolyzable silyl groups in the molecule and (2) one or more ethylenically unsaturated groups and / or mercapto groups. The second graft portion does not include not only the same type of structural unit as the structural unit U1 contained in the polyorganosiloxane and the structural unit U2 contained in the first graft portion, but also all of the "structural units derived from a monomer containing (1) one or more hydrolyzable silyl groups in the molecule and (2) one or more ethylenically unsaturated groups and / or mercapto groups". In order to clarify this, in this specification, the "structural unit derived from a monomer containing (1) one or more hydrolyzable silyl groups in the molecule and (2) one or more ethylenically unsaturated groups and / or mercapto groups" that is not included in the second graft portion is conveniently referred to as the "structural unit U3". Since the second graft portion does not include the structural unit U3, it has the advantage of excellent film-forming properties.

[0083] The second graft part may contain a structural unit other than the structural unit derived from the chain transfer agent. The structural unit other than the structural unit derived from the chain transfer agent is not particularly limited. The second graft part preferably contains, as a structural unit other than the structural unit derived from the chain transfer agent, a structural unit derived from one or more monomers selected from the group consisting of an aromatic vinyl monomer, a vinyl cyan monomer, and a (meth)acrylate monomer. According to this configuration, the second graft part can have the function of solidifying (i) the substantially non-crosslinked polyorganosiloxane and / or (ii) the first graft part. Therefore, according to this configuration, the obtained water-based paint has the advantage of excellent film-forming properties and the coating film of the water-based paint has excellent strength.

[0084] Specific examples of the aromatic vinyl monomer, the vinyl cyan monomer and the (meth)acrylate monomer are the same as those described in the section (First graft portion) above, and therefore the description therein is incorporated by reference and will not be described here.

[0085] From the viewpoint of reactivity during the formation of the second graft portion, the (meth)acrylate monomer is preferably at least one selected from the group consisting of methyl acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate. In addition, by mixing at least one selected from the group consisting of methyl acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate, which have a relatively low glass transition temperature of the homopolymer, with methyl methacrylate, which have a relatively high glass transition temperature of the homopolymer, to prepare a monomer mixture for forming the second graft portion, the glass transition temperature of the resulting second graft portion can be adjusted to a desired temperature.

[0086] The second graft portion may contain only one type of structural unit derived from one or more monomers selected from the group consisting of aromatic vinyl monomers, vinyl cyan monomers, and (meth)acrylate monomers, or may contain a combination of two or more types of structural units.

[0087] The second graft portion preferably contains 95.00% by weight to 99.99% by weight of the constituent units derived from aromatic vinyl monomers, the constituent units derived from vinyl cyan monomers, and the constituent units derived from (meth)acrylate monomers in total, more preferably 97.00% by weight to 99.95% by weight, even more preferably 98.00% by weight to 99.90% by weight, particularly preferably 99.00% by weight to 99.85% by weight, and most preferably 99.20% by weight to 99.82% by weight, in 100% by weight of the second graft portion. This configuration has the advantage that the resulting water-based paint has excellent film-forming properties.

[0088] From the viewpoint of achieving both the film-forming properties of the water-based paint and the reactivity during the formation of the second graft portion, it is preferable that the second graft portion contains a structural unit derived from a (meth)acrylate monomer, and it is more preferable that the second graft portion contains a structural unit derived from methyl methacrylate and a structural unit derived from butyl methacrylate.

[0089] The second graft portion preferably contains 95.00 wt% to 99.99 wt% of constitutional units derived from a (meth)acrylate monomer, more preferably 97.00 wt% to 99.95 wt%, even more preferably 98.00 wt% to 99.90 wt%, particularly preferably 99.00 wt% to 99.85 wt%, and most preferably 99.20 wt% to 99.82 wt%, based on 100 wt% of the second graft portion. This configuration has the advantage of excellent reactivity during the formation of the second graft portion.

[0090] The second graft portion preferably contains 95.00% by weight to 99.99% by weight of structural units derived from methyl methacrylate and structural units derived from butyl methacrylate in total, more preferably 97.00% by weight to 99.95% by weight, even more preferably 98.00% by weight to 99.90% by weight, particularly preferably 99.00% by weight to 99.85% by weight, and most preferably 99.20% by weight to 99.82% by weight, based on 100% by weight of the second graft portion. This configuration has the advantage of being more excellent in reactivity when forming the second graft portion.

[0091] The graft portion preferably contains the first graft portion and the second graft portion in a total amount of 60% by weight or more, more preferably 65% ​​by weight or more, more preferably 70% by weight or more, more preferably 75% by weight or more, more preferably 80% by weight or more, more preferably 85% by weight or more, even more preferably 90% by weight or more, particularly preferably 95% by weight or more, and most preferably 100% by weight. In other words, the graft portion is most preferably composed of only the first graft portion and the second graft portion. When the content of the first graft portion and the second graft portion in the graft portion is within the above-mentioned range, the graft portion has the advantage of excellent film-forming properties and reduced or no occurrence of blisters when the coating film is immersed in water.

[0092] In the graft portion, the content ratio of the first graft portion to the second graft portion is not particularly limited, but for example, with respect to the total of the first graft portion and the second graft portion being 100% by weight, (i) the first graft portion is preferably 10% by weight to 90% by weight and the second graft portion is preferably 10% by weight to 90% by weight, (ii) the first graft portion is more preferably 15% by weight to 85% by weight and the second graft portion is more preferably 15% by weight to 85% by weight, (iii) the first graft portion is more preferably 20% by weight to 80% by weight and the second graft portion is more preferably 20% by weight to 80% by weight, and (iv) the first graft portion is more preferably 25% by weight to 75% by weight and the second graft portion is particularly preferably 25% by weight to 75% by weight. When the content ratio of the first graft portion to the second graft portion in the graft portion is within the above-mentioned range, there is an advantage that a coating film having excellent film formability and a small loss tangent (tan δ) at seawater temperature can be obtained.

[0093] (Structural unit derived from reactive emulsifier) It is preferable that the graft portion further contains a constitutional unit derived from a reactive emulsifier. This constitution has the advantage that the generation of scale during the production of the water-based paint is reduced or eliminated.

[0094] The structural unit derived from the reactive emulsifier may be (i) contained in the first graft portion and not contained in the second graft portion, (ii) not contained in the first graft portion and contained in the second graft portion, or (iii) contained in both the first graft portion and the second graft portion.

[0095] In this specification, the term "reactive emulsifier" refers to an emulsifier having an ethylenically unsaturated double bond. The term "reactive" in the reactive emulsifier refers to the ability to have a polymerizable radical in the presence of a polymerization initiator. Therefore, the "reactive emulsifier" can also be called a "polymerizable emulsifier." The "reactive emulsifier" is sometimes called a "reactive surfactant."

[0096] The type of reactive emulsifier is not particularly limited as long as it has an ethylenically unsaturated double bond. The reactive emulsifier may be a nonionic reactive emulsifier, an anionic reactive emulsifier, or a nonionic reactive emulsifier. As the reactive emulsifier, for example, an anionic reactive emulsifier is preferable because it is easy to control the particle size of the graft copolymer (A) to be fine (specifically, the volume average particle size of the graft copolymer (A) is 30 nm to 200 nm).

[0097] The ethylenically unsaturated double bond of the reactive emulsifier is derived from a group having an ethylenically unsaturated double bond. In other words, the reactive emulsifier has a group having an ethylenically unsaturated double bond. Specific examples of the group having an ethylenically unsaturated double bond include an oxyalkylene group, a (meth)acryloyl group, a vinyl group, an allyl group, an isopropenyl group, a 1-propenyl group, an allyloxy group, and a styryl group.

[0098] The reactive emulsifier preferably has an oxyalkylene group. The reactive emulsifier having an oxyalkylene group has excellent copolymerizability with a monomer. The oxyalkylene group includes an oxyalkylene group having an alkylene group having 2 to 4 carbon atoms, such as an oxyethylene group, an oxypropylene group, and an oxybutylene group. Among these, the oxyalkylene group is preferably an oxyethylene group. The oxyethylene group is more hydrophilic than, for example, an oxypropylene group and an oxybutylene group. Therefore, when the graft portion of the graft copolymer (A) contains a structural unit derived from a reactive emulsifier having an oxyethylene group, a high-density hydration layer can be formed on the surface of the particles of the graft copolymer (A), and as a result, the dispersibility of the particles of the graft copolymer (A) in an aqueous medium tends to be further increased.

[0099] The average number of moles of oxyethylene groups added per mole of reactive emulsifier is not particularly limited, but is preferably 5 moles or more and 40 moles or less, more preferably 10 moles or more and 30 moles or less. According to this constitution, copolymerization with monomers tends to be excellent. In addition, when the average number of moles of oxyethylene groups added is 5 moles or more, the dispersibility of particles of graft copolymer (A) in aqueous medium tends to be improved.

[0100] The above-mentioned reactive emulsifiers may be used alone or in combination of two or more.

[0101] The graft portion preferably contains 0.1% by weight to 20.0% by weight of the constitutional unit derived from the reactive emulsifier, more preferably 0.1% by weight to 15.0% by weight, more preferably 1.0% by weight to 15.0% by weight, more preferably 1.0% by weight to 10.0% by weight, even more preferably 1.0% by weight to 8.0% by weight, even more preferably 1.0% by weight to 5.0% by weight, and particularly preferably 1.0% by weight to 4.0% by weight. This constitution has the advantage that the generation of scale during the production of the water-based paint is further reduced or eliminated.

[0102] When both the first graft portion and the second graft portion contain structural units derived from a reactive emulsifier, the amount of structural units derived from a reactive emulsifier in the graft portion is intended to be the total amount of the structural units derived from a reactive emulsifier in the first graft portion and the amount of structural units derived from a reactive emulsifier in the second graft portion.

[0103] The graft portion may further contain a constituent unit derived from a monomer having a reactive group (hereinafter also referred to as a reactive group-containing monomer). The reactive group-containing monomer is preferably a monomer containing one or more reactive groups selected from the group consisting of an epoxy group, an oxetane group, a hydroxyl group, an amino group, an imide group, a carboxylic acid group, a carboxylic anhydride group, a cyclic ester, a cyclic amide, a benzoxazine group, and a cyanate ester group, and more preferably a monomer containing one or more reactive groups selected from the group consisting of an epoxy group, a hydroxyl group, and a carboxylic acid group. This configuration has the advantage of improving the adhesion of the coating film of the water-based paint to the substrate.

[0104] The structural unit derived from the reactive group-containing monomer may be (i) contained in the first graft portion and not contained in the second graft portion, (ii) not contained in the first graft portion and contained in the second graft portion, or (iii) contained in both the first graft portion and the second graft portion.

[0105] Specific examples of monomers having an epoxy group include glycidyl group-containing vinyl monomers such as glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, and allyl glycidyl ether.

