Positive electrode active material powder, positive electrode containing the same, and lithium secondary battery
Perlithiated manganese-based oxide particles in a single or pseudo-single form address the gas generation and stability issues of conventional hyperlithiated manganese-based oxides, ensuring improved battery performance and life characteristics.
Patent Information
- Application Number
- JP2024523960
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-02-10
- Filing Date
- 2023-02-10
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2043-02-10
AI Technical Summary
Conventional lithium secondary batteries using hyperlithiated manganese-based oxides face issues with gas generation and reduced life characteristics due to changes in crystal structure and increased reaction area with the electrolyte, leading to particle cracking and deterioration.
The use of perlithiated manganese-based oxide particles in a single or pseudo-single particle form with an average diameter of 2.5 μm or less, which reduces particle cracking and electrolyte reaction area, enhancing stability and life characteristics.
This formulation minimizes gas generation and improves battery stability and resistance characteristics by reducing particle cracking and electrolyte interaction, while maintaining high capacity through oxygen-redox reactions.
Smart Images

Figure 2024539233000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0018479 filed on February 11, 2022, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.
[0002] The present invention relates to a positive electrode active material powder, a positive electrode and a lithium secondary battery including the same, and more particularly to a positive electrode active material powder including a perlithiated manganese-based oxide in the form of a single particle or pseudo-single particle, and a positive electrode and a lithium secondary battery including the same. [Background technology]
[0003] Recently, interest in energy storage technology has been gradually increasing, and as its application fields expand to include mobile phones, camcorders, and laptop PCs (personal computers), as well as the energy sources for electric vehicles, efforts in the research and development of electrochemical devices are gradually becoming more concrete.
[0004] Among electrochemical devices, there has been growing interest in the development of rechargeable secondary batteries. In particular, lithium secondary batteries, developed in the early 1990s, have been attracting attention due to their advantages of high operating voltage and extremely high energy density.
[0005] Lithium secondary batteries are generally manufactured by forming an electrode assembly by interposing a separator between a positive electrode including a positive electrode active material made of a lithium-containing transition metal oxide and a negative electrode including a negative electrode active material capable of storing lithium ions, inserting the electrode assembly into a battery case, injecting a non-aqueous electrolyte that serves as a medium for transferring lithium ions, and then sealing the battery case. The non-aqueous electrolyte is generally composed of a lithium salt and an organic solvent capable of dissolving the lithium salt.
[0006] Lithium secondary batteries developed to date mainly use lithium nickel oxide as the positive electrode active material, and carbon-based materials such as natural graphite and artificial graphite as the negative electrode active material. However, such conventional lithium secondary batteries do not fully meet the energy density required for electric vehicle batteries. Therefore, in order to achieve high capacity, a method of using a perlithiated manganese oxide containing excess lithium as the positive electrode active material, or a method of using a silicon-based negative electrode active material with a high theoretical capacity as the negative electrode active material is being actively considered.
[0007] In the case of perlithiated manganese oxides that contain an excess of lithium, the crystal structure is a mixture of a layered phase (LiMO2) and a rock salt phase (Li2MnO3), and as the rock salt phase becomes activated during the charge and discharge process, the capacity due to the oxygen redox reaction is further expressed, resulting in high capacity. However, there is a problem that a large amount of gas is generated during the oxygen-redox reaction, which changes the crystal structure of the positive electrode active material and reduces the life characteristics. Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made to solve the above problems, and aims to provide a positive electrode active material powder that generates little gas, can achieve excellent battery stability and life characteristics, and has excellent resistance characteristics, as well as a positive electrode and a lithium secondary battery using the same. [Means for solving the problem]
[0009] According to one embodiment, the present invention provides perlithiated manganese oxide particles represented by the following [Chemical Formula 1], the perlithiated manganese oxide particles being in the form of a single particle consisting of one nodule or a composite of 2 to 30 nodules, and having an average particle diameter D 50 The positive electrode active material powder has a particle size of 2.5 μm or less, preferably 0.5 μm to 2.5 μm, and more preferably 0.6 μm to 2.5 μm. [Chemical Formula 1] Li a Ni b Co c Mn d M e O2 In Chemical Formula 1 above, M is one or more selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr, 1 < a, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.1, 0.5 ≤ d < 1.0, 0 ≤ e ≤ 0.2, preferably 1.1 ≤ a ≤ 1.5, 0.1 ≤ b ≤ 0.4, 0 ≤ c ≤ 0.05, 0.50 ≤ d ≤ 0.80, 0 ≤ e ≤ 0.1, and more preferably 1.1 ≤ a ≤ 1.3, 0.2 ≤ b ≤ 0.4, 0 ≤ c ≤ 0.05, 0.50 ≤ d ≤ 0.70, 0 ≤ e ≤ 0.1.
[0010] Preferably, the positive electrode active material powder can be composed of positive electrode active material particles having at least one of the above single particle and pseudo single particle forms, and more preferably, it can be composed of positive electrode active material particles in single particle form.
[0011] The over-lithiated manganese-based oxide can have a crystallite size of 30 nm to 200 nm, preferably 40 nm to 150 nm, and more preferably 70 nm to 150 nm.
[0012] According to another embodiment, the present invention provides a positive electrode containing the positive electrode active material powder according to the present invention.
[0013] According to still another embodiment, the present invention provides a lithium secondary battery including a positive electrode containing the positive electrode active material powder according to the present invention, a negative electrode containing a negative electrode active material, a separator interposed between the positive electrode and the negative electrode, and an electrolyte.
Advantages of the Invention
[0014] Compared with conventional perlithiated manganese oxides having a secondary particle form, perlithiated manganese oxides having a single particle or pseudo single particle form have a smaller reaction area with the electrolyte and higher particle strength, so that there is less particle cracking due to rolling during electrode manufacture. Therefore, when perlithiated manganese oxides having a single particle or pseudo single particle form are used as a positive electrode active material as in the present invention, the amount of gas generation is significantly reduced, and thus the effect of improving the life characteristics and stability of the lithium secondary battery can be obtained.
[0015] In the present invention, the average particle size D 50 By using a small positive electrode active material powder having a particle size of 2.5 μm or less, it is possible to realize good output characteristics and resistance characteristics despite the single particle or pseudo single particle form.
