High-purity alumina particle and method for producing the same, and resin composition for electronic device and method for producing the same
Patent Information
- Application Number
- JP2023097978
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-06-14
- Publication Date
- 2024-12-26
AI Technical Summary
【0018】 本発明の高純度アルミナ粒子及び高純度アルミナ粒子の製造方法によると、封止材に添加するフィラー用のアルミナ粒子であって、金属アルミニウムに由来するアルミナ粒子に残存する金属状態のアルミニウム量を低減して純度を高めた高純度アルミナ粒子を得ることができ、併せてその製造方法を確立することができる。
Smart Images

Figure 2024179265000001 
Figure 2024179265000002 
Figure 2024179265000003
Abstract
Description
[Technical field]
[0001] The present invention relates to high-purity alumina particles and a method for producing the same, as well as a resin composition for electronic devices containing high-purity alumina particles and a method for producing the same. [Background technology]
[0002] In the case of sealing materials for sealing precision electronic parts such as semiconductors, inorganic fillers are added to the resin composition. The fillers are required to have insulating properties and a low thermal expansion coefficient. Generally, alumina (aluminum oxide) is widely used.
[0003] Alumina is processed into fillers by crushing natural high-purity ores to a specified particle size. In other words, even if it is high purity, since it is derived from natural ores, the presence of impurities other than aluminum oxide is inevitable. In particular, in the case of alumina derived from natural products, uranium and thorium elements are present. In order to improve the processing speed of semiconductors, processing precision and integration are further promoted. Therefore, the influence of electromagnetic noise that semiconductors receive from the outside is more of a problem than ever before. In the case of alumina derived from natural products, it is known that alpha rays and the like are generated by the radioactive decay of uranium and thorium elements, which are thought to be the cause of malfunction.
[0004] Therefore, a manufacturing method combining pulverization and exposure to flame has been proposed for the purpose of reducing impurities contained in the finished filler, etc. (see Patent Document 1). Furthermore, in order to improve on the manufacturing method of Patent Document 1, etc., a manufacturing method has been proposed in which raw materials in a metallic state such as aluminum are processed into oxides, and then the aluminum impurity is dissolved in a basic solution (see Patent Document 2).
[0005] The conventional manufacturing method has made great progress in reducing impurities. However, it is not easy to dissolve amphoteric metal elements such as aluminum in a basic solution. In particular, in the case of aluminum, depending on the purity of the metal, an oxide film can form on the metal surface, which can inhibit dissolution in a basic solution. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2012-206870 A [Patent Document 2] JP 2014-101239 A Summary of the Invention [Problem to be solved by the invention]
[0007] The inventor then conducted extensive research into the dissolution of metallic aluminum in a basic solution, and as a result, by appropriately controlling the dissolution of the raw material metal in a basic solution, the inventor was able to increase the efficiency of dissolving metallic aluminum in a basic solution and pave the way for reducing impurity components resulting from the metallic raw material.
[0008] The present invention has been made in consideration of the above-mentioned points, and provides high-purity alumina particles for use as a filler to be added to a sealing material, which have an increased purity by reducing the amount of impurities remaining in the alumina particles derived from metallic aluminum and by reducing the amount of aluminum in a metallic state itself, as well as a production method thereof; and a resin composition for electronic devices using the high-purity alumina particles and a production method thereof. [Means for solving the problem]
[0009] That is, the high purity alumina particles of the embodiment are alumina particles derived from metallic aluminum, characterized in that the uranium content in the alumina particles is 5 ppb or less, the thorium content in the alumina particles is 5 ppb or less, the metallic aluminum content in the alumina particles is 5 ppm or less, the sodium content in the alumina particles is 10 ppm or less, and the iron content in the alumina particles is 10 ppm or less.
[0010] Furthermore, in the high purity alumina particles, the amount of residual aluminum particles having a particle size of 20 μm or more derived from the raw material aluminum metal may be 10 or less per 50 g of the alumina particles.
[0011] Furthermore, the resin composition for electronic devices is characterized by having high purity alumina particles and a resin composition.