[0106] Specific examples of monomers having a hydroxyl group include, for example, (a) hydroxy linear alkyl (meth)acrylates (particularly, hydroxy linear C1-6 alkyl (meth)acrylates) such as 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; (b) caprolactone-modified hydroxy (meth)acrylates; (c) hydroxy branched alkyl (meth)acrylates such as α-(hydroxymethyl)methyl acrylate and α-(hydroxymethyl)ethyl acrylate; and (d) hydroxyl group-containing (meth)acrylates such as mono(meth)acrylates of polyester diols (particularly saturated polyester diols) obtained from divalent carboxylic acids (such as phthalic acid) and dihydric alcohols (such as propylene glycol).

[0107] Specific examples of the monomer having a carboxylic acid group include monocarboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid, and dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid. As the monomer having a carboxylic acid group, the above-mentioned monocarboxylic acids are preferably used.

[0108] The reactive group-containing monomers described above may be used alone or in combination of two or more.

[0109] The graft portion preferably contains 0.5% by weight to 90% by weight of the structural unit derived from the reactive group-containing monomer, more preferably 1% by weight to 50% by weight, even more preferably 2% by weight to 35% by weight, and particularly preferably 3% by weight to 20% by weight, based on 100% by weight of the graft portion. When the graft portion contains (a) 0.5% by weight or more of the structural unit derived from the reactive group-containing monomer, the resulting water-based paint can provide a coating film having sufficient adhesion to the substrate, and when (b) 90% by weight or less, the resulting water-based paint can provide a coating film having sufficient adhesion to the substrate, and has the advantage of having good storage stability of the water-based paint.

[0110] The structural unit derived from the reactive group-containing monomer is preferably contained in the graft portion, and more preferably contained only in the graft portion.

[0111] When both the first graft portion and the second graft portion contain structural units derived from reactive group-containing monomers, the amount of structural units derived from reactive group-containing monomers in the graft portions is intended to mean the total amount of structural units derived from reactive group-containing monomers in the first graft portion and the amount of structural units derived from reactive group-containing monomers in the second graft portion.

[0112] (Cross-linked structure of graft portion) By using a multifunctional monomer when preparing the first graft portion, a crosslinked structure can be introduced into the first graft portion. Also, by using a multifunctional monomer when preparing the second graft portion, a crosslinked structure can be introduced into the second graft portion. In one embodiment of the present invention, the graft portion is preferably non-crosslinked. Here, "the graft portion is non-crosslinked" means that the first graft portion, the second graft portion, and all of the other graft portions optionally included are non-crosslinked. Moreover, "the graft portion is non-crosslinked" means that (i) the amount of the polyfunctional monomer used in preparing the first graft portion is 0.50% by weight or less in 100% by weight of the monomer mixture for forming the first graft portion, (ii) the amount of the polyfunctional monomer used in preparing the second graft portion is 0.50% by weight or less in 100% by weight of the monomer mixture for forming the second graft portion, and further (iii) the amount of the polyfunctional monomer used in preparing the other graft portion, which is optionally included, is 0.50% by weight or less in 100% by weight of the monomer mixture for forming the other graft portion. In other words, in one embodiment of the present invention, it is preferable that the graft portion is substantially non-crosslinked, and it is preferable that the amount of the polyfunctional monomer used in preparing the graft portion is 0.50% by weight or less in 100% by weight of the monomer mixture for forming the graft portion. The amount of the polyfunctional monomer used in preparing the first graft portion is preferably 0.50% by weight or less, more preferably 0.20% by weight or less, even more preferably 0.10% by weight or less, and particularly preferably 0.01% by weight or less, based on 100% by weight of the monomer mixture for forming the first graft portion. The amount of the polyfunctional monomer used in preparing the second graft portion is preferably 0.50% by weight or less, more preferably 0.20% by weight or less, even more preferably 0.10% by weight or less, and particularly preferably 0.01% by weight or less, based on 100% by weight of the monomer mixture for forming the second graft portion.

[0113] The first graft portion and the second graft portion may each be composed of only one type of polymer having the same composition (type and content ratio) of the structural units, or may be composed of two or more types of polymers having different compositions (type and content ratio) of the structural units.

[0114] The core part containing polyorganosiloxane and the graft part may have a layer structure. More specifically, the core part containing polyorganosiloxane, the first graft part, and the second graft part may have a layer structure. For example, an embodiment in which the core part containing polyorganosiloxane is the innermost layer (also referred to as the core layer), and a layer of the graft part exists on the outside of the core part as the outermost layer (also referred to as the shell layer) is also one aspect of the present invention. Specifically, in the above-mentioned case C, an embodiment in which the core part containing polyorganosiloxane is the innermost layer (also referred to as the core layer), a layer of the first graft part exists on the outside of the core part, and a layer of the second graft part exists on the outside of the first graft part as the outermost layer is also one aspect of the present invention. In addition, in the above-mentioned case D, the core part containing polyorganosiloxane is the innermost layer (also referred to as the core layer), a layer of the second graft part is present outside the core part, and a layer of the first graft part is present as the outermost layer outside the second graft part, which is also an embodiment of the present invention. A structure in which the core part containing polyorganosiloxane is the core layer and the graft part is the shell layer can be called a core-shell structure. However, as long as the graft part is graft-bonded to the polyorganosiloxane, the graft copolymer (A) is not limited to the above structure.

[0115] (Graft ratio of grafted part) In the preparation of the graft portion in the production of the graft copolymer (A), when a monomer mixture capable of forming the graft portion (monomer mixture for forming the graft portion) is polymerized in the presence of polyorganosiloxane, a polymer having the same structure as the graft portion and not grafted to the polyorganosiloxane may be generated. For example, in the case E described below, when a monomer mixture capable of forming the first graft portion (monomer mixture for forming the first graft portion) is polymerized in the presence of polyorganosiloxane in the preparation of the first graft portion, a polymer having the same structure as the first graft portion and not grafted to the polyorganosiloxane (hereinafter, sometimes referred to as "polymer F1") may be generated. In addition, in case E, when a monomer mixture capable of forming the second graft portion (monomer mixture for forming the second graft portion) is polymerized after the formation of the first graft portion in the preparation of the second graft portion, a polymer having the same structure as the second graft portion and not grafted to either the first graft portion or the polyorganosiloxane (hereinafter, sometimes referred to as "polymer F2") may be generated. Alternatively, in case F described later, when a monomer mixture capable of forming the second graft portion (monomer mixture for forming the second graft portion) is polymerized in the presence of polyorganosiloxane in the preparation of the second graft portion, a polymer having the same structure as the second graft portion and not grafted to the polyorganosiloxane (hereinafter, sometimes referred to as "polymer F3") may be generated. In addition, in case F, when a monomer mixture capable of constituting the first graft portion (monomer mixture for forming the first graft portion) is polymerized after the formation of the second graft portion in the preparation of the first graft portion, a polymer having the same structure as the first graft portion and which is not graft-bonded to either the second graft portion or the polyorganosiloxane (hereinafter sometimes referred to as "polymer F4") may be produced.Alternatively, when the graft portion includes the other graft portion, when a monomer mixture capable of forming the other graft portion (a monomer mixture for forming the other graft portion) is polymerized in the preparation of the other graft portion in the production of the graft copolymer (A), a polymer having the same structure as the other graft portion and not grafted to any of the polyorganosiloxane, the first graft portion, and the second graft portion (hereinafter, sometimes referred to as "polymer F5") may be generated. In this specification, the polymer F1, polymer F2, polymer F3, polymer F4, and polymer F5 are also collectively referred to as "non-graft polymers". The non-graft polymer may or may not be removed from the aqueous latex of the obtained graft copolymer (A). In other words, in one embodiment of the present invention, the water-based paint may have a non-graft polymer. The non-graft polymer contained in the water-based paint corresponds to the polymer (B) described later.

[0116] In this specification, the ratio of the polymer grafted to any other polymer among the polymers obtained in the preparation step of the graft portion is referred to as the graft ratio. The graft ratio can also be expressed as {(weight of the polymer grafted to any other polymer) / [(weight of the polymer grafted to any other polymer)+(weight of the non-grafted polymer)]}×100.

[0117] In the process of preparing the graft portion, in addition to the polymer grafted to any of the polymers and the non-grafted polymer, soluble matter also exists. The soluble matter refers to unpolymerized monomers and secondary raw materials such as initiators.

[0118] As a method for determining whether a polymer is grafted to a polymer, a non-grafted polymer, or a soluble component, for example, a method for determining based on solubility / insolubility in a solvent can be mentioned. For example, a method for determining that a polymer is grafted to a polymer when it is insoluble in MEK, a non-grafted polymer when it is soluble in MEK and insoluble in methanol, and a soluble component when it is soluble in MEK and soluble in methanol can be mentioned.

[0119] In this specification, the graft ratio is calculated as follows. First, an aqueous latex containing the graft copolymer (A) is obtained. Next, an amount of the aqueous latex corresponding to 2 g of solids in the aqueous latex is mixed with 50 ml of methyl ethyl ketone (MEK) to prepare an MEK soluble matter. Then, the obtained MEK soluble matter is separated into a component soluble in MEK (MEK soluble matter) and a component insoluble in MEK (MEK insoluble matter) by centrifugation or the like. Next, 20 ml of the MEK soluble matter is mixed with 200 ml of methanol, and an aqueous calcium chloride solution in which 0.01 g of calcium chloride is dissolved in water is added to the mixture and stirred for 1 hour. Then, the obtained mixture is separated into a methanol soluble matter and a methanol insoluble matter.

[0120] The graft ratio is calculated according to the following formula. Graft rate (%) = 100 - [(weight of methanol insoluble matter) / {(weight of methanol insoluble matter) + (weight of MEK insoluble matter)}] / (total amount of monomer mixture used in preparation of graft portion) x 10,000.

[0121] In this specification, "the total amount of the monomer mixture used to prepare the graft portion" means (i) the total amount of the monomer mixture for forming the first graft portion and the monomer mixture for forming the second graft portion when the graft portion does not contain other graft portions and is composed only of the first graft portion and the second graft portion, and (ii) the total amount of the monomer mixture for forming the first graft portion, the monomer mixture for forming the second graft portion, and the monomer mixture for forming the other graft portion when the graft portion further includes other graft portions.

[0122] In the above-mentioned method of calculating the graft ratio, (a) the MEK insoluble portion is a polymer that is graft-bonded to any other polymer, and (b) the MEK soluble portion and the methanol insoluble portion is a non-grafted polymer.

[0123] The graft ratio of the graft portion is preferably 85.0% or less, more preferably 80.0% or less, more preferably 75.0% or less, more preferably 70.0% or less, more preferably 65.0% or less, more preferably 60.0% or less, more preferably 55.0% or less, more preferably 50.0% or less, more preferably 45.0% or less, more preferably 40.0% or less, even more preferably 35.0% or less, and particularly preferably 30.0% or less. When the graft ratio is 85.0% or less, the water-based paint has the advantage of excellent film-forming properties.