[0016] In addition, the perlithiated manganese oxide contained in the positive electrode active material powder of the present invention has a crystal structure in which a rock salt Li2MnO3 phase and a layered LiM'O2 phase (wherein M' is Ni, Co, Mn) are mixed, and during the activation process, an excess amount of lithium is generated from the Li2MnO3 phase, which can be used to compensate for the irreversible capacity of the negative electrode active material. Therefore, when the positive electrode active material of the present invention is used, the use of a sacrificial anode material or prelithiation for compensating the negative electrode can be minimized, and the capacity of the positive electrode can be maximized. [Brief description of the drawings]
[0017] [Figure 1] 2 is a SEM photograph of the positive electrode active material powder prepared in Example 1. [Diagram 2] 2 is a SEM photograph of the positive electrode active material powder produced in Comparative Example 1. [Diagram 3] 1 is a SEM photograph of a positive electrode active material powder produced in Comparative Example 2. [Figure 4] 1 is a graph showing the resistance characteristics of lithium secondary batteries to which the positive electrode active materials of Examples 1 to 3 and Comparative Example 1 are applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The terms and words used in this specification and the claims are not to be interpreted in a limited manner to their ordinary or dictionary meanings, but are to be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0019] In the present invention, a "single particle" is a particle consisting of one single nodule. In the present invention, a "quasi-single particle" means a particle that is a complex formed of 30 or less nodules.
[0020] In the present invention, the term "nodule" refers to a particle unit body constituting a single particle or a quasi-single particle, and the nodule may be a single crystal lacking a crystalline grain boundary, or a polycrystal having no apparent grain boundary when observed at a magnification of 5,000 to 20,000 using a scanning electron microscope (SEM).
[0021] In the present invention, the term "secondary particle" refers to a particle formed by agglomeration of several tens to several hundreds of primary particles. More specifically, a secondary particle is an agglomeration of 40 or more primary particles.
[0022] The term "particle" as used in the present invention may include any one or all of single particles, quasi-single particles, primary particles, nodules, and secondary particles.
[0023] In the present invention, the "average particle size D 50 " means the particle size at 50% of the volume cumulative particle size distribution of the positive electrode active material powder. 50can be measured using the laser diffraction method. For example, the positive electrode active material powder is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000), and ultrasonic waves of about 28 kHz are irradiated at an output of 60 W. Then, a volume cumulative particle size distribution graph is obtained, and the particle diameter corresponding to 50% of the volume cumulative amount is obtained.
[0024] In the present invention, the average particle size of the primary particles or nodules can be measured by image analysis. Specifically, an image of the particles is obtained using a device such as a scanning electron microscope (SEM) or EBSD, the particle size of the primary particles or nodules confirmed from the obtained image is measured, and the arithmetic average value of these is calculated and measured as the average particle size.
[0025] In the present invention, the "crystalline size" can be quantitatively analyzed using X-ray diffraction analysis (XRD) using Cu-Kα X-rays. Specifically, the crystalline size can be quantitatively analyzed by placing the particles to be measured in a holder, irradiating the particles with X-rays, and analyzing the diffraction grating output. Sampling was performed by placing a powder sample of the particles to be measured in a groove in the center of a general powder holder, making the surface uniform using a slide glass, and making the height of the sample coincide with the periphery of the holder. Then, X-ray diffraction analysis was performed using a Bruker D8 Endeavor (light source: Cu Kα, λ=1.54Å) equipped with a LynxEye XE-T position sensitive detector under the conditions of FDS0.5°, step size 0.02°, and total scan time of about 20 minutes for the region of 2θ=15° to 90°. The measured data were subjected to Rietveld refinement, taking into account the charge at each site (metal ions at transition metal sites are +3, Ni ions at Li sites are +2) and cation mixing. When analyzing the grain size, instrumental broadening was considered using the Fundamental Parameter Approach (FPA) implemented in the Bruker TOPAS program, and the entire peak of the measurement range was used during fitting. Peak shape was fitted using only the Lorenzian contribution as the first principle (FP) among the peak types available in TOPAS, where strain was not considered.
[0026] As a result of intensive research to solve the problems of gas generation and deterioration of life characteristics in secondary batteries applying over-lithiated manganese-based oxides, the inventors have formed the over-lithiated manganese-based oxides into single particles consisting of one nodule or pseudo-single particle forms that are composites of 30 nodules or less, and the average particle size D 50 is adjusted to 2.5 μm or less, by which not only the amount of gas generation can be reduced and the life characteristics can be significantly improved, but also excellent resistance / output characteristics can be realized, and thus the present invention has been completed.
[0027] Hereinafter, the present invention will be described in more detail.
[0028] The positive electrode active material powder according to the present invention contains over-lithiated manganese-based oxide particles represented by the following [Chemical Formula 1]. The over-lithiated manganese-based oxide particles are in the form of single particles consisting of one nodule or pseudo-single particle forms that are composites of 2 to 30 nodules or less, and the average particle size D 50 of the positive electrode active material powder is 2.5 μm or less, preferably 0.5 μm to 2.5 μm, and more preferably 0.6 μm to 2.5 μm.
[0029] [Chemical Formula 1] Li a Ni b Co c Mn d M e O2
[0030] In the above Chemical Formula 1, M is one or more selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr, 1 < a, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.1, 0.5 ≤ d < 1.0, 0 ≤ e ≤ 0.2, preferably 1.1 ≤ a ≤ 1.5, 0.1 ≤ b ≤ 0.4, 0 ≤ c ≤ 0.05, 0.50 ≤ d ≤ 0.80, 0 ≤ e ≤ 0.1, and more preferably 1.1 ≤ a ≤ 1.3, 0.2 ≤ b ≤ 0.4, 0 ≤ c ≤ 0.05, 0.50 ≤ d ≤ 0.70, 0 ≤ e ≤ 0.1.
[0031] Positive electrode active material powder The positive electrode active material powder according to the present invention includes perlithiated manganese oxide particles in the form of a single particle consisting of one nodule or a quasi-single particle that is a composite of 2 to 30 nodules. Preferably, the positive electrode active material powder may be composed of perlithiated manganese oxide particles having at least one of the form of the single particle and the quasi-single particle.
[0032] Conventional perlithiated manganese oxide particles are generally in the form of spherical secondary particles formed by agglomeration of tens to hundreds of primary particles. However, in the case of secondary particles formed by agglomeration of many primary particles, there is a problem that primary particles are easily detached during the rolling process during the manufacture of the positive electrode, and cracks are generated inside the particles during the charge and discharge process. In addition, there is a problem that the contact area with the electrolyte increases, which increases gas generation and active material deterioration due to side reactions with the electrolyte, thereby reducing the life characteristics.
[0033] However, when perlithiated manganese-based oxide particles are formed in the form of single particles or pseudo-single particles as in the present invention, the particle strength is higher than that of conventional perlithiated manganese-based oxide particles in the form of secondary particles, so there is less particle cracking during rolling, and since the number of sub-particle units (i.e., nodules) constituting the particles is small, there is less change due to the volume expansion and contraction of the sub-particle units during charging and discharging, and the occurrence of cracks inside the particles is significantly reduced. In addition, the single particles or pseudo-single particles have a smaller reaction area with the electrolyte than secondary particles, so gas generation due to side reactions with the electrolyte is also reduced.