[0012] The method for producing high purity alumina particles according to the embodiment is characterized by comprising a granulation process in which metallic aluminum powder is introduced into a flame to be vaporized and oxidized, and then spherically shaped by surface tension upon cooling to obtain spherical alumina particles; a dissolution process in which the spherical alumina particles are introduced into a basic solution to dissolve the metallic aluminum remaining within the spherical alumina particles; and a drying process in which the spherical alumina particles are dried.
[0013] Furthermore, in the method for producing high purity alumina particles, the basic solution may be an aqueous solution of an amine compound.
[0014] Furthermore, in the dissolution step of the method for producing high-purity alumina particles, the spherical alumina particles may be dissolved in a basic solution having a pH of 9 or higher and a liquid temperature of 20 to 60°C to dissolve the metallic aluminum remaining in the spherical alumina particles.
[0015] Furthermore, in the dissolving step of the method for producing high purity alumina particles, the spherical alumina particles may be sieved.
[0016] Furthermore, the method for producing high purity alumina particles may further include a washing step of washing the spherical alumina particles.
[0017] In addition, a manufacturing method of a resin composition for electronic devices is characterized by comprising a granulation step in which metallic aluminum powder is introduced into a flame to vaporize and oxidize it, and then spherical alumina particles are obtained through spheroidization due to surface tension upon cooling; a dissolution step in which the spherical alumina particles are introduced into a basic solution having a pH of 9 or more and a liquid temperature of 20 to 60°C to dissolve the aluminum in a metallic state remaining in the spherical alumina particles; a drying step in which the spherical alumina particles are dried; and a resin dispersion step in which the spherical alumina particles that have been subjected to the drying step are dispersed in a resin composition to obtain a resin dispersion. Effect of the Invention
[0018] According to the high-purity alumina particles and the method for producing high-purity alumina particles of the present invention, it is possible to obtain high-purity alumina particles for filler to be added to a sealing material, the amount of metallic aluminum remaining in the alumina particles derived from metallic aluminum being reduced to increase the purity, and also to establish a method for producing the same.
[0019] In addition, the resin composition for electronic devices and its manufacturing method make it possible to reduce the dose of particle rays and electromagnetic waves emitted from the spherical particles contained in the resin composition, which is expected to suppress external disturbance factors such as noise and reduce malfunctions and other problems with the equipment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] In preparing the high-purity alumina particles of the embodiment, a manufacturing method is carried out in which the raw material, metallic aluminum powder, is subjected to the following steps in order. The resin composition for electronic devices is a resin composition containing high-purity alumina particles, and the manufacturing method includes a step of dispersing the high-purity alumina particles in the resin composition in the final stage. The high-purity alumina particles are alumina particles whose total weight is 99.8% or more of which is aluminum oxide.
[0021] First, metallic aluminum powder is prepared as a raw material and is thrown into a flame. In the flame, the metallic aluminum powder vaporizes and is oxidized. The aluminum oxide (alumina) produced by the oxidation cools from a gas to a liquid. At this time, the aluminum oxide (alumina) becomes spheroidal due to surface tension. As a result, fine spherical alumina particles are produced (the "particulation process"). This process is a type of deflagration reaction, and is also known as the VMC method (Vaporized Metal Combustion Method).
[0022] The flame in the granulation process is formed by mixing a combustion supporting gas containing oxygen with a combustible gas and burning it. As an index of the temperature inside the furnace, the temperature of the refractory structure of the furnace is in the range of 900°C to 1500°C at the highest position (furnace body temperature). The furnace body temperature is preferably 900°C to 1100°C as a lower limit and 1300°C to 1500°C as an upper limit. Air and oxygen are used as the combustion supporting gas. When the combustible gas and the combustion supporting gas are supplied into the furnace, they may be supplied separately or in a premixed state.
[0023] The flow velocity of the combustible gas is preferably 0.1 m / s or more, more preferably 0.5 m / s or more, and even more preferably 1 m / s or more. The flow velocity of the combustion supporting gas is preferably 5 m / s or more, more preferably 7 m / s or more, and even more preferably 9 m / s or more. The flow velocity ratio of combustible gas / combustion supporting gas is preferably 0.5 or less, more preferably 0.3 or less, and even more preferably 0.1 or less. The supply amounts of the combustible gas and combustion supporting gas are determined by the amount of the combustible gas that can form a flame large enough to sufficiently heat the raw material particles to be supplied, and the amount of the combustion supporting gas that can sufficiently combust the combustible gas. For example, the amount of the combustible gas per unit weight of the pulverized material to be processed is 0.5 Nm 3 / h or 5Nm 3 / h, oxygen as a combustion support gas is 50Nm 3 / h~500Nm 3 / h.