[0124] The graft ratio of the grafted portion is preferably 30.0% or more, more preferably 35.0% or more, more preferably 40.0% or more, more preferably 45.0% or more, more preferably 50.0% or more, more preferably 55.0% or more, more preferably 60.0% or more, more preferably 65.0% or more, more preferably 70.0% or more, more preferably 75.0% or more, even more preferably 80.0% or more, and particularly preferably 85.0% or more. When the graft ratio is 30.0% or more, there are advantages that (a) the viscosity of the water-based paint does not become too high, and (b) the generation of scale during the production of the water-based paint is reduced or eliminated.

[0125] The graft ratio of the graft portion can be appropriately adjusted by changing the amount of the monomer M1 used in preparing the polyorganosiloxane, the amount of the chain transfer agent used in preparing the second graft portion, and the like.

[0126] (Glass transition temperature of grafted part) The glass transition temperature of the graft portion is not particularly limited. The "glass transition temperature" may be referred to as "Tg" hereinafter. In this specification, the "glass transition temperature of the graft portion" refers to the glass transition temperature of the entire graft portion, including the first graft portion, the second graft portion, and any other graft portions that are optionally included.

[0127] The Tg of the graft portion is not particularly limited, but is preferably 25°C or higher, preferably 25°C to 100°C, more preferably 30°C to 90°C, even more preferably 35°C to 80°C, and particularly preferably 40°C to 70°C. This configuration has the advantage that the water-based paint has excellent film-forming properties. The present inventors have independently found that, when the upper limit of the Tg of the graft portion is 100°C or lower, the generation of scale during the production of the water-based paint is surprisingly reduced or eliminated. The present inventors have independently found that, when the lower limit of the Tg of the graft portion is 25°C or higher, (i) the coating film obtained from the water-based paint has a small loss tangent (tan δ), and as a result, the coating film is considered to have excellent antifouling properties, and (ii) the generation of blisters when the coating film obtained from the water-based paint is immersed in water is reduced or eliminated.

[0128] The Tg of the graft portion can be determined by the composition of the structural units contained in the graft portion, etc. In other words, the Tg of the resulting graft portion can be adjusted by changing the composition of the monomer mixture (e.g., the first graft portion-forming monomer mixture and the second graft portion-forming monomer mixture) used when preparing the graft portion.

[0129] The glass transition temperature Tg of the graft portion can be calculated by the following FOX formula (Formula 1).

[0130] 1 / Tg=w1 / Tg1+w2 / Tg2+···+w n / Tg n (Formula 1) Here, Tg1, Tg2, . . . , Tg nare the Tg(K) of the homopolymers of the components constituting the graft portion (i.e., the monomers used in the production of the graft portion) 1, 2, . . . , n, and w1, w2, . . . , w n are the weight fractions of the components constituting the graft portion (i.e., the monomers used in the production of the graft portion) 1, 2, ..., n, respectively. The Tg of the homopolymer of the monomer can be, for example, the value described in Polymer Handbook Fourth Edition (edited by J. Brandup et al., Jphn Wiley & Sons, Inc.).

[0131] In addition, when the amount of the reactive emulsifier, the chain transfer agent and the monomer M2 used is 20.0% by weight or less, respectively, in the total amount (100% by weight) of the monomer mixture used in the preparation of the graft portion, the glass transition temperature Tg of the graft portion is calculated by the FOX formula (Formula 1) by excluding the reactive emulsifier, the chain transfer agent and the monomer M2 from the monomers used in the preparation of the graft portion. That is, the glass transition temperature Tg of the graft portion is calculated by the FOX formula (Formula 1) by regarding the reactive emulsifier, the chain transfer agent and the monomer M2 as the monomers used in the preparation of the graft portion.

[0132] When the monomer used in the production (polymerization) of the graft portion is unknown, the Tg of the graft portion can also be obtained by performing viscoelasticity measurement using a flat plate made of the graft copolymer (A). Specifically, the Tg can be measured as follows: (1) A dynamic viscoelasticity measurement is performed under tensile conditions on a flat plate made of the graft copolymer (A) using a dynamic viscoelasticity measuring device (e.g., DVA-200, manufactured by IT Measurement & Control Co., Ltd.) to obtain a tan δ graph; (2) The peak temperature of tan δ in the obtained tan δ graph is taken as the glass transition temperature. Here, when multiple peaks are obtained in the tan δ graph, the highest peak temperature is taken as the glass transition temperature of the graft portion.

[0133] (Physical Properties of Graft Copolymer (A)) The physical properties of the graft copolymer (A) will be described below.

[0134] (Volume average particle size of graft copolymer (A)) The volume average particle diameter (Mv) of the graft copolymer (A) is preferably 0.05 μm to 60.00 μm, more preferably 0.10 μm to 20.00 μm, more preferably 0.10 μm to 8.00 μm, more preferably 0.10 μm to 6.00 μm, more preferably 0.10 μm to 4.00 μm, more preferably 0.10 μm to 2.00 μm, even more preferably 0.10 μm to 1.00 μm, and particularly preferably 0.10 μm to 0.80 μm, since a water-based paint having a desired viscosity and high stability can be obtained. According to this configuration, there is an advantage that the polymerization stability of the graft copolymer (A) is excellent, and the water-based paint has excellent storage stability. In this specification, the "volume average particle diameter (Mv) of the graft copolymer (A)" means the volume average particle diameter of the primary particles of the graft copolymer (A) unless otherwise specified. The volume average particle diameter of the graft copolymer (A) can be measured using a water-based paint or a water-based latex containing the graft copolymer (A) as a sample, using a dynamic light scattering particle size distribution measuring device, etc. The volume average particle diameter of the graft copolymer (A) will be described in detail in the following examples.

[0135] The number distribution of the particle size of the graft copolymer (A) in the water-based paint preferably has a half-value width of 0.5 to 1 times the volume average particle size. This configuration has the advantage that the water-based paint has a low viscosity and is easy to handle.

[0136] The method for producing the graft copolymer (A) will be described in detail in the section entitled "Method for producing water-based paint" below.

[0137] In the present water-based paint, the polyorganosiloxane is preferably 55% by weight to 95% by weight, more preferably 55% by weight to 90% by weight, more preferably 60% by weight to 90% by weight, even more preferably 65% ​​by weight to 85% by weight, and particularly preferably 70% by weight to 85% by weight. When the polyorganosiloxane is (a) 55% by weight or more in 100% by weight of the graft copolymer (A), the water-based paint has the advantage of being able to provide a coating film with a smaller loss tangent (tan δ) at seawater temperature, and when it is (b) 95% by weight or less, the water-based paint has the advantage of being more excellent in film formability.

[0138] (2-2. Polymer (B)) The water-based paint preferably contains a polymer (B). The polymer (B) in the water-based paint can contribute to improving the film-forming properties of the water-based paint. The polymer (B) can be mixed mainly in the process of producing the graft copolymer (A). Specifically, in the case where the above-mentioned non-grafted polymer is generated in the preparation step of the graft portion in the production of the graft copolymer (A), and the non-grafted polymer is not removed from the aqueous latex of the obtained graft copolymer (A), the non-grafted polymer can become the polymer (B) in the obtained water-based paint. In particular, in the preparation step of the second graft portion, the non-grafted polymer (polymer F2 or polymer F3) may be generated. Note that the polymer (B) is not limited to the one mixed in the production process of the above-mentioned graft copolymer (A), and also includes a polymer added separately. The polymer added separately as the polymer (B) is obtained, for example, by polymerizing a monomer mixture for forming the polymer (B) separately from the production of the graft copolymer (A).

[0139] The polymer (B) preferably contains a structural unit derived from one or more monomers selected from the group consisting of an aromatic vinyl monomer, a vinyl cyan monomer, and a (meth)acrylate monomer. This structure has the advantage that the resulting water-based paint has excellent film-forming properties.

[0140] Specific examples of the aromatic vinyl monomer, the vinyl cyan monomer and the (meth)acrylate monomer are the same as those described in the section (First graft portion) above, and therefore the description therein is incorporated by reference and will not be described here.

[0141] The polymer (B) preferably contains 60.00% by weight to 99.99% by weight of structural units derived from aromatic vinyl monomers, structural units derived from vinyl cyan monomers, and structural units derived from (meth)acrylate monomers in total, more preferably 80.00% by weight to 99.95% by weight, even more preferably 90.00% by weight to 99.90% by weight, particularly preferably 95.00% by weight to 99.85% by weight, and most preferably 98.0% by weight to 99.82% by weight, in 100% by weight of the polymer (B). This configuration has the advantage that the resulting water-based paint has excellent film-forming properties.

[0142] From the viewpoint of reactivity during the formation (polymerization) of the polymer (B), the (meth)acrylate monomer is preferably one or more selected from the group consisting of methyl acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate. When the polymer (B) is derived from a graft portion, the "reactivity during the formation (polymerization) of the polymer (B)" refers to the "reactivity during the formation of the graft portion." In addition, by mixing one or more selected from the group consisting of methyl acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate, which have a relatively low glass transition temperature of the homopolymer, with methyl methacrylate, which has a relatively high glass transition temperature of the homopolymer, to prepare a monomer mixture for forming a graft portion or a monomer mixture for forming a polymer (B), the glass transition temperature of the resulting polymer (B) can be adjusted to a desired temperature.

[0143] From the viewpoint of achieving both the film-forming properties of the water-based paint and the reactivity during the formation (polymerization) of the polymer (B), the polymer (B) contains a structural unit derived from methyl methacrylate and a structural unit derived from butyl methacrylate.

[0144] The polymer (B) preferably contains 60.00% by weight to 99.99% by weight of the constitutional unit derived from the (meth)acrylate monomer, more preferably 80.00% by weight to 99.95% by weight, even more preferably 90.00% by weight to 99.90% by weight, particularly preferably 95.00% by weight to 99.85% by weight, and most preferably 98.0% by weight to 99.82% by weight, in 100% by weight of the polymer (B). This configuration has the advantages of (i) the glass transition temperature of the polymer (B) being lower (for example, lower than 80°C), thereby providing the water-based paint obtained with even better film-forming properties, and / or (ii) providing excellent reactivity during the formation (polymerization) of the polymer (B).

[0145] The polymer (B) preferably contains 60.00% by weight to 99.99% by weight of structural units derived from methyl methacrylate and structural units derived from butyl methacrylate in total, more preferably 80.00% by weight to 99.95% by weight, even more preferably 90.00% by weight to 99.90% by weight, particularly preferably 95.00% by weight to 99.85% by weight, and most preferably 98.0% by weight to 99.82% by weight, based on 100% by weight of the polymer (B). This configuration has the advantage of being more excellent in reactivity during the formation (polymerization) of the polymer (B).

[0146] (Glass transition temperature of polymer (B)) The Tg of the polymer (B) is not particularly limited, but is preferably 25° C. to 100° C., more preferably 30° C. to 90° C., even more preferably 35° C. to 80° C., and particularly preferably 40° C. to 70° C. This configuration has the advantage that the water-based paint has excellent film-forming properties. Furthermore, the present inventors have independently found that, surprisingly, when the upper limit of the Tg of the polymer (B) is 100° C. or less, the generation of scale during the production of the water-based paint is reduced or eliminated.

