Cold-rolled steel sheet for enamel having excellent fish scale resistance and manufacturing method thereof
A cold-rolled steel sheet with controlled composition and manufacturing process addresses fish scale defects and adhesion issues, achieving high strength and resistance to fish scale, enhancing enameling performance and productivity.
Patent Information
- Application Number
- JP2024536146
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-17
- Filing Date
- 2022-12-16
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2042-12-16
AI Technical Summary
Existing cold-rolled steel sheets for enameling suffer from fish scale defects, reduced productivity due to long annealing times, increased manufacturing costs, and poor adhesion between the steel plate and glaze layer, while also requiring high amounts of titanium which cause nozzle clogging and blister defects.
A cold-rolled steel sheet with controlled composition and oxide layer thickness, including specific ranges of elements like C, Mn, Si, Al, P, Cu, N, Mo, and O, and a manufacturing process involving reheating, hot rolling, cold rolling, annealing, and enameling, to achieve a yield strength of 220 MPa or more with excellent adhesion and fish scale resistance.
The solution provides a high-strength cold-rolled steel sheet with improved enamel adhesion, reduced fish scale resistance, and stable material properties even after high-temperature firing, ensuring excellent enameling properties and productivity.
Smart Images

Figure 2024545259000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel sheet, and more particularly to a cold-rolled steel sheet for enamel having excellent fish scale resistance and a method for producing the same. [Background technology]
[0002] Enameled steel sheets are surface-treated products in which a glassy glaze is applied to a base steel sheet, such as a hot-rolled steel sheet or a cold-rolled steel sheet, and then the surface is fired at high temperatures to improve corrosion resistance, weather resistance, heat resistance, and chemical resistance. The enameled steel sheets are used for building exteriors, home appliances, tableware, and various industrial materials.
[0003] In the early days, rimmed steel was mainly used for the enamel steel sheet, but recently, as the continuous casting method has been used to improve productivity, most materials are continuously cast by the continuous casting method. One of the problems with the enamel steel sheet is a fishscale defect, which occurs when hydrogen dissolved in steel during the manufacturing process of enamel products becomes supersaturated in the steel during the process of cooling after firing, and is released to the surface of the steel over time, causing the enamel layer to fall off in the form of fish scales.
[0004] When fishscale defects occur, rust is generated intensively at the defect sites, which causes a significant decrease in the value of the enamel product. Therefore, in order to prevent fishscale defects in the manufacture of enamel steel sheets, various methods are used that involve forming a large number of sites inside the steel that can capture hydrogen dissolved in the steel.
[0005] Specifically, a method has been proposed to secure workability and fishscale resistance by applying an open coil annealing (OCA) method, which is a type of phase annealing method. However, this method has problems such as a relatively long heat treatment process, which reduces productivity and increases manufacturing costs, as well as causing significant quality deviations within the coil. In addition, since it is difficult to control the decarburization reaction in the heat treatment process, there is also a problem that excessive decarburization softens the grain boundaries of the steel sheet after the enamel firing heat treatment, reducing shape fixability.
[0006] In order to overcome the problems of reduced productivity and increased manufacturing costs due to the long annealing time, recently developed enamel steel sheets utilize a continuous annealing process. Enameled steels produced by the continuous annealing process generally use precipitates such as titanium (Ti) or inclusions obtained by a non-deoxidizing process as hydrogen storage sources based on ultra-low carbon steel. However, even in this case, a large amount of carbonitride-forming elements is required, which leads to increased costs and reduced sheet passing properties, and the problem of surface defects caused by the precipitates and non-deoxidized inclusions is a problem that must be fundamentally solved.
[0007] Enameled steel sheets that utilize titanium-based precipitates contain a large amount of titanium to inhibit the reaction of hydrogen, which causes fish scale, but this causes nozzle clogging due to titanium nitride (TiN) and inclusions during the continuous casting stage of the steelmaking process, which reduces workability and causes direct problems with production loads. In addition, the titanium nitride mixed into the molten steel exists on the top of the steel sheet, causing blister defects, which are a typical bubble defect, and the large amount of titanium added also causes problems such as the formation of a titanium-based oxide layer, which inhibits the adhesion between the steel sheet and the glaze layer.
[0008] In addition, in the case of enamel steel applied to enamel steel plate, the strength of the material is increased by using the material of most structural members, and the weight of the members used is reduced, which enhances competitiveness. For this reason, material properties are required after the firing heat treatment at high temperatures performed to dry the glaze in the enamel process. To meet this requirement, the yield strength of the enamel steel after firing must be secured at 220 MPa or more. Summary of the Invention [Problem to be solved by the invention]
[0009] The technical problem to be solved by the present invention is to provide a high-strength cold-rolled steel sheet for enamel treatment which has a yield strength of 220 MPa or more after enamel treatment, is free of air bubble defects, and has excellent enamel adhesion and fish scale resistance.
[0010] Another technical problem to be solved by the present invention is to provide a method for producing a cold rolled steel sheet having the above-mentioned advantages. [Means for solving the problem]
[0011] According to one embodiment of the present invention, a cold-rolled steel sheet contains, by weight%, C: 0.0003-0.003%, Mn: 0.25-0.55%, Si: 0.001-0.03%, Al: 0.0005-0.0015%, P: 0.01-0.03%, S: 0.001-0.010%, Cu: 0.03-0.08%, N: 0.008-0.015%, Mo: 0.1-0.3%, O: 0.025-0.055%, and the balance being Fe and unavoidable impurities, and includes an oxide layer, the oxide layer formed from the surface toward the inside of the cold-rolled steel sheet having a thickness of 0.006-0.030 μm.
[0012] In one embodiment, the cold-rolled steel sheet satisfies the following formula 1. <Expression 1> 0.014≦([Cu]×[Si) / [P]≦0.080 (In the above formula 1, [Cu], [Si], and [P] represent the weight percent contents of Cu, Si, and P, respectively.)
[0013] In one embodiment, the cold-rolled steel sheet satisfies the following formula 2. <Expression 2> 0.0065≦([Al]×[Mo]) / ([C]+[N])≦0.0310 (In the above formula 2, [Al], [Mo], [C] and [N] respectively represent the weight percent contents of Al, Mo, C and N.)
