Ternary positive electrode material and its manufacturing method, positive electrode plate and lithium ion battery

By optimizing the surface distribution of Co and Al in the Li a (Ni x Co y M 1-x-y ) 1-b M’ b O 2-c A c composition, the method addresses the challenge of maintaining high performance and stability in ternary cathode materials with low Co content, achieving cost-effectiveness and improved cycle life.

JP7574266B2Active Publication Date: 2024-10-28SHANGHAI RUIPU ENERGY CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022200283
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-01-26
Filing Date
2022-12-15
Publication Date
2024-10-28
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

Existing methods for producing ternary cathode materials with low cobalt content struggle to maintain high charge-discharge characteristics and structural stability while reducing production costs, as conventional methods either require high Co content or result in ineffective surface coatings that degrade during cycling.

Method used

A chemical composition of Li a (Ni x Co y M 1-x-y ) 1-b M’ b O 2-c A c is used, where M includes Mn and Al, with controlled surface distribution of Co and Al elements through specific manufacturing processes to ensure high Co content near the surface and prevent Al penetration, maintaining low DC resistance and cycle stability.

Benefits of technology

The method results in a ternary cathode material with reduced Co content, lower production costs, and improved electronic and ionic conduction, along with enhanced cycle stability and long-term performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574266000001
    Figure 0007574266000001
Patent Text Reader

Abstract

To provide a ternary positive electrode material and a manufacturing method thereof, a positive electrode plate, and lithium ion battery in order to overcome defects in a prior art.SOLUTION: A ternary positive electrode material and a manufacturing method thereof, a positive electrode plate, and a lithium ion battery are provided according to the present invention. The ternary positive electrode material has the following chemical composition: Lia(NixCoyM1-x-y)1-bM'bO2-cAc, where 0.75≤a≤1.2, 0.5≤x<1, 0<y≤0.1, 0≤b≤0.01 and 0≤c≤0.2; M is at least one selected from Mn and Al; M' is at least one selected from Al, Zr, Ti, Y, Sr, W and Mg; A is at least one selected from S, F and N; 2%≤CCo1-CCo, and 5%≤CAl-CAl1. The lithium ion battery of the invention is superior in DC internal resistance (DCR), and excellent in long-term charge-discharge cycle characteristic.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of lithium ion batteries, in particular to a ternary positive electrode material having an α-NaFeO2 structure and its manufacturing method, a positive electrode plate and a lithium ion battery. [Background technology]

[0002] LiNiCoMn and LiNiCoAl ternary cathode materials with α-NaFeO2 structure have become one of the mainstream cathode materials for lithium-ion power batteries due to their relatively high capacity per gram and excellent charge-discharge characteristics.

[0003] In the ternary cathode material, the three main transition metal elements play different roles. The Ni element is the main contributor to capacity and energy, which undergoes valence state changes during the charge and discharge process and contributes to charge compensation inside the material during the lithium ion insertion / desorption process. The Co element has two itinerant electrons, which can contribute to the electronic conduction of the material, as well as capacity and energy through valence state changes. The Mn / Al elements can make the crystal structure of the material more stable and improve the stability of the material during the lithium ion insertion / desorption process.

[0004] Co element is important for the charge and discharge characteristics of ternary cathode materials. However, as a precious metal, it is rare and more expensive than the other two major metal elements. In order to reduce the cost of ternary cathode materials, it is necessary to reduce the amount of Co element used while maintaining performance.

[0005] Adjusting the spatial distribution of each metal element is an effective means to improve the Co utilization rate. WO2019120973A1 provides a method for producing a concentration gradient ternary cathode material with a single crystal morphology, but the materials and methods described in the application are only applicable to ternary lithium-containing compounds with a Co content of >10%, and the concentration gradient design cannot be applied to cases with lower Co contents. WO2021153546A1 describes a method for producing a Co-coated ternary cathode active material, but the Co coating temperature in the process is 700°C or higher, and it is difficult to effectively coat other oxide particles that contribute to the material performance at this temperature. In view of the above, a new manufacturing method is needed to obtain a product with high charge / discharge properties and low Co content and surface coating. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2019 / 120973 [Patent Document 2] International Publication No. 2021 / 153546 Summary of the Invention [Problem to be solved by the invention]

[0007] In view of the deficiencies of the prior art, the present invention aims to provide a ternary positive electrode material and its manufacturing method, a positive electrode plate and a lithium ion battery. [Means for solving the problem]

[0008] The object of the present invention is achieved by the following technical means. The first aspect of the present invention is a compound having a chemical composition of Li a (Ni x Co y M 1-x-y ) 1-b M' b O 2-c A cwhere 0.75 ≤ a ≤ 1.2, 0.5 ≤ x < 1, 0 < y ≤ 0.1, 0 ≤ b ≤ 0.01, 0 ≤ c ≤ 0.2, M is at least one selected from Mn and Al, M' includes one or more selected from Al, Zr, Ti, Y, Sr, W, Mg, and A is one or more selected from S, F, N, to provide a ternary cathode material.

[0009] In some embodiments, M' is one or more selected from Al, Zr, Ti, Y, Sr, W, Mg. In some embodiments, M' includes Al and optionally one or more selected from Zr, Ti, Y, Sr, W, Mg. In some embodiments, M' is composed of Al and optionally one or more selected from Zr, Ti, Y, Sr, W, Mg. In some embodiments, M' includes Al and one or more selected from Zr, Ti, Y, Sr, W, Mg. In some embodiments, M' is composed of Al and one or more selected from Zr, Ti, Y, Sr, W, Mg. In some embodiments, M' includes Al and Zr. In some embodiments, M' is composed of Al and Zr.

[0010] In some embodiments, 0.95 ≤ a ≤ 1.1, for example, 0.99 ≤ a ≤ 1.05.

[0011] In some embodiments, 0.55 ≤ x < 0.76, for example, 0.6 ≤ x < 0.76.

[0012] The chemical composition of the ternary cathode material of the present invention is Li a (Ni x Co y M 1-x-y ) 1-b M' b O 2-c A c where, since y ≤ 0.1, the ternary cathode material of the present invention is a low-cobalt ternary cathode material. In some embodiments, 0.05 < y ≤ 0.1, for example, 0.06 < y ≤ 0.09.