[0147] The Tg of the polymer (B) can be determined by the composition of the structural units contained in the polymer (B), etc. In other words, the Tg of the resulting polymer (B) can be adjusted by changing the composition of the monomer mixture (e.g., the monomer mixture for forming the first graft portion and the monomer mixture for forming the second graft portion) used when preparing the graft portion, or the monomer mixture for forming the polymer (B) used when separately preparing the polymer (B).

[0148] When the polymer (B) is a homopolymer of one type of monomer and the monomer used in the production (polymerization) of the polymer (B) is known, the glass transition temperature Tg of the polymer (B) can be regarded as the Tg (°C) of the homopolymer of the monomer. For example, the values ​​described in Polymer Handbook Fourth Edition (edited by J. Brandup et al., Jphn Wiley & Sons, Inc.) can be used for the Tg of the homopolymer.

[0149] The case where polymer (B) is a copolymer of two or more monomers and the monomers used in the production (polymerization) of polymer (B) are known (hereinafter referred to as case A) will be described. In case A, the glass transition temperature Tg of polymer (B) can be calculated by the above-mentioned FOX formula (Formula 1).

[0150] In the case of case A, the amounts of the reactive emulsifier, the chain transfer agent and the monomer M2 used are each 20.0% by weight or less in the total of 100% by weight of the monomer mixture for forming the graft portion and the monomer mixture for forming the polymer (B), when calculating the glass transition temperature Tg of the polymer (B) by the FOX formula (Formula 1), the reactive emulsifier, the chain transfer agent and the monomer M2 are excluded from the monomers used in the production of the polymer (B). That is, the glass transition temperature Tg of the polymer (B) is calculated by the FOX formula (Formula 1) with the monomers other than the reactive emulsifier, the chain transfer agent and the monomer M2 being regarded as the monomers used in the production of the polymer (B).

[0151] In this water-based paint, the content of the polymer (B) is not particularly limited. In this water-based paint, the polymer (B) is preferably 5.0% by weight or more, more preferably 6.0% by weight or more, more preferably 7.0% by weight or more, more preferably 8.0% by weight or more, more preferably 9.0% by weight or more, more preferably 10.0% by weight or more, more preferably 11.0% by weight or more, more preferably 12.0% by weight or more, more preferably 13.0% by weight or more, more preferably 14.0% by weight or more, more preferably 15.0% by weight or more, more preferably 16.0% by weight or more, even more preferably 17.0% by weight or more, and particularly preferably 18.0% by weight or more. According to this configuration, the water-based paint has the advantage of being more excellent in film-forming properties.

[0152] In this water-based paint, the polymer (B) is preferably 30. wt% or less, more preferably 28.0 wt% or less, more preferably 26.0 wt% or less, more preferably 24.0 wt% or less, more preferably 22.0 wt% or less, more preferably 20.0 wt% or less, more preferably 19.0 wt% or less, more preferably 18.0 wt% or less, more preferably 17.0 wt% or less, more preferably 16.0 wt% or less, more preferably 15.0 wt% or less, more preferably 14.0 wt% or less, more preferably 13.0 wt% or less, more preferably 12.0 wt% or less, more preferably 11.0 wt% or less, more preferably 10.0 wt% or less, more preferably 9.0 wt% or less, more preferably 8.0 wt% or less, even more preferably 7.0 wt% or less, and particularly preferably 6.0 wt% or less. This configuration has the advantage that the generation of scale during the production of water-based paint is reduced or eliminated.

[0153] The case where the non-grafted polymer obtained during the production of the graft copolymer (A) is not removed from the aqueous latex of the graft copolymer (A) and a separately prepared polymer is not blended (hereinafter referred to as case B) will be described. In case B, the polymer (B) is derived only from the non-grafted polymer. In case B, the composition (type and content ratio) of the structural units of the grafted portion is the same as the composition of the structural units of the polymer (B). Therefore, the Tg of the grafted portion and the Tg of the polymer (B) are the same value. In case B, when the polymerization conversion rate during the production of the graft copolymer (A) is 100%, the sum of the content (%) of the polymer (B) in the total of 100% by weight of the grafted portion and the polymer (B) and the graft rate is 100%. In case B, the content (%) of polymer (B) in the total of 100% by weight of the graft portion and polymer (B) can be appropriately adjusted by changing the amount of monomer M1 used when preparing the polyorganosiloxane and the amount of chain transfer agent used when preparing the second graft portion, etc.

[0154] In one embodiment of the present invention, a polymer prepared separately from the graft copolymer (A) may be added to the aqueous latex of the graft copolymer (A) or the aqueous paint to obtain the polymer (B). When the non-grafted polymer obtained during the production of the graft copolymer (A) is not removed from the aqueous latex of the graft copolymer (A) and a separately prepared polymer is blended, the polymer (B) is derived from the non-grafted polymer and the polymer prepared separately and blended. When the non-grafted polymer obtained during the production of the graft copolymer (A) is removed from the aqueous latex of the graft copolymer (A) and a separately prepared polymer is blended, the polymer (B) is derived only from the polymer prepared separately and blended.

[0155] In the present water-based paint, the polyorganosiloxane is preferably 55% by weight to 95% by weight, more preferably 55% by weight to 90% by weight, more preferably 60% by weight to 90% by weight, even more preferably 65% ​​by weight to 85% by weight, and particularly preferably 70% by weight to 85% by weight. When the polyorganosiloxane is (a) 55% by weight or more out of the total 100% by weight of the graft copolymer (A) and the polymer (B), the water-based paint has the advantage of being able to provide a coating film with a smaller loss tangent (tan δ) at seawater temperature, and when it is (b) 95% by weight or less, the water-based paint has the advantage of being more excellent in film-forming properties.

[0156] (2-3. Antifouling agents) The water-based paint may further contain an antifouling agent. Since the loss tangent (tan δ) of the water-based paint at seawater temperature is small, it is considered that the water-based paint has antifouling properties against aquatic organisms without containing an antifouling agent. Therefore, the water-based paint can be suitably used as an antifouling paint for underwater structures without containing an antifouling agent. Since the water-based paint can provide a coating film having better antifouling properties against aquatic organisms and / or a coating film in which the antifouling properties against aquatic organisms last for a longer period of time, the water-based paint preferably further contains an antifouling agent. On the other hand, a coating film obtained from a water-based paint that does not contain an antifouling agent is less susceptible to damage than a coating film obtained from a water-based paint that contains an antifouling agent. Therefore, a coating film obtained from a water-based paint that does not contain an antifouling agent has the advantage of being more durable than a coating film obtained from a water-based paint that contains an antifouling agent.

[0157] The antifouling agent is not particularly limited, and any known antifouling agent can be used. Examples of the antifouling agent include inorganic compounds, organic compounds containing metals, and organic compounds not containing metals.

[0158] Examples of the antifouling agent include metal salts such as zinc oxide, cuprous oxide, 2-pyridinethiol-1-oxide zinc salt (also known as zinc pyrithione) and copper salt, pyrithione salt compounds, p-isopropylpyridinemethyldiphenylborane, pyridinetriphenylborane, tetramethylthiuram disulfide, carbamate compounds (e.g., zinc dimethyldithiocarbamate, zinc ethylenebisdithiocarbamate, 3-iodo-2-propylbutylcarbamate, bisdimethyldithiocarbamoylzincethylenebisdithiocarbamate, etc.). Thiocarbamate and manganese-2-ethylenebisdithiocarbamate, 2-methylthio-4-t-butylamino-6-cyclopropylamino-s-triazine, 2,4,5,6-tetrachloroisophthalonitrile, N,N-dimethyldichlorophenylurea, copper rhodanide, 4,5-dichloro-2-n-octyl-3(2H)isothiazolone (also known as 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one), N-(fluorodichloromethylthio)phthalimide, N,N'-dimethyl-N'-phenyl 1,1-Dichloro-N-[(dimethylamino)sulfamide], tetramethylthiuram disulfide, 2,4,6-trichlorophenylmaleimide, 2,3,5,6-tetrachloro-4-(methylsulfonyl)pyridine, diiodomethyl-paratrisulfone, phenyl(bispyridyl)bismuth dichloride, 2-(4-thiazolyl)-benzimidazole, triphenylboron pyridine salt, stearylamine-triphenylboron, laurylamine-triphenylboron, 1,1-dichloro-N-[(dimethylamino)sulfamide] 1,1-dichloro-N-[(dimethylamino)sulfonyl]-1-fluoro-N-(4-methylphenyl)methanesulfenamide, N'-(3,4-dichlorophenyl)-N,N'-dimethylurea, N'-tert-butyl-N-cyclopropyl-6-(methylthio)-1,3,5-triazine-2,4-diamine, 4-bromo-2-(4-chlorophenyl)-5-(trifluoromethyl)-1H-pyrrole-3-carbonitrile, and the like.

[0159] (2-4. Organic solvents) The water-based paint may contain an organic solvent. The water-based paint has the advantage of being excellent in film-forming properties without containing an organic solvent. When the water-based paint contains an organic solvent, the water-based paint has the advantage of being even more excellent in film-forming properties. Examples of organic solvents include hydrocarbons, halogenated hydrocarbons, ethers, esters, ketones, and alcohols. Examples of organic solvents of hydrocarbons include n-hexane, isohexane, n-heptane, n-octane, isooctane, n-decane, n-dodecane, cyclohexane, methylcyclohexane, cyclopentane, toluene, xylene, benzene, ethylbenzene, decalin, white spirit, and naphtha. Examples of organic solvents of halogenated hydrocarbons include methylene chloride, chloroform, tetrachloroethane, and trichloroethylene. Examples of organic solvents of ethers include dioxane, ethyl ether, diethyl ether, butyl diglycol, 2-butoxyethanol, tetrahydrofuran, tetrahydropyran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate (also known as PMAC), propylene glycol methyl ether, dipropylene glycol methyl ether, tripropylene glycol methyl ether, propylene glycol-n-propyl ether, dipropylene glycol-n-propyl ether, propylene glycol-n-butyl ether, dipropylene glycol-n-butyl ether, tripropylene glycol-n-butyl ether, propylene glycol methyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol diacetate, propylene glycol phenyl ether, and dipropylene glycol dimethyl ether.Examples of the organic solvent of the esters include methyl acetate, ethyl acetate, propyl acetate, butyl acetate, benzyl acetate, methoxypropyl acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, n-butyl acetate, and 2-ethoxyethyl acetate. Examples of the organic solvent of the ketones include acetone, methyl ethyl ketone, diethyl ketone, ethyl isobutyl ketone, methyl isobutyl ketone (also known as MIBK), methyl isoamyl ketone, and diacetone alcohol. Examples of the organic solvent of the alcohols include methanol, ethanol, n-propanol, (iso)propanol, n-butanol, isobutanol, benzyl alcohol, ethylene glycol, and propylene glycol. As the organic solvent, a mixture of the above-mentioned alcohol and water can also be used. Examples of the organic solvent include dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone. These organic solvents may be used alone or in combination of two or more.