[0014] In one embodiment, the cold-rolled steel sheet satisfies the following formula 3. <Expression 3> 0.50≦(R max x20S e ) / P c ≦1.05 (In the above formula 3, P c is the number of surface irregularities per unit centimeter (cm), R max is the maximum point roughness value (μm), S e means temper rolling reduction (%))
[0015] In one embodiment, the cold-rolled steel sheet may have a yield strength of 220 MPa or more after enamel firing heat treatment. In one embodiment, the cold-rolled steel sheet may have an enamel adhesion of 95% or more. In one embodiment, the cold-rolled steel sheet may have a hydrogen permeation ratio of 600 sec / mm 2 It may be more than that.
[0016] According to another embodiment of the present invention, a method for producing a cold rolled steel sheet includes reheating a steel slab containing, by weight, 0.0003-0.003% C, 0.25-0.55% Mn, 0.001-0.03% Si, 0.0005-0.0015% Al, 0.01-0.03% P, 0.001-0.010% S, 0.03-0.08% Cu, 0.008-0.015% N, 0.1-0.3% Mo, 0.025-0.055% O, and the balance being Fe and unavoidable impurities, in a temperature range of 1,150-1,280°C. hot rolling the heated slab at a finish hot rolling temperature in the range of 890 to 950°C; coiling the hot rolled hot rolled steel sheet at a temperature in the range of 580 to 720°C; cold rolling the coiled hot rolled steel sheet at a cold reduction of 60 to 90%; annealing the cold rolled cold rolled steel sheet at an annealing temperature of 720 to 850°C for 10 to 70 seconds and temper rolling it to a reduction of 2.5% or less to produce an annealed sheet; and subjecting the annealed sheet to an enamel sintering heat treatment at a temperature in the range of 780 to 850°C.
[0017] In one embodiment, the method for producing a cold-rolled steel sheet satisfies the following formula 1. <Expression 1> 0.014≦([Cu]×[Si) / [P]≦0.080 (In the above formula 1, [Cu], [Si], and [P] represent the weight percent contents of Cu, Si, and P, respectively.)
[0018] In one embodiment, the method for producing a cold-rolled steel sheet satisfies the following formula 2. <Expression 2> 0.0065≦([Al]×[Mo]) / ([C]+[N])≦0.0310 (In the above formula 2, [Al], [Mo], [C] and [N] respectively represent the weight percent contents of Al, Mo, C and N.)
[0019] In one embodiment, the method for producing a cold-rolled steel sheet satisfies the following formula 3. <Expression 3> 0.50≦(R max x20S e ) / P c ≦1.05 (In the above formula 3, P c is the number of surface irregularities per unit centimeter (cm), R max is the maximum point roughness value (μm), S e means temper rolling reduction (%)) Effect of the Invention
[0020] According to an embodiment of the present invention, a cold-rolled steel sheet having excellent enamel adhesion and fish scale resistance is provided by controlling the steel composition, and can be used for various components such as home appliances, chemical equipment, kitchen equipment, sanitary equipment, and building interior and exterior materials.
[0021] A method for producing a cold-rolled steel sheet according to another embodiment of the present invention can provide a method for producing a cold-rolled steel sheet having the above-mentioned advantages. [Brief description of the drawings]
[0022] [Figure 1] FIG. 1 is a cross-sectional schematic diagram of a cold rolled steel sheet according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Terms such as first, second and third are used to describe various parts, components, regions, layers and / or sections, but are not limited thereto. These terms are used only to distinguish one part, component, region, layer or section from another part, component, region, layer or section. Thus, a first part, component, region, layer or section described below may be referred to as a second part, component, region, layer or section without departing from the scope of the present invention.
[0024] The terminology used herein is merely for the purpose of referring to particular embodiments and is not intended to limit the present invention. As used herein, the singular form includes the plural form unless the text clearly indicates otherwise. The term "comprising" as used in the specification embodies certain features, regions, integers, steps, operations, elements and / or components and does not exclude the presence or addition of other features, regions, integers, steps, operations, elements and / or components.
[0025] When an element is referred to as being "on" another element, it may mean that it is directly on top of the other element, or there may be other elements between them. In contrast, when an element is referred to as being "directly on" another element, there are no other elements between them.
[0026] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Terms defined in commonly used dictionaries are additionally interpreted to have a meaning consistent with the relevant technical literature and the currently disclosed content, and are not interpreted in an ideal or very formal sense unless defined.
[0027] Moreover, unless otherwise specified, % means % by weight, and 1 ppm is 0.0001% by weight.
[0028] In one embodiment of the present invention, the term "additionally contain an additional element" means that the remaining iron (Fe) is replaced by an additional amount of the additional element.
[0029] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.
[0030] FIG. 1 is a cross-sectional schematic diagram of a cold rolled steel sheet 100 according to one embodiment.
[0031] 1, the cold-rolled steel sheet 100 includes a steel sheet base material 10 and an oxide layer 20. The cold-rolled steel sheet 10 includes the steel sheet base material 10 and the oxide layer 20 formed from both surfaces of the cold-rolled steel sheet 100 toward the inside and separated from the steel sheet base material 10. Specifically, the cold-rolled steel sheet 100 according to an embodiment of the present invention includes, by weight percent, C: 0.0003-0.003%, Mn: 0.25-0.55%, Si: 0.001-0.03%, Al: 0.0005-0.0015%, P: 0.01-0.03%, S: 0.001-0.010%, Cu: 0.03-0.08%, N: 0.008-0.015%, Mo: 0.1-0.3%, O: 0.025-0.055%, and the balance being Fe and unavoidable impurities.
[0032] The reasons for limiting the alloy components are explained below. Hereinafter, wt% can be expressed as %.
[0033] Carbon (C): 0.0003~0.03% Carbon (C) is an element that affects steel sheet properties such as solid solution strengthening, aging, and bubble defects. The carbon content may be 0.0003 to 0.0030%. Specifically, the carbon content may be in the range of 0.0005 to 0.0028%.
[0034] If the carbon content exceeds the upper limit of the range, the strength increases, but the formability decreases due to the inhibition of the development of texture during annealing, and the enamel layer bubbling during the enamel firing process causes air bubble defects.If the carbon content exceeds the lower limit of the range, the amount of precipitates that act as sites for absorbing hydrogen in the steel decreases, and grain growth occurs due to the purification of grain boundaries during the firing stage, resulting in problems of reduced workability and enamel properties.