[0013] In some embodiments, 0 < b ≤ 0.01, for example, 0.001 ≤ b ≤ 0.005. In some embodiments, c is 0, that is, the A element does not exist.

[0014] In the ternary cathode material of the present invention, 2% ≤ C Co1 -C Co where C Co1 is the atomic ratio of Co element to the total metal elements excluding Li element obtained by measuring the etched cathode material by X-ray photoelectron spectroscopy (XPS), and C Co is the atomic ratio of Co element to the total metal elements excluding Li element obtained by measuring the cathode material by inductively coupled plasma (ICP). In some embodiments, C Co1 is the atomic ratio of Co element to the total metal elements excluding Li element obtained by measuring the etched cathode material at a depth of about 20 - 60 nm from the surface by XPS. The ternary cathode material satisfying this technical feature has a Co content (C Co1 ) at a depth of about 20 - 60 nm from the surface significantly higher than the Co content (C Co ) in the bulk phase, and a lower DC resistance can be obtained. This is because the resistance when electrons and Li ions transition at the interface (the solid-liquid interface between the electrolyte and the cathode material) during the operation process of the lithium-ion battery is greater than the resistance when they transition in the bulk phase (inside the cathode material), and Co has a positive effect on the structural stability and ion / electron conduction of the ternary cathode material. When more Co elements accumulate on the material surface, the conduction speed of electrons and Li ions at the interface is improved, and the transition speeds of electrons and Li ions between the material surface and the bulk phase can be matched, fully exerting the output performance of the material. On the other hand, if the accumulation of Co elements remains only on the material surface or at a depth of <20 nm, the Co-rich coating layer is easily destroyed during the cycle charge and discharge process of the battery, so the DC resistance of the material cannot be maintained. The ternary cathode material of the present invention has a higher surface Co content when etched than the overall Co content of the material, and can maintain a lower DC resistance in the long term during the use process of the material.

[0015] In the ternary positive electrode material of the present invention, 5%≦C Al -C Al1 and C Al is the atomic ratio of Al element in all metal elements excluding Li element obtained by measuring the positive electrode material directly by XPS, and C Al1 is the atomic ratio of Al element to all metal elements excluding Li element obtained by measuring the etched positive electrode material by XPS. In some embodiments, C Al1 is the atomic ratio of Al element in all metal elements excluding Li element obtained by measuring the etched positive electrode material at a depth of about 20 to 60 nm from the surface by XPS. A ternary positive electrode material that satisfies the technical feature has an Al content (C Al ) is the Al content (C Al1 ) and has better cycle stability. This is because the Al element is coated on the surface of the material in the form of an oxide, which can reduce the side reaction between the polyvalent metal ions in the ternary material and the electrolyte. On the other hand, when Al penetrates into the lattice of the material, the diffusion rate of Li ions and the electronic conductivity in the material are reduced, and the capacity per gram of the material is reduced. The surface Al content of the ternary positive electrode material of the present invention before etching is obviously higher than the surface Al content of the material after etching, and a better cycle battery capacity can be obtained within a range that does not affect the capacity of the material.

[0016] In some embodiments, C Al -C Al1 ≧5.3%, for example, ≧7.5%. Preferably, 10%≦C Al -C Al1 It is. Preferably, 10%≦C Al -C Al1 ≦20%.

[0017] In some embodiments, C Co1 -C Co ≧2.7%, for example, ≧3.2%. Preferably, 5%≦C Co1 -C Co It is. Preferably, 5%≦C Co1 -C Co ≦11%.

[0018] Preferably, the etching conditions are Ar + Ion etching, 2500 eV≦E≦3500 eV, 90 s≦t≦100 s, where E is the energy used for etching and t is the etching time.

[0019] Preferably, the ternary cathode material has a single crystal or single crystal-like morphology. Preferably, the particle diameter D when the particle size distribution of the ternary positive electrode material reaches 50% cumulatively v50 2μm≦D v50 This means that the particle diameter of the particles that make up 50% of the total volume is D v50 where D v50 This means that the particle size is within the range of 2 to 5 μm and is a commonly used method of measurement for particle size.

[0020] A second aspect of the present invention is Step S1 of thoroughly mixing a ternary positive electrode precursor comprising Ni, Co, Mn or Ni, Co, Al with a lithium source to form a mixture I, in which a compound comprising element M', such as an oxide of element M', may or may not be added, preferably element M' is element M' other than Al, such as one or more elements selected from Zr, Ti, Y, Sr, W, Mg, in which a compound comprising element A, such as an acid or salt comprising an anion A, may or may not be added; Step S2 of heating the mixture I in an air or oxygen atmosphere, holding it at 700-1100°C for 4-15 hours, and rolling and grinding the mixture to obtain an intermediate product II; Step S3 of thoroughly mixing the intermediate product II, the aluminum-containing solid powder, and the Co-containing solid powder to form a mixture III, in which a compound containing an element M', such as an oxide of the element M', may or may not be added, preferably the element M' is an element M' other than Al, such as one or more elements selected from Zr, Ti, Y, Sr, W, and Mg, in which a compound containing an element A, such as an acid or salt containing an anion A, may or may not be added; and step S4 of heating the mixture III in an air or oxygen atmosphere, maintaining the mixture III at 700-1000°C for 4-15 hours, and rolling and grinding the mixture III to obtain a ternary cathode material having an α-NaFeO2 structure.

[0021] In the present invention, the ternary cathode material may contain one or more elements selected from Zr, Ti, Y, Sr, W, and Mg as the element M', but may not contain these elements. The one or more elements selected from Zr, Ti, Y, Sr, W, and Mg may be doped and / or coated in the ternary cathode material.

[0022] In some embodiments, the element M' in the ternary cathode material includes one or more elements selected from Zr, Ti, Y, Sr, W, and Mg, and a compound including one or more elements selected from Zr, Ti, Y, Sr, W, and Mg is added as the element M' in the process of forming mixture I and / or the process of forming mixture III. The compound including one or more elements selected from Zr, Ti, Y, Sr, W, and Mg as the element M' added in the process of forming mixture I may be a dopant for the ternary cathode material. The compound including one or more elements selected from Zr, Ti, Y, Sr, W, and Mg as the element M' added in the process of forming mixture III may be a coating for the ternary cathode material.

[0023] The compound containing the element M' applicable to the present invention includes, but is not limited to, an oxide of the element M', a hydroxide containing the element M', and the like.

