Carbon nanotube aggregates, carbon nanotube dispersions, conductive materials, electrodes, secondary batteries, planar aggregates, filters, electromagnetic wave shields, and pellicles for extreme ultraviolet rays

A carbon nanotube aggregate with controlled metal contents and structural properties addresses conductivity and dispersibility issues, enhancing performance in conductive materials, electrodes, secondary batteries, filters, and electromagnetic shields.

JP7556170B1Active Publication Date: 2024-09-25SUMITOMO CHEM CO LTD

Patent Information

Application Number
JP2024058121
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-29
Publication Date
2024-09-25
Estimated Expiration
2044-03-29

AI Technical Summary

Technical Problem

Existing carbon nanotube materials do not achieve optimal conductivity and dispersibility in dispersions, which limits their effectiveness in conductive materials, electrodes, and secondary batteries, as well as their application in filters and electromagnetic shields.

Method used

A carbon nanotube aggregate with specific compositions and structural properties, including controlled contents of Fe, Co, Na, and K atoms, and a defined resistivity ratio, along with a bundle structure and pore volume, enhances conductivity and dispersibility.

Benefits of technology

The carbon nanotube aggregate achieves excellent conductivity and dispersibility, leading to improved performance in conductive materials, electrodes, secondary batteries, filters, and electromagnetic shields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556170000002
    Figure 0007556170000002
  • Figure 0007556170000001
    Figure 0007556170000001
Patent Text Reader

Abstract

To provide a carbon nanotube aggregate having excellent electrical conductivity when made into a carbon nanotube dispersion liquid, and applications thereof. [Solution] A carbon nanotube aggregate, a carbon nanotube dispersion, a conductive material, an electrode, a secondary battery, a planar aggregate, a filter, an electromagnetic wave shield, and a pellicle for extreme ultraviolet rays, which satisfy the conditions (1), (2), and (3). (1) At least one of Fe atoms and Co atoms is included, and the total content of Fe atoms and Co atoms is 2000 ppm by mass to 100000 ppm by mass with respect to the total mass of the aggregate of carbon nanotubes. (2) At least one of Na atoms and K atoms is contained, and the total content of Na atoms and K atoms is 50 ppm by mass to 1000 ppm by mass with respect to the total mass of the aggregate of carbon nanotubes. (3) The ratio of volume resistivity under a pressure of 20 kN to volume resistivity under a pressure of 1 kN is 0.21 or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a carbon nanotube aggregate, a carbon nanotube dispersion, a conductive material, an electrode, a secondary battery, a planar aggregate, a filter, an electromagnetic wave shield, and a pellicle for extreme ultraviolet rays. [Background technology]

[0002] Carbon nanotubes are substances with a cylindrical structure formed by rolling up graphene sheets in which carbon atoms are arranged in a hexagonal honeycomb shape. Carbon nanotubes are basically broadly classified into single-walled carbon nanotubes formed from a single layer of graphene sheets and multi-walled carbon nanotubes formed from multiple layers of graphene sheets. Carbon nanotubes have good mechanical and electronic properties and are expected to be used in various applications, and in recent years, various attempts have been proposed to further improve the properties of carbon nanotubes.

[0003] For example, Patent Document 1 describes carbon nanotubes having a cobalt content of 1000 ppm to 30000 ppm, particles containing metal atoms with a specific mass magnetic susceptibility, and a G / D ratio in the Raman spectrum of 0.7 to 1.5, a dispersion, and uses thereof. Patent Document 2 describes a conductive material for secondary batteries that contains carbon nanotubes having a spherical secondary structure in which carbon nanotube units having a diameter of 20 nm to 150 nm are entangled, a true density (TD) to bulk density (BD) ratio (TD / BD) of 30 to 120, and a metal content of 50 ppm or less. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2023-089806 [Patent Document 2] JP 2018-530854 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present disclosure is to provide an aggregate of carbon nanotubes that has excellent electrical conductivity when made into a carbon nanotube dispersion liquid. Another problem to be solved by another embodiment of the present disclosure is to provide a carbon nanotube dispersion liquid which contains the above-mentioned carbon nanotube aggregate and has excellent electrical conductivity. Another problem to be solved by another embodiment of the present disclosure is to provide a conductive material, an electrode, and a secondary battery including the above-mentioned carbon nanotube aggregate. A problem to be solved by another embodiment of the present disclosure is to provide a planar aggregate including the above-mentioned carbon nanotube aggregate having a maximum length of 1000 μm to 30000 μm. Another problem to be solved by another embodiment of the present disclosure is to provide a filter, an electromagnetic wave shield, and a pellicle for extreme ultraviolet rays using the above-mentioned planar assembly. [Means for solving the problem]

[0006] <1> An aggregate of carbon nanotubes that satisfies the following conditions (1), (2), and (3): (1) containing at least one of an Fe atom and a Co atom; The total content of Fe atoms and Co atoms is 2000 ppm by mass to 100000 ppm by mass with respect to the total mass of the aggregate of carbon nanotubes. (2) At least one of Na atoms and K atoms is included, and the total content of Na atoms and K atoms is 50 ppm by mass to 1000 ppm by mass with respect to the total mass of the aggregate of carbon nanotubes. (3) The ratio of volume resistivity under a pressure of 20 kN to volume resistivity under a pressure of 1 kN is 0.21 or less. <2> Including bundle structures, <1> The carbon nanotube aggregate according to claim 1. <3> Pore ​​volume is 0.60 cm 3 / g~3.20cm3 / g, <1> or <2> The carbon nanotube aggregate according to claim 1. <4> <1> ~ <3> 13. A carbon nanotube dispersion comprising the aggregate of carbon nanotubes according to any one of the above items and a dispersion medium. <5> <1> ~ <3> 2. A conductive material comprising the carbon nanotube aggregate according to claim 1 . <6> An electrode active material; <5> and an electrode comprising the conductive material according to claim 1. <7> <6> A secondary battery comprising the electrode according to claim 1. <8> <1> ~ <3> 2. The carbon nanotube aggregate according to claim 1, wherein the carbon nanotube aggregate is a planar aggregate containing carbon nanotubes having a maximum length of 1000 μm to 30000 μm. <9> <8> A filter using the planar assembly described in . <10> <8> Electromagnetic wave shielding using the planar assembly described in 1. <11> <8> A pellicle for extreme ultraviolet light using the planar assembly described in claim 1. Effect of the Invention

[0007] According to an embodiment of the present disclosure, it is possible to provide an aggregate of carbon nanotubes that has excellent electrical conductivity when made into a carbon nanotube dispersion liquid. According to another embodiment of the present disclosure, it is possible to provide a carbon nanotube dispersion liquid containing the aggregate of carbon nanotubes and having excellent electrical conductivity. According to another embodiment of the present disclosure, a conductive material, an electrode, and a secondary battery including the carbon nanotube aggregate can be provided. [Brief description of the drawings]

[0008] [Figure 1] 1 is a scanning electron microscope photograph showing one embodiment of a specific CNT aggregate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the carbon nanotube aggregate, the carbon nanotube dispersion, the conductive material, the electrode, and the secondary battery according to the present disclosure will be described in detail. The following description may be based on representative embodiments of the present disclosure, but the present disclosure is not limited to such embodiments, and can be modified as appropriate within the scope of the purpose of the present disclosure.

[0010] In the present disclosure, a numerical range indicated using "~" means a range that includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in the present disclosure. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples. In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments. In the present disclosure, when there are multiple substances corresponding to each component, the amount of each component means the total amount of multiple substances, unless otherwise specified. In this specification, the term "process" refers not only to an independent process, but also to a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.

[0011] In the present disclosure, the terms "carbon nanotube," "single-walled carbon nanotube," "multi-walled carbon nanotube," "multi-walled carbon nanotube having a maximum length of 1000 μm to 30000 μm," "carbon nanotube aggregate," and "carbon nanotube dispersion" may be abbreviated as "CNT," "SWCNT," "MWCNT," "ULMWCNT," "CNT aggregate," and "CNT dispersion," respectively.

[0012] [Carbon nanotube aggregates] One embodiment of the present disclosure is an aggregate of carbon nanotubes that satisfies the following conditions (1), (2), and (3). (1) The aggregate contains at least one of Fe atoms and Co atoms, and the total content of Fe atoms and Co atoms relative to the total mass of the aggregate is 2,000 ppm by mass to 100,000 ppm by mass. (2) The aggregate contains at least one of Na atoms and K atoms, and the total content of Na atoms and K atoms relative to the total mass of the aggregate is 50 ppm by mass to 1000 ppm by mass. (3) The ratio of volume resistivity under a pressure of 20 kN to volume resistivity under a pressure of 1 kN is 0.21 or more. Hereinafter, the carbon nanotube aggregate of this embodiment will also be referred to as a "specific CNT aggregate."

[0013] The specific CNT aggregate has excellent electrical conductivity when made into a carbon nanotube dispersion. That is, a carbon nanotube dispersion containing the specific CNT aggregate and a dispersion medium that satisfies the above conditions (1), (2), and (3) (hereinafter, also referred to as "specific CNT dispersion") has excellent electrical conductivity.

[0014] The specific CNT dispersion is another embodiment of the present disclosure, and details regarding the specific CNT dispersion other than the specific CNT aggregate will be described later.

[0015] On the other hand, Patent Document 1 specifies the content of Co atoms from the viewpoint of obtaining a carbon nanotube dispersion liquid with excellent conductivity, but does not focus on controlling the total content of N atoms and K atoms, or on setting the ratio of the volume resistivity under a pressure of 20 kN to the volume resistivity under a pressure of 1 kN as specified conditions. Patent Document 2 specifies the ratio (TD / BD) of true density (TD) to bulk density (BD) from the viewpoint of obtaining a carbon nanotube dispersion liquid with excellent conductivity, but does not focus on setting the total content of Fe atoms and Co atoms, the total content of N atoms and K atoms, or further the ratio of the volume resistivity under a pressure of 20 kN to the volume resistivity under a pressure of 1 kN as specified conditions.

[0016] The specific CNT aggregate will be described in detail below. However, the speculations described in the following description are not intended to limit the interpretation of the specific CNT aggregate, but are described as an example.

[0017] <Condition (1)> The specific CNT aggregate contains at least one of Fe atoms and Co atoms, and the total content of Fe atoms and Co atoms is 2000 ppm by mass to 100000 ppm by mass with respect to the total mass of the specific CNT aggregate. The Fe atoms and Co atoms contained in the specific CNT aggregates are believed to originate from the metal catalyst used during CNT production. When CNTs are produced in the presence of a catalyst containing metal atoms such as Fe and Co, there is concern that Fe atoms, Co atoms, etc. derived from the catalyst will be included in the CNTs, resulting in reduced electrical conductivity. To address this issue, conventionally, after CNT production, the CNTs have been washed with acid to remove metal atoms such as Fe and Co atoms. However, according to the investigations of the present inventors, it was found that when the total content of Fe atoms and Co atoms relative to the total mass of the specific CNT aggregate is 2000 ppm by mass to 100,000 ppm by mass, the dispersibility in the dispersion medium is further improved while maintaining the electrical conductivity of the CNT aggregate. The total content of Fe atoms and Co atoms is 2000 ppm by mass to 100000 ppm by mass, preferably 2500 ppm by mass to 80000 ppm by mass, and more preferably 3000 ppm by mass to 60000 ppm by mass.