[0035] Manganese (Mn): 0.25-0.55% Manganese (Mn) is a representative solid solution strengthening element, and is an element that prevents hot shortness by precipitating sulfur dissolved in steel in the form of manganese sulfide (MnS) and promotes the precipitation of carbides. The manganese content may be 0.25 to 0.55%. Specifically, the manganese content may be in the range of 0.27 to 0.53%.
[0036] If the manganese content exceeds the upper limit of the range, problems occur such as a decrease in formability due to the generation of center segregation, and a decrease in the Ar3 transformation temperature of the steel, which causes transformation during enamel firing and deformation of the molded product.If the manganese content exceeds the lower limit of the range, problems occur such that the effects of preventing red brittleness and promoting carbide precipitation are not achieved.
[0037] Silicon (Si): 0.001 to 0.030% Silicon (Si) is an element that promotes the formation of precipitates that increase strength and act as a hydrogen storage source. The silicon content may be 0.001 to 0.030%. Specifically, the silicon content may be in the range of 0.002 to 0.028%.
[0038] If the silicon content exceeds the upper limit of the range, there is a problem that an oxide film is formed on the steel sheet surface, resulting in a decrease in enamel adhesion, whereas if the silicon content exceeds the lower limit of the range, there is a problem that the effect of increasing strength and forming the precipitates acting as a hydrogen storage source is not achieved.
[0039] Aluminum (Al): 0.0005 to 0.0015% Aluminum (Al) is used as a strong deoxidizing agent to remove oxygen from molten steel in the steelmaking process, and is a representative element that fixes dissolved nitrogen. The aluminum content may be 0.0005 to 0.0015%. Specifically, the aluminum content may be in the range of 0.0006 to 0.0014%.
[0040] If the aluminum content exceeds the upper limit of the range, the fraction of inclusions acting as hydrogen storage sources decreases, the generation of fish scale increases significantly, and the amount of dissolved nitrogen decreases, resulting in a problem that the target material quality cannot be secured after sintering.If the aluminum content exceeds the lower limit of the range, the aluminum is used as a deoxidizer and does not exhibit the effect of fixing dissolved nitrogen.
[0041] Phosphorus (P): 0.001 to 0.010% Phosphorus (P) is a solution strengthening element and an element that controls the surface pickling property. The phosphorus content may be 0.01 to 0.03%. Specifically, the phosphorus content may be in the range of 0.011 to 0.028%.
[0042] If the phosphorus content exceeds the upper limit of the range, a segregation layer is formed inside the steel sheet, which not only reduces formability but also promotes sulfuric acid reactivity in the enamel pretreatment process, thereby reducing adhesion.If the phosphorus content exceeds the lower limit of the range, it is difficult to ensure the desired material and surface properties.
[0043] Sulfur (S): 0.001-0.010% Sulfur (S) is an element that combines with manganese (Mn) to induce red shortness. The sulfur content may be 0.001 to 0.010%. Specifically, the sulfur content may be in the range of 0.002 to 0.009%.
[0044] If the sulfur content exceeds the upper limit of the range, not only does the ductility decrease significantly, thereby degrading workability, but also manganese sulfides are excessively precipitated, adversely affecting the fishscale of the product, whereas if the sulfur content exceeds the lower limit of the range, there is a problem of degrading weldability.
[0045] Copper (Cu): 0.03-0.08% Copper (Cu) is an element added to improve solid solution strengthening and adhesion. The copper content may be 0.03 to 0.08%. Specifically, the copper content may be in the range of 0.032 to 0.078%.
[0046] If the copper content exceeds the upper limit of the range, the pickling speed decreases in the acid treatment step, which is a pre-enamel treatment process, and the steel sheet cannot obtain suitable roughness characteristics, resulting in a decrease in adhesion.If the copper content exceeds the lower limit of the range, the effects of solid solution strengthening and improved adhesion cannot be achieved.
[0047] Nitrogen (N): 0.008-0.015% Nitrogen (N) is a typical interstitial solid solution strengthening element along with carbon (C), and is an element for ensuring a target strength level after a sintering process. The nitrogen content may be 0.008 to 0.015%. Specifically, the nitrogen content may be 0.0083 to 0.0145%.
[0048] Molybdenum (Mo): 0.1-0.3% Molybdenum (Mo) is an element that forms various precipitates and oxides to ensure stable strength and provide a hydrogen storage source. The molybdenum content may be 0.1 to 0.3%. Specifically, the molybdenum content may be in the range of 0.11 to 0.29%.
[0049] If the molybdenum content exceeds the upper limit of the range, there is a problem that not only the annealing threadability is deteriorated but also the occurrence rate of surface defects is increased, and if the molybdenum content exceeds the lower limit of the range, there is a problem that the effects of ensuring the strength and providing the hydrogen storage source are not achieved.
[0050] Oxygen (O): 0.025-0.055% Oxygen (O) is an essential element for forming inclusions that act as hydrogen storage sources in enamel steel. The oxygen content may be 0.025 to 0.055%. Specifically, the oxygen content may be in the range of 0.0255 to 0.0540%.
[0051] If the oxygen content exceeds the upper limit of the range, there is a problem that the refractory material is severely eroded during steelmaking, and the occurrence rate of surface defects in the steel sheet is high, whereas if the oxygen content exceeds the lower limit of the range, there is a problem that the effect of forming the inclusions is not achieved.
[0052] The balance is iron (Fe). Inevitable impurities may also be included. Inevitable impurities refer to impurities that are inevitably mixed in during the steelmaking and manufacturing process of grain-oriented electrical steel sheets. Since unavoidable impurities are widely known, a detailed description will be omitted. In one embodiment of the present invention, the addition of elements other than the alloy components described above is not excluded, and various elements are included within a range that does not impair the technical concept of the present invention. When an additional element is further included, it is included in place of the balance Fe.