[0024] In some embodiments, the ternary cathode material includes an element A, and a compound including element A is added in the process of forming mixture I and / or in the process of forming mixture III. The compound including element A added in the process of forming mixture I and the process of forming mixture III may be a modifier of the ternary cathode material.

[0025] In some embodiments, the ternary cathode material includes element A, and a compound including element A is added in the process of forming mixture III.

[0026] The compound containing element A applicable to the present invention includes, but is not limited to, an acid or salt containing an anion A. Preferably, the salt or acid salt containing an anion A may be one or more selected from ammonium fluoride, lithium fluoride, ammonium nitrate, lithium nitrate, ammonium sulfate, ammonium hydrogen sulfate, lithium sulfate, lithium hydrogen sulfate, ammonium sulfide, ammonium hydrogen sulfide, lithium sulfide, and lithium hydrogen sulfide.

[0027] In some embodiments, the element M′ in the ternary cathode material comprises one or more elements selected from Zr, Ti, Y, Sr, W, and Mg, and in step S1, a compound comprising one or more elements selected from Zr, Ti, Y, Sr, W, and Mg is further added in the process of forming mixture I.

[0028] In some embodiments, the ternary cathode material includes element A, and in step S3, a compound including element A is further added in the process to form mixture III.

[0029] In some embodiments, in step S1, the lithium source is one or more selected from lithium carbonate and lithium hydroxide.

[0030] In some embodiments, in step S1, the element M′ in the ternary cathode material comprises Zr element, and a Zr-containing compound is further added in the process of forming mixture I.

[0031] Preferably, in step S1, the Zr-containing compound is any one or more selected from ZrO2, Zr(OH)4.

[0032] In some embodiments, in step S3, the aluminum-containing solid powder is an aluminum oxide powder, and the particle size range of the aluminum-containing solid powder is 100 nm≦D 酸化アルミニウム ≦1000 nm. For example, D 酸化アルミニウム It may be 100 nm, 150 nm, 200 nm, 300 nm, 400 nm, 500 nm, etc.

[0033] Preferably, in step S3, the Co-containing solid powder is any one or more selected from Co3O4, CoO, Co(OH)2, CoOOH, and CoCO3.

[0034] In some embodiments, in step S3, the substance ratio of Co element to intermediate product II in the Co-containing solid powder is (1-3):100, such as 1:100, 1.5:100, 2:100, 2.5:100, etc.

[0035] In some embodiments, in step S3, the mass ratio of Al element to intermediate product II in the aluminum-containing solid powder is (0.02-1.5):100, such as 0.1:100, 0.15:100, 0.2:100, 0.25:100, 0.3:100, 0.5:100, 1:100, etc.

[0036] A third aspect of the present invention provides a positive plate comprising the ternary positive material according to any one of the embodiments herein. The ternary cathode materials and cathode plates of the present invention may be utilized in lithium ion batteries.

[0037] A fourth aspect of the present invention provides a lithium-ion battery comprising a positive plate according to any one of the embodiments herein.

[0038] The design idea of ​​the present invention is that the Co element in the ternary cathode material has high electronic conductivity properties and can stabilize the layered structure of the material, so that the ternary cathode material with a high Co content has better internal resistance and surface stability. However, the content of Co element in the earth is low and the cost is high. In order to obtain a NCM ternary cathode material with higher performance at the same ratio, Co is coated on the surface of the material. However, Co requires a relatively high temperature (>800°C) to form an effective structure, and cannot be used in combination with other commonly used coatings of ternary cathode materials, especially Al2O3, which can effectively inhibit surface side reactions. When Al2O3 is used as a coating agent for high temperature treatment (>800°C) on the surface of the material, the Al element penetrates into the lattice of the ternary cathode material, which not only loses the effect of surface protection, but also makes it difficult for Li ions to be desorbed from the material, resulting in a decrease in the capacity per gram of the material and an increase in impedance. In the ternary cathode material provided by the present invention, Co element is accumulated on the surface, and the Al element is prevented from penetrating into the bulk phase of the material in large quantities, so that the material has low DC resistance and long-term charge-discharge cycle characteristics. In order to achieve this effect, the present application adds a large-particle Al-containing solid powder as a coating agent in addition to the Co-containing solid powder during the secondary sintering of the material. Compared with the small-particle nano-sized aluminum oxide coating agent commonly used in this field, the large-particle aluminum-containing solid powder has a high melting point, a relatively small contact surface with the intermediate product of the ternary cathode material obtained by the primary sintering, and a higher temperature is required to carry out a solid-state reaction with the intermediate product, so that the high-temperature coating process of the present application can accumulate Co on and near the surface of the material, and retain more Al on the surface of the material.

[0039] Compared with the prior art, the present invention has the following advantages: (1) The Co content in the ternary cathode material of the present invention is less than 10%, so that the cost of the material can be obviously reduced. Some Co elements are accumulated on the surface of the material, which reduces the resistance in the interfacial conduction process of lithium ions and electrons, so that the material shows excellent output performance, and the Co element is accumulated near the surface of the material, so that the ratio of the Co element near the surface is higher than the average ratio of the Co element in the material, which ensures low DC resistance in the long-term cycle process of the material. In addition, the Al element is coated on the surface of the material, and the Al element is not penetrated during the sintering process, so that there is an obvious concentration difference (≧5%) between the surface and the near surface of the material. These Al elements can form aluminum oxide or aluminate containing lithium, so that they have an inhibitory effect on the surface side reaction in the battery charge and discharge process of the material, which can further extend the cycle life of the material.

[0040] (2) By treating the material with the method of the present invention, it is possible to etch approximately 20-60 nm of the surface structure of the material, thereby exposing elements near its surface. The relatively high Co content of the material at this depth allows it to maintain a lower DC resistance during long-term cycling processes.

[0041] (3) The positive electrode material of the present invention preferably has particles having a single crystal or single crystal-like morphology, since it has fewer cracks due to lattice constant changes during charge and discharge processes than polycrystalline materials and has excellent stability.

[0042] (4) Preferably, the particle size range of the cathode material of the present invention is 2 to 5 μm when the particle size distribution reaches 50% cumulatively. In this case, since the exposed active area of ​​the material is appropriate, the conduction path of lithium ions in the solid state is not lengthened due to coarse particles, and the surface structure is not deteriorated quickly due to small particles.