[0160] From the viewpoint of environmental conservation and safety and hygiene, the content of organic solvent in the present water-based paint is preferably as small as possible. The content of organic solvent in the present water-based paint is preferably 20 parts by weight or less, more preferably 15 parts by weight or less, even more preferably 10 parts by weight or less, and particularly preferably 5 parts by weight or less, per 100 parts by weight of the water-based paint.

[0161] (2-5. Other optional ingredients) The water-based paint may contain other optional components other than the above-mentioned components as necessary. The other optional components include curing agents, colorants such as pigments and dyes, extender pigments, pigment dispersants, UV absorbers, antioxidants, heat stabilizers (gelling inhibitors), stabilizers, plasticizers, leveling agents, defoamers, silane coupling agents, antistatic agents, flame retardants, lubricants, viscosity reducers, thickeners, viscosity adjusters, thixotropic agents, low-shrinkage agents, inorganic fillers, organic fillers, thermoplastic resins, drying agents, wetting agents, dispersants, anti-sagging agents, color separation inhibitors, anti-settling agents, coating wear adjusters, surface adjusters, film-forming aids, antibacterial agents, antifungal agents, preservatives, antifreeze agents, tackifiers, and rust inhibitors.

[0162] 3. Manufacturing method of water-based paint The method for producing the water-based paint is not particularly limited. For example, the method for producing the water-based paint according to one embodiment of the present invention includes a step 1 of obtaining a polyorganosiloxane by polymerizing a monomer mixture for forming a polyorganosiloxane, the monomer mixture including (a) an organosiloxane and (b) (b-1) a monomer M1 having one or more hydrolyzable silyl groups in the molecule and (b-2) one or more ethylenically unsaturated groups and / or mercapto groups, and a step 2 of polymerizing a monomer mixture for forming a graft portion in the presence of the polyorganosiloxane obtained in the step 1, in which the total amount of the polyfunctional alkoxysilane compound and the polyfunctional monomer used in 100% by weight of the monomer mixture for forming a polyorganosiloxane is 0.50% by weight or less, and the step 2 includes polymerizing a first graft portion. and a step 2b of polymerizing a monomer mixture for forming a second graft portion, in which in the step 2a, the first graft portion-forming monomer mixture contains (a) a monomer M2 derived from a monomer containing (a-1) one or more hydrolyzable silyl groups in the molecule and (a-2) one or more ethylenically unsaturated groups and / or mercapto groups, and does not contain (b) a chain transfer agent, and in the step 2b, the second graft portion-forming monomer mixture contains (a) a chain transfer agent, and does not contain (b) a monomer M3 containing (b-1) one or more hydrolyzable silyl groups in the molecule and (b-2) one or more ethylenically unsaturated groups and / or mercapto groups.

[0163] The manufacturing method of the water-based paint according to one embodiment of the present invention has the above-mentioned configuration, and therefore can provide a water-based paint with excellent film-forming properties that can provide a coating film with a small loss tangent (tan δ) at seawater temperature.

[0164] In this specification, "a method for producing a water-based paint according to one embodiment of the present invention" may also be referred to as "the present production method."

[0165] Each step of the present manufacturing method will be described in detail below, but matters other than those described below (e.g., various components and their amounts to be added, etc.) are not particularly limited, and the explanations in the above section [2. Water-based paint] will be used as appropriate.

[0166] (3-1.Process 1) Step 1 is a step of preparing a polyorganosiloxane.

[0167] The organosiloxane contained in the polyorganosiloxane-forming monomer mixture is not particularly limited. In step 1, for example, it is preferable to use a known organosiloxane so as to obtain a polyorganosiloxane having the structural unit (organosiloxane unit) described in the above (organosiloxane unit).

[0168] In step 1, for example, (a) dimethyldimethoxysilane, dimethyldiethoxysilane, and other dimethyldialkoxysilanes, (b) hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, trimethyltriphenylcyclotrisiloxane, tetradecamethylcycloheptasiloxane, dimethylcyclics (dimethylsiloxane cyclic oligomer trimer to heptamer mixture), and other various organosiloxane-based cyclic compounds having three or more membered rings, and (c) dimethyldichlorosilane, etc., can be used as the raw organosiloxane. In addition, linear or branched organosiloxanes can also be used as the raw organosiloxane.

[0169] A prepolymerized polyorganosiloxane may be used as the organosiloxane in step 1. In this case, the molecular chain terminals of the polyorganosiloxane may be blocked with a hydroxyl group, an alkoxy group, a trimethylsilyl group, a dimethylvinylsilyl group, a methylphenylvinylsilyl group, a methyldiphenylsilyl group, or the like.

[0170] As the organosiloxane raw material used in step 1, various organosiloxane-based cyclic compounds having three or more members, such as hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, trimethyltriphenylcyclotrisiloxane, tetradecamethylcycloheptasiloxane, and dimethylcyclics (mixture of dimethylsiloxane cyclic oligomers 3 to 7 monomers), are preferred because they are easily available and can be used to prepare polyorganosiloxane.

[0171] The monomer M1 contained in the monomer mixture for forming polyorganosiloxane is the same as that explained in the section (structural unit U) above, and therefore the explanation therefor is incorporated by reference and will not be repeated here.

[0172] The amount of the monomer M1 used in step 1 correlates with the content of the structural unit U in the resulting polyorganosiloxane. The amount of the monomer M1 used in step 1 is not particularly limited, but is preferably such that the content of the structural unit U is 0.001% by weight to 10.0% by weight in 100% by weight of the polyorganosiloxane. The amount of the monomer M1 used in step 1 is, for example, preferably 0.001% by weight to 10.0% by weight, more preferably 0.001% by weight to 5.0% by weight, even more preferably 0.01% by weight to 5.0% by weight, and particularly preferably 1.0% by weight to 5.0% by weight in 100% by weight of the monomer mixture for forming the polyorganosiloxane. This configuration has the advantage that the polymerization of the monomer mixture for forming the graft portion in the presence of (a) the polyorganosiloxane can be efficiently carried out.

[0173] In step 1, the method for polymerizing the organosiloxane and the monomer M1 is not particularly limited, but may be, for example, a known emulsion polymerization method carried out in the presence of an acidic emulsifier.

[0174] The acidic emulsifier is not particularly limited, but when using an organosiloxane-based cyclic compound, it is preferable to use one that can open the ring of the organosiloxane-based cyclic compound.As an acidic emulsifier, for example, dodecylbenzenesulfonic acid is preferably mentioned.The amount of the acidic emulsifier used is not particularly limited, and may be appropriately set according to (a) the desired volume average particle size of polyorganosiloxane and graft copolymer (A), (b) the solid content (monomer mixture) concentration in the reaction solution, (c) polymerization conditions such as polymerization temperature, and (d) the presence or absence and amount of additives such as surfactants used.

[0175] The volume average particle size of the resulting polyorganosiloxane can be controlled by (a) the degree of pre-dispersion of the raw materials, (b) the amount of emulsifier used, (c) the polymerization temperature, and (d) the method of supplying the raw materials.

[0176] When polyorganosiloxane is obtained by emulsion polymerization in the presence of an acidic emulsifier, the obtained aqueous latex is strongly acidic, so it is preferable to neutralize it after the polymerization reaction is completed.The basic compound used for neutralization is not particularly limited, and examples thereof include sodium hydroxide, potassium hydroxide, ammonia, triethylamine, etc.The aqueous latex containing polyorganosiloxane can be neutralized by adding these basic compounds directly or in the form of an aqueous solution to the aqueous latex.

[0177] In step 1, the total amount of the polyfunctional alkoxysilane compound and the polyfunctional monomer is 0.50% by weight or less in 100% by weight of the polyorganosiloxane-forming monomer mixture. With this configuration, a non-crosslinked polyorganosiloxane is obtained.

[0178] (3-2.Process 2) Step 2 is a step of preparing a graft portion grafted to the polyorganosiloxane. The graft portion can be formed by polymerizing a monomer (a monomer mixture for forming a graft portion) used for forming the graft portion in the presence of the polyorganosiloxane by known radical polymerization. More specifically, step 2 includes step 2a of polymerizing a monomer mixture for forming a first graft portion and step 2b of polymerizing a monomer mixture for forming a second graft portion.

[0179] When polyorganosiloxane is obtained by emulsion polymerization in the presence of the above-mentioned acidic emulsifier (i.e., when polyorganosiloxane is obtained as an aqueous latex), it is preferable to carry out the polymerization of graft part (first graft part and second graft part) by emulsion polymerization method.The graft part can be produced, for example, according to the method described in International Publication WO2005 / 028546.

[0180] The order of performing steps 2a and 2b is not particularly limited. In this production method, (a) step 2a may be performed after step 1, and step 2b may be performed after step 2a, or (b) step 2b may be performed after step 1, and step 2a may be performed after step 2b.

[0181] A case where step 2a is carried out after step 1, and step 2b is carried out after step 2a (hereinafter also referred to as "case E") will be described. In case E, step 2a can be said to be a step of polymerizing a monomer mixture for forming a first graft portion in the presence of the polyorganosiloxane obtained in step 1 to prepare a first graft portion formed outside the polyorganosiloxane. In case E, step 2b is a step of polymerizing a monomer mixture for forming a second graft portion in the presence of the copolymer having polyorganosiloxane and the first graft portion formed outside the polyorganosiloxane obtained in step 2a to prepare a second graft portion formed outside the first graft portion. In case E, at least a part of the first graft portion can be graft-bonded to the polyorganosiloxane.

[0182] A case where step 2b is carried out after step 1, and step 2a is carried out after step 2b (hereinafter also referred to as "case F") will be described. In case F, step 2b can be said to be a step of polymerizing a monomer mixture for forming a second graft portion in the presence of the polyorganosiloxane obtained in step 1 to prepare a second graft portion formed outside the polyorganosiloxane. In case F, step 2a is a step of polymerizing a monomer mixture for forming a first graft portion in the presence of the copolymer having polyorganosiloxane and a second graft portion formed outside the polyorganosiloxane obtained in step 2b to prepare a first graft portion formed outside the second graft portion. In case F, at least a part of the second graft portion can be graft-bonded to the polyorganosiloxane.

[0183] The monomer mixture for forming the first graft portion contains (a) (a-1) a monomer M2 derived from a monomer containing one or more hydrolyzable silyl groups in the molecule and (a-2) one or more ethylenically unsaturated groups and / or mercapto groups, and (b) does not contain a chain transfer agent. This configuration has the advantages of (i) providing a coating film with a small loss tangent (tan δ) at seawater temperature and (ii) reducing or eliminating the occurrence of blisters when a coating film obtained from the water-based paint is immersed in water. In addition, since the monomer mixture for forming the first graft portion does not contain a chain transfer agent, the amount of polymer that is a polymer having the same structure as the first graft portion (i.e., a polymer containing the structural unit U2) and is not graft-bonded to any polymer (e.g., polyorganosiloxane) is not generated at all or is very small, if any. As a result, the degree of crosslinking of the coating film is low, and there is also the advantage of excellent film formability.