[0018] Fe and Co atoms are close to each other in the periodic table and are thought to have similar mechanisms of action. By having the total content of Fe atoms and Co atoms relative to the total mass of the specific CNT aggregate be in the range of 2,000 ppm by mass to 100,000 ppm by mass, the number of contact points between the CNTs contained in the specific CNT aggregate is maintained within an appropriate range, and therefore conductive paths are easily connected, and it is believed that good conductivity can be obtained in the resulting specific dispersion.

[0019] As a catalyst containing Fe or Co atoms used in the production of CNTs, a metal catalyst such as iron (Fe) or cobalt (Co) may be used alone as a main catalyst, or the main catalyst may be used in the form of a main catalyst-co-catalyst composite catalyst together with a co-catalyst such as molybdenum (Mo), vanadium (V) or chromium (Cr). Specific examples of the composite catalyst include FeCo, CoMo, CoV, FeCoMo, FeMoV, FeV, or FeCoMoV, and any one or a mixture of two or more of these may be used. In addition, the co-catalyst may be used in an amount of 0.01 mol to 1 mol, more specifically 0.05 mol to 0.5 mol, relative to 1 mol of the main catalyst.

[0020] The respective contents (ppm by mass) of Fe atoms and Co atoms relative to the total mass of a specific CNT aggregate can be measured, for example, by the following method. The specific CNT aggregate is completely dissolved in an acid such as hydrochloric acid or nitric acid. In order to completely dissolve the specific CNT aggregate in acid, a pretreatment such as dry ashing, wet ashing, or melting treatment may be performed. The solution in which the specific CNT aggregate is completely dissolved in acid is subjected to inductively coupled plasma atomic emission spectroscopy (ICP-AES), inductively coupled plasma mass spectrometry (ICP-MS), or the like to measure the Fe atom and Co atom contents. ICP-MS is preferably performed because it allows for more sensitive measurement.

[0021] When the content of Fe atoms and Co atoms is less than 10 ppm, it may be technically difficult to detect the peaks derived from the respective elements by ICP-MS or ICP-AES, and therefore difficult to calculate the content accurately. Therefore, the content of less than 10 ppm may be treated as 0.

[0022] CNTs may contain 0.01% by mass to 50% by mass of Fe atoms or Co atoms derived from the iron catalyst used during production. CNTs may contain Fe atoms or Co atoms, for example, in a state of being adsorbed on the surface of the CNTs or in a state of being incorporated inside the fibrous CNTs formed during production. That is, in the present disclosure, the Fe atoms and Co atoms contained in the specific CNT aggregate may respectively include Fe atoms and Co atoms derived from the catalyst used in the production of the MWCNTs. In the specific CNT aggregate, taking into consideration the content of catalyst-derived Fe atoms and Co atoms contained in the CNTs, it is preferable to adjust the total content of Fe atoms and Co atoms to the target content within a range of 4000 mass ppm to 60000 mass ppm relative to the total mass of the aggregate. Note that, when the total content of catalyst-derived Fe atoms or Co atoms relative to the total mass of the aggregate is the target content, it goes without saying that there is no need to take any particular measure to adjust the content of Fe atoms.

[0023] When the total content of Fe atoms and Co atoms relative to the total mass of the specific CNT aggregate exceeds 60,000 ppm by mass, the total content of Fe atoms and Co atoms relative to the total mass of the specific CNT aggregate can be adjusted to 60,000 ppm by mass or less by a known method, for example, by washing the aggregate with water, acid, or an aqueous acid solution (for example, a 35% by mass aqueous solution of hydrochloric acid) to wash and remove some of the Fe atoms. If the total content of Fe atoms and Co atoms relative to the total mass of the specific CNT aggregate is less than 2000 ppm by mass, the aggregate can be immersed in an approximately 5% by mass iron nitrate aqueous solution or an approximately 40% by mass iron chloride aqueous solution as a source of Fe atoms to adsorb Fe atoms onto the surface of the fibrous ULMWCNT, thereby improving the content of Fe atoms relative to the total mass of the aggregate, and the total content of Fe atoms and Co atoms can be adjusted to 2000 ppm by mass or more. Also, the aggregate can be immersed in an approximately 5% by mass cobalt nitrate aqueous solution or an approximately 40% by mass cobalt chloride aqueous solution as a source of Co atoms to adsorb Co atoms onto the surface of the fibrous ULMWCNT, thereby improving the content of Co atoms relative to the total mass of the aggregate, and the total content of Fe atoms and Co atoms can be adjusted to 2000 ppm by mass or more.

[0024] <Condition (2)> The specific CNT aggregate contains at least one of Na atoms and K atoms, and the total content of Na atoms and K atoms relative to the total mass of the specific CNT aggregate is 50 ppm by mass to 1000 ppm by mass. The total content of Na atoms and K atoms relative to the total mass of the specific CNT aggregate is preferably 60 ppm by mass to 900 ppm by mass, and more preferably 70 ppm by mass to 700 ppm by mass. The Na atoms and K atoms contained in the specific CNT aggregate are considered to be derived from the catalyst raw material used in the production of CNTs. The Na atoms and K atoms are preferably derived from atoms contained as impurities in the catalyst raw material, such as ferrocene. The dispersant used to prepare the CNT dispersion may contain Na atoms and K atoms as counter ions. According to the study by the present inventors, it is considered that Na atoms and K atoms originate from the catalyst raw material, and are effective for the conductivity of the carbon nanotube dispersion when they are contained in a state of being adsorbed on the surface of the CNT during the production of the CNT, or in a state of being incorporated inside the fibrous CNT formed during the production. This is considered to be because the Na ions and K ions contained in the dispersant have unstable adsorption to the CNT in the dispersion.

[0025] It is not clear why the conductivity of the specific CNT dispersion is improved when the total content of Na atoms and K atoms relative to the total mass of the specific CNT aggregate is 50 ppm by mass to 1000 ppm by mass, but the inventors consider it as follows. After the reaction during CNT production, the surfaces of the catalyst-derived Fe and Co atoms are partially covered with oxide, but it is speculated that the presence of at least one type selected from Na and K atoms during CNT production results in the formation of a complex oxide. The formation of the complex oxide increases the affinity of the specific CNT aggregates to water, allowing them to be more stably dispersed in the dispersion liquid, and as a result, it is believed that the resulting specific CNT dispersion liquid is more likely to form conductive paths and provide good conductivity.

[0026] Examples of the composite oxide include NaFeO3, Na2FeO4, NaCoO3, Na2CoO4, KFeO3, K2FeO4, KCoO3, K2CoO4, etc. It is presumed that the above-mentioned effect is achieved because the above-mentioned composite oxide is formed in small amounts on the surfaces of Fe atoms, Co atoms, etc., which are catalyst residues.

[0027] In a specific CNT aggregate, if the total content of Fe atoms and Co atoms is too high, the formation of a conductive path tends to be hindered, and if the total content of Fe atoms and Co atoms is too low, the CNTs become more likely to aggregate and the dispersibility of the CNT aggregate in solvents such as water tends to decrease, making it difficult to achieve the effect of improving the conductivity of the dispersion. In addition, if the total content of Na atoms and K atoms is too high, the ionic strength on the surface will be too strong, which suggests the possibility that the formation of a conductive path may become difficult due to some reason such as electrostatic repulsion between CNTs. Conversely, if the total content of Na atoms and K atoms is too low, it may be difficult to achieve the effect of improving the dispersibility of the CNT aggregates in solvents such as water, and it is believed that this will make it difficult to achieve the effect of improving the conductivity of the dispersion.

[0028] The respective contents of Na atoms and K atoms contained in the specific CNT aggregate can be measured by a method similar to the method for measuring the Fe atom content described above.

[0029] The total content of Na atoms and K atoms contained in the specific CNT aggregate can be adjusted by controlling the content of Na atoms and K atoms contained as impurities in the catalyst raw material, such as ferrocene. For example, when ferrocene using sodium cyclopentadienyl and iron chloride is used as a catalyst starting material, the content of Na atoms contained as impurities may be high. By using a sodium compound and a potassium compound as starting materials for the catalyst raw material in this way, the respective contents of Na atoms and K atoms contained in the obtained CNTs can be increased to a predetermined content. On the other hand, when CNTs having a total content of Na atoms and K atoms exceeding the predetermined range are obtained, the total content can be adjusted to the predetermined range by removing some of the Na atoms and K atoms through an appropriate acid washing treatment as described above.

[0030] <Condition (3)> The specific CNT aggregate has a ratio of the volume resistivity under a pressure of 20 kN to the volume resistivity under a pressure of 1 kN (hereinafter also simply referred to as "resistivity ratio") of 0.21 or less.

[0031] Since the specific CNT aggregates have a resistivity ratio of 0.21 or more, they do not tend to aggregate when in a powdered state and have good dispersibility in the dispersion medium, allowing them to be widely and finely dispersed in the dispersion. For this reason, it is assumed that the conductive paths formed between the CNTs in the dispersion tend to be of an appropriate length, resulting in a dispersion with excellent conductivity. Furthermore, there is no particular upper limit to the resistivity ratio in the specific CNT aggregate, but it can be set to 0.35 or less because this makes the contact between the CNTs appropriately strong and facilitates the stable formation of conductive paths.

[0032] In particular, in one embodiment, the resistivity ratio of the specific CNT aggregate is preferably 0.21 or more and 0.24 or less. When the resistivity ratio is 0.21 or more and 0.24 or less, the specific CNT aggregates do not have a high tendency to aggregate in a powder state and it is easy to ensure their dispersibility in the dispersion medium. This ensures communication between the CNTs finely dispersed in the dispersion liquid, and it is presumed that this improves the conductivity of the dispersion liquid. In another embodiment, the resistivity ratio of the specific CNT aggregate is preferably 0.25 or more and 0.29 or less. When the resistivity ratio is 0.25 or more and 0.29 or less, it is presumed that the coagulation tendency in the powder state is not too high, and the conductivity of the specific CNT dispersion liquid can be more stably ensured.

[0033] In the present disclosure, the volume resistivity of the CNT aggregate is measured by a four-probe method using a resistivity meter at 25° C. A Loresta device can be used as the resistivity meter. Specifically, using a Loresta device (product name: powder resistivity measurement system MCP-PD51, low resistivity meter Loresta-GP, low resistivity probe for powder MCP-PD511 (constant current application type 4-probe method), all manufactured by Nitto Seiko Analytech Co., Ltd.), the measurement sample is introduced into the resistivity measurement probe unit, and a pressure of 1 kN or 20 kN is applied using the attached hydraulic pump until the target load is reached, at which point the volume resistivity (Ω·cm) is measured.

[0034] As a sample for measuring the volume resistivity, a powder of CNT aggregate is used. When the CNT aggregate is in a form other than powder (for example, fiber or sheet), the CNT aggregate may be pulverized to obtain a powder. The pulverization is not particularly limited, and any pulverization process capable of crushing the CNT aggregate into small pieces may be used. As the pulverization, a process using a freeze pulverization method may be used.

[0035] In the present disclosure, the resistivity ratio is calculated by dividing the volume resistivity measured under a pressure of 20 kN by the volume resistivity measured under a pressure of 1 kN, and rounding off to two decimal places.

[0036] The resistivity ratio of the specific CNT aggregate can be adjusted by a conventional method. Methods for adjusting the resistivity ratio of a specific CNT aggregate include, for example, controlling the amount of impurities contained in the CNTs, controlling structural defects in the CNTs, controlling the length of the CNTs, and controlling the specific surface area of ​​the CNTs.