[0053] In one embodiment, the cold-rolled steel sheet 100 can contain titanium (Ti), niobium (Nb), chromium (Cr), and vanadium (V). The cold-rolled steel sheet for enamel having excellent fish scale resistance can selectively further contain one or more of Ti: 0.005% or less, Nb: 0.005% or less, Cr: 0.05% or less, and V: 0.003% or less.
[0054] In this way, the cold-rolled steel sheet 100 of the present invention not only does not include any arbitrary addition of elements such as titanium (Ti), which has a higher oxidizing property than iron (Fe), but also improves properties such as enamel adhesion between the steel sheet and the glaze by controlling the surface oxide layer.
[0055] The oxide layer 20 is formed from both surfaces of the cold rolled steel sheet 100, which is the base material 10, toward the inside, and can be classified based on a point containing 5% oxygen. Specifically, the thickness of the oxide layer was classified based on a point containing 5% oxygen by analyzing the oxygen concentration from the surface to the inside of the steel sheet cross section. More specifically, the thickness of the oxide layer was measured using Glow Discharge Spectroscopy (GDS) starting from a point containing 5% oxygen.
[0056] In one embodiment, the thickness of the oxide layer 20 may be in the range of 0.006 to 0.030 μm. Specifically, the thickness of the oxide layer 20 may be 0.007 to 0.028 μm. If the thickness of the oxide layer 20 exceeds the upper limit of the above range, there is a problem that the surface characteristics of the steel sheet are deteriorated. If the thickness of the oxide layer 20 exceeds the lower limit of the above range, there is a problem that the bonding strength between the glaze layer and the steel sheet is reduced, making it difficult to ensure enamel adhesion, and fishscale resistance is also deteriorated.
[0057] Thus, enamel products are products in which an organic glaze is applied to a steel sheet, and it is extremely important to ensure adhesion between the steel sheet and the glaze. The main component of the glaze is specifically composed of silicon-oxide (SiO2)-based, and there is a problem in that expensive glazes such as NiO, which are one of the glaze components, are used to prevent a decrease in adhesion to the steel sheet. The high-strength cold-rolled steel sheet for enamel, which has excellent enamel adhesion and fish scale resistance according to one embodiment of the present invention, can improve enamel adhesion by controlling the thickness of the oxide layer on the steel sheet surface. By controlling the thickness of the oxide layer composed of 90% by weight or more of iron oxide (FeO-based) within a certain range, it is possible to promote covalent bonding with silicon (Si) atoms in the glaze layer and improve enamel adhesion.
[0058] In one embodiment, the cold rolled steel sheet 100 satisfies the following formula 1. <Expression 1> 0.014≦([Cu]×[Si) / [P]≦0.080 (In the above formula 1, [Cu], [Si], and [P] represent the weight percent contents of Cu, Si, and P, respectively.)
[0059] The above formula 1 represents the correlation between copper (Cu) and silicon (Si) with respect to phosphorus (P). The above formula 1 may be in the range of 0.014 to 0.080. Specifically, the above formula 1 may be in the range of 0.0142 to 0.0798. By satisfying the above range, the cold-rolled steel sheet 100 can suppress enamel adhesion and surface bubble defects.
[0060] If the value of the formula 1 exceeds the upper limit of the range, the inflow of gas into the surface of the steel sheet increases, causing surface defects such as air bubbles, which reduces product reliability.If the value of the formula 1 falls below the lower limit of the range, the surface is not modified in the sulfuric acid pretreatment process, which reduces enamel properties such as enamel adhesion.
[0061] In one embodiment, the cold rolled steel sheet 100 satisfies the following formula 2. <Expression 2> 0.0065≦([Al]×[Mo]) / ([C]+[N])≦0.0310 (In the above formula 2, [Al], [Mo], [C] and [N] respectively represent the weight percent contents of Al, Mo, C and N.)
[0062] The above formula 2 is the correlation between aluminum (Al) and molybdenum (Mo) with carbon (C) and nitrogen (N). In the case of carbon (C) and nitrogen (N) in steel, they react with aluminum (Al) and molybdenum (Mo) to form carbonitrides, and the excess solute elements not only provide excellent control of shape fixability by suppressing structure growth even during high-temperature heat treatment such as the enamel firing process, but these precipitates also serve as a hydrogen storage source.
[0063] Therefore, it is necessary to take into consideration not only the reactivity of each alloy element but also the reactivity of the composite solute elements. The above formula 2 may be 0.0065 to 0.0310. Specifically, the above formula 2 may be in the range of 0.0067 to 0.0305.
[0064] When the value of the above formula 2 exceeds the upper limit of the range, the workability is good, but the rolling and annealing passability are deteriorated, and the amount of expensive alloy elements used is increased, which causes a problem of an increase in production costs.When the value of the above formula 2 is below the lower limit of the range, not only is precipitation not promoted, so that fishscale resistance is deteriorated, but also the amount of interstitial solid solution elements is increased, which causes a problem of a decrease in workability.
[0065] In one embodiment, the cold rolled steel sheet 100 satisfies the following formula 3. <Expression 3> 0.50≦(R max x20S e ) / P c ≦1.05 (In the above formula 3, P c is the number of surface irregularities per unit centimeter (cm), R max is the maximum point roughness value (μm), S e means temper rolling reduction (%))
[0066] The above formula 3 may be 0.50 to 1.05. Specifically, the above formula 3 may be in the range of 0.505 to 1.00. If the value of the above formula 3 exceeds the upper limit of the range, there is a problem that the crystal grains of the steel sheet grow after the enamel firing treatment, and the target material properties and enamel characteristics are secured. If the value of the above formula 3 falls below the lower limit of the range, there is a problem that the wedge effect of the steel sheet surface decreases, and the adhesion to the glaze decreases.
[0067] In one embodiment, the cold-rolled steel sheet 100 may have a yield strength of 220 MPa or more after the enamel firing heat treatment. The yield strength of materials used in structural members is a physical property that determines the dent resistance and shape fixability of the members. In the case of enamel products, the yield strength at the processing inlet side as well as the yield strength after a long-term heat treatment at high temperature for drying after the enamel glaze treatment act as major factors in examining the stability of the product. When the yield strength after the enamel firing heat treatment is 220 MPa or more, there is an advantage that the product has excellent stability during the heat treatment stage for drying after the enamel treatment.