[0034] The perlithiated manganese oxide particles according to the present invention may have a composition represented by the following [Chemical Formula 1].
[0035] [Chemical formula 1] Li a Ni b Co c Mn d M e O2
[0036] In the above Chemical Formula 1, M can be one or more selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr.
[0037] On the other hand, a is the molar ratio of Li in the over-lithiated manganese-based oxide, and it can be 1 < a, 1.1 ≤ a ≤ 1.5, or 1.1 ≤ a ≤ 1.3. When a satisfies the above range, a crystal structure in which a layered phase and a rock salt phase coexist can be formed. During charge and discharge, it is possible to realize the capacity by the oxidation-reduction reaction (oxygen redox) of oxygen, and high-capacity characteristics can be realized.
[0038] The above b is the molar ratio of Ni in the over-lithiated manganese-based oxide, and it can be 0 ≤ b ≤ 0.5, 0.1 ≤ b ≤ 0.4, or 0.2 ≤ b ≤ 0.4.
[0039] The above c is the molar ratio of Co in the over-lithiated manganese-based oxide, and it can be 0 ≤ c ≤ 0.1, 0 ≤ c ≤ 0.08, or 0 ≤ c ≤ 0.05. When c exceeds 0.1, it is difficult to ensure a high capacity, and gas generation and deterioration of the positive electrode active material become severe, and the life characteristics may deteriorate.
[0040] The above d is the molar ratio of Mn in the over-lithiated manganese-based oxide, and it can be 0.5 ≤ d < 1.0, 0.50 ≤ d ≤ 0.80, or 0.50 ≤ d ≤ 0.70. When d is less than 0.5, the ratio of the rock salt phase becomes excessively small, and the capacity improvement effect is not significant.
[0041] The above e is the molar ratio of the doping element M in the over-lithiated manganese-based oxide, and it can be 0 ≤ e ≤ 0.2, 0 ≤ e ≤ 0.1, or 0 ≤ e ≤ 0.05. If the content of the doping element is too large, it may have an adverse effect on the capacity of the active material.
[0042] The perlithiated manganese oxide has a crystal structure in which a layered phase (LiMO2) and a rock salt phase (Li2MnO3) are mixed. The rock salt phase is activated at a high voltage of 4.4 V or more, which enables further capacity to be achieved through the oxygen-oxidation-reduction reaction during charging and discharging, thereby enabling the realization of a high capacity.
[0043] Meanwhile, in the perlithiated manganese oxide represented by the formula 1, the ratio of the number of moles of Li to the number of moles of all metal elements other than Li (Li / Me) can be 1.2 to 1.5, 1.25 to 1.5, or 1.25 to 1.4. When the Li / Me ratio is within the above range, the rate characteristics and capacity characteristics are excellent. If the Li / Me ratio is too high, the electrical conductivity decreases and the rock salt phase (Li2MnO3) increases, which may increase the rate of deterioration, while if the Li / Me ratio is too low, there is little effect in improving the energy density.
[0044] Meanwhile, the composition of the perlithiated manganese oxide may be represented by the following [Chemical Formula 2].
[0045] [Chemical formula 2] XLi2MnO3·(1-X)Li[Ni 1-y-z-w Mn y Co z M w ]O2
[0046] In the above [Chemical Formula 2], M may be at least one selected from the group consisting of metal ions Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr.
[0047] The X means the ratio of the Li2MnO3 phase in the perlithiated manganese oxide, and may be 0.2≦X≦0.5, 0.25≦X≦0.5, or 0.25≦X≦0.4. When the ratio of the Li2MnO3 phase in the perlithiated manganese oxide satisfies the above range, high capacity characteristics can be achieved.
[0048] The y is LiM'O2 (where M' = Ni 1-y-z-w Mn yCo z M w ) the molar ratio of Mn in the layered phase, which can be 0.4≦y<1, 0.4≦y≦0.8, or 0.4≦y≦0.7.
[0049] The z is a molar ratio of Co in the LiM'O2 layered phase, and may be 0≦z≦0.1, 0≦z≦0.08, or 0≦z≦0.05. If z exceeds 0.1, gas generation and deterioration of the positive electrode active material may become severe, resulting in reduced life characteristics.
[0050] The w is the molar ratio of the doping element M in the LiM'O2 layered phase, and can be 0≦w≦0.2, 0≦w≦0.1, or 0≦w≦0.05.
[0051] Meanwhile, in the perlithiated manganese oxide, the average particle size of the nodules may be 0.5 μm or more, 1.0 μm or more, or 1.5 μm or more, and may be 3.5 μm or less, 3 μm or less, 2.5 μm or less, or 2.0 μm or less. The average particle size of the nodules may be 0.5 μm to 3.5 μm. For example, the average particle size of the nodules may be 0.5 μm to 3.5 μm, 0.5 μm to 3 μm, 1 μm to 3 μm, or 1 μm to 2.5 μm. If the average particle size of the nodules is less than 0.5 μm, the overall specific surface area of the positive electrode active material may increase, and electrolyte side reactions may increase, and if it exceeds 3.5 μm, the lithium mobility in the positive electrode active material may decrease, and the output characteristics of the battery may decrease.
[0052] In addition, the perlithiated manganese oxide may have a crystalline size of 30 nm to 200 nm, preferably 40 nm to 150 nm, and more preferably 70 nm to 150 nm. When the crystallite size is within the above range, the degree of completion of the crystal structure can be improved and excellent electrochemical performance can be ensured. If the crystallite size is too small, the crystal structure cannot be properly formed and the stability of the crystal structure can be reduced, which can reduce the life performance and increase gas generation. On the other hand, if the crystal size is too large, the structural stability increases, but an impurity structure can be generated on the surface, which can increase the resistance, and the Li migration path can be lengthened, which can reduce the rate characteristics.
[0053] Meanwhile, the perlithiated manganese-based oxide may be prepared by mixing a transition metal precursor and a lithium source material and then calcining the mixture.
[0054] Examples of the lithium source material include lithium-containing carbonates (e.g., lithium carbonate, etc.), hydrates (e.g., lithium hydroxide hydrate (LiOH·H2O), etc.), hydroxides (e.g., lithium hydroxide), nitrates (e.g., lithium nitrate (LiNO3), etc.), and chlorides (e.g., lithium chloride (LiCl), etc.), and among these, one kind may be used alone or two or more kinds may be used in combination.
[0055] Meanwhile, the transition metal precursor may be in the form of a hydroxide, oxide or carbonate. When a precursor in the form of a carbonate is used, it is more preferable in that a positive electrode active material having a relatively high specific surface area can be prepared.