[0037] It is believed that when the load pressure is low, the impurities contained in the CNTs are sandwiched between the CNTs, and the effect of blocking the conductive path is large, resulting in a high resistivity. On the other hand, as the load pressure increases, the number of contact points between the CNTs increases, and the effect of the increase in resistance due to the impurities decreases, resulting in a low resistivity. For this reason, for example, the resistance ratio can be controlled by controlling the content of Fe atoms and / or Co atoms derived from the catalyst, which are substances that are effective as impurities. The amount of structural defects in CNTs can be measured by the G / D intensity ratio in Raman spectroscopy. When the G / D intensity ratio is high, there are fewer structural defects, and the resistivity tends to decrease. The G / D intensity ratio can be controlled by selecting the conditions for the CNT manufacturing method described below.

[0038] The longer the CNT, the lower the resistivity tends to be. Taking this into consideration, one of the control methods is to include ULMWCNT. ULMWCNT can be obtained, for example, by controlling the manufacturing method of CNT.

[0039] The resistivity ratio of a specific CNT aggregate can also be controlled by the specific surface area of ​​the CNT. If the specific surface area is small, it is difficult to secure contact points between CNTs, but it is presumed that the effect of increasing contact points due to load and pressure is significant. On the other hand, if the specific surface area is large, it is easy to secure contact points between CNTs, but it is presumed that the effect of increasing contact points due to load and pressure is small. The specific surface area of ​​the CNT can be controlled by adjusting the conditions in the CNT manufacturing method described below. For example, the mixing ratio of CNTs with a large specific surface area and CNTs with a small G / D intensity ratio may be controlled and the two may be mixed uniformly.

[0040] <Bundle structure> From the viewpoint of improving handleability, the specific CNT aggregate preferably includes a bundle structure. The bundle structure refers to an aggregate in which multiple CNTs are aggregated together by van der Waals forces or the like to form a bundle. It is presumed that the specific CNT aggregate contains a bundle structure of an appropriate size, which improves the handleability as a CNT aggregate and further improves stability. However, on the other hand, if the bundle structure contained in the specific CNT aggregate becomes too large, the size of the CNT aggregate itself becomes too large, and it becomes difficult to separate and disperse the CNTs contained in the bundle structure, which may reduce dispersibility in the dispersion medium.

[0041] For this reason, from the viewpoint of achieving both the handleability of the CNT aggregate and its dispersibility in a solvent, the width of each bundle structure contained in the specific CNT aggregate, i.e., the size in the width direction of the fiber bundle, is preferably 5 nm to 500 nm, and more preferably 10 nm to 300 nm. The content of the bundle structure in the specific CNT aggregate is preferably 10 mass % to 100 mass %, and more preferably 20 mass % to 90 mass %, with respect to the total mass of the specific CNT aggregate. The presence or absence of a bundle structure in a specific CNT aggregate can be confirmed by observing the specific CNT aggregate with an optical microscope, a scanning electron microscope (SEM), etc. The width of the bundle structure can be found by identifying the location where the bundle structure exists in the specific CNT aggregate and measuring the length using a photographed image of the bundle structure.

[0042] The bundle structure in a specific CNT aggregate can be formed, for example, by controlling the catalyst particle size distribution in production by chemical vapor deposition (CVD) and by controlling the cooling rate in the cooling process.

[0043] <Pore volume> The specific CNT aggregate of the present disclosure has a pore volume of 0.60 cm 3 / g~3.20cm3 It is preferred that the molecular weight is / g.

[0044] The specific CNT aggregate has a pore volume of 0.60 cm 3 / g~3.20cm 3 / g, friction between the specific CNT aggregates falls within a suitable range, and when dispersed, conductive paths are easily formed stably, improving the conductivity of the dispersion.

[0045] In contrast, the pore volume is 0.60 cm 3 / g, the CNT aggregates have fewer projections and recesses on their surfaces, which reduces friction between the CNT aggregates and makes it difficult to maintain a stable contact state, presumably resulting in an unstable conductive path.

[0046] Also, the pore volume is 3.20 cm 3 It is presumed that CNT aggregates larger than this value will have greater friction between the CNT aggregates, resulting in insufficient dispersion in the dispersion liquid, which is detrimental to the formation of conductive paths.

[0047] Furthermore, the pore volume is 3.20 cm 3 If it is larger than 1 / g, the amount of cavities in the CNT aggregate increases, which may reduce the physical strength of the CNT aggregate. This is not preferable because the physical strength of the CNT aggregate decreases, and the aggregate may not be able to withstand a process in which a shear force is applied to the aggregate, such as a process of dispersing the CNT aggregate (for example, the pores may be partially blocked, or the CNT aggregate may be partially destroyed). In addition, if the pore volume is too large, the amount of cavities in the CNT aggregate increases, and the conductive paths in the CNT aggregate may become too long, which may increase the resistance, which is not preferable.

[0048] In the present disclosure, the pore volume of a CNT aggregate is the volume (cm) of pores that a CNT aggregate has per unit mass (g). 3 The form of the CNT aggregate to be measured for pore volume is not limited, and may be any form such as powder, fiber, sheet, etc.

[0049] In the present disclosure, the pore volume of the CNT aggregate is measured by a constant volume method. A specific surface area / pore distribution measuring device can be used as the measuring device.

[0050] Pore ​​volume of CNT aggregates (cm 3 / g) is specifically measured according to the following procedure. First, a CNT aggregate to be measured is subjected to a vacuum degassing treatment at 300° C. for 3 hours to prepare a measurement sample. The nitrogen adsorption and desorption isotherms of the prepared samples are measured using the constant volume method. The BJH method is used for the analysis to calculate the pore volume. Measurement equipment: Specific surface area / pore distribution measurement equipment (product name "BEL SORP-miniII", manufactured by Microtrack Bell) Measurement temperature: 77K Adsorbate: Nitrogen Saturated vapor pressure: Actual measurement Adsorbate cross section: 0.162nm 2 Waiting time after reaching adsorption equilibrium: 500 seconds

[0051] <Other matters regarding specific CNT aggregates> In the present disclosure, the CNTs contained in the specific CNT aggregate may be SWCNTs or MWCNTs, but it is preferable for the specific CNT aggregate to contain MWCNTs, since these have a wall number distribution and are slightly less uniform, making it easier to improve dispersibility.

[0052] In general, SWCNTs have a lower volume resistivity than MWCNTs, and the lower the volume resistivity, the smaller the change in resistivity due to applied pressure. The number of walls of CNTs can be controlled by selecting the manufacturing method for CNTs.

[0053] The longer the CNT, the lower its volume resistivity tends to be. The length of the CNT can be controlled by selecting the manufacturing method of the CNT.

[0054] In one embodiment, the specific CNT aggregate may be an aggregate that contains MWCNTs having a maximum length of 500 μm or less as a main component and does not contain MWCNTs having a maximum length of more than 500 μm and 30,000 μm or less. Here, the main component means that 90 mass % or more of the CNTs constituting the specific CNT aggregate are MWCNTs having a maximum length of 500 μm or less. The specific CNT aggregate may contain SWCNTs having a maximum length of 500 μm or less.

[0055] In one embodiment, the specific CNT aggregate preferably includes MWCNTs having a maximum length of 10 μm to 30,000 μm. In one aspect, the MWCNTs preferably include ULMWCNTs.

[0056] ULMWCNT is MWCNT with a maximum length of 1000 μm to 30000 μm, which is longer than general-purpose MWCNT and can take the shape of a fiber.

[0057] By taking on a fibrous shape, ULMWCNTs have the property of easily entangling with each other. The MWCN contains at least one ULMWCNT, and from the viewpoint that the MWCNTs are easily entangled with each other to form a more stable aggregate, it is preferable that the MWCN is an aggregate containing multiple ULMWCNTs. Hereinafter, an aggregate containing ULMWCNTs may be abbreviated as "ULMWCNT aggregate."

[0058] Here, the term "fiber" is generally used to refer to a structure in which one dimension is larger than the other two. The fibers may be thread-like fibers with a circular cross section, ribbon-like fibers with a rectangular cross section, hollow, or have other shapes. From the viewpoint of increasing electrical conductivity, the cross section of the ULMWCNT is preferably circular, and preferably hollow.

[0059] The aggregate of MWCNTs may be an aggregate having a three-dimensional structure in which the MWCNTs are entangled with one another. Fig. 1 is a scanning electron microscope (SEM) photograph showing one embodiment of an aggregate of MWCNTs according to the present disclosure. From the SEM photograph shown in Fig. 1, it can be seen that a plurality of fibrous ULMWCNTs are entangled to form an aggregate. Thus, the entangled state of the ULMWCNTs according to the present disclosure can be confirmed by SEM observation.

[0060] The length of ULMWCNTs can be measured by focusing on one ULMWCNT and observing multiple SEM images taken at adjacent viewing angles. Here, "ULMWCNT length" refers to the measured length of the ULMWCNT in the longitudinal direction, and the maximum value of the measured lengths is taken as the "maximum length." When observing an SEM photograph, if one MWCNT with a maximum length in the range of 1000 μm to 30000 μm is observed within the viewing angle of the SEM photograph, it can be confirmed that the observed MWCNT includes ULWMCNT.

[0061] It is preferable that a plurality of ULMWCNTs are present within the viewing angle of the SEM photograph. Focusing on 100 MWCNTs included in the viewing angle of the SEM photograph, the maximum length of each is measured, and from the viewpoint of further improving the stability of the MWCNT aggregate due to the entanglement of the ULMWCNTs, it is preferable that 10% or more of the observed MWCNTs (i.e., ULMWCNTs) have a maximum length in the range of 1000 μm to 30000 μm, calculated as a number, be present, more preferably 20% or more, even more preferably 30% or more, and particularly preferably 50% or more.

[0062] The diameter of ULMWCNT can be measured by observing SEM or transmission electron microscope (TEM) photographs. Here, the diameter refers to the length in the direction perpendicular to the longitudinal direction of the ULMWCNT, and the diameter is measured at 10 different points on one ULMWCNT, and the average value is the diameter of that ULMWCNT.

[0063] The length of the ULMWCNT is in the range of 1000 μm to 30000 μm, preferably in the range of 1050 μm to 25000 μm, more preferably in the range of 1100 μm to 20000 μm, further preferably in the range of 1200 μm to 18000 μm, and particularly preferably in the range of 1300 μm to 15000 μm. The diameter of the ULMWCNT is preferably 1 nm to 100 nm, more preferably in the range of 2 nm to 80 nm, further preferably in the range of 3 nm to 50 nm, and particularly preferably in the range of 5 nm to 30 nm.

[0064] The length / diameter ratio of the ULMWCNT, so-called aspect ratio, is preferably 1,000 or more, more preferably 3,000 or more, further preferably 5,000 or more, and particularly preferably 10,000 or more. The aspect ratio can be calculated from the ratio of the maximum length to the diameter of one ULMWCNT. From the viewpoint of measurement accuracy, it is preferable to use the average value of the measurements of 20 or more ULMWCNTs.

[0065] From the viewpoint of dispersibility, the specific gravity of the ULMWCNT aggregate is preferably in the range of 1.5 to 2.5, more preferably in the range of 1.7 to 2.4, and further preferably in the range of 1.8 to 2.2. The specific gravity of the ULMWCNT aggregate can be measured by the method described in JIS Z8807:2012 "Method of measuring density and specific gravity of solids."

[0066] The purity of the MWCNT in the ULMWCNT aggregate can be measured by thermogravimetric analysis. For example, using a thermal analyzer (manufactured by Shimadzu Corporation, DTG-60), the thermogravimetric (TG) curve and differential thermal analysis (DTA) curve of the ULMWCNT aggregate are obtained. The largest exothermic peak in the DTA curve with a peak top appearing around 650°C to 750°C is regarded as the combustion of MWCNT, and the exothermic peaks appearing otherwise are regarded as the combustion of substances other than MWCNT. The purity of MWCNT is determined from the weight loss rate of the TG curve. From the perspective of the conductivity obtained, the purity of the ULMWCNT aggregate is preferably 50% by mass or more, more preferably 65% by mass or more, still more preferably 80% by mass or more, and particularly preferably 95% by mass or more.