[0184] The monomer M2 is the same as that explained above in the section (Structural unit U2), and therefore the explanation therefor is incorporated by reference and will not be repeated here.

[0185] The monomer mixture for forming the second graft portion contains (a) a chain transfer agent and does not contain (b) a monomer M3 containing (b-1) one or more hydrolyzable silyl groups in the molecule and (b-2) one or more ethylenically unsaturated groups and / or mercapto groups. This configuration has the advantage of (i) being able to provide a water-based paint with better film-forming properties. In addition, this configuration has the advantage of not generating any polymers that are polymers containing structural units derived from monomers containing (1) one or more hydrolyzable silyl groups in the molecule and (2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule and that are not graft-bonded to any of the polymers, or if any, they are generated, they are very small. As a result, the degree of crosslinking of the coating film is low, and the coating film has the advantage of excellent film-forming properties.

[0186] The chain transfer agent is the same as that explained above in the section (Structural Units Derived from Chain Transfer Agents), and therefore the explanation therefor is incorporated by reference and will not be repeated here.

[0187] The type and amount of the constituent units of the first graft portion to be obtained can be determined by the type and amount of the monomers contained in the monomer mixture for forming the first graft portion. Therefore, the type and amount of the monomers contained in the monomer mixture for forming the first graft portion may be appropriately set so that the first graft portion described in the above section (First graft portion) is obtained. Furthermore, the type and amount of the monomers contained in the monomer mixture for forming the second graft portion may be appropriately set so that the second graft portion described in the above section (Second graft portion) is obtained.

[0188] In the case where an emulsion polymerization method is adopted in step 2 (step 2a and step 2b), a thermally decomposable initiator can be used as the radical polymerization initiator. Examples of the thermally decomposable initiator include known initiators such as 2,2'-azobisisobutyronitrile, hydrogen peroxide, potassium persulfate, and ammonium persulfate.

[0189] As the radical polymerization initiator, a redox type initiator can also be used. The redox type initiator is an initiator in which (a) a peroxide such as an organic peroxide or an inorganic peroxide is used in combination with (b) a reducing agent such as sodium formaldehyde sulfoxylate or glucose, if necessary, a transition metal salt such as iron (II) sulfate, if necessary, a chelating agent such as disodium ethylenediaminetetraacetate, if necessary, and a phosphorus-containing compound such as sodium pyrophosphate, if necessary. Examples of the organic peroxide include t-butyl peroxyisopropyl carbonate, paramenthane hydroperoxide, cumene hydroperoxide, dicumyl peroxide, t-butyl hydroperoxide, di-t-butyl peroxide, and t-hexyl peroxide. Examples of the inorganic peroxide include hydrogen peroxide, potassium persulfate, and ammonium persulfate.

[0190] In step 2b, 0.01 to 5.00 parts by weight of a chain transfer agent is used per 100 parts by weight of the monomer mixture for forming the second graft portion. According to this configuration, a water-based paint containing the polymer (B) in an amount of, for example, 5.0% by weight or more based on the total of 100% by weight of the graft copolymer (A) and the polymer (B) can be obtained. As a result, this production method has the advantage of being able to provide a water-based paint with excellent film-forming properties.

[0191] The amount of the chain transfer agent used relative to 100 parts by weight of the second graft portion-forming monomer mixture is preferably 0.01 parts by weight to 5.00 parts by weight, more preferably 0.05% by weight to 3.0% by weight, even more preferably 0.10% by weight to 2.0% by weight, and particularly preferably 0.15% by weight to 1.0% by weight. This configuration has the advantage of being able to provide a water-based coating material with excellent film-forming properties.

[0192] On the other hand, as described above, in step 2a, the first graft portion-forming monomer mixture does not contain a chain transfer agent, in other words, no chain transfer agent is used in step 2a.

[0193] In this production method, the polyorganosiloxane-forming monomer mixture is preferably contained in an amount of 55% by weight to 90% by weight out of the total amount of the polyorganosiloxane-forming monomer mixture and the graft portion-forming monomer mixture, which is 100% by weight. This configuration has the advantage of providing a water-based paint that can provide a coating film with excellent water repellency. In this production method, the total amount of the polyorganosiloxane-forming monomer mixture is more preferably 55% by weight to 95% by weight, more preferably 60% by weight to 90% by weight, even more preferably 65% ​​by weight to 85% by weight, and particularly preferably 70% by weight to 85% by weight out of the total amount of the polyorganosiloxane-forming monomer mixture and the graft portion-forming monomer mixture, which is 100% by weight. This configuration has the advantage of providing a water-based paint that can provide a coating film with excellent water repellency and has excellent film formability.

[0194] The graft ratio of the graft portion (including preferred embodiments) is the same as that described in the above section (Graft ratio of the graft portion), and therefore the description is incorporated herein by reference and will not be repeated here.

[0195] The glass transition temperature of the graft portion (including preferred embodiments) is the same as that described in the above section (Glass transition temperature of the graft portion), and therefore the description is incorporated herein by reference and will not be repeated here.

[0196] As described above, in step 2, a non-grafted polymer may be obtained together with the grafted portion. In particular, in step 2b, a non-grafted polymer (polymer F2) may be obtained. By not removing the non-grafted polymer from the aqueous latex obtained in step 2, an aqueous latex containing the graft copolymer (A) and the polymer (B) can be obtained. The ratio of the grafted portion and the non-grafted polymer obtained in step 2 can be appropriately adjusted by (i) the amount of the monomer M1 in the monomer mixture for forming the polyorganosiloxane in step 1, and (ii) the amount of the chain transfer agent in the monomer mixture for forming the second grafted portion in step 2b, etc. In addition, a polymer (B) prepared separately may be further added to the aqueous latex of the graft copolymer (A) or the aqueous latex containing the graft copolymer (A) and the non-grafted polymer.

[0197] The first graft portion-forming monomer mixture in step 2a and the second graft portion-forming monomer mixture in step 2b each preferably contain a reactive emulsifier. The reactive emulsifier is the same as that described in the above section (Constituent units derived from reactive emulsifier), and therefore the description is incorporated herein by reference and will not be described here. For example, the amount of reactive emulsifier used in step 2a is preferably 0.1% by weight to 20.0% by weight, more preferably 0.1% by weight to 15.0% by weight, more preferably 1.0% by weight to 15.0% by weight, more preferably 1.0% by weight to 10.0% by weight, even more preferably 1.0% by weight to 8.0% by weight, even more preferably 1.0% by weight to 5.0% by weight, and particularly preferably 1.0% by weight to 4.0% by weight, based on 100% by weight of the first graft portion-forming monomer mixture. For example, the amount of reactive emulsifier used in step 2b is preferably 0.1% by weight to 20.0% by weight, more preferably 0.1% by weight to 15.0% by weight, more preferably 1.0% by weight to 15.0% by weight, more preferably 1.0% by weight to 10.0% by weight, even more preferably 1.0% by weight to 8.0% by weight, even more preferably 1.0% by weight to 5.0% by weight, and particularly preferably 1.0% by weight to 4.0% by weight. When the amount of reactive emulsifier used in steps 2a and 2b is within the above-mentioned range, there is an advantage that the generation of scale during the production of the water-based paint is further reduced or eliminated.

[0198] In addition to the above-mentioned components, an emulsifier and a surfactant can be used in the polymerization of each monomer mixture in the production of the water-based paint. The types and amounts of the emulsifier and surfactant used are within the known ranges.

[0199] In the production of the water-based paint, known conditions such as polymerization temperature, pressure, and deoxidation in the polymerization of each monomer mixture can be used.

[0200] The aqueous latex containing the graft copolymer (A) and the polymer (B) obtained by the above-mentioned production method may be used as it is or diluted with water (e.g., deionized water) as necessary as an aqueous paint. An antifouling agent and / or other optional components may be further added to the aqueous latex containing the graft copolymer (A) and the polymer (B) obtained by the above-mentioned production method to form an aqueous paint. In other words, the present production method may further include a step of adding an antifouling agent. The antifouling agent and other optional components are the same as those described above in (2-3. Antifouling Agent) and (2-5. Other Optional Components), respectively, and therefore the description is incorporated herein by reference and will not be repeated here.

[0201] [4. How to use water-based paint (how to manufacture water-based coating film)] The method of using the water-based paint can be said to be a method of applying a coating film (e.g., an antifouling coating film) using the water-based paint. The method of using the water-based paint has a step of applying the water-based paint to an underwater structure. Specifically, the method of using the water-based paint according to one embodiment of the present invention includes a step of applying the water-based paint according to one embodiment of the present invention described in the above section [2. Water-based paint] or the water-based paint obtained by the method of producing the water-based paint according to one embodiment of the present invention described in the above section [3. Method of producing the water-based paint] to an underwater structure. The method of using the water-based paint can be said to be a method of producing a water-based coating film. Specifically, the method of producing a water-based coating film according to one embodiment of the present invention includes a step of applying the water-based paint according to one embodiment of the present invention described in the above section [2. Water-based paint] or the water-based paint obtained by the method of producing the water-based paint according to one embodiment of the present invention described in the above section [3. Method of producing the water-based paint] to an underwater structure. According to this configuration, a coating film having a small loss tangent (tan δ) at seawater temperature can be formed on the surface or inner surface of the underwater structure. A coating film with a small loss tangent (tan δ) at seawater temperature is considered to have excellent antifouling properties at seawater temperature (e.g., antifouling properties against aquatic organisms). Therefore, the method of using the present water-based paint can provide a coating film with excellent antifouling properties at seawater temperature (e.g., antifouling properties against aquatic organisms) on the surface or inner surface of an underwater structure. In addition, the present water-based paint has excellent film-forming properties. Therefore, by applying the water-based paint to an underwater structure, a coating film with antifouling properties can be easily formed on the surface or inner surface of the underwater structure.

[0202] In the coating step, the method of coating the water-based coating material is not particularly limited, and any known method can be used. Examples of the coating method that can be used include casting, dipping, spraying, brushing, roller, dip coater, electrostatic coating, and electrodeposition coating.

[0203] In the coating step, a coating robot may be used. The coating robot may be used to apply the water-based paint by extruding the water-based paint onto the underwater structure in a bead, monofilament or swirl shape. The water-based paint may also be applied onto the underwater structure by using a jet spray method or a streaming method.

[0204] The water-based paint applied to the underwater structure may be dried. As described above, by applying the water-based paint to the underwater structure and optionally drying the water-based paint, a coating film having a small loss tangent (tan δ) at seawater temperature can be formed on the surface or inner surface of the underwater structure. As a result, by applying the water-based paint to the underwater structure and optionally drying the water-based paint, a coating film having antifouling properties at seawater temperature can be formed.

[0205] The method for producing a water-based coating film according to one embodiment of the present invention may be configured as follows.

