Gas separation membrane

The gas separation membrane with a porous and separation layer configuration addresses the trade-off in existing membranes by enhancing mechanical strength and selectivity for carbon dioxide separation with reduced energy consumption.

JP2024170941APending Publication Date: 2024-12-11SEIKO EPSON CORP

Patent Information

Application Number
JP2023087719
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-12-11

AI Technical Summary

Technical Problem

Existing gas selectively permeable membranes require large differential pressures for separation, leading to high energy consumption, and face a trade-off between permeability and separation performance.

Method used

A gas separation membrane with a porous layer and a separation layer, where the porous layer has a specific thickness and pore diameter ratio, and the separation layer is made of organopolysiloxane, ensuring both mechanical strength and selective permeability for carbon dioxide.

Benefits of technology

The membrane achieves efficient carbon dioxide separation with reduced energy consumption and improved mechanical properties, allowing for both high selectivity and permeability while maintaining durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024170941000001_ABST
    Figure 2024170941000001_ABST
Patent Text Reader

Abstract

To provide a gas separation membrane that is excellent in mechanical characteristics and can achieve both a gas selectivity ratio for carbon dioxide and gas permeability for carbon dioxide.SOLUTION: A gas separation membrane for separating carbon dioxide from mixed gas containing the carbon dioxide and a non-target component includes: a porous layer; and a separation layer formed of a polymer material and in close contact with one surface of the porous layer. In the gas separation membrane, t is 5 nm or more and 500 nm or less, a ratio d / t is more than 2.0 and 100 or less, and a ratio T / t is 100 or more and 10000 or less, where t is an average thickness of the separation layer, d is an average hole diameter of the porous layer, and T is an average thickness of the porous layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to gas separation membranes. [Background technology]

[0002] To achieve carbon neutral or carbon negative, technologies are being considered for capturing and capturing carbon dioxide emitted from thermal power plants, boiler facilities, etc., and carbon dioxide in the atmosphere. One known technology for this purpose is the membrane separation method, which separates carbon dioxide using a gas separation membrane.

[0003] For example, Patent Document 1 discloses a gas selective permeable membrane that selectively allows a specific gas to pass through. This gas selective permeable membrane is manufactured through a process of laminating a thin film of a siloxane compound on a film-shaped polymeric porous support, subjecting the surface layer of the thin film to plasma treatment with a non-polymerizable gas, and depositing a plasma polymerized membrane on the thin film. It is also disclosed that these processes result in a gas selective permeable membrane with strong adhesion between the thin film and the plasma polymerized membrane, and that the thickness of the thin film is 1 μm to 30 μm. It is also disclosed that this gas selective permeable membrane is used to selectively allow gases such as oxygen, hydrogen, and helium to pass through, and the separated gas is collected. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 60-75320 Summary of the Invention [Problem to be solved by the invention]

[0005] The gas selective permeable membrane described in Patent Document 1 requires a large pressure difference to allow a specific component to pass through. This poses the problem of a large amount of energy consumption in separating the components. Another problem is that increasing the permeability of a specific component reduces the separation performance of that component, and conversely, increasing the separation performance of a specific component reduces the permeability of that component.

[0006] Therefore, there is a demand for realizing a gas separation membrane that is excellent in mechanical properties and can achieve both a high gas selectivity for carbon dioxide and a high gas permeability for carbon dioxide. [Means for solving the problem]

[0007] The gas separation membrane according to the application example of the present invention is A porous layer; a separation layer made of a polymer material and in close contact with one surface of the porous layer; A gas separation membrane for separating carbon dioxide from a mixed gas containing carbon dioxide and a non-target component, The average thickness of the separation layer is t, The average pore diameter of the porous layer is d, When the average thickness of the porous layer is T, t is 5 nm or more and 500 nm or less, The ratio d / t is more than 2.0 and 100 or less, The ratio T / t is 100 or more and 10,000 or less. [Brief description of the drawings]

[0008] [Figure 1] 1 is a cross-sectional view illustrating a gas separation membrane according to an embodiment. [Diagram 2] FIG. 11 is a cross-sectional view that illustrates a gas separation membrane according to a modified example of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, the gas separation membrane of the present invention will be described in detail based on the embodiments shown in the accompanying drawings. 1. Gas separation membrane First, the configuration of the gas separation membrane according to the embodiment will be described.

[0010] FIG. 1 is a cross-sectional view that illustrates a gas separation membrane 1 according to an embodiment. The gas separation membrane 1 shown in Fig. 1 has the function of selectively allowing carbon dioxide to permeate from a mixed gas containing carbon dioxide and non-target components. The gas separation membrane 1 shown in Fig. 1 has a porous layer 2 and a separation layer 3. The non-target components refer to gas components other than carbon dioxide that are contained in the mixed gas.

[0011] The porous layer 2 is a porous membrane having pores 23 as shown in Fig. 1. Such a porous layer 2 has good gas permeability and supports the separation layer 3. This makes it possible to improve the mechanical properties of the entire gas separation membrane 1 without impairing the good gas selectivity of the separation layer 3.