[0068] In one embodiment, the cold-rolled steel sheet 100 may have an enamel adhesion in the range of 95% or more. Specifically, the enamel adhesion may be 96% or more. In this range, the cold-rolled steel sheet 100 can be used as an enamel material even when an inexpensive glaze is used. If the enamel adhesion is lower than the above range, there is a problem that the rate of fish scale generation due to hydrogen in the steel increases.
[0069] In one embodiment, the cold rolled steel sheet 100 has a hydrogen permeation ratio of 600 sec / mm 2 Specifically, the hydrogen permeation ratio is 610 sec / mm 2 The upper limit of the hydrogen permeability ratio is not particularly limited, but may be, for example, 1,700 sec / mm 2 The hydrogen permeability ratio is a representative index for evaluating fishscale resistance, which indicates resistance to fishscale defects that are fatal defects when enamel steel is used, and means the ability to fix hydrogen in the cold-rolled steel sheet.
[0070] Specifically, the hydrogen permeability ratio is a value obtained by measuring the time it takes for hydrogen to be generated in one direction of the steel sheet and for the hydrogen to permeate and exit in the opposite direction of the steel sheet, and dividing the measured value by the square of the thickness of the material. If the hydrogen permeability ratio is excessively low, when the resistance to fishscale defects is evaluated by performing accelerated heat treatment at 200°C for 24 hours after enameling, the defect rate is 50% or more, which is problematic for use as a stable enamel product.
[0071] According to another embodiment of the present invention, a method for producing a cold rolled steel sheet 100 includes, in weight percent, C: 0.0003 to 0.003%, Mn: 0.25 to 0.55%, Si: 0.001 to 0.03%, Al: 0.0005 to 0.0015%, P: 0.01 to 0.03%, S: 0.001 to 0.010%, Cu: 0.03 to 0.08%, N: 0.008 to 0.015%, Mo: 0.1 to 0.3%, The method includes the steps of reheating a steel slab containing 0.025-0.055% Fe and the balance Fe and inevitable impurities, hot rolling the heated slab, coiling the hot-rolled hot-rolled steel sheet, cold rolling the coiled hot-rolled steel sheet, annealing and temper rolling the cold-rolled cold-rolled steel sheet to produce an annealed sheet, and subjecting the annealed sheet to enameling heat treatment. The detailed description of the steel slab is the same as that of the above-mentioned cold-rolled steel sheet to the extent that it does not contradict the above-mentioned cold-rolled steel sheet, so that a duplicated description will be omitted.
[0072] The step of reheating the steel slab is a step for facilitating the subsequent hot rolling process and homogenizing the steel slab. The heating may refer to reheating.
[0073] In one embodiment, the step of reheating the steel slab may be a step of hot rolling in a range of 1,150 to 1,280°C. Specifically, the reheating temperature range may be 1,150 to 1,280°C. If the temperature exceeds the upper limit of the temperature range, the amount of surface scale increases at the slab heating temperature, resulting in a large material loss, as well as a problem of increased energy costs due to an increase in the heat source. If the temperature falls below the lower limit of the temperature range, a problem of reduced hot workability due to a rapid increase in rolling load in the hot rolling process may arise.
[0074] In one embodiment, the step of reheating the steel slab is performed at a finish hot rolling temperature in the range of 890 to 950° C. Specifically, the finish hot rolling temperature is in the range of 900 to 945° C.
[0075] If the finish hot rolling temperature exceeds the upper limit of the range, there are problems in that the peelability of the surface scale is reduced, the incidence of surface defects is increased, and uniform hot rolling properties are not ensured, resulting in reduced impact toughness.If the finish hot rolling temperature is below the lower limit of the range, there are problems in that the hot rolling is finished in a low temperature region, resulting in rapid grain mixing, resulting in reduced rollability and workability.
[0076] In one embodiment, the step of coiling the hot-rolled steel sheet is performed at a temperature range of 580 to 720° C. Specifically, the temperature range may be 590 to 700° C. The hot-rolled steel sheet may be cooled on a run-out table (ROT) before coiling.
[0077] If the temperature exceeds the upper limit of the above range, there are problems in that the corrosion resistance during coiling is reduced, and the grain boundary segregation of phosphorus (P) is promoted, which reduces cold rolling properties and adversely affects the workability of the final product.If the temperature is below the lower limit of the above range, there is a problem in that the temperature non-uniformity in the width direction increases during the cooling and soaking processes, which increases the material deviation due to the difference in precipitation behavior, which reduces the enameling properties.
[0078] In an embodiment, the method may further include pickling the hot-rolled steel sheet after the step of coiling the hot-rolled steel sheet. The pickling may remove scale generated during hot rolling.
[0079] In one embodiment, the step of cold rolling the coiled hot-rolled steel sheet is performed at a cold reduction of 60 to 90%. Specifically, the cold reduction is performed in the range of 63 to 88%.
[0080] If the cold rolling reduction exceeds the upper limit of the range, the material hardens, reducing workability, and the load on the cold rolling mill increases, reducing workability.If the cold rolling reduction is below the lower limit of the range, the driving force for recrystallization in the subsequent heat treatment process is not secured, resulting in localized unrecrystallized grains remaining, reducing workability.
[0081] In one embodiment, the step of annealing and temper rolling the cold-rolled steel sheet to produce an annealed sheet is performed at an annealing temperature range of 720 to 850° C. for 10 to 70 seconds.
[0082] If the annealing temperature exceeds the upper limit of the annealing temperature range, there is a problem that the annealing passability is deteriorated due to softening caused by a decrease in high-temperature strength, whereas if the annealing temperature is below the lower limit of the annealing temperature range, there is a problem that deformation caused by cold rolling is not sufficiently removed, resulting in a significant decrease in workability and failure to ensure enamel properties.
[0083] When the annealing holding time exceeds the upper limit of the range, the workability is good, but the degree of non-uniformity of the crystal grains increases, which causes a problem of deteriorating enamel properties, whereas when the annealing holding time is below the lower limit of the range, the recrystallization is not completed and unrecrystallized grains remain, which causes a problem of deteriorating formability.