[0067] ULMWCNT may contain 0.01% to 50% by mass of Fe atoms derived from iron, which is the catalyst used in production. ULMWCNT may contain Fe atoms, for example, in a state adsorbed on the surface of ULMWCNT or in a state incorporated into the interior of the fibrous ULMWCNT formed during production.

[0068] The obtained fibrous ULMWCNT is preferably flexible and strong. Also, the conductivity of ULMWCNT itself is preferably 5000 ohm -1 ·m -1 or more, and more preferably 10000 ohm -1 ·m -1 or more. Note that the conductivity of ULMWCNT itself is usually 1000000 ohm -1 ·m -1 or less.

[0069] <Manufacturing method of CNT> The manufacturing method of CNT in the present disclosure is not particularly limited. For example, as the manufacturing method of MWCNT in the present disclosure, methods such as a conventionally known chemical vapor deposition (CVD) method and a method of reacting a gaseous reactant containing a carbon source in the presence of a catalyst can be applied.

[0070] The CNTs in the present disclosure can be produced by referring to the methods described in, for example, JP 2016-102047 A and JP 2021-527611 A.

[0071] The method for producing CNTs according to the present disclosure will be described below with reference to examples, although the method for producing CNTs according to the present disclosure is not limited to the following examples.

[0072] =Manufacturing method X= An example of a method for producing CNTs referred to in this disclosure is the method described in JP 2016-102047 A. That is, the method includes a step of passing a gaseous reactant containing one or more carbon sources through a reactor, a step of reacting the one or more gaseous reactants in the presence of a catalyst in a reaction zone of the reactor to form product particles containing carbon, agglomerating the product particles into aggregates, and a step of applying a force to the aggregates to continuously move the aggregates out of the reaction zone (hereinafter also referred to as "production method X").

[0073] According to the production method X, MWCNTs, including ULMWCNTs, can be obtained in the form of fibrous aggregates or other aggregate forms that are easy to handle.

[0074] In the manufacturing method X, the force applied to the product particles may be a mechanical force. When the agglomerates are fibrous MWCNTs, the mechanical force applied to the product particles can be exerted by a rotating spindle around which the agglomerates are wound. The fibrous CNTs can be collected on the spindle or can be accumulated elsewhere by successively unwinding the spindle after one or more revolutions around the spindle.

[0075] The spindle is preferably oriented with the spindle axis perpendicular or parallel to the flow direction of the gaseous reactant(s), but may be oriented at other orientations, for example a spindle with the spindle axis oriented at an angle of 25° to the flow direction of the gaseous reactants may also be suitable for applying mechanical forces to the product particles.

[0076] The spindle can rotate about two axes (e.g., two perpendicular axes). In particular, the spindle can rotate about axes perpendicular and parallel to the flow direction of the gaseous reactants. Such a spindle can pull and twist the fibrous CNT aggregates to control the number and length of twists.

[0077] The spindle may be made of metal, ceramic, or plastic. The spindle can have different suitable shapes depending on the material properties and the intended use of the MWCNTs. The spindle can be used as a mold for producing carbon products, for example, by a spin-coating process. A preferred spindle shape is a rod or box shape.

[0078] Fibrous MWCNTs are deposited on a spindle or elsewhere, and the coating thickness and its orientation can be controlled by controlling the reaction time and conditions, or by the conditions under which an electric or other field is applied to the carbon product. The coating thickness and orientation of the carbon product can be controlled, for example, by gas flow forces.

[0079] The rotation speed of the spindle is preferably 0.01 rpm (revolutions / minute; the same applies below) to 10,000 rpm, and more preferably 0.1 rpm to 100 rpm. The spinning speed (i.e., the rotational speed of the spindle) may be adjusted so that the material is collected at a similar rate as it is produced. The rotational speed of the spindle may control the thickness of the accumulated MWCNT filaments. In a preferred embodiment, as the spindle rotates, the MWCNT filaments are processed in the axial direction of the spindle, such that the MWCNT filaments are wrapped evenly along the spindle, rather than only at one particular point on the spindle.

[0080] The MWCNT fibers may be collected, for example, on the reactor wall by a substrate placed in the reactor. The substrate may be a fixed substrate or a rotating guide that is used to apply a strong and equal force to the MWCNT fibers as they are collected. Suitable substrate configurations for fiber technology include a substrate consisting of two guides positioned at right angles to each other.

[0081] In process X, the mechanical force applied to the product particles may be a force applied by an accelerating gas flow. The accelerating gas flow may be generated by passing the product particles through a reactor having a narrow diameter or through a capillary tube downstream of the reaction zone. A vacuum may be applied to the product particles.

[0082] Other forces that can be applied to the product particles include electrostatic forces, suitably applied by a charged plate. Electrostatic forces require that the product particles be charged. The use of a charged plate allows the MWCNTs to be produced in the form of intertwined sheets on the charged plate.

[0083] Other forces applied to the product particles may also be magnetic forces or photon pressure applied by a light source.

[0084] The CNT source may be injected in the form of a liquid containing a carbon source instead of a gaseous reactant containing a carbon source. When a liquid is used as the CNT source, it can be injected through a single inlet or multiple inlets, for example in a showerhead arrangement.

[0085] Preferably, the gaseous reactant or reactants are reacted at between 500° C. and 1600° C., more preferably between 1000° C. and 1500° C. A temperature gradient is preferably maintained within the reactor, with the reaction zone being maintained at a higher temperature than the product zone of the reactor.

[0086] The gaseous reactants may be mixed with one or more gases that act as diluents. The gaseous reactants may be mixed with gases that do not play a direct role in the reaction but play a supporting role. It is also preferred to use a diluent gas that can react with the amorphous carbon by-product to keep the reactive sites on the catalyst intact to produce nanotubes.

[0087] Examples of gases that can be used as a diluent include argon or other inert gases, hydrogen, nitrogen, ammonia, carbon dioxide, and helium. Among these, hydrogen is particularly preferred as a gas that can be used as a diluent. The flow rate of the gas as a diluent is preferably 2000 mL (milliliters) / min or less, and more preferably 400 mL / min to 800 mL / min.

[0088] The gas pressure of the gaseous reactants and any diluents is preferably between 0.1 bar and 50 bar, more preferably between 0.5 bar and 5 bar, and even more preferably between 1 bar and 2 bar. In case of gas effluent from the furnace, the effluent gas can be recycled with or without cleaning.

[0089] The composition of the product particles can be controlled by monitoring the agglomerates and changing the reaction conditions based on the information obtained. For example, the agglomerates can be monitored by online Raman spectroscopy, which provides data indicative of single-walled or multi-walled CNTs. It also provides data indicative of the diameter and crystallinity of the CNTs. The agglomerates can also be monitored by online conductivity measurements, gas analysis, measuring the opacity of the reaction zone and / or measuring the winding force.

[0090] When the agglomerates are removed from the reactor, it is preferable to prevent air from entering the reactor, which is particularly important when the diluent gas contains hydrogen, for example to prevent an explosive mixture of hydrogen and air from forming in the reactor.

[0091] The product particles in production method X contain ULMWCNTs. Depending on the production conditions, SWCNTs may also be contained in addition to MWCNTs.

[0092] The product particles may be produced by chemical vapor deposition, where a gaseous reactant, a carbon source, is reacted in the presence of a catalyst.

[0093] Carbon-containing compounds suitable as carbon sources include carbon monoxide, carbon dioxide, aromatic hydrocarbons (e.g., benzene, toluene, xylene, cumene, ethylbenzene, naphthalene, or mesitylene), non-aromatic hydrocarbons (e.g., methane, ethane, propane, butane, pentane, hexane, cyclohexane, ethylene, propylene, or acetylene), and oxygen-containing hydrocarbons (e.g., formaldehyde, acetaldehyde, acetone, methanol, ethanol, diethyl ether, polyethylene glycol, 1-propanol, ethyl formate, and hydrocarbons including mixtures of two or more thereof). The carbon-containing compound is preferably carbon monoxide, methane, ethylene or acetylene.

[0094] The carbon source preferably contains oxygen. Ethanol is a particularly preferred carbon source. Oxygen can be introduced into the reactor by other methods, such as by using a diluent gas or a carbon source containing water.

[0095] The gaseous reactant that is the carbon source is preferably injected into the reactor at a rate of 0.01 mL / min to 10 mL / min, more preferably 0.08 mL / min to 0.25 mL / min.

[0096] The catalyst is preferably a transition metal group, in particular chromium (Cr), molybdenum (Mo), tungsten (W) or VIIIB transition metal group. Specifically, the catalyst is preferably, for example, iron (Fe), cobalt (Co), nickel (Ni), ruthenium (Ru), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir) and platinum (Pt) or manganese (Mn), or a mixture thereof. Metals from the lanthanide and actinide series (e.g. yttrium (Y)) can also be used as catalyst. Fe, Ni, Co, Mo and mixtures thereof, for example, a mixture of Ni and Co (mass ratio: 50 / 50), a mixture of Fe and Ni, or a mixture of Fe and Mo are more preferred. Any of these transition metals may be used alone or in combination with any of the other transition metals listed to act as a catalyst for CNT growth, with it being particularly preferred that the catalyst is a mixture of two or more of the metals listed.

[0097] The catalyst is preferably formed by decomposition of a precursor. The precursor is preferably a thermally or photo- or plasma-decomposable compound of one or more of the above metals, such as a carbonyl or cyclopentadienyl organometallic compound. Ferrocene, iron pentacarbonyl, nickelocene and cobaltocene are particularly preferred precursors. Suitably, at least 0.01% by weight of the precursor is contained in the carbon source, and preferably 0.2% to 2.5% by weight of the precursor is contained in the carbon source. In one embodiment, 0.23% to 2.3% by weight of the precursor is contained in the carbon source. The catalyst may be used supported on a carrier, and preferred carriers include silica and magnesium oxide.

[0098] The carbon source is preferably reacted in the presence of a promoter. Suitable promoters are one or more of sulfur, phosphorus, molybdenum and organic compounds of these elements. Thiophene is also one of the preferred promoters. Suitably, up to 10% by weight of the promoter is included in the carbon source. Preferably, 0.2% to 6% by weight of the promoter is included in the carbon source. When high or low concentrations of thiophene are used as the promoter, MWCNTs are formed. For example, MWCNTs are well formed using ethanol containing 0 mass % or 1.5 mass % to 4.0 mass % thiophene and 0.5 mass % to 5.0 mass % (particularly 2.3 mass %) ferrocene under conditions of an injection rate of 3.0 mL / hour to 12.0 mL / hour (particularly 7.5 mL / hour), a hydrogen flow rate of 400 mL / min to 800 mL / min, and a synthesis temperature of 1100°C to 1180°C.

[0099] According to the production method X, it is possible to obtain fibrous CNTs having a length of at least 500 μm, for example, at least 1 mm. The fibrous CNTs can take the form of a thread or a sheet. The length of the fibrous CNTs can be controlled, for example, by the winding capacity of a spindle used in producing the fibrous CNTs.

[0100] The manufacturing method X preferably includes a step of reacting a carbon source in a reaction zone of a reactor to generate CNTs, and a step of aggregating the CNTs into aggregates by applying a force to the CNTs. According to this manufacturing method, fibrous CNTs can be easily manufactured.