[0024] The method for supplying the aluminum metal powder to the flame is not particularly limited, but the aluminum metal powder can be supplied to the flame in a dispersed state in a carrier gas, such as air, oxygen, or nitrogen.
[0025] In the spherical alumina particles produced by the granulation process, not all of the metallic aluminum is necessarily oxidized to aluminum oxide, and a small amount of metallic aluminum may remain. Therefore, in order to remove the metallic aluminum, the spherical alumina particles are put into a basic solution, and the metallic aluminum remaining in the spherical alumina particles is dissolved ("dissolving process").
[0026] The basic solution used when dissolving metallic aluminum, which is an amphoteric element, in a basic solution is a solution that does not contain an alkali metal. In general, aqueous solutions of hydroxides of alkali metals, such as lithium hydroxide, sodium hydroxide, and potassium hydroxide, are strongly basic. However, if the alkali metal in the basic solution remains in the spherical alumina particles, it is undesirable because it reduces the purity of the spherical alumina particles that are finally produced.
[0027] Therefore, an aqueous solution of an amine compound is used as a basic solution that does not contain an alkali metal. Examples of the amine compound include ammonia, primary amines, secondary amines, tertiary amines, quaternary ammonium hydroxides (ammonium salts), arylamines, silazanes, and hydrazines.
[0028] More specifically, the amine compound is one or more compounds selected from ammonia, methylamine, ethylamine, propylamine, dimethylamine, diethylamine, pyrrolidine, trimethylamine, triethylamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrabutylammonium hydroxide, benzyltrimethylammonium hydroxide, methyltriamylammonium hydroxide, methyltributylammonium hydroxide, pyrrolidine, piperidine, pyridine, quinoline, imidazole, indole, pyrimidine, hexamethyldisilazane, hydrazine, diazabicycloundecene, diazabicyclononene, etc. When preparing the aqueous solution, the amine compound may be a single type or a mixture of two or more types.
[0029] When an amine compound, which is an organic compound, is used, the compound molecules volatilize and decompose with the subsequent process. Therefore, it is desirable that the amine compound hardly remains in the spherical alumina particles that are finally produced. Of course, regarding the concentration of the amine compound in the aqueous solution, when dissolving the metallic aluminum remaining in the spherical alumina particles, the pH of the basic solution is 9 or more, more preferably 10 or more, and the metallic aluminum remaining in the spherical alumina particles is heated by the basic solution at a liquid temperature of 20 to 60°C, more preferably at a liquid temperature of approximately 40 to 60°C. If the temperature is less than 40°C, the time until precipitation is long. Also, if the temperature exceeds 60°C, precipitation is difficult to occur due to the influence of the liquid temperature. From the examples described below, it is based on the knowledge that mainly controlling the pH and temperature conditions is effective in reducing the amount of metallic aluminum that remains undissolved.
[0030] Regarding the relationship between the amount of base and the amount of metallic aluminum to be dissolved, the amount of base (wt%) relative to the amount of metallic aluminum (Al) (g) is preferably in the range of 0.04 to 2 wt%. The amount of base is converted from a molar amount to wt% (weight percent) to make it easier to measure.
[0031] It is known that the metallic aluminum remaining in the spherical alumina particles forms an oxide film of alumina (such as anodized aluminum) on the metal surface when reacting with an acid or base. By forming an oxide film on the surface, the base does not come into contact with the metallic aluminum inside the oxide film, and the hydroxide reaction ends. In other words, undissolved metallic aluminum (residual) is inevitably generated. Therefore, it is necessary to promote hydroxide formation by reacting metallic aluminum with a basic solution (aqueous solution of an amine compound) as vigorously as possible. It is speculated that the oxide film formed on the surface of high-purity aluminum, that is, high-purity alumina, is so pure that a base such as ammonia cannot completely dissolve the oxide film, and as a result, the dissolution of the internal aluminum does not proceed.