[0012] The separation layer 3 is provided on one surface of the porous layer 2, and is made of a polymer material that is denser (has a lower porosity) than the porous layer 2. Such a separation layer 3 blocks the upper ends of the pores 23. The separation layer 3 has a good gas selectivity ratio that selectively allows carbon dioxide in the mixed gas supplied to the upstream side of the gas separation membrane 1 to permeate to the downstream side. This enables the gas separation membrane 1 to separate carbon dioxide in the mixed gas. In the following description, the upper side of the gas separation membrane 1 shown in FIG. 1 will be referred to as the "upstream side" or simply "top", and the lower side will be referred to as the "downstream side" or simply "bottom".

[0013] The non-target components include, for example, nitrogen, methane, etc., and in particular, nitrogen. Therefore, the above-mentioned mixed gas includes a mixed gas of carbon dioxide and nitrogen.

[0014] 1.1.Porous layer As described above, the porous layer 2 is a porous membrane having pores 23, and has good gas permeability. In addition, the porous layer 2 has higher rigidity than the separation layer 3, and ensures the self-supporting property and durability of the gas separation membrane 1 as a whole.

[0015] Examples of materials for the porous layer 2 include polymeric materials, ceramic materials, and metal materials. These materials have high rigidity and are therefore particularly useful in terms of improving the mechanical properties of the gas separation membrane 1. The material for the porous layer 2 may also be a composite material of these materials and other materials.

[0016] Examples of polymeric materials include polyolefin resins such as polyethylene and polypropylene, fluorine-containing resins such as polytetrafluoroethylene, polyvinyl fluoride and polyvinylidene fluoride, polystyrene, cellulose, cellulose acetate, polyurethane, polyacrylonitrile, polyphenylene oxide, polysulfone, polyethersulfone, polyimide, polyaramid, nylon, and the like.

[0017] Examples of the ceramic material include alumina, cordierite, mullite, silicon carbide, zirconia, etc. Examples of the metal material include stainless steel, etc.

[0018] Among these, a ceramic material is preferably used as the constituent material of the porous layer 2. A ceramic material has high rigidity and, being a sintered material, contains continuous pores. For this reason, by using a ceramic material as the constituent material of the porous layer 2, a gas separation membrane 1 having excellent mechanical properties and high gas permeability to carbon dioxide can be obtained.

[0019] The shape of the porous layer 2 may be a flat plate as shown in FIG. 1, or may be a spiral, tubular, hollow fiber, or other shape.

[0020] The average thickness T of the porous layer 2 is not particularly limited, but is preferably 10 μm or more and 500 μm or less, more preferably 20 μm or more and 300 μm or less, and even more preferably 30 μm or more and 200 μm or less. This allows the porous layer 2 to have a necessary and sufficient rigidity to support the gas separation membrane 1. If the average thickness T of the porous layer 2 is below the lower limit, the rigidity may be insufficient. On the other hand, if the average thickness T of the porous layer 2 is above the upper limit, the rigidity of the porous layer 2 may be too high, which may reduce the handleability of the gas separation membrane 1 or reduce the adhesion of the separation layer 3.

[0021] The average thickness T of the porous layer 2 is an average value of thicknesses in the stacking direction measured at 10 points of the porous layer 2. The thickness of the porous layer 2 can be measured using, for example, a thickness gauge.

[0022] The porous layer 2 has pores 23, and the average inner diameter of the pores is called the "average pore diameter d". The average pore diameter d of the porous layer 2 is preferably 5 nm or more and 1000 nm or less, more preferably 10 nm or more and 800 nm or less, even more preferably 50 nm or more and 400 nm or less, and particularly preferably 100 nm or more and 300 nm or less. This makes it possible to sufficiently ensure the gas permeability of carbon dioxide in the porous layer 2 while suppressing the separation layer 3 from escaping to the downstream side of the porous layer 2. If the average pore diameter d of the porous layer 2 is below the lower limit, the gas permeability of carbon dioxide in the porous layer 2 may decrease. On the other hand, if the average pore diameter d of the porous layer 2 is above the upper limit, the separation layer 3 may escaping to the downstream side of the porous layer 2.

[0023] The average pore diameter d of the porous layer 2 is measured by a through-pore diameter evaluation device after removing the separation layer 3 from the gas separation membrane 1 to obtain the single porous layer 2. An example of the through-pore diameter evaluation device is a Perm Porometer manufactured by PMI.

[0024] The porosity of the porous layer 2 is preferably 20% or more and 90% or less, and more preferably 30% or more and 80% or less, so that the porous layer 2 can have both good gas permeability and sufficient rigidity.

[0025] The porosity of the porous layer 2 is measured after removing the separation layer 3 from the gas separation membrane 1 using the through-pore diameter evaluation device described above.

[0026] 1.2. Separation layer The separation layer 3 is formed on the upstream surface of the porous layer 2. Therefore, the separation layer 3 is substantially a dense membrane and has good affinity with carbon dioxide molecules. Due to this affinity, the separation layer 3 selectively allows carbon dioxide to permeate.