[0206] A method for producing a water-based coating film, comprising the steps of: applying a water-based paint to an underwater structure; Here, the water-based paint is Contains a graft copolymer (A), The graft copolymer (A) includes a polyorganosiloxane and a graft portion graft-bonded to the polyorganosiloxane, The polyorganosiloxane (a) comprises a structural unit U1 derived from a monomer containing (a-1) one or more hydrolyzable silyl groups and (a-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule, and (b) is non-crosslinked; the graft portion includes a first graft portion and a second graft portion; the first graft portion (a) contains (a-1) a structural unit U2 derived from a monomer containing one or more hydrolyzable silyl groups and (a-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule, and (b) does not contain a structural unit derived from a chain transfer agent; The second graft portion (a) contains a structural unit derived from a chain transfer agent, and does not contain a structural unit U3 derived from a monomer containing (b-1) one or more hydrolyzable silyl groups and (b-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule.

[0207] [5. Coating] A coating film formed by the method described in the above section [4. Method for using water-based paint (method for producing water-based coating film)] is also one embodiment of the present invention. That is, (a) a coating film made of the present water-based paint described in the above section [2. Water-based paint], or (b) a coating film made of the water-based paint produced by the present production method described in the above section [3. Method for producing water-based paint] is also one embodiment of the present invention. Hereinafter, the "coating film according to one embodiment of the present invention" may be referred to as the "present coating film".

[0208] This coating has the advantage that the loss tangent (tan δ) at seawater temperature is small.

[0209] The contact angle of the present coating film (for example, a coating film of the present water-based paint having a thickness of 100 μm) is not particularly limited, but is preferably greater than 90, more preferably 93 or more, more preferably 95 or more, more preferably 98 or more, even more preferably 100 or more, even more preferably 102 or more, and particularly preferably 104 or more. When the contact angle of the coating film is greater than 90, the coating film can be said to have excellent water repellency. A coating film having excellent water repellency can also have excellent antifouling properties. That is, when the contact angle of the present coating film is within the above-mentioned range, the coating film has the advantage of having excellent antifouling properties against aquatic organisms. The method for measuring the contact angle of the coating film will be described in detail in the examples below.

[0210] When the loss tangent (tan δ) of a coating film (e.g., a coating film having a thickness of 100 μm) is 0.60 or less at 25° C. or 0.20 or less at 0° C., the coating film can be said to have excellent antifouling properties. The lower the loss tangent (tan δ) of the coating film, the better the antifouling properties of the coating film. The loss tangent (tan δ) of this coating film (e.g., a coating film having a thickness of 100 μm made of this water-based paint) is preferably 0.60 or less at 25° C. (at a coating film at 25° C.), more preferably 0.50 or less, more preferably 0.40 or less, more preferably 0.30 or less, more preferably 0.20 or less, even more preferably 0.10 or less, and particularly preferably 0.05 or less. The loss tangent (tan δ) of the present coating film (for example, a 100 μm thick coating film made of the present water-based paint) at 0° C. (coating film at 0° C.) is preferably 0.20 or less, more preferably 0.18 or less, more preferably 0.16 or less, more preferably 0.14 or less, more preferably 0.12 or less, more preferably 0.10 or less, more preferably 0.08 or less, more preferably 0.06 or less, more preferably 0.04 or less, even more preferably 0.02 or less, and particularly preferably 0.01 or less.

[0211] [6.Applications] The water-based paint can be suitably used as an antifouling paint for preventing the surface or inner surface of various underwater structures from being fouled. Examples of underwater structures include ships, materials for aquaculture and fishing (e.g., ropes, fishing nets, fishing gear, floats, buoys, tetrapods, etc.), oil fences, water supply and drainage outlets of thermal or nuclear power plants, piping for cooling water pipes and seawater utilization equipment, undersea tunnels, undersea bases, megafloats, port facilities, various marine civil engineering works such as canals and waterways, industrial water facilities, bridges, buoys, etc. EXAMPLES

[0212] Hereinafter, one embodiment of the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited thereto. One embodiment of the present invention can be practiced with appropriate modifications within the scope of the above or below-mentioned purpose, and all of these modifications are included in the technical scope of the present invention. In the following examples and comparative examples, "parts" and "%" mean parts by weight or % by weight.

[0213] <Evaluation method> First, the evaluation methods for the graft copolymers, polymer (B) and water-based paints produced in the examples and comparative examples will be described below.

[0214] (Measurement of volume average particle size) The volume average particle size (Mv) of the polyorganosiloxane or graft copolymer dispersed in the aqueous latex was measured using Nanotrac WaveII-EX150 (manufactured by Microtrackbell Co., Ltd.). The aqueous latex was diluted with deionized water and used as the measurement sample. The measurement was performed by inputting the refractive index of water and the polyorganosiloxane or graft copolymer obtained in each production example, adjusting the sample concentration so that the measurement time was 120 seconds and the loading index was within the range of 1 to 10.

[0215] (Method of calculating glass transition temperature of graft portion) The Tg of the graft portion was calculated according to the above-mentioned FOX formula (Formula 1) using the Tg values ​​of homopolymers of the following monomers.

[0216] Methyl methacrylate (MMA) 105℃ Butyl methacrylate (BMA) 20℃ (Method for evaluating the film-forming properties of water-based paints) The film-forming properties of the water-based paints were evaluated by the following method: (1) Each water-based paint was applied to an aluminum plate with an applicator so that the film thickness after drying would be 100 μm; (2) The obtained aluminum plate was left to stand overnight at 25° C. to form a coating film of the water-based paint; (3) The state of the coated surface of the obtained aluminum plate was visually inspected, and the film-forming properties were evaluated according to the following criteria. 2 (Good): No cracks, 1 (Fault): Crack present.

[0217] (Method of measuring the contact angle of water-based paint coating and method of evaluating water repellency) The contact angle of the coating film of the water-based paint was measured by the following method: (1) an epoxy-based heavy-duty anticorrosive paint was applied to a glass plate; (2) the obtained glass plate was further coated with each water-based paint by an applicator so that the film thickness after drying was 100 μm; (3) the obtained glass plate was left at 25 ° C. overnight to prepare a coating film of the epoxy-based heavy-duty anticorrosive paint and the water-based paint; (4) the obtained glass plate was immersed in water and left at rest for one week; (5) after leaving it at rest, the contact angle of the coating film on the glass plate was measured by the sessile drop method based on JIS R 3257 using a contact angle meter (DropMaster, manufactured by Kyowa Interface Science Co., Ltd.). In the examples, when the contact angle of the coating film obtained by the above-mentioned method is greater than 90, the coating film is judged to have excellent water repellency.

[0218] (Method of measuring tan δ of water-based paint film) The tan δ of the coating film of the water-based paint was evaluated by the following method: (1) Each water-based paint was poured into a silicone mold so that the film thickness after drying was 0.3 mm; (2) The silicone mold containing the water-based paint was left to stand overnight at 25°C to prepare a coating film of the water-based paint; (3) The obtained coating film was subjected to dynamic viscoelasticity measurement under tensile conditions using a dynamic viscoelasticity measuring device (e.g., DVA-200, manufactured by IT Measurement and Control Co., Ltd.), and a graph of tan δ was obtained. From the obtained graph, the tan δ of each water-based paint at 0°C or 25°C was calculated.

[0219] Example 1 (Preparation of an aqueous latex containing a graft copolymer and polymer (B)) (Process 1) 251 parts by weight of deionized water, 0.5 parts by weight of SDS, and a mixture of monomers for forming polyorganosiloxane (a mixture consisting of 100 parts by weight of octamethylcyclotetrasiloxane and 2 parts by weight of γ-acryloyloxypropyldimethoxymethylsilane as monomer M) were mixed. The resulting mixture was stirred at 10,000 rpm for 5 minutes using a homomixer to prepare an emulsion. The resulting emulsion was poured into a five-neck glass container all at once. Here, the glass container had a thermometer, a stirrer, a reflux condenser, a nitrogen inlet, and an addition port for the monomer and emulsifier. While stirring the charged raw materials, (i) a 10% aqueous solution of dodecylbenzenesulfonic acid (DSA) was added to the glass container in an amount equivalent to 1 part by weight of the solid content in the aqueous solution, then (ii) the temperature in the glass container was raised to 80°C over about 40 minutes, and (iii) the mixture in the glass container was then reacted at 80°C for 6 hours. The temperature in the glass container was then cooled to 25°C, and after the temperature in the glass container reached 25°C, the reaction solution in the glass container was left for 20 hours. The polymerization was then terminated by adjusting the pH of the reaction solution to pH 6.8 using sodium hydroxide. By the above operations, an aqueous latex (R-1) containing polyorganosiloxane was obtained. The polymerization conversion rate of the monomer component was 97%. The volume average particle diameter of the polyorganosiloxane contained in the obtained aqueous latex (R-1) was 280 nm.

[0220] (Process 2) (Step 2a) Next, 275.5 parts by weight of the aqueous polyorganosiloxane latex (R-1) (containing 70 parts by weight of polyorganosiloxane) and 121 parts by weight of deionized water were added to the glass reactor. Here, the glass reactor had a thermometer, a stirrer, a reflux condenser, a nitrogen inlet, and a monomer addition device. The raw materials added at 60°C were stirred while the gas in the glass reactor was replaced with nitrogen. Next, 0.004 parts by weight of EDTA, 0.001 parts by weight of ferrous sulfate heptahydrate, and 0.13 parts by weight of SFS were added to the glass reactor and stirred for 10 minutes. Then, the monomer mixture for forming the first graft portion was continuously added to the glass reactor. Then, 0.013 parts by weight of BHP was added to the glass reactor, and the mixture in the glass reactor was stirred for another hour to complete the polymerization.

[0221] Next, the second graft monomer mixture was continuously added to the glass reactor, followed by adding 0.013 parts by weight of BHP to the glass reactor, and continuing to stir the mixture in the glass reactor for another hour to complete the polymerization.

[0222] As the "monomer mixture for forming the first graft portion", a mixture of compounds listed in the "first graft portion" column of Table 1 was used, and as the "monomer mixture for forming the second graft portion", a mixture of compounds listed in the "second graft portion" column of Table 1 was used. By the above operations, an aqueous latex (L-1) containing a graft copolymer (A) and a polymer (B) was obtained. The polymerization conversion rate of the monomer components was 97% or more. The volume average particle diameter of the graft copolymer (A) contained in the obtained aqueous latex (L-1) was 293 nm.

[0223] 61.85 parts by weight of the obtained water-based latex, 7 parts by weight of deionized water, 1.5 parts by weight of CS-12 (manufactured by JNC) and 3 parts by weight of Dowanol DPnB (manufactured by Dow Chemical Japan) as a film-forming aid, 1.2 parts by weight of SN Thickener 612NC (manufactured by San Nopco) as a thickener, 0.15 parts by weight of BYK-333 (manufactured by BYK Japan) as a leveling agent, and 0.3 parts by weight of Agitan 295 (manufactured by MUNZING CHEMIE) as an antifoaming agent were mixed to obtain a water-based paint. The obtained water-based paint was evaluated for film-forming properties, and the contact angle was measured to evaluate the water repellency. In addition, a coating film was prepared using the obtained water-based paint by the above-mentioned method, and the tan δ of the coating film at 0 ° C. and 25 ° C. was measured. The results are shown in Table 1.