[0101] In another embodiment, the MWCNTs comprising ULMWCNTs may be produced in a reaction zone by the methods described above, followed by condensation to form MWCNTs comprising ULMWCNTs, and continuously withdrawing the MWCNTs from near the reaction zone. In another embodiment, the method may include producing MWCNTs containing ULMWCNTs in a reaction zone, continuously electrostatically attracting the MWCNTs containing ULMWCNTs from the reaction zone, and recovering the MWCNTs containing ULMWCNTs.

[0102] =Manufacturing method Y= In the present disclosure, as an example of a method for producing CNTs, the method described in JP2021-527611A can be referred to. That is, the method includes a step (1) of supporting a mixture containing a main catalyst precursor and a co-catalyst precursor on γ-Al2O3 to produce an active support, a step (2) of drying the active support by multi-stage drying including vacuum drying, a step (3) of subjecting the dried active support to a heat treatment to produce a supported catalyst, and a step (4) of producing CNTs in the presence of the supported catalyst (hereinafter also referred to as "production method Y").

[0103] ·Process (1) In step (1), a mixture containing a main catalyst precursor and a co-catalyst precursor is supported on γ-Al2O3 to produce an active support.

[0104] In order to uniformly support the main catalyst precursor and the co-catalyst precursor on γ-Al2O3, the mixture may further contain a solvent, and the main catalyst precursor and the co-catalyst precursor may be in a state of being dissolved in the solvent. The solvent may be one or more selected from the group consisting of water, methanol, and ethanol, and is preferably water.

[0105] Since γ-Al2O3 has high porosity and a spinel structure, the main catalyst and the promoter can be arranged randomly in γ-Al2O3. The CNTs grown from the randomly arranged main catalyst can be produced in an entangled state.

[0106] The main catalyst may be one or more selected from the group consisting of cobalt, iron, nickel, manganese and chromium, with cobalt being preferred.

[0107] The main catalyst precursor may be one or more selected from the group consisting of nitrates, sulfates, carbonates and acetates of the main catalyst, with nitrates of the main catalyst being preferred.

[0108] The main catalyst precursor may be one or more selected from the group consisting of Co(NO3)2, Co(NO3)2·6H2O, Co2(CO)8, Co2(CO)6[HC=C(C(CH3)3)], Co(CH3CO2)2, Fe(NO3)3, Fe(NO3)2·nH2O, Fe(CH3CO2)2, Ni(NO3)2, Ni(NO3)2·6H2O, Mn(NO3)2, Mn(NO3)2·6H2O, Mn(CH3CO2)2·n(H2O) and Mn(CO)5Br, of which Co(NO3)2·6H2O, Fe(NO3)2·nH2O and Ni(NO3)2·6H2O are preferred.

[0109] The co-catalyst improves the dispersibility of the main catalyst, and may be one or more selected from the group consisting of vanadium and molybdenum.

[0110] The promoter precursors were NH4VO3, NaVO3, V2O5, V(C5H7O2)3, and (NH4)6Mo7O. 24 4H2O, NH4VO3 and (NH4)6Mo7O 24 Preferably, one or more selected from the group consisting of 4H2O.

[0111] When the mixture contains two or more kinds of promoter precursors, that is, when it contains both a vanadium precursor and a molybdenum precursor, the molar ratio of the sum of vanadium and molybdenum to vanadium can be 1:0.45 to 1:0.95 or 1:0.5 to 1:0.9, and preferably 1:0.5 to 1:0.9. When the above conditions are satisfied, the CNT structure can be stably maintained and CNTs having a desired pore volume can be produced.

[0112] The mixture may contain the main catalyst precursor and the cocatalyst precursor such that the molar ratio of the main catalyst to the cocatalyst is 1:0.01 to 1:0.5, 1:0.1 to 1:0.4, or 1:0.1 to 1:0.25, and preferably 1:0.1 to 1:0.25. If the above molar ratio is satisfied, the dispersibility of the main catalyst can be improved, and CNTs having the desired pore volume can be produced.

[0113] The mixture may further include an organic acid which serves to inhibit precipitation of the main catalyst precursor and the co-catalyst precursor.

[0114] The organic acid may be one or more selected from the group consisting of citric acid, tartaric acid, fumaric acid, malic acid, acetic acid, butyric acid, palmitic acid and oxalic acid, with citric acid being preferred.

[0115] The mixture may contain the organic acid and the cocatalyst precursor in a molar ratio of 1:1 to 1:20, 1:2 to 1:10, or 1:3 to 1:6, and preferably contains the organic acid and the cocatalyst precursor in a ratio of 1:3 to 1:6. If the above range is satisfied, there are advantages in that a transparent catalyst metal solution can be produced during catalyst production, and a catalyst in which fine powder is suppressed during impregnation can be produced.

[0116] After step (1), a step of aging may be further included.

[0117] The aging may be performed for 1 to 60 minutes or 10 to 50 minutes. It is preferably performed for 10 to 50 minutes. When the above-mentioned conditions are satisfied, the main catalyst precursor and the co-catalyst precursor can be sufficiently supported on the γ-Al2O3. In addition, air bubbles existing in the support are removed to the maximum extent, and the main catalyst precursor and the co-catalyst precursor can be sufficiently supported even in the fine pores inside the support.

[0118] ·Process (2) The active support is then dried by multi-stage drying, including vacuum drying.

[0119] Multi-stage drying may mean that a drying process including vacuum drying is performed two or more times. Specifically, multi-stage drying may include atmospheric drying and vacuum drying, or may include vacuum drying two or more times.

[0120] The vacuum drying may be performed at 80° C. to 300° C. or 120° C. to 250° C., and is preferably performed at 120° C. to 250° C. If the above conditions are satisfied, the main catalyst precursor, i.e., the coordinate bond of the main catalyst, can be easily decomposed to form the main catalyst oxide, and energy consumption can be minimized.

[0121] The vacuum drying may be performed at 1 mbar to 200 mbar or 30 mbar to 150 mbar, and is preferably performed at 30 mbar to 150 mbar. If the above conditions are met, the main catalyst precursor, i.e., the coordinate bond of the main catalyst, is rapidly decomposed and discharged, so that the main catalyst oxide can be more easily formed under vacuum conditions and energy consumption can be minimized.

[0122] The vacuum drying can be performed for 10 minutes to 3 hours or 10 minutes to 2 hours, and is preferably performed for 10 minutes to 2 hours. If the above conditions are met, the main catalyst precursor can be easily decomposed and converted into the main catalyst oxide, and energy consumption can be minimized.

[0123] On the other hand, when the multi-stage drying includes atmospheric drying and vacuum drying, the atmospheric drying can be performed before the above-mentioned vacuum drying, and the atmospheric drying can remove the solvent that may be present in the active support.

[0124] The normal pressure drying may be performed at 80° C. to 160° C. or 100° C. to 140° C., and is preferably performed at 100° C. to 140° C. If the above conditions are satisfied, the solvent present in the active support can be sufficiently removed, and energy consumption can be minimized.

[0125] The normal pressure drying may be performed at 900 mbar to 1,100 mbar, and preferably at 950 mbar to 1,050 mbar. If the above conditions are met, the solvent present in the active support can be sufficiently removed, and energy consumption can be minimized.

[0126] Drying at normal pressure may be performed for 1 to 12 hours, preferably for 3 to 9 hours. If the above conditions are met, the solvent present in the active support can be sufficiently removed, and energy consumption can be minimized.

[0127] On the other hand, when the multi-stage drying includes two or more vacuum dryings, the multi-stage drying may include two or more vacuum dryings performed at different temperatures, more specifically, a primary vacuum drying performed at a first temperature and a secondary vacuum drying performed at a second temperature higher than the first temperature.

[0128] The primary vacuum drying can remove any solvent that may be present in the active support.

[0129] The first temperature may be 80° C. to 160° C., and is preferably 100° C. to 140° C. If the above conditions are met, the solvent present in the active support can be sufficiently removed, and energy consumption can be minimized.

[0130] The primary vacuum drying can be performed for 1 to 12 hours, preferably 3 to 9 hours. If the above conditions are met, the solvent present in the active support can be sufficiently removed, and energy consumption can be minimized.

[0131] The primary vacuum drying may be performed at 1 mbar to 200 mbar, 1 mbar to 150 mbar, or 80 mbar to 150 mbar, and is preferably performed at 80 mbar to 150 mbar. If the above conditions are met, the solvent present in the active support can be sufficiently removed, and energy consumption can be minimized.

[0132] The secondary vacuum drying is as described above in the description of the vacuum drying.

[0133] The second temperature may be 175 to 300° C., and is preferably 180 to 280° C. If the above conditions are satisfied, the main catalyst precursor, i.e., the coordinate bond of the main catalyst, can be easily decomposed to form the main catalyst oxide, and energy consumption can be minimized.

[0134] The secondary vacuum drying may be performed at 1 mbar to 200 mbar, 1 mbar to 150 mbar, or 1 mbar to 70 mbar, and more preferably at 1 mbar to 70 mbar. If the above conditions are met, the main catalyst precursor, i.e., the coordinate bond of the main catalyst, is rapidly decomposed and discharged, so that the main catalyst oxide can be more easily formed under vacuum conditions and energy consumption can be minimized.

[0135] The secondary vacuum drying may be performed for 10 minutes to 3 hours or 10 minutes to 2 hours, and is preferably performed for 10 minutes to 2 hours. If the above conditions are met, the main catalyst precursor can be easily decomposed and converted into the main catalyst oxide, and energy consumption can be minimized.

[0136] ·Process (3) The dried active support is then subjected to a heat treatment to produce a supported catalyst.

[0137] By carrying out the heat treatment, a supported catalyst is produced in which the main catalyst and the promoter are present in a coated state on the surface and in the pores of the γ-Al2O3.

[0138] The heat treatment may be carried out at 600°C to 800°C or 620°C to 750°C, and is preferably carried out at 620°C to 750°C. If the above conditions are met, a supported catalyst can be produced in a state in which the main catalyst and the co-catalyst are uniformly coated on the surface and pores of γ-Al2O3, and energy consumption can be minimized.

[0139] The heat treatment may be performed for 1 to 12 hours or 2 to 8 hours, and is preferably performed for 2 to 8 hours. When the above-mentioned time is satisfied, a supported catalyst in which the catalyst precursor is present in a state of being uniformly coated on the surface and pores of γ-Al2O3 can be produced.

[0140] ·Process (4) CNTs are then produced in the presence of a supported catalyst.

[0141] In particular, CNTs can be produced by contacting a supported catalyst with a carbon-based compound, and more specifically, by carrying out a chemical vapor synthesis method.

[0142] The steps for producing CNTs are described in detail below. First, the supported catalyst can be loaded into a horizontal fixed bed reactor or a fluidized bed reactor. Then, the gaseous carbonaceous compound or a mixture of the gaseous carbonaceous compound, a reducing gas (e.g., hydrogen, etc.) and a carrier gas (e.g., nitrogen, etc.) is injected at a temperature equal to or higher than the thermal decomposition temperature of the gaseous carbonaceous compound or equal to or lower than the melting point of the catalyst supported on the supported catalyst, and CNTs can be grown by chemical vapor synthesis through the decomposition of the gaseous carbonaceous compound.

[0143] The CNTs produced by the above-mentioned chemical vapor synthesis method have a crystal growth direction nearly parallel to the tube axis, and the graphite structure has high crystallinity in the tube length direction. As a result, CNTs with small unit diameters and high electrical conductivity and strength can be produced.