[0056] The transition metal precursor may be prepared by a co-precipitation process. For example, the transition metal precursor may be prepared by dissolving each transition metal-containing raw material in a solvent to prepare a metal solution, mixing the metal solution, an ammonium cation complexing agent, and a basic compound, and then performing a co-precipitation reaction. If necessary, an oxidizing agent or oxygen gas may be further added during the co-precipitation reaction.
[0057] Here, the transition metal-containing raw material may be acetate, carbonate, nitrate, sulfate, halide, sulfide, etc. of each transition metal. Specifically, the transition metal-containing raw material may be NiO, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, Mn2O3, MnO2, Mn3O4, MnCO3, Mn(NO3)2, MnSO4·H2O, manganese acetate, manganese halide, cobalt oxide, cobalt nitrate, cobalt sulfate, cobalt carbonate, cobalt acetate, cobalt halide, etc.
[0058] The ammonium cation complexing agent can be one or more selected from the group consisting of NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, and NH4CO3.
[0059] The basic compound may be one or more selected from the group consisting of NaOH, Na2CO3, KOH, and Ca(OH)2. The form of the precursor may vary depending on the type of basic compound used. For example, when NaOH is used as the basic compound, a precursor in the form of a hydroxide is obtained, and when Na2CO3 is used as the basic compound, a precursor in the form of a carbonate is obtained. Also, when a basic compound and an oxidizing agent are used together, a precursor in the form of an oxide is obtained.
[0060] Meanwhile, the transition metal precursor and the lithium source material may be mixed in an amount such that the total transition metal (Ni+Co+Mn):Li molar ratio is 1:1.05 to 1:2, preferably 1:1.1 to 1:1.8, and more preferably 1:1.3 to 1:1.8.
[0061] Meanwhile, the calcination is carried out at a temperature at which single particles or pseudo-single particles can be formed. In order to form single particles or pseudo-single particles, the calcination should be carried out at a higher temperature than that used in the manufacture of conventional lithium transition metal composite oxides in the form of secondary particles. For example, when the composition of the precursor is the same, the calcination should be carried out at a temperature about 30°C to 100°C higher than that used in the manufacture of conventional lithium transition metal composite oxides in the form of secondary particles. The calcination temperature for forming single particles or pseudo-single particles may vary depending on the composition of the metal in the precursor, and may be, for example, about 800°C to 1100°C, preferably about 950°C to 1050°C.
[0062] The firing may be carried out for 5 to 35 hours in an oxygen atmosphere. Here, the oxygen atmosphere refers to an atmosphere containing a sufficient amount of oxygen for firing, including an air atmosphere. In particular, it is preferable to carry out the firing in an atmosphere having a higher oxygen partial pressure than the air atmosphere.
[0063] Meanwhile, the positive electrode active material according to the present invention may further include a coating layer on the surface of the perlithiated manganese-based oxide particles, if necessary.
[0064] When the positive electrode active material includes a coating layer, the coating layer prevents contact between the perlithiated manganese oxide and the electrolyte, thereby reducing electrolyte side reactions, thereby providing better effects in reducing gas generation and improving life characteristics.
[0065] The coating layer is a coating element M 1 The coating element M 1 may be, for example, one or more selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr and Zr, preferably Al, Co, Nb, W and combinations thereof, more preferably Al, Co and combinations thereof. 1may contain two or more elements, for example, Al and Co. The coating elements are in the form of oxides in the coating layer, i.e., M 1 It can exist as Oz, where 1≦z≦4.
[0066] The coating layer can be formed by dry coating, wet coating, chemical vapor deposition (CVD), physical vapor deposition (PVD), atomic layer deposition (ALD), etc. Among them, the coating layer is preferably formed by atomic layer deposition, since it can be formed to have a large area.
[0067] The area on which the coating layer is formed may be 10 to 100%, preferably 30 to 100%, and more preferably 50 to 100%, of the total surface area of the perlithiated manganese oxide particles.
[0068] On the other hand, the positive electrode active material powder according to the present invention has an average particle size D 50 The average particle diameter D may be 2.5 μm or less, preferably 0.5 μm to 2.5 μm, and more preferably 0.6 μm to 2.5 μm. As described above, the positive electrode active material in the form of single particle or pseudo single particle has the advantage of excellent particle strength, small contact area with the electrolyte, suppressing gas generation, and thus realizing excellent life characteristics. However, since there are few interfaces between primary particles that become the migration path of lithium ions inside the positive electrode active material particles, lithium mobility is lower than that of a positive electrode active material in the form of secondary particles, and in the process of over-firing at high temperatures to form single particles, a rock salt phase with no electrical activity is formed on the surface of the particles, resulting in an increase in resistance. Such an increase in resistance becomes more severe as the particle size increases, and the increase in resistance leads to a decrease in capacity and output characteristics. Therefore, in the present invention, the average particle diameter D 50 By using small positive electrode active material powder with a particle size of 2.5 μm or less, the movement distance of lithium ions inside the positive electrode active material particles is minimized, thereby minimizing the decrease in lithium mobility and the increase in resistance.
[0069] The positive electrode active material powder has a BET specific surface area of 0.5 to 5 m 2 / g or 1~3m 2 / g. When the BET specific surface area of the positive electrode active material powder satisfies the above range, appropriate electrochemical properties can be ensured. If the specific surface area is too small, the electrochemical properties can be deteriorated as the reaction sites are reduced, and if it is too large, the reaction area with the electrolyte increases, which can activate side reactions at high voltages.
[0070] In addition, the positive electrode active material powder according to the present invention preferably has an initial irreversible capacity of about 5 to 70%, 5 to 50%, or 10 to 30%. When the initial irreversible capacity of the positive electrode active material satisfies the above range, the irreversible capacity of the silicon-based negative electrode active material can be compensated for without a separate compensation material such as a sacrificial anode material or a prior lithium compensation process such as prelithiation.
[0071] positive electrode Next, the positive electrode according to the present invention will be described.
[0072] The positive electrode according to the present invention includes a positive electrode active material powder including a perlithiated manganese oxide in the form of a single particle or a pseudo single particle according to the present invention. Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector and including the positive electrode active material powder. The positive electrode active material powder has been described above, so the remaining components will be described below.
[0073] In the positive electrode, the positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can usually have a thickness of 3 to 500 μm, and fine irregularities can be formed on the surface of the positive electrode current collector to increase the adhesive force of the positive electrode active material. For example, it can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0074] Meanwhile, the positive electrode active material layer may contain a conductive material and a binder in addition to the positive electrode active material powder.
[0075] The conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery that is constructed and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and one or more of these can be used alone or in combination. The conductive material can usually be contained in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, based on the total weight of the positive electrode active material layer.