[0224] (Examples 2 to 11) Except for changing the "monomer mixture for forming the first graft portion" used to a mixture of compounds listed in the "first graft portion" column of Table 1, and changing the "monomer mixture for forming the second graft portion" used to a mixture of compounds listed in the "second graft portion" column of Table 1, an aqueous latex containing a graft copolymer (A) and a polymer (B) was obtained by the same method as in Example 1. Using the aqueous latex obtained in each example, an aqueous paint was obtained by the same method as in Example 1. The film-forming property of the obtained aqueous paint was evaluated, and the contact angle was measured to evaluate the water repellency. In addition, a coating film was prepared by the above-mentioned method using the obtained aqueous paint, and the tan δ of the coating film at 0 ° C. and 25 ° C. was measured. The results are shown in Table 1.

[0225] Comparative Example 1 (Preparation of an aqueous latex containing a graft copolymer and polymer (B)) (Process 1) 251 parts by weight of deionized water, 0.5 parts by weight of SDS, and a mixture of monomers for forming polyorganosiloxane (a mixture consisting of 100 parts by weight of octamethylcyclotetrasiloxane and 2 parts by weight of γ-acryloyloxypropyldimethoxymethylsilane as monomer M) were mixed. The resulting mixture was stirred at 10,000 rpm for 5 minutes using a homomixer to prepare an emulsion. The resulting emulsion was poured into a five-neck glass container all at once. Here, the glass container had a thermometer, a stirrer, a reflux condenser, a nitrogen inlet, and an addition port for the monomer and emulsifier. While stirring the charged raw materials, (i) a 10% aqueous solution of dodecylbenzenesulfonic acid (DSA) was added to the glass container in an amount equivalent to 1 part by weight of the solid content in the aqueous solution, then (ii) the temperature in the glass container was raised to 80°C over about 40 minutes, and (iii) the mixture in the glass container was then reacted at 80°C for 6 hours. The temperature in the glass container was then cooled to 25°C, and after the temperature in the glass container reached 25°C, the reaction solution in the glass container was left for 20 hours. The polymerization was then terminated by adjusting the pH of the reaction solution to pH 6.8 using sodium hydroxide. By the above operations, an aqueous latex (R-1) containing polyorganosiloxane was obtained. The polymerization conversion rate of the monomer component was 97%. The volume average particle diameter of the polyorganosiloxane contained in the obtained aqueous latex (R-1) was 280 nm.

[0226] (Process 2) Next, 275.5 parts by weight of the aqueous polyorganosiloxane latex (R-1) (containing 70 parts by weight of polyorganosiloxane) and 121 parts by weight of deionized water were added to the glass reactor. Here, the glass reactor had a thermometer, a stirrer, a reflux condenser, a nitrogen inlet, and a monomer addition device. The raw materials added were stirred at 60°C while the gas in the glass reactor was replaced with nitrogen. Next, 0.004 parts by weight of EDTA, 0.001 parts by weight of ferrous sulfate heptahydrate, and 0.13 parts by weight of SFS were added to the glass reactor and stirred for 10 minutes. Then, a mixture of monomers for forming a graft portion (a mixture consisting of 28.5 parts by weight of BMA, 1 part by weight of an ether sulfate type anionic surfactant (having an allyloxy group) (ADEKA, Adeka Reasoap SR1025) as a reactive emulsifier, and 1.5 parts by weight of 3-methacryloxypropylmethyldimethoxysilane as a monomer M), 0.24 parts by weight of t-dodecyl mercaptan as a chain transfer agent, and 0.085 parts by weight of BHP was continuously added to the glass reactor over a period of 120 minutes. Then, 0.013 parts by weight of BHP was added to the glass reactor, and the mixture in the glass reactor was stirred for another hour to complete the polymerization. By the above operations, an aqueous latex (CL-1) containing a graft copolymer and a polymer (B) was obtained. The polymerization conversion rate of the monomer components was 97% or more. The volume average particle diameter of the graft copolymer (A) contained in the obtained aqueous latex (CL-1) was 293 nm.

[0227] The obtained water-based latex was used to obtain a water-based paint in the same manner as in Example 1. The obtained water-based paint was evaluated for film-forming property and the contact angle was measured to evaluate the water repellency. In addition, the obtained water-based paint was used to prepare a coating film in the above-mentioned manner, and the tan δ of the coating film at 0°C and 25°C was measured. The results are shown in Table 1.

[0228] Comparative Example 2 An aqueous latex containing a graft copolymer and a polymer (B) was obtained by the same method as in Comparative Example 1, except that the "monomer mixture for forming a graft portion" used was changed to a mixture of compounds listed in the "first graft portion" column of Table 1. A water-based paint was obtained by the same method as in Example 1 using the obtained aqueous latex. The film-forming property of the obtained water-based paint was evaluated, and the contact angle was measured to evaluate the water repellency. In addition, a coating film was prepared by the above-mentioned method using the obtained water-based paint, and the tan δ of the coating film at 0°C and 25°C was measured. The results are shown in Table 1.

[0229] In all the examples and comparative examples, an ether sulfate type anionic surfactant (having an allyloxy group) (ADEKA Corporation, Adeka Reasoap SR1025) was used as the reactive emulsifier, 3-methacryloxypropylmethyldimethoxysilane was used as the monomer M1, and t-dodecyl mercaptan was used as the chain transfer agent. In addition, in all the examples and comparative examples, after preparing the graft copolymer, the water-based paint was obtained without removing the non-grafted polymer that may have been generated during the preparation of the graft portion from the obtained aqueous latex. In addition, in all the examples and comparative examples, the core portion of the graft copolymer (A) was composed only of polyorganosiloxane. In other words, the volume average particle diameter of the polyorganosiloxane contained in the aqueous latex (R-1) can be said to be the volume average particle diameter of the core portion.

[0230] [Table 1] [Industrial Applicability]

[0231] According to one embodiment of the present invention, a water-based paint having excellent film-forming properties and capable of providing a coating film having excellent water repellency can be provided. In addition, the water-based paint according to one embodiment of the present invention can provide a coating film having a small loss tangent (tan δ) at seawater temperature. Therefore, the water-based paint according to one embodiment of the present invention and a coating film made of the water-based paint can be suitably used for ships, materials for aquaculture and fishing, oil fences, water supply and drainage outlets of thermal or nuclear power plants, piping for cooling water pipes and seawater utilization equipment, various marine civil engineering works such as undersea tunnels, undersea bases, megafloats, port facilities, canals and waterways, industrial water system facilities, bridges, buoys, and other underwater structures.

Claims

1. Contains a graft copolymer (A), The graft copolymer (A) includes a polyorganosiloxane and a graft portion graft-bonded to the polyorganosiloxane, The polyorganosiloxane comprises (a) a structural unit U derived from a monomer containing (a-1) one or more hydrolyzable silyl groups and (a-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule. 1 and (b) is non-crosslinked; the graft portion includes a first graft portion and a second graft portion; The first graft portion is a structural unit U derived from a monomer containing (a-1) one or more hydrolyzable silyl groups and (a-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule. 2 and (b) does not contain any structural units derived from a chain transfer agent; The second graft portion includes (a) a structural unit derived from a chain transfer agent, and (b) a structural unit U derived from a monomer containing (b-1) one or more hydrolyzable silyl groups and (b-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule. 3 Contains no water-based paint.

2. The graft portion is composed of 100% by weight of the structural unit U 2 The water-based paint according to claim 1, comprising 7.0% by weight to 20.0% by weight of

3. 3. The water-based paint according to claim 1, wherein the glass transition temperature of the graft portion is 25° C. or higher.

4. The polyorganosiloxane contains the structural unit U 1 The water-based paint according to claim 1 or 2, comprising 0.001% by weight to 10.0% by weight of the above.

5. The water-based paint according to claim 1 or 2, wherein the graft portion further comprises a structural unit derived from a reactive emulsifier.

6. The water-based paint according to claim 5, wherein the graft portion contains 0.1% by weight to 20.0% by weight of a constituent unit derived from the reactive emulsifier, based on 100% by weight of the graft portion.

7. The water-based paint according to claim 1 or 2, wherein the volume average particle diameter of the polyorganosiloxane is 0.03 μm to 50.00 μm.

8. 2. The water-based paint according to claim 1, wherein the polyorganosiloxane is 55% by weight to 90% by weight in 100% by weight of the graft copolymer (A).

9. The water-based coating material further contains a polymer (B), The water-based paint according to claim 1 or 2, wherein the polymer (B) contains a structural unit derived from one or more monomers selected from the group consisting of an aromatic vinyl monomer, a vinyl cyan monomer, and a (meth)acrylate monomer.

10. The water-based paint according to claim 1 or 2, further comprising an antifouling agent.

11. The water-based paint according to claim 9, wherein the polymer (B) accounts for 5.0% by weight or more of the total of the graft copolymer (A) and the polymer (B) being 100% by weight.

12. A method for producing a water-based coating film, comprising a step of applying the water-based coating material according to claim 1 or 2 to an underwater structure.

13. (a) an organosiloxane, and (b) a monomer M containing (b-1) one or more hydrolyzable silyl groups and (b-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule; 1 Step 1 of polymerizing a monomer mixture for forming a polyorganosiloxane, comprising the steps of: obtaining a polyorganosiloxane; Step 2 of polymerizing the graft portion-forming monomer mixture in the presence of the polyorganosiloxane obtained in step 1; In the step 1, the total amount of the polyfunctional alkoxysilane compound and the polyfunctional monomer is 0.50% by weight or less in 100% by weight of the monomer mixture for forming the polyorganosiloxane, The step 2 includes a step 2a of polymerizing a first graft portion-forming monomer mixture and a step 2b of polymerizing a second graft portion-forming monomer mixture, In the step 2a, the first graft portion-forming monomer mixture is a monomer mixture containing (a) (a-1) a monomer M derived from a monomer containing one or more hydrolyzable silyl groups and (a-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule. 2 and (b) does not contain a chain transfer agent; In the step 2b, the monomer mixture for forming the second graft portion contains (a) a chain transfer agent and (b) a monomer M containing (b-1) one or more hydrolyzable silyl groups and (b-2) one or more ethylenically unsaturated groups and / or mercapto groups in the molecule. 3 A method for producing water-based paints that does not contain

Citation Information

Patent Citations

  • Water-based antifouling coating composition

    JP2007191531A

  • Aqueous coating material

    JP2008260883A

  • Preparation method of polymer emulsion and water-based coating material

    JP2010059267A

Cited By

  • Water-based paint

    CN122563425A

  • Water-based coatings

    JP2026137075A

  • JPWO2021200647A1