[0043] (5) The manufacturing method of the present invention includes a normal mixing and calcination process, but the temperature (700-1100°C) used in step S4 is higher than that of the normal process. In this case, if normal highly active and small nano-oxide particles are used as the coating material added in step S3, these coating materials tend to penetrate into the bulk phase of the material at high temperatures, and the purpose of coating cannot be achieved. Therefore, it is preferable to use aluminum-containing particles with a particle size of 100 nm or more for coating, and utilize their low reaction activity to suppress the reaction rate and retain it on the material surface.

[0044] (6) The positive electrode plate and the lithium ion battery manufactured using the positive electrode material of the present invention have excellent DC internal resistance and excellent long-term charge / discharge cycle characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0045] The present invention will be described in detail below with reference to specific examples. The following examples are provided for those skilled in the art to have a deeper understanding of the present invention, but are not intended to limit the present invention in any manner. Those skilled in the art may make some changes and improvements without departing from the concept of the present invention, which are within the scope of protection of the present invention.

[0046] Example 1 Ni 0.66 Co 0.06 Mn 0.28The (OH)2 precursor and lithium carbonate (molar ratio of precursor:lithium 1:1.05) were mixed, 0.12 wt% (vs. precursor) nano-sized ZrO2 powder was added, and the mixture was mixed uniformly in a high-speed mixer to obtain mixture I. The mixture was placed in a sagger, heated to 940°C at a heating rate of 5°C / min in a roller hearth kiln, and held for 8 hours. The block was cooled, passed through a jaw crusher, and placed in a jet mill for crushing to obtain the product of the primary firing (intermediate product II). The primary firing product was mixed uniformly in a high-speed mixer with 2.0% molar ratio Co(OH)2 and 0.25 wt% mass ratio Al2O3 powder (particle size of primary particles approximately 150 nm), (mixture III), placed in a sagger, heated to 850°C at a heating rate of 10°C / min in a roller hearth kiln, and held for 5 hours to perform secondary firing. The cooled powder is the cathode material product. The cathode material product has a single crystal form and the particle diameter D when the particle size distribution reaches 50% cumulatively. v50 is 2.3 μm.

[0047] The composition of the material was measured by ICP and found to be Li 0.99 (Ni 0.65 Co 0.08 Mn 0.27 ) 0.998 Zr 0.001 Al 0.001 O2, i.e. C Co = 7.98%. As a result of measurement by XPS, the ratio of metal elements other than Li on the surface was 20.2% Al, 14.1% Co, 29.1% Mn, 33.7% Ni, and 2.9% Zr, that is, C Al = 20.2%. The material is Ar + The etching was performed using ions under the conditions of a spot diameter of 1.5 mm, energy of 3000 eV, and duration of 100 s. The etching process was performed on the material and the results of measurement by XPS showed that the ratio of metal elements other than Li on the surface was 10.2% Al, 17.5% Co, 30.7% Mn, 40.1% Ni, and 1.5% Zr, i.e., C. Co1 =17.5%, C Al1 =10.2%.

[0048] Example 2 Ni 0.66 Co 0.06Mn 0.28 The (OH)2 precursor and lithium carbonate (molar ratio of precursor:lithium 1:1.05) were mixed, 0.12 wt% (vs. precursor) nano-sized ZrO2 powder was added, and the mixture was mixed uniformly in a high-speed mixer to obtain mixture I. The mixture was placed in a sagger, heated to 940°C at a heating rate of 5°C / min in a roller hearth kiln, and held for 8 hours. The block was cooled, passed through a jaw crusher, and placed in a jet mill for crushing to obtain a primary sintered product (intermediate product II). The primary sintered product was mixed uniformly in a high-speed mixer with 1.0% molar ratio Co(OH)2 and 0.20 wt% mass ratio Al2O3 powder (particle size of primary particles approximately 110 nm), (mixture III), placed in a sagger, heated to 820°C at a heating rate of 10°C / min in a roller hearth kiln, and held for 5 hours to perform secondary sintering. The cooled powder is the cathode material product. The cathode material product has a single crystal form and the particle diameter D when the particle size distribution reaches 50% cumulatively. v50 is 2.5 μm.

[0049] The composition of the material was measured by ICP and found to be Li 1.01 (Ni 0.65 Co 0.07 Mn 0.28 ) 0.9975 Zr 0.001 Al 0.0015 O2, i.e. C Co = 6.98%. As a result of measurement by XPS, the ratio of metal elements other than Li on the surface was 25.7% Al, 7.8% Co, 31.0% Mn, 33.1% Ni, and 2.4% Zr, that is, C Al =25.7%. The material is Ar + The etching was performed with ions under the conditions of a spot diameter of 1.5 mm, energy of 2700 eV, and duration of 95 seconds. The etching process was performed on the material, and the results of the measurement by XPS showed that the ratio of metal elements other than Li on the surface was 9.4% Al, 9.7% Co, 38.7% Mn, 41.0% Ni, and 1.2% Zr, i.e., C Co1 =9.7%, C Al1 =9.4%.

[0050] Example 3 Ni 0.64 Co0.06 Mn 0.30 The (OH)2 precursor and lithium carbonate (precursor:lithium molar ratio 1:1.05) were mixed, 0.12 wt% (vs. precursor) nano-sized ZrO2 powder was added, and the mixture was mixed uniformly in a high-speed mixer to obtain mixture I. The mixture was placed in a sagger, heated to 940°C at a heating rate of 5°C / min in a roller hearth kiln, and held for 8 hours. The block was cooled, passed through a jaw crusher, and placed in a jet mill for crushing to obtain a primary sintered product (intermediate product II). The primary sintered product was mixed uniformly in a high-speed mixer with 2.5% molar ratio Co(OH)2 and 0.15 wt% mass ratio Al2O3 powder (particle size of primary particles approximately 200 nm), and the mixture was placed in a sagger, heated to 840°C at a heating rate of 10°C / min in a roller hearth kiln, and held for 5 hours to perform secondary sintering. The cooled powder is the cathode material product. The cathode material product has a single crystal form and the particle diameter D when the particle size distribution reaches 50% cumulatively. v50 is 2.7 μm.