[0076] The binder serves to improve the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, more preferably 1 to 10% by weight, based on the total weight of the positive electrode active material layer.
[0077] The positive electrode may be manufactured by a conventional method for manufacturing a positive electrode. For example, the positive electrode may be manufactured by mixing a positive electrode active material, a binder, and / or a conductive material in a solvent to prepare a positive electrode slurry, applying the positive electrode slurry onto a positive electrode current collector, and then drying and rolling the positive electrode slurry. Here, the types and contents of the positive electrode active material, binder, and conductive material are as described above.
[0078] The solvent may be a solvent commonly used in the art, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., and one or more of these may be used alone or in combination. The amount of the solvent used is sufficient to have a viscosity that can dissolve or disperse the positive electrode active material, conductive material, and binder and provide excellent thickness uniformity during subsequent coating for the production of a positive electrode, taking into consideration the coating thickness of the slurry and the manufacturing yield.
[0079] Alternatively, the positive electrode can be produced by casting the positive electrode slurry on a separate support, peeling the resulting film from the support, and laminating the film on a positive electrode current collector.
[0080] Lithium secondary battery The lithium secondary battery of the present invention comprises a positive electrode containing the positive electrode active material powder of the present invention, a negative electrode containing a negative electrode active material, a separator interposed between the positive electrode and the negative electrode, and an electrolyte.
[0081] When using the positive electrode active material powder according to the present invention, a high energy density can be achieved by performing an activation process at a high voltage of 4.6 V or more, and then repeating charge and discharge at a charge cut-off voltage of 4.2 to 4.5 V, and deterioration of life characteristics due to gas generation can be minimized.
[0082] In addition, since the perlithiated manganese-based oxide represented by Chemical Formula 1 has a high initial irreversible capacity, even when it is used together with a negative electrode active material having a large irreversible capacity such as a silicon-based negative electrode active material, it is possible to minimize the addition of a sacrificial anode material or prelithiation for compensating for the irreversible capacity of the negative electrode active material.
[0083] The positive electrode has been described above, so the remaining components will be described below.
[0084] negative electrode The negative electrode according to the present invention includes a negative electrode active material layer including a negative electrode active material, and the negative electrode active material layer may further include a conductive material and / or a binder, if necessary.
[0085] The negative electrode active material may be any of various negative electrode active materials used in the art, such as silicon-based negative electrode active materials, carbon-based negative electrode active materials, metal alloys, and the like.
[0086] Preferably, the negative electrode active material includes a silicon-based negative electrode active material.
[0087] Silicon-based negative electrode active materials have a higher theoretical capacity and a faster reaction rate with lithium than carbon-based negative electrode active materials, and therefore, when a silicon-based negative electrode active material is included in a negative electrode, the energy density and rapid charging performance are improved. However, silicon-based negative electrode active materials have a large irreversible capacity and a large volume expansion during charging and discharging, which results in poor life characteristics. In particular, when used in combination with a perlithiated manganese oxide that generates a lot of gas, there is a problem that the deterioration of life characteristics becomes even more severe. However, when a perlithiated manganese oxide in the form of a single particle or pseudo-single particle is applied as in the present invention, the deterioration of life characteristics can be minimized because less gas is generated than in the conventional perlithiated manganese oxide in the form of a secondary particle, and the excess lithium generated from the rock salt phase during the activation process of the perlithiated manganese oxide can compensate for the irreversible capacity of the silicon-based negative electrode active material.
[0088] The silicon-based negative electrode active material is, for example, Si, SiOw (where 0 < w ≦ 2), Si-C composite, Si-M a alloy (M a is one or more selected from the group consisting of Al, Sn, Mg, Cu, Fe, Pb, Zn, Mn, Cr, Ti, Ni) or a combination thereof.
[0089] On the other hand, the silicon-based negative electrode active material can be doped with M b metal as needed, where the M b metal can be a Group 1 alkali metal element and / or a Group 2 alkaline earth metal element, and can be, for example, Li, Mg, etc. Specifically, the silicon negative electrode active material is Si, SiO b doped with M w (where 0 < w ≦ 2), Si-C composite, etc. In the case of a metal-doped silicon-based negative electrode active material, although the active material capacity decreases due to the doping element, high efficiency can achieve a high energy density.
[0090] In addition, the silicon-based negative electrode active material can further include a carbon coating layer on the surface of the particles as needed. Here, the carbon coating amount can be 20 wt% or less, preferably 0.1 - 20 wt% based on the total weight of the silicon-based negative electrode active material. When applying the carbon coating, the electrical conductivity of the surface of silicon is improved, the uniformity of the SEI layer is improved, and the initial efficiency and life characteristics are improved.
[0091] The carbon coating layer can be formed by methods such as dry coating, wet coating, chemical vapor deposition (CVD), physical vapor deposition (PVD), atomic layer deposition (ALD).
[0092] On the other hand, the silicon-based negative electrode active material has a capacity of 1000 to 4000 mAh / g, preferably 1000 to 3800 mAh / g, and more preferably 1200 to 3800 mAh / g. When a silicon-based negative electrode active material that satisfies the above capacity range is used, high capacity characteristics can be realized.
[0093] The silicon-based negative electrode active material may have an initial efficiency of 60 to 95%, 70 to 95%, and preferably 75 to 95%. The initial efficiency of the silicon-based negative electrode active material means a percentage of a discharge capacity relative to a charge capacity measured by charging and discharging between 0.01 V and 1.5 V at a 0.1 C rate after preparing a half cell using a negative electrode that uses 100% silicon-based negative electrode active material as a negative electrode active material and a lithium counter electrode. When the initial efficiency of the silicon-based negative electrode active material satisfies the above range, lithium provided from the positive electrode can be reversibly used, and excellent rapid charging performance can be realized.
[0094] The particle diameter of the silicon-based negative electrode active material is D 50 is 3 μm to 8 μm, preferably 4 μm to 7 μm, and D min ~D max When the particle size of the silicon-based negative electrode active material falls within the above range, sufficient electrode density can be ensured when mixed with a carbon-based negative electrode or used alone.
[0095] In addition, the negative electrode may further include a carbon-based negative electrode active material as a negative electrode active material, if necessary. The carbon-based negative electrode active material may be, for example, artificial graphite, natural graphite, graphitized carbon fiber, amorphous carbon, soft carbon, hard carbon, etc., but is not limited thereto.
[0096] Meanwhile, the silicon-based negative electrode active material may be included in an amount of 1 to 100 wt%, 1 to 50 wt%, 1 to 30 wt%, 1 to 15 wt%, 10 to 70 wt%, or 10 to 50 wt%, based on the total weight of the negative electrode active material.