[0027] The constituent material of the separation layer 3 is a polymeric material. Examples of the polymeric material include polyolefin resins such as polyethylene and polypropylene, fluorine-containing resins such as polytetrafluoroethylene, polyvinyl fluoride and polyvinylidene fluoride, polystyrene, cellulose, cellulose acetate, polyurethane, polyacrylonitrile, polyphenylene oxide, polysulfone, polyethersulfone, polyimide, polyaramid, organopolysiloxane, polyethylene terephthalate (PET), polyacetal (POM), polylactic acid (PLA), etc. The constituent material of the separation layer 3 may be one or a composite material of two or more of these polymeric materials.

[0028] Among these, organopolysiloxane is preferably used as the constituent material of the separation layer 3. One molecule of organopolysiloxane has the following basic constituent units: 1 SiO 3 / 2 Units expressed in (T units), R 2 R 3 SiO 2 / 2 Units expressed by (D units) and R 4 R 5 R 6 SiO 1 / 2 Each unit contains at least the unit (M unit) represented by R 1 ~R6 is an aliphatic hydrocarbon or a hydrogen atom. One molecule of organopolysiloxane is composed of a combination of these T units, D units and M units.

[0029] Specific examples of organopolysiloxane include polydimethylsiloxane, polymethylphenylsiloxane, polydiphenylsiloxane, polysulfone / polyhydroxystyrene / polydimethylsiloxane copolymer, dimethylsiloxane / methylvinylsiloxane copolymer, dimethylsiloxane / diphenylsiloxane / methylvinylsiloxane copolymer, methyl-3,3,3-trifluoropropylsiloxane / methylvinylsiloxane copolymer, dimethylsiloxane / methylphenylsiloxane / methylvinylsiloxane copolymer, diphenylsiloxane / dimethylsiloxane copolymer terminal vinyl, polydimethylsiloxane terminal vinyl, polydimethylsiloxane terminal amino, polydimethylsiloxane terminal phenyl, polydimethylsiloxane terminal H, dimethylsiloxane-methylhydrosiloxane copolymer, etc. The notation "terminal vinyl" indicates that at least one end of the main chain contained in the organopolysiloxane is substituted with a substituent such as a vinyl group. These also include those in which a crosslinked product is formed. The constituent material of the separation layer 3 may be a composite of one or more of these materials, or a composite material in which, by mass ratio, organopolysiloxane is the main component in combination with other resin components.

[0030] In addition, organopolysiloxane has a good affinity for carbon dioxide, so that the gas separation membrane 1 having the separation layer 3 containing organopolysiloxane exhibits a high gas selectivity ratio for carbon dioxide.

[0031] The average thickness t of the separation layer 3 is 5 nm or more and 500 nm or less. If the average thickness t is within the above range, the separation layer 3 is unlikely to have defects, and therefore has sufficient gas permeability while ensuring a good gas selectivity ratio. As a result, a gas separation membrane 1 can be realized that has good carbon dioxide selectivity and can reduce the amount of energy input required for separation, specifically, can reduce the pressure difference between the upstream and downstream sides of the gas separation membrane 1. If the average thickness t of the separation layer 3 is below the lower limit, the probability of defects occurring in the separation layer 3 increases, or the separation layer 3 becomes more susceptible to subsequent damage. On the other hand, if the average thickness t of the separation layer 3 exceeds the upper limit, the gas permeability of carbon dioxide in the separation layer 3 decreases, increasing the amount of energy input required for separation, or reducing the flexibility of the separation layer 3.

[0032] The average thickness t of the separation layer 3 is preferably 7 nm or more and 300 nm or less, and more preferably 10 nm or more and 100 nm or less.

[0033] The average thickness t of the separation layer 3 is determined, for example, by observing the cross section of the gas separation membrane 1 at a magnification and averaging the thicknesses at 10 points. For example, a scanning electron microscope or a transmission electron microscope is used for the magnification observation.

[0034] Furthermore, an arbitrary intermediate layer may be interposed between the separation layer 3 and the porous layer 2. The intermediate layer may have, for example, a function of increasing the adhesion between the separation layer 3 and the porous layer 2, a function of preventing the separation layer 3 from penetrating into the pores 23, etc.

[0035] If necessary, any functional group may be introduced using a coupling agent or the like on the upstream surface of the separation layer 3. By appropriately selecting the functional group, it is possible to further increase the affinity for carbon dioxide.

[0036] The separation layer 3 may be a functionally gradient layer configured such that the composition or structure changes along the thickness direction. In the functionally gradient layer, the function can be changed, for example, so that the affinity with carbon dioxide is increased on the upstream side of the separation layer 3 and the permeability to carbon dioxide is increased on the downstream side. This makes it possible to particularly increase both the gas selectivity and gas permeability of carbon dioxide.