[0032] The above conditions are for ensuring the pH required for forming aluminum hydroxide and for the reaction to proceed slowly at a mild temperature close to room temperature. Of course, the conditions are adjusted depending on the type and concentration of the amine compound used.
[0033] In the dissolving step, the spherical alumina particles are sieved if necessary. Although the spherical alumina particles can be spheroidized in the granulation step, the particle size of the spherical alumina particles cannot be homogenized. In the dissolving step, the spherical alumina particles may be broken down due to the influence of the strong base during dissolution. Therefore, prior to the next step, the spherical alumina particles with non-uniform particle sizes are removed by sieving. For sieving, a known sieve or the like is used to separate the spherical alumina particles according to the specified particle size.
[0034] After the dissolving process, the spherical alumina particles are dried (the "drying process"). Before the drying process, the spherical alumina particles are washed to remove the basic solution (the "washing process"). First, in the washing process, the spherical alumina particles are washed with water. The washing device and number of times are appropriate, and the washing is completed when the pH of the wastewater after washing reaches approximately 7. The drying process may be performed by natural drying or drying by exposing the particles to warm or hot air using a dryer, as appropriate.
[0035] The spherical alumina particles that are completed through the drying process tend to be large and non-uniform due to aggregation during the process. Therefore, crushing is added to adjust the final product to a homogeneous quality. Either wet crushing or dry crushing may be used for crushing. As a crushing device, a known device for crushing solids such as a ball mill, a vibration mill, a chopper stirring type crusher, a jet mill, or an atomizer is used. In the embodiment, the solidified material and alumina balls are placed in a crushing pod, and the pod is rotated to crush the solidified material by a wet method. The rotation time of the pod (crushing time) is adjusted according to the target particle size. After the wet crushing, the crushed material collected from the pod is dried by spray drying or the like.
[0036] Here, the average particle size of the spherical alumina particles in each process is the median diameter (D 50 ) means the average particle diameter of the spherical alumina particles (D 50 ) is preferably 30 μm or less, more preferably 20 μm or less.
[0037] As explained above, the spherical alumina particles (i.e., high-purity alumina particles) produced from metallic aluminum through a granulation process, a dissolution process, a drying process, and optionally washing have a significantly reduced total amount of impurities such as uranium and thorium, as well as sodium and iron, compared to the metallic aluminum raw material stage. As will be clear from the examples described later, the metallic aluminum contained in the spherical particles (components that were not oxidized to alumina) is reduced to 1 / 10 or less, or even 6 / 100 or less, of the amount contained in the original metallic aluminum raw material. This makes it possible to further reduce the dose of particle rays such as alpha rays and beta rays, and electromagnetic waves such as gamma rays, emitted from the spherical particles, thereby reducing the impact on electronic components, etc.
[0038] The spherical aluminum particles produced by the oxidation of the aluminum metal powder are dissolved in a basic solution, and the aluminum metal remaining in the spherical aluminum particles changes from a metallic state to aluminum hydroxide, which is a hydroxide. At this point, the amount of impurities contained in the raw aluminum metal is considered to be less than the amount dissolved in the basic solution. Heavy elements such as U (uranium) and Th (thorium) are not amphoteric elements, so they are difficult to dissolve in a basic solution and remain as insoluble components. This ease of dissolution in a basic solution makes it possible to separate the uranium and thorium elements and other impurity components. Therefore, it is possible to further reduce impurities compared to the preparation of oxides for fillers in the past.
[0039] In addition, depending on the dissolution conditions in the basic solution, the oxide coating that forms on the surface of the metallic aluminum upon contact with the basic solution is also dissolved, making it possible to reduce the amount of metallic aluminum that remains undissolved on the high-purity alumina particles.
[0040] The high purity alumina particles are characterized by being prepared from alumina particles derived from metallic aluminum. The content of uranium in the alumina particles is 5 ppb or less, preferably 1 ppb or less, and the content of thorium in the alumina particles is 5 ppb or less, preferably 1 ppb or less. The amounts of uranium and thorium, which are particularly desired to be reduced, can be significantly reduced.