[0051] The composition of the material was measured by ICP and found to be Li 1.03 (Ni 0.63 Co 0.08 Mn 0.29 ) 0.9978 Zr 0.001 Al 0.0012 O2, i.e. C Co = 7.98%. As a result of measurement by XPS, the ratio of metal elements other than Li on the surface was 19.7% Al, 13.0% Co, 29.1% Mn, 33.7% Ni, and 4.5% Zr, that is, C Al = 19.7%. The material is Ar + The etching was performed using ions under the conditions of a spot diameter of 1.5 mm, energy of 3300 eV, and duration of 90 seconds. The etching process was performed on the material, and the results of the measurement using XPS showed that the ratio of metal elements other than Li on the surface was 12.2% Al, 18.5% Co, 29.7% Mn, 38.6% Ni, and 1.0% Zr, i.e., C. Co1 =18.5%, C Al1 =12.2%.

[0052] Example 4 Ni0.61 Co 0.07 Mn 0.32 The (OH)2 precursor and lithium carbonate (molar ratio of precursor:lithium 1:1.05) were mixed, 0.12 wt% (vs. precursor) nano-sized ZrO2 powder was added, and the mixture was mixed uniformly in a high-speed mixer to obtain mixture I. The mixture was placed in a sagger, heated to 930°C at a heating rate of 5°C / min in a roller hearth kiln, and held for 8 hours. The block was cooled, passed through a jaw crusher, and placed in a jet mill for crushing to obtain a primary sintered product (intermediate product II). The primary sintered product was mixed uniformly in a high-speed mixer with 1.5% molar ratio Co(OH)2 and 0.20 wt% mass ratio Al2O3 powder (particle size of primary particles approximately 300 nm), placed in a sagger, heated to 840°C at a heating rate of 10°C / min in a roller hearth kiln, and held for 5 hours to perform secondary sintering. The cooled powder is the cathode material product. The cathode material product has a single crystal form and the particle diameter D when the particle size distribution reaches 50% cumulatively. v50 is 2.5 μm.

[0053] The composition of the material was measured by ICP and found to be Li 1.03 (Ni 0.60 Co 0.09 Mn 0.31 ) 0.9979 Zr 0.001 Al 0.0011 O2, i.e. C Co The results of XPS measurements showed that the ratio of metal elements other than Li on the surface was 27.3% Al, 10.5% Co, 27.8% Mn, 31.9% Ni, and 2.5% Zr. Al =27.3%. The material is Ar + The etching was performed with ions under the conditions of a spot diameter of 1.5 mm, energy of 3400 eV, and duration of 90 seconds. The etching process was performed on the material, and the results of the measurement by XPS showed that the ratio of metal elements other than Li on the surface was 8.0% Al, 14.4% Co, 35.7% Mn, 39.9% Ni, and 2.0% Zr, i.e., C Co1 =14.4%, C Al1 =8.0%.

[0054] Example 5 Ni0.61 Co 0.07 Mn 0.32 The (OH)2 precursor and lithium carbonate (precursor:lithium molar ratio 1:1.05) were mixed, 0.12 wt% (vs. precursor) nano-sized ZrO2 powder was added, and the mixture was mixed uniformly in a high-speed mixer to obtain mixture I. The mixture was placed in a sagger, heated to 930°C at a heating rate of 5°C / min in a roller hearth kiln, and held for 8 hours. The block was cooled, passed through a jaw crusher, and placed in a jet mill for crushing to obtain a primary sintered product (intermediate product II). The primary sintered product was mixed uniformly with 2.0% molar ratio Co(OH)2 and 0.16 wt% mass ratio Al2O3 powder (particle size of primary particles approximately 150 nm) in a high-speed mixer, placed in a sagger, heated to 850°C at a heating rate of 10°C / min in a roller hearth kiln, and held for 5 hours to perform secondary sintering. The cooled powder is the cathode material product. The cathode material product has a single crystal form and the particle diameter D when the particle size distribution reaches 50% cumulatively. v50 is 3.1 μm.

[0055] The composition of the material was measured by ICP and found to be Li 1.03 (Ni 0.60 Co 0.09 Mn 0.31 ) 0.998 Zr 0.001 Al 0.001 O2, i.e. C Co = 8.98%. As a result of measurement by XPS, the ratio of metal elements other than Li on the surface was 22.1% Al, 12.5% ​​Co, 29.0% Mn, 34.7% Ni, and 1.7% Zr, that is, C Al =22.1%. The material is Ar + The etching was performed using ions under the conditions of a spot diameter of 1.5 mm, energy of 2600 eV, and duration of 100 s. The etching process was performed on the material and the results of measurement by XPS showed that the ratio of metal elements other than Li on the surface was 10.8% Al, 16.6% Co, 31.7% Mn, 38.6% Ni, and 2.3% Zr, i.e., C. Co1 =16.6%, C Al1 =10.8%.

[0056] Example 6 Ni 0.61 Co 0.07 Mn 0.32 The (OH)2 precursor and lithium carbonate (precursor:lithium molar ratio 1:1.05) were mixed, 0.12 wt% (vs. precursor) nano-sized ZrO2 powder was added, and the mixture was mixed uniformly in a high-speed mixer to obtain mixture I. The mixture was placed in a sagger, heated to 930°C at a heating rate of 5°C / min in a roller hearth kiln, and held for 8 hours. The block was cooled, passed through a jaw crusher, and placed in a jet mill for crushing to obtain a primary sintered product (intermediate product II). The primary sintered product was mixed uniformly with 2.5% molar ratio Co(OH)2 and 0.12 wt% mass ratio Al2O3 powder (particle size of primary particles approximately 150 nm) in a high-speed mixer, placed in a sagger, heated to 860°C at a heating rate of 10°C / min in a roller hearth kiln, and held for 5 hours to perform secondary sintering. The cooled powder is the cathode material product. The cathode material product has a single crystal form and the particle diameter D when the particle size distribution reaches 50% cumulatively. v50 is 3.6 μm.

[0057] The composition of the material was measured by ICP and found to be Li 1.03 (Ni 0.60 Co 0.09 Mn 0.31 ) 0.998 Zr 0.001 Al 0.001 O2, i.e. C Co = 8.98%. As a result of measurement by XPS, the ratio of metal elements other than Li on the surface was 18.8% Al, 14.2% Co, 28.6% Mn, 35.9% Ni, and 2.5% Zr, that is, C Al =18.8%. The material is Ar + The etching was performed using ions under the conditions of a spot diameter of 1.5 mm, energy of 3000 eV, and duration of 100 s. The etching process was performed on the material and the results of measurement by XPS showed that the ratio of metal elements other than Li on the surface was 13.5% Al, 17.4% Co, 30.3% Mn, 36.7% Ni, and 2.1% Zr, i.e., C. Co1 =17.4%, C Al1 =13.5%.