[0037] 1.3. Ratio d / t of average pore diameter d of porous layer 2 to average thickness t of separation layer 3 In the gas separation membrane 1, the ratio d / t of the average pore diameter d of the porous layer 2 to the average thickness t of the separation layer 3 is more than 2.0 and not more than 100. If the ratio d / t is within the above range, both the carbon dioxide gas selectivity and the carbon dioxide gas permeability of the gas separation membrane 1 can be increased. If the ratio d / t is below the lower limit, the average pore diameter d becomes too small and the gas permeability of the porous layer 2 decreases, so that the carbon dioxide gas permeability of the gas separation membrane 1 decreases. On the other hand, if the ratio d / t exceeds the upper limit, the average pore diameter d becomes too large and the separation layer 3 enters the pores 23, making it difficult to form a uniform separation layer 3. If this happens, the coverage rate of the porous layer 2 by the separation layer 3 decreases, and the carbon dioxide gas selectivity of the gas separation membrane 1 decreases. The ratio d / t is preferably 2.5 or more and 80 or less, more preferably 3.0 or more and 50 or less, and further preferably 5.0 or more and 30 or less.

[0038] 1.4. Ratio of average thickness T of porous layer 2 to average thickness t of separation layer 3, T / t In the gas separation membrane 1, the ratio T / t of the average thickness T of the porous layer 2 to the average thickness t of the separation layer 3 is 100 or more and 10,000 or less. If the ratio T / t is within the above range, both the gas selectivity ratio of carbon dioxide and the gas permeability of carbon dioxide are increased, and the gas separation membrane 1 having excellent mechanical properties is obtained. If the ratio T / t is below the lower limit, the average thickness T of the porous layer 2 becomes too thin and the mechanical properties are reduced, for example, the self-supporting property of the gas separation membrane 1 is impaired. If the self-supporting property is impaired, the handling property of the gas separation membrane 1 is reduced. On the other hand, if the ratio T / t exceeds the upper limit, the average thickness T of the porous layer 2 becomes too thick and the difference with the average thickness t of the separation layer 3 becomes large, so that the tracking property of the porous layer 2 is reduced when the gas separation membrane 1 is deformed. If this happens, the separation layer 3 may peel off or be damaged.

[0039] The ratio T / t is preferably 1,000 or more and 9,000 or less, more preferably 2,000 or more and 8,000 or less, and further preferably 3,000 or more and 7,000 or less.

[0040] 2. Gas separation membrane manufacturing method Next, a method for producing the gas separation membrane 1 shown in FIG. 1 will be described.

[0041] First, the separation layer 3 is formed on one surface of the porous layer 2. Examples of the method for forming the separation layer 3 include a sol-gel method, a coating method, a plasma CVD method, a plasma polymerization method, and an ALD (Atomic Layer Deposition) method. Among these, examples of the coating method include a dipping method, a dropping method, an inkjet method, a dispenser method, a spray method, a screen printing method, a coater coating method, and a spin coating method.

[0042] Among these, when the constituent material of the separation layer 3 is organopolysiloxane, the plasma polymerization method is preferably used. According to the plasma polymerization method, the organopolysiloxane can be deposited while cleaning and activating the porous layer 2. As a result, the separation layer 3 formed is more firmly adhered to the porous layer 2. In addition, since the plasma polymerization method is a type of vapor phase film formation method, a part of the deposited molecules also adheres to the inner wall of the pores 23 of the porous layer 2. This can further increase the adhesion of the separation layer 3. Furthermore, since the film formed by the plasma polymerization method (plasma polymerized film) is densified, a separation layer 3 with fewer through holes (defects) can be formed. In addition, in the case of the plasma polymerization method, the average thickness t can be controlled by adjusting the film formation time, for example.

[0043] Examples of the raw material gas used in the plasma polymerization method include organosiloxanes such as methylsiloxane, octamethyltrisiloxane, decamethyltetrasiloxane, decamethylcyclopentasiloxane, octamethylcyclotetrasiloxane, and methylphenylsiloxane.

[0044] The pressure in the chamber used for plasma polymerization is 133.3×10 -5 Pa or more and 1333Pa or less (1×10 -5 Torr or more and 10 Torr or less) is preferable.

[0045] The temperature of the porous layer 2 subjected to the plasma polymerization method is preferably about 25° C. or more and 100° C. or less, and the film formation time is preferably about 1 minute or more and 10 minutes or less.

[0046] Furthermore, when the constituent material of the separation layer 3 is organopolysiloxane, the separation layer 3 can also be formed by the following coating method. In the coating method, for example, a resin solution obtained by mixing organopolysiloxane before a curing reaction with a solvent is used. This resin solution is applied to one side of the porous layer 2 and then cured. In this way, the separation layer 3 is obtained.

[0047] 3. Variations Next, a gas separation membrane 1 according to a modified example of the embodiment will be described. FIG. 2 is a cross-sectional view that illustrates a gas separation membrane 1 according to a modified example of the embodiment.

[0048] The following describes a modification of the embodiment, but in the following description, the differences from the above embodiment will be mainly described, and the description of the similar items will be omitted. Note that in Fig. 2, the same items as in Fig. 1 are denoted by the same reference numerals.