[0144] The chemical vapor synthesis method may be carried out at 600° C. to 800° C. or 650° C. to 750° C., and is preferably carried out at 650° C. to 750° C. If the above-mentioned temperature is satisfied, CNTs can be produced while minimizing the generation of amorphous carbon.

[0145] The heat source for the reaction may be induction heating, radiant heat, laser, IR, microwave, plasma, surface plasmon heating, or the like.

[0146] Furthermore, any carbonaceous compound can be used without particular limitation as long as it can supply carbon and can exist in a gaseous state at a temperature of 300° C. or higher.

[0147] The carbon-based compound may be a carbon-based compound having 6 or less carbon atoms, and may be one or more selected from the group consisting of carbon monoxide, methane, ethane, ethylene, ethanol, acetylene, propane, propylene, butane, butadiene, pentane, pentene, cyclopentadiene, hexane, cyclohexane, benzene, and toluene.

[0148] After the CNTs are grown by the above-mentioned reaction, a cooling step may be optionally performed to arrange the CNTs more regularly. Specifically, the cooling step may be performed by natural cooling by removing the heat source or by using a cooler or the like.

[0149] The above manufacturing method X and manufacturing method Y are merely examples, and the manufacturing method for CNTs that can be contained in the specific CNT aggregate is not limited to the above.

[0150] [Carbon nanotube dispersion liquid] The carbon nanotube dispersion liquid (specific CNT dispersion liquid) according to the present disclosure contains a specific CNT aggregate and a dispersion medium. The specific CNT dispersion liquid has good dispersibility of the specific CNT aggregate according to the present disclosure in a dispersion medium and has excellent electrical conductivity. The specific CNT dispersion liquid is preferably used for forming electrodes, forming transparent conductive films, as a resin additive, a conductive ink, a coating agent, an antistatic agent, a paint, and the like.

[0151] <Specific CNT aggregate> The specific CNT aggregate contained in the specific CNT dispersion liquid is the same as the specific CNT aggregate according to the present disclosure described above, and therefore a description thereof will be omitted here.

[0152] <Dispersion medium> The dispersion medium preferably contains water, and more preferably contains water as a main component. "Containing water as a main component" means that the proportion of water in the dispersion medium is more than 50% by mass. The proportion of water in the dispersion medium is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 99% by mass or more, and may be, for example, 100% by mass.

[0153] The water is not particularly limited, but is preferably distilled water, ion-exchanged water, pure water, or the like, which contains fewer impurities.

[0154] The dispersion medium may be a mixture of water and a hydrophilic solvent. Examples of hydrophilic solvents include carbonate compounds such as ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, and butylene carbonate; ether compounds such as tetrahydrofuran; ketone compounds such as acetone; lower alcohol compounds such as methanol and ethanol; and acetonitrile. When the dispersion medium contains a hydrophilic solvent, the proportion of the hydrophilic solvent in the dispersion medium is preferably 10 mass % or less, more preferably 5 mass % or less, and even more preferably 1 mass % or less.

[0155] The specific CNT dispersion may further contain other components that can be used in a dispersion, in addition to the specific CNT aggregates and the dispersion medium. Examples of other components include dispersants, antifoaming agents, antistatic agents, conductive assistants other than the conductive assistant according to the present disclosure, etc. Furthermore, the composition may further contain a trace amount of impurity components, so-called inevitable impurities, etc.

[0156] <Dispersant> The carbon nanotube dispersion liquid may contain a dispersant for the purpose of further improving the dispersibility and dispersion stability of the specific CNT aggregates. The dispersant is not particularly limited, and examples thereof include various surfactants. Examples of the dispersant also include polymer compounds such as resins. The dispersant is preferably a surfactant. The surfactant may be an ionic surfactant or a nonionic surfactant, and is not particularly limited. In the specific CNT dispersion liquid, the surfactant may be used alone or in combination of two or more kinds.

[0157] Examples of ionic surfactants include anionic surfactants, cationic surfactants, and amphoteric surfactants. Examples of the anionic surfactant include aromatic sulfonic acid surfactants such as alkylbenzene sulfonates (e.g., dodecylbenzene sulfonate) and dodecylphenyl ether sulfonate; ether sulfate surfactants; phosphate surfactants; and carboxylic acid surfactants. Examples of the cationic surfactant include alkylamine salts and quaternary ammonium salts. Examples of the amphoteric surfactant include alkyl betaine surfactants and amine oxide surfactants. As the ionic surfactant, an ionic surfactant having an aromatic ring (so-called aromatic ionic surfactant) is preferred, and aromatic sulfonic acid surfactants such as alkylbenzene sulfonate and dodecyl phenyl ether sulfonate are more preferred. Aromatic ionic surfactants tend to be excellent in dispersibility, dispersion stabilization, and concentration of multi-walled carbon nanotubes.

[0158] Examples of nonionic surfactants include sugar ester surfactants such as sorbitan fatty acid esters and polyoxyethylene sorbitan fatty acid esters; fatty acid ester surfactants such as polyoxyethylene resin acid esters and polyoxyethylene fatty acid diethyl esters; ether surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers and polyoxyethylene polypropylene glycols; and aromatic nonionic surfactants such as polyoxyalkylene octyl phenyl ether, polyoxyalkylene nonyl phenyl ether, polyoxyalkyl dibutyl phenyl ether, polyoxyalkyl styryl phenyl ether, polyoxyalkyl benzyl phenyl ether, polyoxyalkyl bisphenyl ether, polyoxyalkyl cumyl phenyl ether and polyoxyalkylene phenyl ether. As the nonionic surfactant, an ionic surfactant having an aromatic ring (so-called aromatic nonionic surfactant) is preferable, polyoxyalkylene phenyl ether is more preferable, and polyoxyethylene phenyl ether is further preferable. Aromatic nonionic surfactants tend to be excellent in dispersibility, dispersion stabilization, and concentration of multi-walled carbon nanotubes.

[0159] Other dispersants that are excellent in dispersibility, dispersion stability, and high concentration of CNTs include DEMOL (registered trademark: the same applies below) N, DEMOL RN, and DEMOL T (manufactured by Kao Corporation), which are sodium salts of β-naphthalenesulfonic acid formalin condensates, Brij S 100 (manufactured by Sigma-Aldrich), which is a polyoxyethylene stearyl ether, polyvinylpyrrolidone K30 (for example, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), carboxymethylcellulose (CMC) (for example, manufactured by Daicel Miraize Co., Ltd.), sodium deoxycholate (for example, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and SOLSPERSE. TM W100, SOLSPERSE TM W150 (manufactured by Lubrizol Japan, Inc.) etc. From the viewpoint of excellent dispersibility, dispersion stabilization ability and high concentration of multi-walled carbon nanotubes, CMC is particularly preferable.

[0160] When the specific CNT dispersion liquid contains a dispersant, the amount of the dispersant used is not particularly limited and can be set appropriately depending on the type of dispersant, the amount of multi-walled carbon nanotubes, the amount of dispersion medium, and the like.

[0161] [Method for producing specific CNT dispersion liquid] The method for producing the specific CNT dispersion liquid is not particularly limited. The specific CNT dispersion liquid can be produced by dispersing the specific CNT aggregate in a dispersion medium. That is, the specific CNT dispersion liquid can be produced by a method including a step of dispersing the specific CNT aggregate in a dispersion medium (also referred to as a "dispersion step"). The dispersion medium that can be used in the dispersion step is as described above.

[0162] The dispersion method is not particularly limited. Examples of the dispersion method include methods using a dispersion device such as a stirrer, a homogenizer, a colloid mill, a flow jet mixer, a dissolver, a paint conditioner, a Manton emulsifier, a jet mill, or an ultrasonic device. Examples of the dispersion method include methods using known pulverization means, such as ball milling (e.g., ball mill, vibration ball mill, planetary ball mill, bead mill, etc.), sand milling, colloid milling, jet milling, roller milling, and dispersing machines such as vertical or horizontal agitator mills, attritors, colloid mills, three-roll mills, pearl mills, super mills, impellers, dispersers, KD mills, dynatrons, and pressure kneaders. As a dispersion method, a method using a jet mill is preferable, and a method using a wet jet mill is more preferable. A wet jet mill is a dispersion device that pressure-feeds a mixture in a solvent as a high-speed flow from a nozzle arranged in a sealed pressure-resistant container. In the wet jet mill, multi-walled carbon nanotubes are dispersed in a pressure-resistant container by collisions between opposing flows, collisions with the container wall, turbulence caused by high-speed flows, shear flows, and the like. As a wet jet mill, an ultra-high pressure homogenizer (models: NAGS20, NAGS100, JAGS200, NAGS1000, etc.) manufactured by Jokou Corporation can be suitably used. However, the wet jet mill is not limited to this. When the above-mentioned ultra-high pressure homogenizer is used as the dispersing device, the dispersion treatment pressure is preferably 10 MPa to 250 MPa.

[0163] The method for producing the specific CNT dispersion liquid may include a step of drying the specific CNT aggregate (also referred to as a "drying step") prior to the above-mentioned dispersion step.

[0164] If moisture adheres to the CNTs, the CNTs will tend to adhere to each other due to the surface tension of the water, which may result in a decrease in dispersibility. Therefore, by carrying out a drying process of the conductive assistant body before the dispersion process, moisture adhered to the CNTs is removed, and adhesion between multi-walled carbon nanotubes due to moisture adhesion is suppressed, thereby further improving the dispersibility of the CNTs in the dispersion medium. The drying method is not particularly limited. Examples of the drying method include heat drying, vacuum drying, and heat vacuum drying. The drying method is preferably heated vacuum drying. The drying temperature is not particularly limited, and is preferably from 40°C to 100°C, for example. The drying time is not particularly limited, and can be appropriately set depending on the drying temperature, the degree of moisture adhesion to the multi-walled carbon nanotubes in the present disclosure, and the like.

[0165] An example of the production of the specific CNT dispersion liquid is shown below, but the production of the specific CNT dispersion liquid is not limited to the following.

[0166] <Production Example 1: Example of production of dispersion liquid> 0.040 g of the specific CNT aggregate according to the present disclosure is weighed and placed in a three-neck flask. After the specific CNT aggregate is placed in the flask, a large excess of ion-exchanged water as a dispersion medium is poured (for example, 20 mL) and stirred at room temperature (25°C, the same applies below). At this time, a known dispersant (for example, carboxymethylcellulose) may be added as appropriate. Next, a conductive assistant is dispersed in the dispersion medium using a known dispersion device (for example, an ultrasonic irradiation device or a wet jet mill). The obtained dispersion is further stirred with a stirrer at room temperature for a long period of time (for example, 1 hour to 48 hours). In this manner, a specific CNT dispersion is obtained.

[0167] [Conductive materials] The conductive material according to the present disclosure includes a specific CNT aggregate. As described above, the specific CNT aggregates contained in the conductive material according to the present disclosure have excellent conductivity when made into a dispersion liquid, and are therefore suitable as a conductive auxiliary. Since the conductive material according to the present disclosure contains the specific CT aggregate according to the present disclosure, it has excellent conductive efficiency and can effectively impart high conductivity to the object of use.

[0168] The conductive material according to the present disclosure may contain a known conductive assistant such as graphite, Ketjen black, etc. Furthermore, the conductive material according to the present disclosure may contain CNTs other than the specific CNT aggregate.

[0169] The conductive material according to the present disclosure can be used as one of electrode materials. An example of an electrode formed using the electrode material is an electrode included in a secondary battery. Hereinafter, an embodiment of the electrode and the secondary battery including the electrode will be described.