[0041] The sodium content in the alumina particles is 10 ppm or less, preferably 5 ppb or less, and more preferably 1 ppb or less, and the iron content in the alumina particles is 10 ppm or less, preferably 5 ppb or less, and more preferably 1 ppm or less. In this way, impurity components other than aluminum are reduced, so that very pure high-purity alumina particles can be obtained.
[0042] In addition, the content of metallic aluminum in the high-purity alumina particles (alumina particles) is 5 ppm or less, preferably 3 ppb or less, and more preferably 1 ppm or less. In other words, metallic aluminum remaining in the final high-purity alumina particles (spherical alumina particles) is suppressed as much as possible. If metallic aluminum remains in the high-purity alumina particles, as described above, the influence of the uranium and thorium elements remaining in the metallic aluminum cannot be eliminated. In addition, since metallic aluminum is a conductor, there is a risk of electrical conduction when the high-purity alumina particles are used as a filler for electronic materials. Therefore, in order to promote the dissolution of metallic aluminum in a basic solution as much as possible, the amount of metallic aluminum remaining in the final high-purity alumina particles (spherical alumina particles) is specified.
[0043] Furthermore, the amount of residual aluminum particles having a particle size of 20 μm or more derived from the metallic aluminum used as the raw material is 10 or less, preferably 5 or less, more preferably 0 (not detected) per 50 g of high-purity alumina particles (spherical alumina particles). If metallic aluminum particles having a size of 20 μm or more remain in the final high-purity alumina particles (spherical alumina particles), the electrical insulation of the high-purity alumina particles is reduced. In other words, since metallic aluminum is conductive, the insulating performance as a filler is reduced. This may cause electrical defects such as short circuits at the site where the resin composition containing the high-purity alumina particles as a filler is applied. Therefore, the metallic aluminum particles present in the high-purity alumina particles can be suppressed to control the quality of the high-purity alumina particles.
[0044] The high-purity alumina particles prepared by the method for producing high-purity alumina particles according to the embodiment described above are mainly used as a filler for electronic materials. The high-purity alumina particles are added to a resin to prepare a resin composition for electronic devices (a filler-containing resin composition for electronic materials) (the "resin dispersion step" in the method for producing a resin composition for electronic devices).
[0045] Resins to which the epoxy resin can be added include thermoplastic resins such as polyethylene, polypropylene, polyvinyl chloride, polyethylene terephthalate, polystyrene, other olefin resins, polyimide resins, liquid crystal polymers, etc., fluororesins, urea resins, phenolic resins, polyphenylene ether, bismaleimide, etc. Furthermore, the epoxy resin can be added to elastic resins such as styrene butadiene rubber, isoprene rubber, etc., silicone resins, etc. For example, when manufacturing resin substrates such as electronic component packaging substrates and interlayer insulating films, epoxy resins are used as the resin.
[0046] Examples of epoxy resins used in the resin composition include bisphenol A type epoxy resins, bisphenol F type epoxy resins, biphenyl type epoxy resins, phenol novolac type epoxy resins, naphthalene type epoxy resins, and phenoxy type epoxy resins. The weight of the high purity alumina particles blended in the resin composition is preferably large from the viewpoints of heat resistance and thermal expansion coefficient. It is desirable to add 80 mass% or more of high purity alumina particles (filler for electronic materials) to the total mass of the resin composition.
[0047] Furthermore, the high purity alumina particles (filler for electronic materials) of the embodiment can be prepared as a slurry for electronic materials having a liquid dispersion medium that is substantially free of moisture by dispersing the filler for electronic materials. As the dispersion medium, for example, a solvent such as methyl alcohol, ethyl alcohol, isopropyl alcohol, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, methyl acetate, ethyl acetate, toluene, N-methylpyrrolidone, γ-butyrolactone, propylene glycol monomethyl ether, and propylene glycol monomethyl ether acetate is used. The dispersion medium can be used alone or in combination. It is also possible to use an appropriate dispersant.
[0048] As explained above about the high purity alumina particles, the characteristic property of the resin composition for electronic devices (resin composition containing filler for electronic materials) is that it is possible to reduce the dose of particle rays and electromagnetic waves emitted from the spherical particles contained in the resin composition. Therefore, it is possible to reduce the effects of particle rays and electromagnetic waves on electronic components and the like from the processed parts of the resin composition. As a result, it is expected that disturbance factors such as noise will be suppressed and malfunctions such as malfunctions of equipment will be reduced. EXAMPLES
[0049] In order to verify the manufacturing method of high purity alumina particles, Test Examples 1 to 29 were prepared and the physical properties of each Test Example were evaluated. The following describes the raw materials used, the manufacturing method, and the measurement and evaluation methods in that order. For details of each prototype, see Tables 1 to 6 below.