[0049] The gas separation membrane 1 shown in FIG. 2 is similar to the gas separation membrane 1 shown in FIG.

[0050] Since the intermediate layer 4 is formed on the upstream surface of the porous layer 2, it inherits the porosity of the porous layer 2 and has pores 43. Therefore, the intermediate layer 4 obtains a strong adhesive force through the adhesion between the porous layer 2 and the separation layer 3, and has good gas permeability without blocking the pores 23 of the porous layer 2.

[0051] The intermediate layer 4 is made of an organopolysiloxane. The organopolysiloxane used may be the same as or different from the material used for the separation layer 3.

[0052] The intermediate layer 4 is chemically bonded to the separation layer 3. Examples of chemical bonds include hydrogen bonds and covalent bonds, with covalent bonds being particularly preferred. This allows the separation layer 3 to adhere more firmly to the porous layer 2 via the intermediate layer 4. As a result, the gas separation membrane 1 has particularly good mechanical properties.

[0053] Such good mechanical properties allow for flexibility in the shape of the gas separation membrane 1 during use. For example, the gas separation membrane 1 may be used in a curved or folded state. If the gas separation membrane 1 is used in such a state, peeling may occur between the porous layer 2 and the separation layer 3 if the adhesion strength is low.

[0054] In contrast, by interposing the intermediate layer 4, the adhesion strength can be increased and the occurrence of peeling can be suppressed. As a result, the gas separation membrane 1 is less likely to break even when used in a curved or folded state. In a folded state, for example, the surface area of ​​the gas separation membrane 1 can be increased without increasing the area of ​​the module using the gas separation membrane 1. Therefore, the module using the gas separation membrane 1 can be made highly dense.

[0055] The average thickness of the intermediate layer 4 is not particularly limited, but is preferably 1000 nm or less, more preferably 3 nm or more and 500 nm or less, and even more preferably 5 nm or more and 300 nm or less. This allows the intermediate layer 4 to have sufficient adhesion. In addition, the intermediate layer 4 does not become too thick and has pores 43, so that the intermediate layer 4 has good gas permeability like the porous layer 2.

[0056] The sum of the average thickness of the separation layer 3 and the average thickness of the intermediate layer 4 is preferably 1500 nm or less, more preferably 50 nm or more and 500 nm or less, and even more preferably 100 nm or more and 400 nm or less. This allows the separation layer 3 to adhere strongly to the porous layer 2 via the intermediate layer 4, and makes it difficult for the intermediate layer 4 to inhibit the good gas permeability of the porous layer 2.

[0057] The average thickness of the intermediate layer 4 may be equal to or greater than the average thickness of the separation layer 3, but is preferably set to be thinner than the separation layer 3. In this case, the difference between the average thickness of the separation layer 3 and the average thickness of the intermediate layer 4 is preferably greater than 0 nm and equal to or less than 300 nm, more preferably equal to or greater than 10 nm and equal to or less than 150 nm, and even more preferably equal to or greater than 15 nm and equal to or less than 100 nm. This provides a good balance between the thicknesses of the separation layer 3 and the intermediate layer 4, making it difficult for peeling to occur due to an excessive difference in film thickness, and allowing the separation layer 3 and the intermediate layer 4 to perform their respective functions well. This difference is the average thickness of the separation layer 3 minus the average thickness of the intermediate layer 4.

[0058] Next, a method for producing a gas separation membrane according to a modified embodiment will be described. First, a film of organopolysiloxane is formed on one surface of the porous layer 2. In this way, the intermediate layer 4 is obtained.

[0059] Examples of methods for forming a film of organopolysiloxane include the sol-gel method, coating method, plasma CVD method, plasma polymerization method, and ALD (Atomic Layer Deposition) method. Among these, the plasma polymerization method is preferably used. According to the plasma polymerization method, the organopolysiloxane can be deposited while cleaning and activating the porous layer 2. As a result, the intermediate layer 4 formed is more firmly adhered to the porous layer 2. In addition, since the plasma polymerization method is a type of vapor phase film formation method, a part of the deposited molecules also adheres to the inner walls of the pores 23 of the porous layer 2. This can further increase the adhesion of the intermediate layer 4. Furthermore, since the film formed by the plasma polymerization method (plasma polymerized film) is densified, the intermediate layer 4 can more firmly fix the separation layer 3 to the porous layer 2.

[0060] Examples of the raw material gas used in the plasma polymerization method include organosiloxanes such as methylsiloxane, octamethyltrisiloxane, decamethyltetrasiloxane, decamethylcyclopentasiloxane, octamethylcyclotetrasiloxane, and methylphenylsiloxane.

[0061] The pressure in the chamber used for plasma polymerization is 133.3×10 -5 Pa or more and 1333Pa or less (1×10 -5 Torr or more and 10 Torr or less) is preferable.

[0062] The temperature of the porous layer 2 subjected to the plasma polymerization method is preferably about 25° C. or more and 100° C. or less, and the film formation time is preferably about 1 minute or more and 10 minutes or less.

[0063] Next, a sheet to be a sacrificial layer is prepared, and on the surface thereof, a separation layer 3 is formed. The method for forming the separation layer 3 is as described above.