[0084] In one embodiment, the step of manufacturing an annealed sheet by annealing and temper rolling the cold-rolled cold-rolled steel sheet is performed at a rolling reduction of 2.5% or less during the temper rolling. The shape of the material can be controlled by the temper rolling to obtain a desired surface roughness. Specifically, the temper rolling is performed at a rolling reduction of 0.3 to 2.2%.
[0085] If the reduction ratio exceeds the upper limit of the range, the material hardens due to work hardening, which reduces workability. Also, if the temper reduction ratio is high during the firing heat treatment in the enamel process, strain induced crystal grains grow abnormally, which significantly reduces the yield strength of the enamel product and reduces dent resistance.
[0086] In one embodiment, the step of subjecting the annealed sheet to an enamel firing heat treatment may be a step of subjecting the annealed sheet to an enamel firing heat treatment at a temperature range of 780 to 850° C. The enamel firing heat treatment may be a step for drying an enameled glaze. Specifically, the temperature range may be 790 to 840° C.
[0087] If the temperature exceeds the upper limit, the thickness of the oxide layer increases, which increases the rate of surface defects, and the energy consumption increases, which increases the manufacturing cost.If the temperature is below the lower limit, the wettability of the glaze decreases, which makes it difficult to ensure the adhesion of the enamel.
[0088] Hereinafter, the high strength cold rolled steel sheet for enamel having excellent fish scale resistance and the manufacturing method thereof according to the present invention will be described in detail with reference to the following examples and comparative examples. The following examples are provided for reference in order to explain the present invention in detail, and the present invention is not limited thereto and may be realized in various forms.
[0089] A method for producing a cold-rolled steel sheet according to another embodiment of the present invention includes the steps of heating a steel slab containing carbon (C): 0.11 to 0.13%, silicon (Si): 0.05% or less, manganese (Mn): 0.1 to 0.6%, aluminum (Al): 0.02 to 0.06%, phosphorus (P): 0.015% or less, sulfur (S): 0.015% or less, nitrogen (N): 0.006% or less, the balance being Fe and other inevitable impurities, hot rolling the heated slab, cooling the hot-rolled hot-rolled steel sheet, coiling the cooled hot-rolled steel sheet, cold rolling the coiled hot-rolled steel sheet, annealing the cold-rolled cold-rolled steel sheet, and secondary rolling the annealed cold-rolled steel sheet. The detailed description of the steel slab is the same as that of the cold-rolled steel sheet described above to the extent that it does not contradict the above, so duplicated description will be omitted.
[0090] First, the steel slab is heated. The step of heating the steel slab is performed at 1,150°C or higher. The step of heating the steel slab requires a temperature of 1,150°C or higher because the precipitates formed in the steel must be re-dissolved.
[0091] Next, in the step of hot rolling the heated slab, the heated slab is hot rolled to obtain a hot-rolled steel sheet. In one embodiment, the steel slab is hot-finish rolled at a temperature of Ar3 or more. The temperature of Ar3 or more may be 890°C or more. By performing the hot-finish rolling at a temperature of Ar3 or more, rolling is performed in an austenite single phase region. If rolling is performed in a temperature range beyond the above range, there is a problem that rolling stability is reduced due to non-uniform material.
[0092] The step of cooling the hot-rolled steel sheet is carried out for a time period of 150 to 1,200 seconds. If the time period is less than the lower limit of the above range, a large amount of pearlite phase is formed, which may cause large carbides in the final material. If the carbides are large, they may become the starting point of cracks, which may reduce the hole expansion rate.
[0093] If the upper limit of the time range is exceeded, the formation of pearlite phase is suppressed, but there is a problem that a thick surface oxide layer is formed due to oxidation of the surface of the hot-rolled steel sheet. If the surface oxide layer is formed thickly, not only does the pickling time before cold rolling become longer, but the possibility of inducing surface defects increases significantly. Specifically, the step of cooling the hot-rolled hot-rolled steel sheet may be cooled to 710°C by maintaining the temperature between 710°C and 860°C for 150 to 1,200 seconds.
[0094] The step of coiling the cooled hot-rolled steel sheet may be performed at a temperature of 560 to 700° C. In order to ensure a grain size appropriate for strength and workability, the step of coiling the cooled hot-rolled steel sheet may be controlled within the above coiling temperature range. If the coiling temperature is too low, the grains may become too fine, whereas if the coiling temperature is too high, the grains may become too coarse.
[0095] The coiled hot-rolled steel sheet may be cold-rolled at a rolling reduction of 80 to 95% to produce a cold-rolled steel sheet. The thickness of the hot-rolled steel sheet is usually 2 to 4 mm, and a rolling reduction of 80% or more is required to reduce the thickness by 0.4 mm.
[0096] If the reduction exceeds the upper limit, the deformation resistance during rolling increases excessively, making rolling difficult, whereas if the reduction falls below the lower limit, the cold rolled steel sheet cannot reach a target thickness.
[0097] In an embodiment, the method may further include pickling the coiled hot-rolled steel sheet before cold rolling the coiled hot-rolled steel sheet. The pickling may remove scale generated during hot rolling.
[0098] The step of annealing the cold-rolled steel sheet is performed at a temperature of 620 to 760°C to manufacture an annealed steel sheet. The annealing of the cold-rolled steel sheet can remove internal stress formed during cold rolling and ensure workability. In order to remove the internal stress and ensure the workability, a process of annealing at a sufficiently high temperature to cause recrystallization is required.
[0099] If the temperature exceeds the upper limit, the high temperature strength may decrease, resulting in sheet fracture defects, whereas if the temperature is below the lower limit, there is a problem that recrystallization does not occur in the cold rolled steel sheet having the composition of the present invention.
[0100] In the step of second rolling the annealed cold-rolled steel sheet, the annealed cold-rolled steel sheet may be second-rolled at a rolling reduction of 6 to 18% to produce a final steel sheet. If the rolling reduction exceeds the upper limit, there is a problem that the desired level of workability cannot be secured due to a decrease in elongation rate. If the rolling reduction is below the lower limit, there is a problem that the target strength cannot be obtained. EXAMPLES
[0101] Hereinafter, the high strength cold rolled steel sheet for enamel having excellent fish scale resistance and the manufacturing method thereof according to the present invention will be described in detail with reference to the following examples and comparative examples. The following examples are provided for reference in order to explain the present invention in detail, and the present invention is not limited thereto and may be realized in various forms.