[0058] Example 7 The difference between this example and Example 1 is that no ZrO2 powder is added after mixing the precursor with lithium carbonate. The cathode material product has a single crystal morphology and a particle diameter D when the particle size distribution reaches 50% cumulatively. v50 is 3.6 μm.

[0059] The composition of the material was measured by ICP and found to be Li 0.99 (Ni 0.65 Co 0.08 Mn 0.27 ) 0.999 Al 0.001 O2, i.e. C Co = 7.99%. As a result of measurement by XPS, the ratio of metal elements other than Li on the surface was 20.7% Al, 14.9% Co, 30.1% Mn, and 34.3% Ni, i.e., C Al = 20.7%. The material is Ar + The etching was performed using ions under the conditions of a spot diameter of 1.5 mm, energy of 3000 eV, and duration of 100 s. The etching process was performed on the material, and the results of the measurement using XPS showed that the ratio of metal elements other than Li on the surface was 10.5% Al, 18.0% Co, 31.2% Mn, and 40.3% Ni, i.e., C. Co1 =18.0%, C Al1 =10.5%.

[0060] Example 8 Ni 0.77 Co 0.04 Al 0.19The (OH)2 precursor and lithium carbonate (molar ratio of precursor:lithium 1:1.05) were mixed, 0.12 wt% (vs. precursor) nano-sized ZrO2 powder was added, and the mixture was mixed uniformly in a high-speed mixer to obtain mixture I. The mixture was placed in a sagger, heated to 930°C at a heating rate of 5°C / min in a roller hearth kiln, and held for 8 hours. The block was cooled, passed through a jaw crusher, and placed in a jet mill for crushing to obtain a primary sintered product (intermediate product II). The primary sintered product was mixed uniformly with 2.5% molar ratio Co(OH)2 and 0.12 wt% mass ratio Al2O3 powder (particle size of primary particles approximately 150 nm) in a high-speed mixer, placed in a sagger, heated to 840°C at a heating rate of 10°C / min in a roller hearth kiln, and held for 5 hours to perform secondary sintering. The cooled powder is the cathode material product. The cathode material product has a single crystal form and the particle diameter D when the particle size distribution reaches 50% cumulatively. v50 is 2.6 μm.

[0061] The composition of the material was measured by ICP and found to be Li 1.02 (Ni 0.76 Co 0.06 Al 0.18 ) 0.999 Zr 0.001 O2, i.e. C Co = 5.99%. As a result of measurement by XPS, the ratio of metal elements other than Li on the surface was 26.8% Al, 11.2% Co, 59.1% Ni, and 2.9% Zr, that is, C Al =26.8%. The material is Ar + The etching was performed with ions under the conditions of a spot diameter of 1.5 mm, energy of 3000 eV, and duration of 100 s. The etching process was performed on the material and the results of measurement by XPS showed that the ratio of metal elements other than Li on the surface was 16.5% Al, 9.2% Co, 71.6% Ni, and 2.7% Zr, i.e., C Co1 =9.2%, C Al1 =16.5%.

[0062] Comparative Example 1 The difference between this comparative example and Example 1 is that no Al2O3 powder is added during secondary sintering. The other conditions and methods for manufacturing the material are the same as those in Example 1. The cathode material product has a single crystal form, and the particle diameter D v50 is 2.3 μm.

[0063] The composition of the material was measured by ICP and found to be Li 1.01 (Ni 0.65 Co 0.07 Mn 0.28 ) 0.999 Zr 0.001 O2, i.e. C Co = 6.99%. As a result of measurement by XPS, the ratio of metal elements other than Li on the surface was 0% Al (ND), 10.9% Co, 40.4% Mn, 44.1% Ni, and 4.6% Zr, that is, C Al =0%. The material is Ar + The etching was performed with ions under the conditions of a spot diameter of 1.5 mm, energy of 3000 eV, and duration of 100 s. The etching process was performed on the material and the results of measurement by XPS showed that the ratio of metal elements other than Li on the surface was 0% Al (ND), 9.5% Co, 42.7% Mn, 45.4% Ni, and 2.4% Zr, i.e., C. Co1 =9.5%, C Al1 =0%.

[0064] Comparative Example 2 The difference between this comparative example and Example 1 is that Co(OH)2 is not added during the secondary firing. The other conditions and methods for manufacturing the material are the same as those in Example 1. The cathode material product has a single crystal form, and the particle diameter D when the particle size distribution reaches 50% cumulatively is 1. v50 is 2.3 μm.

[0065] The composition of the material was measured by ICP and found to be Li 1.01 (Ni 0.66 Co 0.06 Mn 0.28 ) 0.9975 Zr 0.001 Al 0.0015 O2, i.e. C Co= 5.99%. As a result of measurement by XPS, the ratio of metal elements other than Li on the surface was 27.3% Al, 4.1% Co, 32.3% Mn, 34.9% Ni, and 1.4% Zr, that is, C Al =27.3%. The material is Ar + The etching was performed using ions under the conditions of a spot diameter of 1.5 mm, energy of 3000 eV, and duration of 100 s. The etching process was performed on the material and the results of measurement by XPS showed that the ratio of metal elements other than Li on the surface was 8.2% Al, 6.3% Co, 39.6% Mn, 43.0% Ni, and 2.9% Zr, i.e., C Co1 =6.3%, C Al1 =8.2%.

[0066] Comparative Example 3 The difference between this comparative example and Example 1 is that in this comparative example, neither Al2O3 powder nor Co(OH)2 is added during secondary sintering. The other conditions and methods for manufacturing the material are the same as those in Example 1. The cathode material product has a single crystal form, and the particle diameter D when the particle size distribution reaches 50% cumulatively is 1. v50 is 2.3 μm.