[0050] [Raw materials used] As the metallic aluminum in Test Examples 1 to 6, a general-purpose aluminum powder having an average particle diameter of 20 μm was used. The metallic aluminum used in Test Examples 7 to 22 was a high-purity aluminum powder with an average particle size of 20 μm. The alumina particles used in Test Examples 23, 25, and 27 were high purity alumina particles with an average particle diameter of 0.2 μm. The alumina particles used in Test Examples 24, 26, 28, and 29 were high purity alumina particles with an average particle diameter of 10 μm.
[0051] The following amine compounds were used in preparing the basic solution: Ammonia: Fujifilm Wako Pure Chemical Industries, Ltd. Dimethylamine: Fujifilm Wako Pure Chemical Industries, Ltd. Tetramethylammonium hydroxide (hereafter referred to as TMAH): Fujifilm Wako Pure Chemical Industries, Ltd. Diazabicycloundecene (hereinafter referred to as DBU): Manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0052] [Confirmation of solubility of metallic aluminum] Test Examples 1 to 22 0.2 g of metallic aluminum particles of each test example, 100 g of ion-exchanged water, and an aqueous solution of the base species shown in the table were mixed and stirred for the test time indicated while heating to 40° C. Test examples 1 to 12 were a 28% aqueous ammonia solution, test examples 13 to 20 were a 50% aqueous dimethylamine solution, test example 21 was a 25% TMAH solution, and test example 22 was an aqueous DBU solution.
[0053] [Verification of the production of high-purity alumina particles] Test Examples 23 to 29 Test Examples 23 to 29 use alumina particles as the starting material. These are a type of deflagration reaction, and are verifications aimed at removing metallic aluminum remaining within alumina particles prepared by the VMC method (Vaporized Metal Combustion Method).
[0054] For each test example, 100 g of alumina particles were mixed with 100 g of ion-exchanged water, to which an amine compound was added as a base species and dissolved. The amount of the base species was determined according to the test example in the table. The solution of each test example was then stirred at 25°C for 5 hours. After stirring, the solution was dried at 160°C, and the spherical alumina particles were collected.
[0055] ·Component analysis In analyzing the atomic composition contained in the oxide powder, Shimadzu Corporation's ICP (inductively coupled plasma atomic emission spectrometry) equipment ICP-MS (measurement of U, Th) and ICP-AES (measurement of alumina and other impurities) were used. For the measurement, the alumina powder of each test example was completely dissolved in sulfuric acid to form a solution, and then the solution was subjected to the measurement.
[0056] Measurement of residual metallic aluminum content When measuring the amount of residual metallic aluminum, 50 g of alumina powder samples of each test example (both before and after immersion in the basic solution) were weighed and placed in a 500 mL Erlenmeyer flask. 220 mL of 2 M sodium hydroxide solution was added to the flask, which was quickly sealed and stirred at 1000 to 1200 rpm using a magnetic stirrer. The temperature at the start of stirring: T1, was then measured.
[0057] Stirring was continued in a sealed state for the time (approximately 15 minutes) that was considered to be the time when the reaction between metallic aluminum and sodium hydroxide was completed, and the generated hydrogen was collected in an Erlenmeyer flask. Immediately after stirring was stopped, a hydrogen detector tube (Kitagawa-type gas detector hydrogen 137U, manufactured by Komyo Rikagaku Kogyo Co., Ltd.) was inserted through the airtight stopper, and a gas sampler for the detector tube (Kitagawa-type gas sampler AP-20, manufactured by Komyo Rikagaku Kogyo Co., Ltd.) was attached, and 50 mL of gas was sucked from the sealed Erlenmeyer flask to measure the hydrogen concentration.
[0058] The detector tube and gas sampler were removed, and the temperature in the Erlenmeyer flask, T3, was measured through a tightly sealed stopper. Water was then poured into the Erlenmeyer flask, and the volume of the space in the Erlenmeyer flask, V, was measured from the volume of the water.