[0064] Examples of the material for the sacrificial layer include materials that dissolve in a solvent. Examples of the material for the sacrificial layer include water-soluble resins such as polyvinyl alcohol, polyethylene oxide, and gelatin, and acrylic resins. Among these, water-soluble resins are suitable as the material for the sacrificial layer because they are easily dissolved in water-based solvents.

[0065] Next, the intermediate layer 4 is subjected to an activation treatment. Examples of the activation treatment include a method of irradiating the intermediate layer 4 with energy rays, a method of heating the intermediate layer 4, a method of exposing the intermediate layer 4 to plasma or corona, and a method of exposing the intermediate layer 4 to ozone gas. Examples of the energy rays include infrared rays, ultraviolet rays, and visible light. When the activation treatment is performed, a part of the organic groups of the organopolysiloxane constituting the intermediate layer 4 is eliminated. After the elimination of the organic groups, H atoms or moisture are adsorbed to the dangling bonds to generate active species. Examples of the active species include Si-H groups and Si-OH groups. The activation treatment may be performed as necessary, and may be omitted if sufficient active species are present. In addition, the activation treatment can clean the intermediate layer 4, which can contribute to further improving the bonding strength.

[0066] Similarly, the activation treatment is also performed on the separation layer 3. As a result, active species are generated in the separation layer 3. This activation treatment may also be performed as necessary, and may be omitted if sufficient active species are present.

[0067] Next, the surfaces of the separation layer 3 and the intermediate layer 4 that have been subjected to the activation treatment are brought into contact with each other. Then, in this state, they are pressurized. As a result, the surfaces that have been subjected to the activation treatment are bonded to each other. This bonding is based on chemical bonding. Specifically, when the surfaces are brought into contact with each other, for example, hydrogen bonds are generated between the activated species. Next, when the separation layer 3 and the intermediate layer 4 are pressurized, dehydration condensation polymerization occurs between the activated species. As a result, the surfaces are bonded to each other by covalent bonds.

[0068] According to this method, no inclusions are present at the bonded interface, and therefore gas permeation is not inhibited at the bonded interface, resulting in a gas separation membrane 1 with good mechanical properties, gas permeability, and selective separation properties.

[0069] Next, the sacrificial layer is removed. This results in the gas separation membrane 1. The sacrificial layer is removed, for example, by contacting the sacrificial layer with a solvent containing water, an organic solvent, or the like. This allows the sacrificial layer to be dissolved and removed. With this method, even if the separation layer 3 is thin, the sacrificial layer can be removed without affecting it. This makes it possible to manufacture a gas separation membrane 1 having a separation layer 3 that is thin but has a low porosity.

[0070] Furthermore, the surface of the separation layer 3 from which the sacrificial layer has been removed exposes a clean surface of the constituent material. This surface allows the constituent material's affinity with carbon dioxide to be fully exerted. For this reason, the gas separation membrane 1 produced by the above method has excellent selective separation properties, particularly for carbon dioxide.

[0071] 4. Applications of gas separation membranes The gas separation membrane 1 according to the embodiment can be used for gas separation and recovery, gas separation and purification, etc. For example, the gas separation membrane 1 is used when efficiently separating carbon dioxide from a mixed gas containing gas components such as hydrogen, helium, carbon monoxide, carbon dioxide, hydrogen sulfide, oxygen, nitrogen, ammonia, sulfur oxides, nitrogen oxides, as well as saturated hydrocarbons such as methane and ethane, unsaturated hydrocarbons such as propylene, and perfluorohydrocarbons such as tetrafluoroethane. This allows the gas separation membrane 1 to be effectively used in, for example, a technology for separating and recovering carbon dioxide contained in the atmosphere (direct air capture (DAC)) and a technology for separating and recovering carbon dioxide from crude oil-associated gas and natural gas, the main component of which is methane.

[0072] 5. Advantages of the above embodiment As described above, the gas separation membrane 1 according to the embodiment has the porous layer 2 and the separation layer 3, and separates carbon dioxide from a mixed gas containing carbon dioxide and a non-target component. The separation layer 3 is in close contact with one surface of the porous layer 2 and is made of a polymer material. When the average thickness of the separation layer 3 is t, the average pore diameter of the porous layer 2 is d, and the average thickness of the porous layer 2 is T, t is 5 nm or more and 500 nm or less, the ratio d / t is more than 2.0 and 100 or less, and the ratio T / t is 100 or more and 10,000 or less.

[0073] According to such a configuration, a gas separation membrane 1 can be obtained which has excellent mechanical properties and can satisfactorily achieve both a gas selectivity ratio for carbon dioxide and a gas permeability for carbon dioxide.

[0074] The polymer material preferably contains organopolysiloxane. With this configuration, a separation layer 3 having good affinity for carbon dioxide can be obtained, and therefore a gas separation membrane 1 exhibiting a high gas selectivity ratio for carbon dioxide can be obtained.

[0075] The average pore diameter d of the porous layer 2 is preferably 5 nm or more and 1000 nm or less.