[0170] [Electrodes and secondary batteries] The electrode according to the present disclosure includes an electrode active material and a conductive material according to the present disclosure. The secondary battery according to the present disclosure includes the electrode according to the present disclosure. The electrode according to the present disclosure contains the conductive material according to the present disclosure, and therefore has excellent conductive path formation properties within the electrode, and therefore the secondary battery according to the present disclosure has excellent cycle characteristics. Hereinafter, an embodiment of an electrode and a secondary battery including the electrode will be described.

[0171] <Electrode> The electrodes can include specific CNT aggregates. In the electrode, the specific CNT aggregates can function as a conductive additive. The CNT aggregate contained in the electrode described below is synonymous with the specific CNT aggregate, and the preferred embodiments are also the same, so description of the CNT aggregate will be omitted below.

[0172] The electrode may be at least one of a positive electrode and a negative electrode. The electrode may include an electrode active material layer, or may include a current collector and an electrode active material layer disposed on the current collector.

[0173] There are no particular limitations on the current collector, so long as it does not induce a chemical change in the battery and has electrical conductivity. The current collector may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel whose surface has been treated with carbon, nickel, titanium, silver, etc. Specifically, a transition metal such as copper or nickel that has good carbon adsorption properties may be used as the current collector.

[0174] The electrode active material layer can include an electrode active material. The electrode active material is preferably electrode active material particles. When the electrode is a positive electrode, the electrode active material is not particularly limited, and the electrode active material layer can contain a positive electrode active material that is commonly used as an electrode material for a positive electrode. Specifically, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; a lithium iron oxide such as LiFe3O4; 1+c1 Mn 2-c1Lithium manganese oxides such as O4 (0 ≦ c1 ≦ 0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7; chemical formula LiNi 1-c2 M c2 O2 (where M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, and satisfies 0.01 ≦ c2 ≦ 0.66).) The Ni-site type lithium nickel oxide represented by; chemical formula LiMn 2-c3 M c3 O2 (where M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01 ≦ c3 ≦ 0.1.), or lithium manganese composite oxide represented by Li2Mn3MO8 (where M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn).); examples include LiMn2O4 in which a part of the Li in the chemical formula is substituted with an alkaline earth metal ion.

[0175] When the electrode is a negative electrode, the electrode active material is not particularly limited, and the electrode active material layer can contain a negative electrode active material usually used for a negative electrode material. Specifically, the negative electrode active material can contain graphite-based active material particles or silicon-based active material particles. As the graphite-based active material particles, at least one selected from the group consisting of artificial graphite, natural graphite, graphitized carbon fiber, and graphitized mesocarbon microbeads may be used. By using artificial graphite as the graphite-based active material particles, the rate characteristics can be improved. As the silicon-based active material particles, at least one selected from the group consisting of Si, SiOx (0 < x < 2), Si-C composite, and Si-Y alloy (where Y is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a transition metal, a Group 13 element, a Group 14 element, a rare earth element, and a combination thereof) may be used. By using the silicon-based active material particles, the battery can be made to have a higher capacity.

[0176] The electrode active material layer can further contain a binder. The binder is not particularly limited, and the electrode active material layer can contain a binder that is commonly used in electrode materials. Examples of the binder include at least one polymer selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, and polyacrylic acid, as well as polymers in which the hydrogen atoms of these polymers have been substituted with Li, Na, Ca, or the like.

[0177] <Secondary battery> The secondary battery may include a negative electrode, a positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte. At least one of the positive electrode and the negative electrode is an electrode formed using a conductive material containing the specific CNT aggregate as an electrode material.

[0178] The separator separates the negative electrode and the positive electrode and provides a path for lithium ion migration, and is not particularly limited as long as it is a separator that is usually used as a separator in a secondary battery. The separator preferably has low resistance to ion migration of the electrolyte and is excellent in the ability to wet the electrolyte solution. A specific example of the separator is a porous polymer film. The porous polymer film may be, for example, a porous polymer film made from a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer, or a laminate structure in which two or more of these films are laminated. The separator may be a typical porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. The separator may be coated with a ceramic component or a polymeric substance to ensure heat resistance or mechanical strength. The separator may optionally be of single layer or multi-layer construction.

[0179] The electrolyte is not particularly limited, and examples thereof include electrolytes such as organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used when manufacturing lithium secondary batteries.

[0180] Specifically, the electrolyte can include a non-aqueous organic solvent and a metal salt. Examples of non-aqueous organic solvents include aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydroxyfuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphate triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.

[0181] Among carbonate-based organic solvents, cyclic carbonates such as ethylene carbonate and propylene carbonate are preferably used as non-aqueous organic solvents because they have a high dielectric constant as a high-viscosity organic solvent and dissociate lithium salts well. It is more preferable to use such a cyclic carbonate mixed with a linear carbonate having a low viscosity and a low dielectric constant such as dimethyl carbonate or diethyl carbonate in an appropriate ratio as a non-aqueous organic solvent, since an electrolyte having a high electrical conductivity can be obtained.

[0182] The metal salt may be a lithium salt. The lithium salt is a substance that is easily dissolved in the non-aqueous electrolyte. The anion portion of the lithium salt is, for example, F - , Cl - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , and (CF3CF2SO2)2N - Examples include:

[0183] In addition to the non-aqueous organic solvent and metal salt, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, and aluminum trichloride for the purposes of improving the life characteristics of the battery, suppressing a decrease in battery capacity, and improving the discharge capacity of the battery.

[0184] The above-mentioned secondary battery can be configured into a battery module including the secondary battery as a unit cell, and a battery pack including the battery module. The battery module and the battery pack can be used as a power source for a medium to large device selected from the group consisting of, for example, an electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, and a power storage system.

[0185] The planar aggregate of the present disclosure is the aggregate of carbon nanotubes of the present disclosure, and the aggregate of carbon nanotubes includes carbon nanotubes having a maximum length of 1000 μm to 30000 μm. The ratio of carbon nanotubes having a maximum length of 1000 μm to 30000 μm contained in the planar assembly of the present disclosure is usually 1 mass % or more. The planar assembly of the present disclosure may contain other components such as a carbon nanotube aggregate containing carbon nanotubes having a maximum length of less than 1000 μm, that is, a carbon nanotube aggregate not containing carbon nanotubes having a maximum length of 1000 μm to 30000 μm. The planar aggregate of the present disclosure can be produced, for example, as a nonwoven fabric-like planar aggregate, by dispersing a carbon nanotube aggregate containing carbon nanotubes with a maximum length of 1000 μm to 30000 μm, or the carbon nanotube aggregate and other components such as a carbon nanotube aggregate containing carbon nanotubes with a maximum length of less than 1000 μm, in water or other fluid, and filtering once or twice or more times.

[0186] The planar assembly of the present disclosure includes, for example, a film. The planar assemblies of the present disclosure are useful, for example, in filters, electromagnetic shields, and extreme ultraviolet (EUV) pellicles. EXAMPLES

[0187] The specific CNT aggregate and the dispersion containing the specific CNT aggregate according to the present disclosure will be described in more detail below with reference to examples. The aggregate and dispersion according to the present disclosure are not limited to the following examples as long as they do not deviate from the gist of the disclosure. Unless otherwise specified, "%" means "% by mass" and "ppm" means "ppm by mass".

[0188] Example 1 1. Production of sheet-shaped CNT aggregate 1 The sheet-like CNT aggregate 1 was prepared by a floating catalyst method (CVD method) that directly interacts with the self-assembly of CNT bundles in the gas phase. First, ferrocene as a metal catalyst precursor containing Fe atoms and thiophene as a promoter were introduced into a continuous flow of carrier gas in a once-through reactor whose temperature was controlled at 400°C to 700°C. A mixture of nitrogen and argon was used as the carrier gas. The flow rate of the carrier gas was 30,000sccm (standard cubic centimeter per minute). By maintaining the temperature in the flow-through reactor within the above range, the metal catalyst precursor was produced as a particulate metal catalyst. The region in which the metal catalyst was produced is referred to as the first temperature zone.

[0189] The carbon source, methane, was then released into the carrier gas stream. The metal catalyst and carbon source were fed into a second temperature zone downstream of the first temperature zone, which was temperature-controlled at 1400° C. The second temperature zone was maintained at a temperature sufficient to produce carbon nanotube aggregates.

[0190] In the second temperature zone, an electric field was generated within the temperature-controlled flow reactor, which generated CNT aggregates. The aggregates of CNTs were continuously discharged through the outlet of a flow-type reactor whose temperature was controlled at 100°C to 500°C, and a sheet-like CNT aggregate was collected by continuous discharge. The obtained sheet-shaped CNT aggregate 1 contains MWCNTs. The obtained sheet-like CNT aggregate was washed with pure water for 10 seconds in order to adjust the contents of Fe atoms, Co atoms, Na atoms, and K atoms, thereby obtaining a sheet-like CNT aggregate 1, which is a specific CNT aggregate.

[0191] 2. Preparation of CNT Dispersion 1 The following materials were mixed and pre-dispersed by processing for 1 hour with an Ace Homogenizer manufactured by Nippon Seiki Co., Ltd. to obtain a pre-dispersion liquid 1. Note that the sheet-like CNT aggregate 1 was cut into small pieces of 1 cm x 1 cm with scissors before mixing so that the sheet-like CNT aggregate 1 would not become entangled with the blades of the homogenizer.

[0192] (Dispersion liquid composition) 1.1g of the sheet-like CNT aggregate 1 obtained above ·CARBOXYMETHYL CELLULOSE SODIUM SALT HIGH VISCOSITY (manufactured by MP Biomedicals) 1.65g ·Pure water 547.25g

[0193] The pre-dispersion liquid 1 was subjected to main dispersion using an ultra-high pressure homogenizer (model: NAGS100) manufactured by Jokou Corporation as a wet jet mill under the following conditions, to obtain CNT dispersion liquid 1, which is a specific CNT dispersion liquid. (dispersion condition) Nozzle diameter: 0.22mm Pressure: 85MPa Number of times: 8 Method: Circulation method

[0194] 3. Evaluation 3-1. Contents of Fe atoms, Co atoms, Na atoms, and K atoms relative to the total mass of the aggregate The contents of Fe atoms, Co atoms, Na atoms, and K atoms contained in the sheet-like CNT aggregate 1 of Example 1 were measured using an inductively coupled plasma mass spectrometry (ICP-MS) device (PerkinElmer, NexION 2000C). The sheet-like CNT aggregate 1 was subjected to low-temperature ashing / acid dissolution as a pretreatment, and measured with the above device. As a result, the content of Fe atoms relative to the total mass of the aggregate in the sheet-like CNT aggregate 1 of Example 1 was 56000 ppm, the content of Co atoms was less than 10 ppm (below the detection limit), the content of Na atoms was 100 ppm, and the content of K atoms was 500 ppm. In other words, the total content of Fe atoms and Co atoms was 56000 ppm, and the total content of Na atoms and K atoms was 600 ppm.

[0195] 3-2.Volume resistivity The sheet-like CNT aggregate 1 of Example 1 was pulverized using a freeze-pulverization method. Using a Loresta device (product name: powder resistivity measurement system MCP-PD51, low resistivity meter Loresta-GP, low resistance probe for powder MCP-PD511 (constant current application type 4-probe method), all manufactured by Nitto Seiko Analytech Co., Ltd.), the pulverized sheet-like CNT aggregate 1 was introduced into a powder resistivity measurement probe unit, and pressed at 1 kN and 20 kN using an attached hydraulic pump until the target load was reached, and then the volume resistivity (Ω·cm) was measured. As a result, the volume resistivity is 1.7×10 at 1 kN. -2 Ω cm, and 5.0×10 at 20 kN -3 The ratio of the volume resistivity at 20 kN to the volume resistivity at 1 kN (referred to as "resistivity ratio" in Table 1) was 0.29.