[0067] The composition of the material was measured by ICP and found to be Li 1.01 (Ni 0.66 Co 0.06 Mn 0.28 ) 0.999 Zr 0.001 O2, i.e. C Co = 5.99%. As a result of measurement by XPS, the ratio of metal elements other than Li on the surface was 0% Al (ND), 6.7% Co, 39.8% Mn, 51.3% Ni, and 2.2% Zr, that is, C Al =0%. The material is Ar + The etching was performed with ions under the conditions of a spot diameter of 1.5 mm, energy of 3000 eV, and duration of 100 s. The etching process was performed on the material and the results of measurement by XPS showed that the ratio of metal elements other than Li on the surface was 0% Al (ND), 7.1% Co, 37.3% Mn, 52.9% Ni, and 2.7% Zr, i.e., C. Co1 =7.1%, C Al1 =0%.

[0068] Comparative Example 4 The difference between this comparative example and Example 1 is that the particle diameter of the Al2O3 primary particles added during secondary sintering in this comparative example is 10 nm. The other conditions and methods for manufacturing the material are the same as those in Example 1. The cathode material product has a single crystal form, and the particle diameter D v50 is 2.3 μm.

[0069] The composition of the material was measured by ICP and found to be Li 1.01 (Ni 0.65 Co 0.07 Mn 0.28 ) 0.9975 Zr 0.001 Al 0.0015 O2, i.e. C Co = 6.98%. As a result of measurement by XPS, the ratio of metal elements other than Li on the surface was 19.3% Al, 9.2% Co, 28.7% Mn, 40.3% Ni, and 2.5% Zr, that is, C Al = 19.3%. The material is Ar + The etching was performed using ions under the conditions of a spot diameter of 1.5 mm, energy of 3000 eV, and duration of 100 s. The etching process was performed on the material and the results of measurement by XPS showed that the ratio of metal elements other than Li on the surface was 18.2% Al, 10.1% Co, 30.3% Mn, 39.6% Ni, and 1.8% Zr, i.e., C. Co1 = 10.1%, C Al1 =18.2%.

[0070] Comparative Example 5 The difference between this comparative example and Example 1 is that the temperature during secondary sintering in this comparative example is 550°C. Other conditions and methods for manufacturing the material are the same as those in Example 1. The cathode material product has a single crystal form, and the particle diameter D v50 is 2.1 μm.

[0071] The composition of the material was measured by ICP and found to be Li 1.01 (Ni 0.65 Co 0.07 Mn 0.28 ) 0.9975 Zr0.001 Al 0.0015 O2, i.e. C Co = 6.98%. As a result of measurement by XPS, the ratio of metal elements other than Li on the surface was 23.1% Al, 15.6% Co, 24.4% Mn, 34.8% Ni, and 2.1% Zr, that is, C Al =23.1%. The material is Ar + The etching was performed with ions under the conditions of a spot diameter of 1.5 mm, energy of 3000 eV, and duration of 100 s. The etching process was performed on the material and the results of measurement by XPS showed that the ratio of metal elements other than Li on the surface was 15.5% Al, 8.3% Co, 33.2% Mn, 40.3% Ni, and 2.7% Zr, i.e., C Co1 =8.3%, C Al1 =15.5%.

[0072] The cathode materials of the above examples and comparative examples are used to manufacture batteries in the following manner. The positive electrode active material, carbon black as a conductive agent, and polyvinylidene fluoride (PVDF) as an adhesive were mixed in a mass ratio of 97:1.7:1.3, and then added to N-methyl-2-pyrrolidone (NMP), an organic solvent, and stirred at high speed to obtain a uniform dispersion. After high-speed stirring, the mixture was degassed using negative pressure in a stirring tank to obtain a positive electrode paste suitable for application. The obtained positive electrode paste was applied to aluminum foil using a transfer type coater, and then dried, cold pressed, and cut to obtain a positive electrode plate of the required shape. The cold pressing process resulted in a compressed density of 3.2 g / cm in the area coated with the positive electrode active material. 3 ~3.6g / cm 3 Manage it so that it stays within the range.

[0073] The negative electrode active material, conductive carbon black, adhesive, and sodium carboxymethylcellulose (CMC-Na) were mixed in a mass ratio of 96.8:1.2:1.2:0.8, added to deionized water, and stirred at high speed to form a uniform dispersion. After high-speed stirring, the mixture was degassed using negative pressure in a stirring tank to obtain a negative electrode paste suitable for application. The obtained negative electrode paste was applied to copper foil using a transfer coater, and then dried, cold pressed, and cut to obtain a negative electrode plate of the required shape. The cold pressing process reduced the compression density of the negative electrode active material application area to 1.5 g / cm. 3 ~1.8g / cm 3 Manage it so that it stays within the range.

[0074] The positive and negative plates were placed on either side of a 9 μm thick PE separator, wound to form a core, and connected by ultrasonic welding, leaving uncoated areas and nickel lugs. The core was covered with an aluminum plastic film and heat sealed, leaving one side open for liquid filling.

[0075] The lithium salt LiPF6 (13 wt% calculated based on the total mass of the electrolyte) and additives vinylene carbonate (1 wt% calculated based on the total mass of the electrolyte) and ethylene sulfate (DTD) (2 wt% calculated based on the total mass of the electrolyte) were added to a mixed solvent of EC, EMC, and DEC (mass ratio 3:5:2) to prepare an electrolyte, which was then filled into an aluminum plastic film covering the core. The resulting product was then vacuum-packed, left to stand, and chemically converted to obtain a lithium-ion battery.

[0076] The performance of the positive electrode material and the resulting battery were measured and the results are shown in Table 1. The measurement methods are as follows.

[0077] Particle size D v50Measurement: 5 g of ternary cathode material sample was weighed and placed in a 100 mL beaker, 50 mL of deionized water and 1 mL of sodium hexametaphosphate solution (concentration 1 wt%) were added, and ultrasonic waves were applied for 1 min before placing in the Mastersizer 3000 sample injection system. The total amount of sample and deionized water was made 500 mL, and the particle size distribution was measured under the conditions of mixer rotation speed 2800 rpm, particle refractive index 1.8, particle absorption rate 1.0, and solvent refractive index 1.33. The D of the particle size distribution data was v It read 50.

[0078] ICP measurement: 0.4 g of the positive electrode material sample was weighed and placed in a 250 ml beaker, 10 ml of HCl solution (HCl to water volume ratio 1:1) was added, and the mixture was heated to 180°C to dissolve it. The heated liquid was transferred to a volumetric flask, made to a constant volume with pure water, diluted to a measurable range, and measured with an ICP device. The chemical formula of the positive electrode material is Li a (Ni x Co y M 1-x-y ) 1-b M' b O 2-c A c In the above, the x and y values ​​of Ni, Co, and Mn elements were calculated by comparing with the relative contents from the ICP measurement results, and a, b, and c were obtained by ICP measurement. When there are multiple M's and A's, b and c are the total contents of each element.