[0076] With such a configuration, the separation layer 3 can be prevented from escaping to the downstream side of the porous layer 2 while the gas permeability of the porous layer 2 to carbon dioxide is sufficiently ensured.

[0077] The average thickness T of the porous layer 2 is preferably 10 μm or more and 500 μm or less.

[0078] With this configuration, the porous layer 2 has necessary and sufficient rigidity to support the gas separation membrane 1 .

[0079] The material constituting the porous layer 2 may be a polymeric material, a ceramic material, or a metal material.

[0080] With this configuration, the material constituting the porous layer 2 has high rigidity, and therefore the mechanical properties of the gas separation membrane 1 can be improved.

[0081] Although the gas separation membrane according to the present invention has been described above based on the preferred embodiment, the present invention is not limited thereto.

[0082] For example, the gas separation membrane of the present invention may be one in which each part of the above-mentioned embodiment is replaced with a component having a similar function, or one in which any component is added to the above-mentioned embodiment. EXAMPLES

[0083] Next, specific examples of the present invention will be described. 6. Preparation of Gas Separation Membrane 6.1. Sample No. 1 First, an organopolysiloxane film was formed by plasma polymerization on one side of a porous layer made of alumina (Al2O3). This resulted in a separation layer. The raw material gas used was octamethyltrisiloxane, and the constituent material of the obtained separation layer was organopolysiloxane. The porosity of the porous layer was 50%. The composition of the gas separation membrane is as shown in Table 1.

[0084] 6.2. Samples No. 2 to 16 Except for changing the configuration of the gas separation membrane as shown in Table 1, a gas separation membrane was produced in the same manner as in the case of Sample No. 1.

[0085] 6.3. Sample No. 17 A gas separation membrane was produced in the same manner as in the case of Sample No. 1, except that the configuration of the gas separation membrane was changed as shown in Table 2. The method for producing the gas separation membrane of Sample No. 17 is as follows.

[0086] First, an organopolysiloxane film was formed on one surface of the porous layer made of alumina by plasma polymerization. The intermediate layer was thus obtained. The raw material gas used was octamethyltrisiloxane.

[0087] Next, a film of organopolysiloxane was formed on one surface of the water-soluble film as a sacrificial layer by plasma polymerization, thereby obtaining a separation layer. Note that octamethyltrisiloxane was used as the raw material gas.

[0088] Next, the intermediate layer and the separation layer were each subjected to an activation treatment by irradiating them with ultraviolet light. Then, the layers were stacked so that the surfaces that had been subjected to the activation treatment were in contact with each other, and the layers were heated and pressed to obtain a gas separation membrane.

[0089] 6.4. Samples No. 18 and 19 Except for changing the configuration of the gas separation membrane as shown in Table 2, a gas separation membrane was produced in the same manner as in the case of Sample No. 17.

[0090] 6.5. Sample No. 20 A gas separation membrane was produced in the same manner as in the case of Sample No. 1, except that the configuration of the gas separation membrane was changed as shown in Table 3. The method for producing the gas separation membrane of Sample No. 20 is as follows.

[0091] First, an O / W type emulsion containing polylactic acid (PLA) was prepared, and then this O / W type emulsion was mixed with glycerin, triethylene glycol monobutyl ether, and 2-pyrrolidone to prepare an ink.

[0092] Next, the prepared ink was used to form an inkjet coating by an inkjet method, thereby obtaining a separation layer.

[0093] 6.6. Samples No. 21 and 22 Except for changing the configuration of the gas separation membrane as shown in Table 3, a gas separation membrane was produced in the same manner as in the case of sample No. 20.

[0094] In Tables 1 to 3, gas separation membranes corresponding to the present invention are designated as "Examples," and gas separation membranes not corresponding to the present invention are designated as "Comparative Examples." In Tables 1 and 2, "p-OPS" refers to organopolysiloxane produced by plasma polymerization, "a-OPS" refers to polydimethylsiloxane with amino terminals formed by coating, and "ph-OPS" refers to polydimethylsiloxane with phenyl terminals formed by coating.

[0095] 7. Evaluation of gas separation membranes The gas separation membranes of each of the Examples and Comparative Examples were evaluated as follows.

[0096] 7.1. Coverage of the separation layer For each of the gas separation membranes of the Examples and Comparative Examples, the cross section of the separation layer was observed with an electron microscope, and the area of ​​defects was calculated. The area of ​​the defect-free area relative to the area of ​​the observed area was calculated as the "coverage rate of the separation layer." The calculation results are shown in Tables 1 to 3.

[0097] 7.2. Gas permeability and gas selectivity for carbon dioxide A test sample was prepared by cutting the gas separation membrane of each Example and Comparative Example into a circle with a diameter of 5 cm. Next, a gas mixture of carbon dioxide and nitrogen in a volume ratio of 13:87 was supplied to the upstream side of the test sample using a gas permeability measuring device. The total pressure on the upstream side was adjusted to 5 MPa, the partial pressure of carbon dioxide to 0.65 MPa, the flow rate to 500 mL / min, and the temperature to 40°C. The gas components that permeated the test sample were then analyzed by gas chromatography.