[0097] The carbon-based negative electrode active material may be included in an amount of 0 to 99 wt%, 50 to 99 wt%, 70 to 99 wt%, 85 to 99 wt%, 30 to 90 wt%, or 50 to 90 wt%, based on the total weight of the negative electrode active material.
[0098] According to one embodiment, the negative electrode active material may be a mixture of a silicon-based negative electrode active material and a carbon-based negative electrode active material, and the mixing ratio of the silicon-based negative electrode active material to the carbon-based negative electrode active material may be 1:99 to 50:50, preferably 3:97 to 30:70, by weight. When the mixing ratio of the silicon-based negative electrode active material to the carbon-based negative electrode active material satisfies the above range, the capacity characteristics can be improved and the volume expansion of the silicon-based negative electrode active material can be suppressed, thereby ensuring excellent cycle performance.
[0099] The negative electrode active material may be included in an amount of 80 to 99 wt % based on the total weight of the negative electrode active material layer. When the content of the negative electrode active material is in this range, excellent capacity characteristics and electrochemical characteristics can be obtained.
[0100] Examples of the conductive material include spherical or flaky graphite; carbonaceous materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, single-walled carbon nanotubes, and multi-walled carbon nanotubes; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and one or more of these may be used alone or in combination. The conductive material may be included in an amount of 0.1 to 30% by weight, 1 to 20% by weight, or 1 to 10% by weight based on the total weight of the negative electrode active material layer.
[0101] Preferably, the conductive material may be a single-walled carbon nanotube. When the single-walled carbon nanotube is used as the conductive material, a conductive path is uniformly formed on the surface of the negative electrode active material, thereby improving cycle characteristics.
[0102] Examples of the binder include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylic acid, polyacrylamide, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 to 20% by weight, 2 to 20% by weight, or 2 to 10% by weight based on the total weight of the negative electrode active material layer.
[0103] The negative electrode may have a single-layered or multi-layered structure in which the negative electrode active material layer is composed of two or more layers. When the negative electrode active material layer is composed of two or more layers, each layer may have a different type and / or content of the negative electrode active material, binder and / or conductive material. For example, the negative electrode according to the present invention may have a lower layer with a higher content of the carbon-based negative electrode active material than the upper layer, and the upper layer with a higher content of the silicon-based negative electrode active material. In this case, the effect of improving the fast charging performance can be obtained compared to the case in which the negative electrode active material layer is formed as a single layer.
[0104] The negative electrode active material layer may have a porosity of 20% to 70% or 20% to 50%. If the porosity of the negative electrode active material layer is too small, the electrolyte impregnation property may decrease, and the lithium mobility may decrease, whereas if the porosity is too large, the energy density may decrease.
[0105] Meanwhile, the lithium secondary battery of the present invention is preferably configured so that the N / P ratio, which is the ratio of the negative electrode discharge capacity to the positive electrode discharge capacity, is different depending on the type of negative electrode active material used.
[0106] For example, when a mixture of SiO and a carbon-based negative electrode active material is used as the negative electrode active material, the N / P ratio may be about 100% to 150%, preferably about 100% to 140%, and more preferably about 100% to 120%. If the negative electrode discharge capacity relative to the positive electrode discharge capacity deviates from the above range, the balance between the positive electrode and the negative electrode is not achieved, and the life characteristics may decrease or lithium deposition may occur.
[0107] When 100% of Si is used as the negative electrode active material, the N / P ratio may be about 150% to 300%, preferably about 160% to 300%, and more preferably about 180% to 300%. If the negative electrode discharge capacity relative to the positive electrode discharge capacity deviates from the above range, the balance between the positive electrode and the negative electrode is not achieved, and the life characteristics may decrease or lithium deposition may occur.
[0108] The negative electrode may be manufactured by a method for manufacturing a negative electrode well known in the art. For example, the negative electrode may be manufactured by applying a negative electrode slurry, which is prepared by dissolving or dispersing a negative electrode active material and, optionally, a binder and a conductive material in a solvent, onto a negative electrode current collector, followed by rolling and drying, or by casting the negative electrode slurry onto a separate support, peeling off the support, and laminating the resulting film onto the negative electrode current collector.
[0109] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may have a thickness of usually 3 μm to 500 μm, and like the positive electrode current collector, the surface of the current collector may be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0110] The solvent may be a solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., and one or more of these may be used alone or in combination. The amount of the solvent used is not particularly limited as long as it can be adjusted to an appropriate viscosity of the negative electrode slurry in consideration of the coating thickness of the negative electrode mixture, production yield, workability, etc.
[0111] Separator In the lithium secondary battery of the present invention, the separator separates the negative electrode and the positive electrode to provide a path for lithium ions to move, and any separator that is generally used in lithium secondary batteries can be used without any particular limitation, and in particular, a separator that has low resistance to ion movement of the electrolyte and has excellent electrolyte humidification ability is preferred. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting glass fiber, polyethylene terephthalate fiber, etc. can be used. In addition, a coated separator containing a ceramic component or a polymeric material can be used to ensure heat resistance or mechanical strength, and can be selectively used in a single-layer or multi-layer structure.
[0112] electrolyte Examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.
[0113] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0114] The organic solvent can be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of solvents that can be used include carbonate-based solvents such as polycarbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a straight-chain, branched or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; and sulfolanes.
[0115] The lithium salt can be used without any particular limitation as long as it is a compound that can provide lithium ions used in lithium secondary batteries. Specifically, the anion of the lithium salt is F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 -, CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - The lithium salt may be one or more selected from the group consisting of LiPF6, LiN(FSO2)2, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, LiB(C2O4)2, etc. The lithium salt may be used in a concentration range of 0.1M to 5.0M.
[0116] The electrolyte may contain additives for the purpose of improving the life characteristics of the battery, suppressing the capacity decrease, suppressing gas generation, etc. Examples of the additives include various additives used in the art, such as fluoroethylene carbonate (FEC), vinylene carbonate (VC), vinyl ethylene carbonate (VEC), ethylene sulfate (ESa), lithium difluorophosphate (LiPO2F2), lithium bisoxalate borate (LiBOB), lithium tetrafluoroborate (LiBF4), lithium difluorooxalate borate (LiDFOB), lithium difluorobisoxalate phosphate (LiDFBP), lithium tetrafluorooxalate phosphate (LiTFOP), lithium methyl sulfate (LiMS), lithium ethyl sulfate (LiES), propane sultone (PS), propene sultone (PRS), succinonitrile (SN), and adiponitrile (AND). , 1,3,6-hexene tricarbonitrile (HTCN), 1,4-dicyano-2-butene (DCB), fluorobenzene (FB), ethyl di(prop-2-ynyl)phosphate (EDP), 5-methyl-5-propargyloxylcarbonyl-1,3-dioxane-2-one (MPOD), a compound represented by the following chemical formula A (Chemical formula 1) (e.g., cyanoethyl polyvinyl alcohol, PVA-CN), a compound represented by the following chemical formula B (Chemical formula 2) (e.g., heptafluorobutyl cyanoethyl polyvinyl alcohol, PF-PVA-CN), a compound represented by the following chemical formula C (Chemical formula 3) (e.g., propargyl 1H-imidazole-1-carboxylate, PAC), and / or a compound represented by the following chemical formula D (Chemical formula 4) (e.g., aryl imidazole such as CHN), etc. may be used.