[0196] 3-3. Electrical conductivity of dispersion liquid CNT dispersion liquid 1 was dropped onto a glass substrate (10 cm × 10 cm) and formed into a film using a stainless steel applicator with a gap size of 150 μm. After that, it was heated on a hot plate at 110°C for 10 minutes and dried. The surface resistivity of the film was measured using Loresta GXII manufactured by Nitto Seiko Analytech Co., Ltd. Measurements were performed at five points on the film, and the average of the five values ​​was taken as the surface resistivity. As a result, the surface resistivity was 164.42 Ω / □.

[0197] 3-4. Check the bundle structure The obtained sheet-like CNT aggregate 1 of Example 1 was observed with an SEM (apparatus name: S-4800, manufactured by Hitachi High-Technologies Corporation) and was confirmed to contain a bundle structure. Lengths were measured at 20 points and the average value was calculated, resulting in a width of the bundle structure of 70 nm.

[0198] 3-5. Pore volume The pore volume was measured using a gas adsorption measurement device (product name "BELSORP-miniII", manufactured by Microtrack-Bel). The sheet-shaped CNT aggregate 1 obtained in Example 1 was used as a measurement sample. The pore volume was measured after the sheet-like CNT aggregate 1 was subjected to a vacuum degassing treatment at 300°C for 3 hours using a pretreatment device (product name "BELPREP-vacII", manufactured by Microtrack-Bel). For the sheet-shaped CNT aggregate 1 after the vacuum degassing treatment, the nitrogen adsorption / desorption isotherm was measured using a constant volume method. The measurement temperature was 77K, the adsorbate was nitrogen, the saturated vapor pressure was measured, and the adsorbate cross section was 0.162 nm 2 The waiting time after the adsorption equilibrium state was reached was set to 500 seconds. The pore volume was calculated from the obtained adsorption / desorption isotherms using the BJH method. As a result, the pore volume of the sheet-like CNT aggregate 1 was 2.06 cm 3 / g.

[0199] The above evaluation results are shown in Table 1. In the section on confirmation of bundle structure, if the bundle structure was confirmed, it is recorded as "Yes", and if it was not confirmed, it is recorded as "-".

[0200] Example 2 1. Production of fibrous CNT aggregate 2 Like the sheet-like CNT aggregate 1, the fibrous CNT aggregate 2 was also produced by the floating catalyst method (CVD method) which directly interacts with the self-aggregation of CNT bundles in the gas phase. First, ferrocene as a metal catalyst precursor containing Fe atoms and thiophene as a promoter were introduced into a continuous flow of carrier gas in a once-through reactor whose temperature was controlled at 400°C to 700°C. A mixture of nitrogen and argon was used as the carrier gas. The flow rate of the carrier gas was 30,000sccm. By maintaining the temperature in the flow-through reactor within the above range, the metal catalyst precursor was produced as a particulate metal catalyst. The region in which the metal catalyst was produced is referred to as the first temperature zone.

[0201] The carbon source, methane, was then released into the carrier gas stream. The metal catalyst and carbon source were fed into a second temperature zone downstream of the first temperature zone, which was temperature-controlled at 1400° C. The second temperature zone was maintained at a temperature sufficient to produce carbon nanotube aggregates.

[0202] In the second temperature zone, an electric field was generated within a temperature-controlled flow reactor, which produced fibrous CNT aggregates. The carbon nanotube aggregates were continuously discharged through the outlet of a flow-type reactor whose temperature was controlled at 100° C. to 500° C., and fibrous CNT aggregates were collected by continuous discharge. The obtained fibrous CNT aggregate contains MWCNTs. The obtained fibrous CNT aggregate was washed with pure water for 10 seconds in order to adjust the contents of Fe atoms, Co atoms, Na atoms, and K atoms, and a fibrous CNT aggregate 2 was obtained.

[0203] 2. Preparation of CNT Dispersion 2 Using the obtained fibrous CNT aggregate 2, a CNT dispersion liquid 2 was obtained in the same manner as in Example 1.

[0204] 3. Evaluation The fibrous CNT aggregate 2 and the CNT dispersion 2 of Example 2 were evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1.

[0205] Example 3 1. Production of sheet-shaped CNT aggregate 3 The sheet-like CNT aggregate obtained in Example 1 was immersed in a polytetrafluoroethylene (PTFE) tray containing hydrochloric acid (special grade reagent, manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) for 24 hours. After that, the sheet-like CNT aggregate was taken out of the tray and washed with deionized water until the pH of the washing water became 7, and a sheet-like CNT aggregate 3 was obtained.

[0206] 2. Preparation of CNT Dispersion 3 Using the obtained sheet-shaped CNT aggregate 3, a CNT dispersion 3 was obtained in the same manner as in Example 1.

[0207] 3. Evaluation The sheet-shaped CNT aggregate 3 and the CNT dispersion 3 of Comparative Example 1 were evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1.

[0208] Comparative Example 1 1. Preparation of Powdered CNT Aggregates 4. As the powdered CNT aggregate 4, "multi-walled carbon nanotubes" (catalog number: 901019, 50-90 nm diameter, >95% carbon basis, manufactured by Sigma-Aldrich) were prepared.

[0209] 2. Preparation of CNT Dispersion 4 Using the prepared powdered CNT aggregate 4, a CNT dispersion liquid 4 was obtained in the same manner as in Example 1.

[0210] 3. Evaluation The powdered CNT aggregate 4 and the CNT dispersion liquid 4 of Comparative Example 1 were evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1.

[0211] Comparative Example 2 1. Preparation of Powdered CNT Aggregates 5 As the powdered CNT aggregate 5, "multi-walled carbon nanotubes" (catalog number: FT7000, manufactured by C-nano Corporation) were prepared.

[0212] 2. Preparation of CNT Dispersion 5 Using the prepared powdered CNT aggregate 4, a CNT dispersion liquid 5 was obtained in the same manner as in Example 1.

[0213] 3. Evaluation The powdered CNT aggregate 5 and the CNT dispersion liquid 5 of Comparative Example 2 were evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0214] Comparative Example 3 1. Preparation of Powdered CNT Aggregates 6. As the powdered CNT aggregate 6, "single-walled carbon nanotubes" (catalog number: TUBALL TM A 1000-milliliter (manufactured by OCSiAl) was prepared.

[0215] 2. Preparation of CNT Dispersion 6 Using the prepared powdered CNT aggregate 6, a CNT dispersion liquid 6 was obtained in the same manner as in Example 1.

[0216] 3. Evaluation The powdered CNT aggregate 6 and the CNT dispersion liquid 6 of Comparative Example 3 were evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0217] Comparative Example 4 1. Preparation of Powdered CNT Aggregates 7 As the powdered CNT aggregate 7, "multi-walled carbon nanotubes" (catalog number: FT6120, manufactured by C-nano Corporation) were prepared.

[0218] 2. Preparation of CNT Dispersion 7 Using the prepared powdered CNT aggregate 7, a CNT dispersion 7 was obtained in the same manner as in Example 1.

[0219] 3. Evaluation The powdered CNT aggregate 7 and the CNT dispersion 7 of Comparative Example 4 were evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0220] [Table 1]

[0221] As shown in Table 1, it is understood that the CNT dispersion obtained by dispersing the CNT aggregates of the example has good electrical conductivity. On the other hand, the CNT aggregates of Comparative Example 1 and Comparative Example 2, in which the total content of Na atoms and K atoms was less than 50 ppm or more than 1000 ppm and the ratio of the volume resistivity at 20 kN to the volume resistivity at 1 kN was less than 0.21, had problems with the conductivity of the CNT dispersion obtained by dispersing. It is clear that the CNT aggregates of Comparative Example 1 and Comparative Example 2 are inferior as conductive materials. In addition, the CNT aggregate of Comparative Example 3, in which the total content of Fe atoms and Co atoms is greater than 100,000 ppm and the total content of Na atoms and K atoms is greater than 1,000 ppm, and the CNT aggregate of Comparative Example 4, in which the total content of Fe atoms and Co atoms is less than 2,000 ppm, both had problems with the conductivity of the CNT dispersion obtained by dispersion. It is clear that the CNT aggregates of Comparative Example 3 and Comparative Example 4 are inferior as conductive materials.

Claims

1. An aggregate of carbon nanotubes which satisfies the following conditions (1), (2), and (3): (1) At least one of Fe atoms and Co atoms is contained, and the total content of Fe atoms and Co atoms is 2000 ppm by mass to 60000 ppm by mass with respect to the total mass of the aggregate of carbon nanotubes. (2) At least one of Na atoms and K atoms is contained, and the total content of Na atoms and K atoms is 50 ppm by mass to 700 ppm by mass with respect to the total mass of the aggregate of carbon nanotubes. (3) The ratio of the volume resistivity under a pressure of 20 kN to the volume resistivity under a pressure of 1 kN is 0.21 or more.

2. The carbon nanotube aggregate according to claim 1 , comprising a bundle structure.

3. Pore ​​volume is 0.60 cm 3 / g ~ 3.20 cm 3 The carbon nanotube aggregate according to claim 1 or 2, wherein the aggregate is a tensile strength of 1 / g.

4. A carbon nanotube dispersion comprising the aggregate of carbon nanotubes according to claim 1 or 2 and a dispersion medium.

5. A conductive material comprising the carbon nanotube aggregate according to claim 1 or 2.

6. An electrode comprising an electrode active material and the conductive material according to claim 5 .

7. A secondary battery comprising the electrode according to claim 6.

8. The carbon nanotube aggregate according to claim 1 or 2, The carbon nanotube aggregate includes carbon nanotubes having a maximum length of 1000 μm to 30000 μm.

9. A filter using the planar assembly according to claim 8.

10. 9. An electromagnetic wave shield using the planar assembly according to claim 8.

11. A pellicle for extreme ultraviolet rays using the planar assembly according to claim 8.

Citation Information

Patent Citations

  • Method of purifying composition containing carbon nanotube

    JP2004277279A

  • Method for cleaning carbon nanotubes, carbon nanotube substrate, and use thereof

    JP2016527171A

  • Conductive material for secondary battery and secondary battery containing the same

    JP2018530854A

  • Precursor materials and methods for producing nanostructured carbon materials - Patents.com

    JP2021521094A

  • Carbon nanotube dispersion composition, and resin composition using the same, electrode film, secondary battery, and vehicle

    JP2023069017A

Cited By

  • Carbon nanotube aggregates, conductive materials, electrodes, secondary batteries, planar aggregates, laminates, filters, electromagnetic shielding, and pellicles for extreme ultraviolet radiation.

    JP2026129611A

  • Carbon nanotube aggregates, conductive materials, electrodes, secondary batteries, planar aggregates, laminates, filters, electromagnetic shielding, and pellicles for extreme ultraviolet radiation.

    JP2026129621A

  • Carbon nanotube aggregates, conductive materials, electrodes, secondary batteries, planar aggregates, laminates, filters, electromagnetic shielding, and pellicles for extreme ultraviolet radiation.

    JP2026129624A

  • Carbon nanotube aggregates, conductive materials, electrodes, secondary batteries, planar aggregates, laminates, filters, electromagnetic shielding, and pellicles for extreme ultraviolet radiation.

    JP2026162818A

  • Carbon nanotube aggregates, conductive materials, electrodes, secondary batteries, planar aggregates, filters, electromagnetic shielding, and pellicles for extreme ultraviolet radiation.