[0098] Next, from the analysis results, the carbon dioxide gas permeability R of the gas separation membrane is calculated. CO2 and nitrogen gas permeability R N2 and the gas selectivity R of carbon dioxide to nitrogen CO2 / R N2 The calculation results are shown in Tables 1 to 3.

[0099] 7.3. Mechanical properties 7.3.1. Independence For the gas separation membranes of each Example and Comparative Example, the end of the test sample prepared in 7.2 was clamped with a jig and fixed so that the clamped part was horizontal. Next, the sagging distance of the test sample was measured. Specifically, the vertical distance between the lowest part of the test sample and the jig was measured. The measured distance was evaluated against the following evaluation criteria. In the following evaluation criteria, the distance measured for the test sample No. 13 is set as the "reference value." The evaluation results are shown in Tables 1 to 3.

[0100] A: The sagging distance is small (less than half the standard value) B: The sagging distance is slightly small (more than half the standard value but less than the standard value) C: The sagging distance is large (above the standard value)

[0101] 7.3.2. Folding resistance The gas separation membranes of each of the examples and comparative examples were folded into an accordion shape, and then stretched. This operation was repeated 10 times, and the gas separation membranes were then cut into circles with a diameter of 5 cm to prepare test samples.

[0102] Next, the gas selectivity R of the test sample was measured in the same manner as in 7.2. CO2 / R N2 The gas selectivity R before the bending test was calculated. CO2 / R N2 and the gas selectivity R after the bending test. CO2 / R N2 The difference between and is the gas selectivity R CO2 / R N2 This decrease was calculated as the decrease in the gas selectivity R CO2 / R N2 The calculated degree of decrease was compared with the following evaluation criteria to relatively evaluate the mechanical properties of the gas separation membrane. The evaluation results are shown in Tables 1 to 3.

[0103] A: Gas selection ratio R CO2 / R N2 The decrease is small (less than 3) B: Gas selectivity R CO2 / R N2 The decline is moderate (3 or more but less than 6) C: Gas selectivity R CO2 / R N2 The decrease is large (6 or more)

[0104] [Table 1]

[0105] [Table 2]

[0106] [Table 3]

[0107] As is clear from Tables 1 to 3, the gas separation membranes of the examples have superior mechanical properties compared to the gas separation membranes of the comparative examples, and it was found that they achieve both a good gas selectivity ratio for carbon dioxide and a good gas permeability for carbon dioxide. It was also found that the mechanical properties could be particularly improved when an intermediate layer was interposed between the separating layer and the porous layer. [Explanation of symbols]

[0108] 1...gas separation membrane, 2...porous layer, 3...separation layer, 4...intermediate layer, 23...hole, 43...hole

Claims

1. A porous layer; a separation layer made of a polymer material and in close contact with one surface of the porous layer; A gas separation membrane for separating carbon dioxide from a mixed gas containing carbon dioxide and a non-target component, The average thickness of the separation layer is t, The average pore diameter of the porous layer is d, When the average thickness of the porous layer is T, t is 5 nm or more and 500 nm or less, The ratio d / t is more than 2.0 and not more than 100; A gas separation membrane having a ratio T / t of 100 or more and 10,000 or less.

2. 2. The gas separation membrane of claim 1, wherein the polymeric material comprises an organopolysiloxane.

3. 3. The gas separation membrane according to claim 1, wherein the average pore diameter d of the porous layer is 5 nm or more and 1000 nm or less.

4. 3. The gas separation membrane according to claim 1, wherein the average thickness T of the porous layer is 10 μm or more and 500 μm or less.

5. 3. The gas separation membrane according to claim 1, wherein the porous layer is made of a polymeric material, a ceramic material or a metallic material.

Citation Information

Patent Citations

  • Permeselective composite membrane for gas and its preparation

    JP1985075320A

Cited By

  • Therapeutic agent for brain metastatic tumors, comprising n-(4-(4-amino-6-ethynyl-5-(quinolin-3-yl)-7h-pyrrolo [2, 3-d] pyrimidin-7-yl) bicyclo [2.2. 1] heptane-1-yl)-5-methylpyrazine-2-carboxamide or salt thereof as active ingredient

    CN122438686A

  • Brain-migrating tumor treatment agent containing, as active ingredient, n-(4-(4-amino-6-ethynyl-5-(quinolin-3-yl)-7h-pyrrolo[2,3-d]pyrimidin-7-yl) bicyclo[2.2.1]heptan-1-yl)-5-methylpyrazine-2-carboxamide or salt thereof

    EP4825380A1

  • Brain-migrating tumor treatment agent containing, as active ingredient, n-(4-(4-amino-6-ethynyl-5-(quinolin-3-yl)-7h-pyrrolo[2,3-d]pyrimidin-7-yl) bicyclo[2.2.1]heptan-1-yl)-5-methylpyrazine-2-carboxamide or salt thereof

    WO2025127108A1