[0102] <Steel slabs made from inventive steels 1-5 and comparative steels 1-5> Table 1 below shows the compositions of the main components of the invention steels 1 to 5 and the comparative steels 1 to 5. Slabs were produced using alloy components according to the compositions in Table 1 below, through the converter, secondary refining, and continuous casting processes. In addition, the values of formulas 1 and 2 are shown according to the compositions of the main components. Formula 1 above shows ([Cu]×[Si]) / [P], and formula 2 above shows ([Al]×[Mo]) / ([C]+[N]). [Cu], [Si], [P], [Al], [Mo], [C], and [N] in formulas 1 and 2 above each mean weight percent.
[0103] [Table 1]
[0104] From Table 1, it can be seen that the comparative steels are not within the steel composition range of the present invention compared to the inventive steels, and therefore it can be seen that they are not within the values of Formulas 1 and 2 above.
[0105] <Examples 1 to 9 and Comparative Examples 1 to 9> The slab was used to produce cold-rolled steel sheets under the manufacturing conditions shown in Table 2. Specifically, the slab was held in a heating furnace for 2 hours and then hot-rolled to a thickness of 4.0 mm. The hot-rolled steel sheets were pickled to remove the oxide film on the surface, and then cold-rolled at the respective reduction ratios.
[0106] [Table 2]
[0107] As shown in Table 2, Examples 1 to 9 were performed using slabs of invention steels 1 to 5, which are within the composition range of the present invention, and were performed within the slab reheating temperature, finish hot rolling temperature, coiling temperature, cold rolling reduction, annealing temperature, holding time, temper rolling reduction, and enamel firing temperature ranges of the present invention. In contrast, Comparative Examples 1 to 4 were performed using slabs of invention steels 1 to 4, which are within the composition range of the present invention, and were controlled so that at least one of the manufacturing conditions in Table 2 did not correspond to the conditions of the present invention. Comparative Examples 5 to 9 were performed using comparative steels 1 to 5 in Table 1, and were controlled so that the manufacturing conditions in Table 2 were within the range of the present invention.
[0108] <Measurement results of cold-rolled steel sheet properties> Table 3 below shows the oxide layer thickness, passability, yield strength, presence or absence of bubble defects, presence or absence of fish scale generation, enamel adhesion, and hydrogen permeability ratio for Examples 1 to 9 and Comparative Examples 1 to 9, which were produced using the inventive steel and comparative steel in Table 1 under the production conditions in Table 2.
[0109] The thickness of the oxide layer was determined by analyzing the oxygen concentration from the steel sheet surface to the inside using GDS (Glow Discharge Spectroscopy), dividing the oxide layer from the base material based on the point containing 5% oxygen, and measuring the thickness up to the point containing 5% oxygen, and this was measured three times and the average value was expressed. In the case of the threadability, if the operability in the continuous casting, hot rolling, and cold rolling processes is 90% or more compared to the productivity of normal material, it is indicated as good (indicated by "○"), and if the productivity is less than 90% and the defect occurrence rate is 10% or more, it is indicated as poor (indicated by "X").
[0110] The yield strength was measured by preparing tensile test pieces (standard ASTM 13B) from test pieces that were heat-treated for 15 minutes at each temperature in a firing furnace to replicate the enamel drying process for the steel plate, and conducting a tensile test at a crosshead speed of 10 mm / min.
[0111] The enamel-treated test pieces were cut to the appropriate size for each purpose depending on the test purpose, and the enamel-treated test pieces that had completed the heat treatment were completely degreased and then coated with a standard glaze (Check Frit) that is relatively weak against fish scale defects, and then kept at 300℃ for 10 minutes to remove moisture. After drying, the test pieces were fired for 15 minutes at each firing temperature in order to highlight the differences in enamel properties such as adhesion, and then cooled to room temperature, and the atmospheric conditions in the firing furnace were set at a dew point of 20℃, which is a harsh condition that is likely to cause fish scale defects.
[0112] The test pieces that had completed the enamel treatment were subjected to an accelerated fishscale experiment in which they were kept in an oven at 200° C. for 24 hours. After the accelerated fishscale treatment, the presence or absence of fishscale defects was observed with the naked eye, and if no fishscale defects were found, the result was marked as good (represented by an "O"), and if the fishscale defects were found, the result was marked as bad (represented by an "X").
[0113] Enamel adhesion, which evaluates the adhesion between the steel sheet and the glaze, is defined in the American Society for Testing and Materials standard, ASTM C313-78, by applying a certain load to the enamel layer with a steel ball, and then evaluating the degree of electrical current at this point, thereby expressing the degree of detachment of the enamel glaze layer as an index. In the present invention, the evaluation result of enamel adhesion is set to a target of ensuring 95% or more adhesion in order to ensure application stability with relatively low-cost glazes.
[0114] The porosity defects were judged to be excellent (represented by "○") or poor (represented by "×") by visually observing the enamel surface of test pieces that had been kept in an oven at 200°C for 24 hours after the enamel treatment. The hydrogen permeability ratio is one of the indices for evaluating the resistance to fish scale, a fatal defect in enamel, and is determined by measuring the time (ts, unit: seconds) for hydrogen to be generated in one direction of the steel plate using an experimental method described in the European standard (EN10209-2013) and for the hydrogen to permeate and exit on the other side. This is expressed as the square of the thickness of the material (t, unit: mm), and is expressed as ts / t2 (unit: seconds / mm). 2 )
[0115] [Table 3]
[0116] Referring to Table 3, Examples 1 to 9 of the present invention, which satisfy various characteristics such as the component composition, manufacturing conditions, surface characteristics, and oxide layer thickness of the present invention, not only have good threading properties, but also related indexes such as the oxide layer thickness satisfy the range of the present invention. In addition, Examples 1 to 9 of the present invention do not generate enamel defects such as fish scale and bubble defects, and have a hydrogen permeability of 600 sec / mm 2As described above, the enamel adhesion index is 95% or more, and the yield strength after enamel firing heat treatment is 220 MPa or more, and the properties targeted by the present invention are secured. In contrast, in the case of Comparative Examples 5 to 9, which do not satisfy the composition of the present invention, not only do most of them not satisfy the thickness of the surface oxide layer, hydrogen permeability ratio, and enamel adhesion proposed by the present invention, but in most cases, fish scales and bubble defects occur even when observed with the naked eye after enamel treatment, making them unsuitable for the intended use. In addition, in Comparative Examples 1 to 4, which satisfy the composition of the present invention but whose manufacturing conditions in the annealing steps during hot rolling do not satisfy the control range of the present invention, the thickness of the surface oxide layer exceeds the range proposed by the present invention, the enamel adhesion is less than 95%, and it is confirmed that enamel defects such as bubble defects or fish scales occur after enamel treatment, the plate passing property is poor, and the yield strength after enamel firing heat treatment is less than 220 MPa, so that the overall targeted properties cannot be secured.