[0117] [ka]
[0118] In the above chemical formula A, m and n each independently represent an integer of 1-100.
[0119] [ka]
[0120] [ka]
[0121] In the above chemical formula C, R 16 is a linear or non-linear alkylene group having 1 to 3 carbon atoms; R 17 ~R 19 are each independently at least one selected from the group consisting of hydrogen, an alkyl group having 1 to 3 carbon atoms, and -CN, and D is CH or N.
[0122] [ka]
[0123] In the above chemical formula D, R1, R2, R3, and R4 each independently represent hydrogen; or an alkyl group having 1 to 5 carbon atoms, a cyano group (CN), an allyl group, a propargyl group, an amine group, a phosphate group, an ether group, a benzene group, a cyclohexyl group, a silyl group, an isocyanate group (-NCO), or a fluoro group (-F).
[0124] Preferably, the additive may be a compound that acts as an oxygen scavenger. In addition to tristri(methylsilyl)phosphite (TMSPi), tristrimethylphosphite (TMPi), tris(2,2,2-trifluoroethyl)phosphite (TTFP), phosphite-based materials (see Chemical Formula E (Chemical Formula 5)), tristri(methylsilyl)phosphate (TMSPa), polyphosphate trimethylsilyl ester (PPSE), tris(pentafluorophenyl)borane (TPFPB), coumarin-3-carbonitrile (CMCN), 7-ethynylcoumarin (ECM), 3-a Compounds that can be used as oxygen scavengers include cetylcoumarin (AcCM), 3-[(trimethylsilyl)oxyl]-2H-1-benzopyran-2-one (TMSOCM), 3-(trimethylsilyl)coumarin (TMSCM), 3-(2-propyn-1-yloxyl)-2H-1-benzopyran-2-one (POCM), 2-propyn-1-yl-2-iodine-2H-1-benzopyran-3-carboxylate (OBCM), and compounds containing a coumarin structure (see chemical formula F (chemical formula 6)).
[0125] [ka]
[0126] [ka]
[0127] In the chemical formulas E and F, R1 to R6 are each independently a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms and a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, and may include cyan (nitrile), fluoro (F), ether (COC), carboxyl (OC=O), trimethylsilyl (-TMS), isocyanate (-NCO), and / or isothiocyanate (-NCS) functional groups.
[0128] The lithium secondary battery according to the present invention can be usefully used in portable devices such as mobile phones, notebook computers, and digital cameras, and in electric vehicles such as hybrid electric vehicles (HEVs).
[0129] Therefore, according to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.
[0130] The battery module or battery pack may be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0131] The external shape of the lithium secondary battery of the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.
[0132] The lithium secondary battery according to the present invention can be used as a battery cell used as a power source for a small device, and can also be preferably used as a unit battery in a medium- to large-sized battery module including a large number of battery cells.
[0133] The present invention will now be described in detail with reference to specific examples.
[0134] Example 1 Average particle size D 50 Ni with a thickness of 0.8 μm 0.25 Mn 0.75(OH)2 and lithium hydroxide (LiOH) were added to a Henschel mixer (700 L) so that the molar ratio of Li:transition metals (Ni+Mn) was 1.4:1, and mixed at 300 rpm for 20 minutes. The mixed powder was placed in an alumina crucible of 330 mm x 330 mm size, and maintained at 500°C for 10 hours in an oxygen atmosphere, and then fired at 850°C for 30 hours to produce a positive electrode active material powder. A SEM image of the produced positive electrode active material powder is shown in Figure 1. Referring to Figure 1, it can be seen that the produced positive electrode active material powder has a single particle morphology.
[0135] Example 2 Average particle size D 50 Ni with a thickness of 1.0 μm 0.35 Mn 0.65 (OH)2 and lithium hydroxide (LiOH) were added to a Henschel mixer (700L) so that the molar ratio of Li:transition metals (Ni+Mn) was 1.33:1, and mixed at 300 rpm for 20 minutes. The mixed powder was placed in an alumina crucible of 330mm x 330mm size, and kept at 500℃ in an oxygen atmosphere for 10 hours, and then calcined at 850℃ for 30 hours to produce perlithiated manganese oxide.
[0136] The perlithiated manganese oxide and aluminum oxide were mixed and then heat-treated to prepare a positive electrode active material powder in which the surface of the perlithiated manganese oxide was coated with 1500 ppm of Al.
[0137] Example 3 Average particle size D 50 Ni with a thickness of 1.8 μm 0.25 Mn 0.75 (OH)2 and lithium hydroxide (LiOH) were added to a Henschel mixer (700L) so that the molar ratio of Li:transition metals (Ni+Mn) was 1.4:1, and mixed at 300 rpm for 20 minutes. The mixed powder was placed in an alumina crucible of 330mm x 330mm size, and maintained at 500℃ in an oxygen atmosphere for 10 hours, and then calcined at 880℃ for 30 hours to produce a positive electrode active material powder.
[0138] Comparative Example 1 D 50 Ni with a thickness of 3 μm 0.25 Mn 0.75 (OH)2 powder and lithium hydroxide (LiOH) were added to a Henschel mixer (700 L) so that the molar ratio of Li:transition metals (Ni+Mn) was 1.4:1, and mixed at 300 rpm for 20 minutes. The mixed powder was placed in an alumina crucible of 330 mm x 330 mm size and fired at 900°C for 10 hours in an oxygen atmosphere to produce a positive electrode active material powder. An SEM image of the produced positive electrode active material powder is shown in Figure 2. Referring to Figure 2, it can be seen that the particles of the produced positive electrode active material have a pseudo-single particle morphology.
[0139] Comparative Example 2 A positive electrode active material powder was prepared in the same manner as in Comparative Example 1, except that after maintaining at 500°C for 10 hours, the material was calcined at 850°C for 10 hours instead of at 900°C for 30 hours. A SEM image of the prepared positive electrode active material powder is shown in Figure 3. Referring to Figure 3, it can be seen that the particles of the prepared positive electrode active material are in the form of secondary particles formed by agglomeration of several hundred primary particles.