[0059] From the above measured values, the residual metallic aluminum concentration was measured using the following equation, which follows the equation of state for an ideal gas and Boyle's law: (Remaining metallic aluminum concentration: ppm) = Hydrogen concentration (%) x (273 (K) + T1 (℃)) x (V (mL) + Gas intake volume (mL)) / {V (mL) x (273 (K) + T3 (℃))} x 10000 x V (mL) / 1000 x 1 / {22.4 (L) x (273 (K) + T1 (℃)) / 273 (K)} x (Reaction molar ratio of remaining metallic material and hydrogen) x Atomic weight of unburned metal x 1 / Amount of sample used (g) Here, (the reaction molar ratio of remaining metallic aluminum to hydrogen) is a value indicating how many moles of hydrogen are produced per mole of remaining metallic aluminum, and in the case of metallic aluminum, it is 1.5.
[0060] Measurement of residual metallic aluminum particles Along with the residual metallic aluminum concentration, the residual metallic aluminum in granular form was measured as the amount of conductive aluminum particles of 20 μm or more. 300 g of alumina powder sample (both before and after immersion in the basic solution) was weighed out, 0.1 g of sodium hexametaphosphate was added, and the sample was sieved through a 20 μm sieve. Isopropanol was sprayed continuously from above the sieve for about 8 hours to wash the alumina powder, and then it was left to stand and dry for 24 hours.
[0061] After drying, the number of objects that appeared to be foreign bodies in the alumina powder was counted by visual inspection using an optical microscope, and these were then separated from the alumina powder. Electrical continuity was confirmed for the separated foreign bodies using a tungsten needle. For foreign bodies that were confirmed to have electrical continuity, qualitative analysis was performed using an energy dispersive X-ray analyzer (SEM-EDX) to confirm that they were aluminum.
[0062] [result] The results of Test Examples 1 to 22 are shown in Tables 1 to 4. In each table, from the top, the weight (g) of metallic aluminum, the amount of water (g) of the basic solution, the type of base, the amount of base (mol%) relative to the amount (mol) of metallic aluminum (Al), pH, temperature (°C), time (h), the amount of uranium and thorium in the final state (ppb), the amount of sodium and iron in the final state (ppm), and the solubility evaluation (A, B, C, and D) are shown.
[0063] The solubility is evaluated according to the following four levels, with A being the best, B being good, C being average, and D being poor. A rating of A indicates that all metal particles have turned white and converted to aluminum hydroxide. A rating of B indicates that although some whitening has occurred, the metallic aluminum can still be seen with the naked eye. Grade C indicates a greater amount of metallic aluminum than the grade B above. A rating of D indicates that little or no change to aluminum hydroxide was observed.
[0064] Test Examples 23 to 29 correspond to a method in which dissolution in a basic solution is added to the conventional method of producing alumina powder by the VMC method starting from metal powder. Here, the VMC method is a method for producing spherical oxide fine particles by utilizing the deflagration phenomenon of metal powder.
[0065] [Table 1]
[0066] [Table 2]
[0067] [Table 3]
[0068] [Table 4]
[0069] [Considerations on dissolving metallic aluminum powder] Test Examples 1 to 6 are general-purpose aluminum metal powders, and generally contain a large amount of impurities compared to the high-purity aluminum metal powders of Test Examples 7 to 22. Since the purity of aluminum is not high, adjusting the pH of the dissolution conditions in the basic solution has little effect on the solubility evaluation (see Test Examples 4, 5, and 6). In contrast, the solubility evaluation of Test Examples 10, 11, and 12, which are high-purity aluminum metal powders, deteriorated even though similar conditions were used. Therefore, it is difficult to use the conditions for dissolving a general-purpose aluminum metal powder in a basic solution as the conditions for dissolving a high-purity aluminum metal powder in a basic solution.
[0070] Therefore, as shown in Test Examples 13 to 22, by controlling the type of amine compound in the basic solution, its base amount, pH, and dissolution time, it was possible to achieve good dissolution of high-purity metallic aluminum powder in the basic solution.