[0117] As described above, the cold-rolled steel sheet for enamel having excellent enamel adhesion and fish scale resistance according to one embodiment of the present invention satisfies the above-mentioned alloy composition and alloy range, so that the thickness of the oxide layer formed in the inward direction can be controlled to an appropriate level, thereby providing a high-strength cold-rolled steel sheet for enamel having excellent fish scale resistance.
[0118] In addition, the cold-rolled steel sheet has significantly improved enamel properties even through high-speed continuous annealing operation, and can maintain a high level of strength after enamel firing heat treatment. The surface roughness characteristics can be optimized in the heat treatment and temper rolling stages in the continuous annealing furnace to improve adhesion. Furthermore, by suppressing grain growth during enamel firing, such as residual nitrogen in the inner surface layer of the steel sheet, stable material properties can be ensured even after high-temperature firing.
[0119] The present invention is not limited to the above-described embodiments and / or examples, and can be manufactured in various different forms, and a person skilled in the art to which the present invention pertains will understand that the present invention can be embodied in other specific forms without changing the technical idea or essential features of the present invention. Therefore, the above-described embodiments and / or examples should be understood to be illustrative in all respects and not limiting.
Claims
1. Containing, by weight, C: 0.0003-0.003%, Mn: 0.25-0.55%, Si: 0.001-0.03%, Al: 0.0005-0.0015%, P: 0.01-0.03%, S: 0.001-0.010%, Cu: 0.03-0.08%, N: 0.008-0.015%, Mo: 0.1-0.3%, O: 0.025-0.055%, and the balance being Fe and unavoidable impurities, Contains an oxide layer, The thickness of the oxide layer formed from the surface toward the inside of the cold-rolled steel sheet is 0.006 to 0.030 μm.
2. The cold rolled steel sheet according to claim 1, which satisfies the following formula 1. <Formula 1> 0.014≦([Cu]×[Si) / [P]≦0.080 (In the above formula 1, [Cu], [Si], and [P] respectively represent the weight percent contents of Cu, Si, and P.)
3. The cold rolled steel sheet according to claim 1, which satisfies the following formula 2. <Formula 2> 0.0065≦([Al]×[Mo]) / ([C]+[N])≦0.0310 (In the above formula 2, [Al], [Mo], [C] and [N] respectively represent the weight percent contents of Al, Mo, C and N.)
4. The cold-rolled steel sheet according to claim 1 , which satisfies the following formula 3: <Formula 3> 0.50≦(R max ×20S e ) / P c ≦1.05 (In the above formula 3, P c is the number of surface irregularities per unit centimeter (cm), R max is the maximum point roughness value (μm), S e means temper rolling reduction (%))
5. The cold-rolled steel sheet according to claim 1, having a yield strength of 220 MPa or more after enamel firing heat treatment.
6. The cold-rolled steel sheet according to claim 1, having an enamel adhesion of 95% or more.
7. Hydrogen permeability is 600 seconds / mm 2 The cold rolled steel sheet according to claim 1 .
8. reheating a steel slab containing, by weight, 0.0003-0.003% C, 0.25-0.55% Mn, 0.001-0.03% Si, 0.0005-0.0015% Al, 0.01-0.03% P, 0.001-0.010% S, 0.03-0.08% Cu, 0.008-0.015% N, 0.1-0.3% Mo, 0.025-0.055% O, and the balance being Fe and unavoidable impurities, in a temperature range of 1,150-1,280°C; hot rolling the heated slab at a finish hot rolling temperature in the range of 890 to 950°C; Coiling the hot-rolled steel sheet at a temperature in the range of 580 to 720°C; cold rolling the coiled hot-rolled steel sheet at a cold reduction of 60 to 90%; annealing the cold-rolled steel sheet at an annealing temperature of 720 to 850° C. for 10 to 70 seconds, and temper rolling the cold-rolled steel sheet at a rolling reduction of 2.5% or less to produce an annealed sheet; and subjecting the annealed steel sheet to an enamel sintering heat treatment at a temperature in the range of 780 to 850°C.
9. The method for producing a cold-rolled steel sheet according to claim 8, which satisfies the following formula 1. <Formula 1> 0.014≦([Cu]×[Si) / [P]≦0.080 (In the above formula 1, [Cu], [Si], and [P] respectively represent the weight percent contents of Cu, Si, and P.)
10. The method for producing a cold-rolled steel sheet according to claim 8, which satisfies the following formula 2. <Formula 2> 0.0065≦([Al]×[Mo]) / ([C]+[N])≦0.0310 (In the above formula 2, [Al], [Mo], [C] and [N] respectively represent the weight percent contents of Al, Mo, C and N.)
11. The method for producing a cold-rolled steel sheet according to claim 8, which satisfies the following formula 3. <Formula 3> 0.50≦(R max ×20S e ) / P c ≦1.05 (In the above formula 3, P c is the number of surface irregularities per unit centimeter (cm), R max is the maximum point roughness value (μm), S e means temper rolling reduction (%))
Citation Information
Patent Citations
Steel sheet for porcelain enameling having remarkably excellent deep drawability
JP1991166336A
Steel sheet for porcelain enameling, excellent in weldability, and its production
JP1996120406A
Steel sheet for enameling excellent in fish-scale resistance, adhesion and workability and its producing method
JP2001316760A
Steel sheet for enameling having excellent processability, aging property and enameling characteristic and its production method
JP2002080934A
Steel sheet for enameling having good adhesion to enameling, production method therefor, and enameled product
JP2006037215A