[0140] Experimental Example 1 The average particle size D of the positive electrode active material powders produced in Examples 1 to 3 and Comparative Examples 1 and 2 50 The average particle size of the nodules / primary particles was measured. 50 was measured using a Microtrac MT 3000 and the average particle size of the nodules / primary particles was measured by SEM image analysis.
[0141] The measurement results are shown in Table 1 below.
[0142] [Table 1]
[0143] <Manufacturing lithium secondary batteries> The positive electrode active materials, carbon nanotubes, and PVDF binder prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were mixed in N-methylpyrrolidone in a weight ratio of 92.5:3:4.5 to prepare positive electrode slurries. The positive electrode slurries were applied to one side of an aluminum current collector sheet, dried at 120°C, and rolled to prepare positive electrodes.
[0144] Anode active material (a mixture of graphite:SiO = 95:5 by weight): conductive material (super C): styrene butadiene rubber (SBR): carboxymethyl cellulose (CMC) were mixed in water in a weight ratio of 95.8:1.0:2.2:1.0 to prepare anode slurry. The anode slurry was applied to one side of a copper current collector sheet, dried at 150°C, and rolled to prepare anode.
[0145] An electrode assembly was prepared by interposing a separator between the positive electrode and the negative electrode prepared as described above. The electrode assembly was inserted into a battery case, and an electrolyte was injected to assemble a lithium secondary battery. The battery was then charged at a constant current of 0.1 C at 45° C. to 4.65 V, and then discharged at a constant current of 0.1 C to 2.0 V to perform an activation process.
[0146] Experimental Example 2 The amount of gas generated and the number of cycles until the discharge capacity reached 80% of the lithium secondary batteries of Examples 1 to 3 and Comparative Example 2 prepared as described above were measured by the following method. The measurement results are shown in Table 2 below.
[0147] (1) Amount of gas generated (unit: μL / Ah): The lithium secondary battery was stored at 60° C. for 4 weeks, and then the amount of gas generated was measured.
[0148] (2) Number of cycles to reach 80%: A lithium secondary battery was charged at 25°C with a constant current of 0.33 C until the voltage reached 4.35 V, and then discharged at a constant current of 0.33 C until the voltage reached 2.5 V. One cycle consisted of repeated charging and discharging. The number of times that the discharge capacity after the cycle reached 80% of the initial discharge capacity was measured.
[0149] [Table 2]
[0150] Referring to Table 2 above, it can be seen that the lithium secondary batteries of Examples 1 to 3, in which perlithiated manganese oxide in the form of single particle / quasi-single particle is used, generate less gas and have excellent life characteristics compared to the lithium secondary battery of Comparative Example 2, in which perlithiated manganese oxide in the form of secondary particles is used.
[0151] Experimental Example 3 The lithium secondary batteries of Examples 1 to 3 and Comparative Example 1 prepared as above were charged and discharged while measuring the resistance according to SOC by a hybrid pulse power characterization test (HPPC). Specifically, the lithium secondary batteries were charged to 4.65V at a rate of 0.1C in CCCV mode at room temperature (25°C) and then discharged to 2.5V at 0.33C. Then, the batteries were charged to 4.65V in CCCV mode at a rate of 0.3C and then discharged while being discharged at a rate of 1.5C according to SOC, and the voltage drop resistance was measured for 10 seconds.
[0152] The measurement results are shown in Figure 4. As shown in Figure 4, it can be seen that the lithium secondary batteries of Examples 1 to 3, in which a perlithiated manganese oxide having an average particle size of 2.5 μm or less is used, have lower resistance characteristics than the lithium secondary battery of Comparative Example 1, in which a perlithiated manganese oxide having an average particle size of 3.4 μm is used.
Claims
1. A positive electrode active material powder containing perlithiated manganese oxide particles represented by the following [chemical formula 1], The perlithiated manganese-based oxide particles are in the form of a single particle consisting of one nodule or a quasi-single particle consisting of a composite of 2 to 30 nodules; The average particle size D of the positive electrode active material powder 50 is 2.5 μm or less, [Chemical formula 1] Li a Ni b Co c Mn d M e O 2 In the above Chemical Formula 1, 1<a, 0≦b≦0.5, 0≦c≦0.1, 0.5≦d<1.0, 0≦e≦0.2, and M is at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr.
2. The positive electrode active material powder according to claim 1 , wherein the positive electrode active material powder is made of perlithiated manganese oxide particles having at least one of the form of a single particle and a quasi-single particle.
3. The average particle size D of the positive electrode active material powder 50 The positive electrode active material powder according to claim 1, wherein the particle size is 0.5 μm to 2.5 μm.
4. 2. The positive electrode active material powder according to claim 1, wherein, in Chemical Formula 1, 1.1≦a≦1.5, 0.1≦b≦0.4, 0≦c≦0.05, 0.5≦d≦0.80, and 0≦e≦0.
1.
5. 2. The positive electrode active material powder according to claim 1, wherein the perlithiated manganese oxide particles have a crystal structure in which a layered phase and a rock salt phase are mixed.
6. 2. The positive electrode active material powder according to claim 1, wherein the nodules have an average particle size of 0.5 μm to 3.5 μm.
7. 2. The positive electrode active material powder according to claim 1, wherein the perlithiated manganese oxide particles have a crystallite size of 30 nm to 200 nm.
8. A positive electrode comprising the positive electrode active material powder according to claim 1 .
9. The positive electrode according to claim 8 , a negative electrode including a negative electrode active material; a separator interposed between the positive electrode and the negative electrode; and an electrolyte.
10. The lithium secondary battery according to claim 9 , wherein the negative electrode comprises a silicon-based negative electrode active material.
11. 10. The lithium secondary battery of claim 9, wherein the negative electrode comprises a mixture of a silicon-based negative electrode active material and a carbon-based negative electrode active material.
12. The negative electrode active material is made of Si, 10. The lithium secondary battery according to claim 9, wherein the N / P ratio of the lithium secondary battery is 150% to 300%.
13. the negative electrode active material is a mixture of silicon oxide and a carbon-based negative electrode active material, 10. The lithium secondary battery according to claim 9, wherein the N / P ratio of the lithium secondary battery is 100% to 150%.
Citation Information
Patent Citations
Lithium-enriched manganese-based material precursor as well as preparation method, lithium-enriched manganese-based anode material and preparation method thereof, lithium battery
CN108557905A
Single crystal lithium-rich manganese-based anode material, preparation method thereof, lithium ion battery
CN108598457A
Single-crystal-like lithium-rich layered oxide positive electrode material with adjustable total concentration gradient and preparation
CN113497227A
Lithium ion secondary battery
JP2011181235A
Secondary battery and charging method of the same
JP2013012336A