[0071] The results of Test Examples 23 to 29 are shown in Tables 5 and 6. In each table, from the top, the weight (g) of the alumina powder, the amount of water (g) of the basic solution, the type of base, the amount of base (mol%) relative to the amount of metallic aluminum (Al) (mol), pH, temperature (°C), time (h), the amount of metallic aluminum in the alumina powder (both before and after immersion in the basic solution) (ppm), the amount of conductive aluminum particles of 20 μm or more (both before and after immersion in the basic solution) (pieces / 50 g), the amount of uranium and thorium in the final state (ppb), and the amount of sodium and iron in the final state (ppm).
[0072] [Table 5]
[0073] [Table 6]
[0074] [Considerations on dissolving alumina powder] In Test Examples 23 to 29, even though the amount and number of metallic aluminum particles were large before immersion in the basic solution, it was confirmed that the amount and number of metallic aluminum particles decreased after immersion in the basic solution, regardless of the initial amount. Specifically, it was less than 1 ppm and there were zero particles. Therefore, the effectiveness of immersing alumina particles (powder) in a basic solution after the fact was clear. It is considered that the amount of base in Test Example 27 was too small.
[0075] From this series of results, it is possible to reduce impurities in the preparation of alumina powder starting from metallic aluminum, and subsequently reduce poorly soluble metallic aluminum from the alumina powder, dramatically improving the properties of the filler in the alumina powder. This is expected to contribute to the improvement of resin compositions for electronic devices.
Claims
1. Alumina particles derived from metallic aluminum, The content of uranium element in the alumina particles is 5 ppb or less, The content of thorium element in the alumina particles is 5 ppb or less, The content of metallic aluminum in the alumina particles is 5 ppm or less, The sodium content in the alumina particles is 10 ppm or less, The iron content in the alumina particles is 10 ppm or less. High purity alumina particles.
2. 2. The high purity alumina particles according to claim 1, wherein the amount of residual aluminum particles having a particle size of 20 μm or more derived from the raw material aluminum metal is 10 or less per 50 g of the alumina particles.
3. A composition comprising the high-purity alumina particles according to claim 1 and a resin composition. A resin composition for electronic devices comprising:
4. 2. A method for producing high purity alumina particles according to claim 1, comprising the steps of: a granulation step in which metallic aluminum powder is introduced into a flame to vaporize and oxidize it, and then spherical alumina particles are obtained by spheroidization due to surface tension during cooling; a dissolving step of dissolving the metallic aluminum remaining in the spherical alumina particles by introducing the spherical alumina particles into a basic solution; and a drying step of drying the spherical alumina particles. A method for producing high purity alumina particles, comprising:
5. 5. The method for producing high purity alumina particles according to claim 4, wherein the basic solution is an aqueous solution of an amine compound.
6. 5. The method for producing high purity alumina particles according to claim 4, wherein in the dissolving step, the spherical alumina particles are dissolved in the basic solution having a pH of 9 or higher and a liquid temperature of 20 to 60°C to dissolve the metallic aluminum remaining in the spherical alumina particles.
7. The method for producing high purity alumina particles according to claim 4, wherein the spherical alumina particles are sieved in the dissolving step.
8. The method for producing high purity alumina particles according to claim 4, further comprising the step of washing the spherical alumina particles prior to the drying step.
9. A method for producing the resin composition for electronic devices according to claim 3, comprising the steps of: a granulation step in which metallic aluminum powder is introduced into a flame to vaporize and oxidize it, and then spherical alumina particles are obtained by spheroidization due to surface tension during cooling; a dissolving step of dissolving the metallic aluminum remaining in the spherical alumina particles by immersing the spherical alumina particles in a basic solution having a pH of 9 or more and a temperature of 20 to 60° C.; a drying step of drying the spherical alumina particles; and a resin dispersion step of dispersing the spherical alumina particles that have been subjected to the drying step in a resin composition to obtain a resin dispersion.
2. The method for producing a resin composition for electronic devices, comprising:
Citation Information
Patent Citations
Method for producing spherical silica powder and method for producing semiconductor sealing material
JP2012206870A
Manufacturing method of metal oxide particles, and manufacturing method of resin composition for electronic equipment
JP2014101239A
Cited By
Adhesive for tennis ball
US12344770B2
Adhesive for tennis ball
US12415902B2