[0079] XPS measurement: The powder sample of the cathode material was spread on an aluminum foil with double-sided tape, and the sample was compressed and molded by a tablet press, and then the material was measured by an XPS instrument. The measurement process consisted of first performing a full spectrum scan to identify the possible element types present, and then performing a narrow spectrum scan for the elements present. The atomic relative content of the elements was calculated from the area of ​​the signal peak with reference to the elemental sensitivity factor.

[0080] Etching: Ar+ ion etching was used, with a spot diameter of 1.5 mm, 2500 eV≦E≦3500 eV, and 90 s≦t≦100 s. Here, E is the energy used for etching, and t is the etching time. After the material was processed, it was measured by an XPS device. For detailed etching parameters, please refer to the specific examples and comparative examples. Under the above conditions (Ar + The relative atomic content of an arbitrary element obtained by measuring a cathode material etched by ion etching (spot diameter 1.5 mm, 2500 eV≦E≦3500 eV, 90 s≦t≦100 s) using XPS is the relative atomic content of the element at a depth of 20 to 60 nm from the surface.

[0081] Direct current resistance (DCR) measurement: Using a charge / discharge device, adjust the battery's state of charge (SOC state) to 10% (i.e., charge the battery from a fully discharged state to 10% of the rated capacity) at a rate of 0.33C (i.e., the current magnitude is 0.33 times the battery's rated capacity Ah), leave it for 30 minutes, and then discharge the battery at a constant current of 3C A. When the voltage change ΔV during the discharge process is recorded, DCR = ΔV / A.

[0082] Cycle life: The battery is cycled at 1C using a charge / discharge device, and the capacity retention rate after 1,000 cycles is recorded.

[0083] DCR increase rate measurement: For a 1000-cycle battery, adjust the battery's SOC state to 50% (i.e., charge the battery from a fully discharged state to 50% of the rated capacity) at a rate of 0.33C (i.e., the current is 0.33 times the battery's rated capacity Ah) using a charge / discharge device, leave it for 30 minutes, then discharge the battery at a constant current of 3C A, and record the voltage change ΔV during the discharge process. DCR1000=ΔV / A. DCR increase rate=(DCR1000 / DCR)-1.

[0084] [Table 1]

[0085] Since the technical characteristics of the materials according to Examples 1 to 8 are within the preferred range of the present application, the batteries manufactured with the materials have low initial direct current resistance (DCR), excellent cycle capacity retention and cycle DCR increase rate. Co1 -C Co is the difference between the Co atomic ratio near the material surface and the average Co atomic content in the material. If the difference is ≥ 2%, the Co is relatively abundant near the material surface, and the electronic conductivity and ionic transition of the material are improved. Al -C Al1 is the difference between the Al atomic ratio on the material surface and the Al atomic ratio near the surface, and when the difference is ≧5%, the material surface is coated with Al and Al atoms do not penetrate into the material. Comparing the data of Example 1 and Comparative Example 1, when there is no Al coating on the material surface, C Al -C Al1 <5%, which is outside the preferred range, and the cycle capacity retention rate of the material is obviously decreased. Co1 -C Co <2%, which is outside the preferred range, and the capacity retention rate of the material is maintained at a high level, but the DC impedance is high. Comparing the data of Example 1 and Comparative Example 3, when the material surface does not have the two coatings, C Al -C Al1 and C Co1 -C Co is outside the preferred range, and the DC impedance, cycle capacity retention rate, and cycle DC resistance (DCR) increase rate of the material are poor. Comparing the data of Example 1 and Comparative Example 4, when the coating process is performed with a small particle coating agent, the Al element penetrates near the surface and into the inside of the material, and the C Al -C Al1 <5%, which not only fails to protect the material during long-term cycle processes, but also inhibits the transition of electrons and ions, improving the DC resistance of the material. Comparing the data of Example 1 and Comparative Example 5, when the secondary firing temperature is not high and the Co element does not penetrate near the material surface, the C Co1 -C Co<2%, where the material has excellent DC impedance and cycling capacity retention, but cannot maintain the DC impedance of the battery at a low level during long-term cycling processes.

[0086] The above describes specific examples of the present invention. The present invention is not limited to the above embodiments, and those skilled in the art may make various changes or modifications within the scope of the claims without affecting the substantial content of the present invention. The examples and features of the examples may be arbitrarily combined with each other without causing any inconsistency.

Claims

1. The chemical composition is Li a (Ni x Co y M 1-x-y ) 1-b M' b O 2-c A c wherein 0.75≦a≦1.2, 0.5≦x<1, 0<y≦0.1, 0<b≦0.01, 0≦c≦0.2, M is at least one selected from Mn and Al, M′ includes Al and optionally one or more selected from Zr, Ti, Y, Sr, W, and Mg, and A is one or more selected from S, F, and N; However, 2%≦C Co1 -C Co And C Co1 is the atomic ratio of Co to all metal elements excluding Li, obtained by measuring the surface structure of the cathode material etched to a depth of 20 to 60 nm from the surface by XPS, and C Co is the atomic ratio of Co to all metal elements excluding Li, obtained by measuring the positive electrode material by ICP, 5%≦C Al -C Al1 And C Al is the atomic ratio of Al element in all metal elements excluding Li element obtained by measuring the positive electrode material directly by XPS, and C Al1 is an atomic ratio of Al element to all metal elements excluding Li element, obtained by measuring a cathode material having a surface structure etched by 20 to 60 nm from the surface by XPS.

2. 5.3%≦C Al -C Al1 and preferably, 10%≦C Al -C Al1 and / or 2.7%≦C Co1 -C Co and preferably, 5%≦C Co1 -C Co The ternary cathode material of claim 1 ,

3. The etching conditions were Ar + 2. The ternary cathode material of claim 1, characterized in that: ion etching, spot diameter 1.5 mm, 2500 eV≦E≦3500 eV, 90 s≦t≦100 s, where E is the energy utilized for etching and t is the etching time.

4. Chemical composition Li a (Ni x Co y M 1-x-y ) 1-b M' b O 2-c A c 2. The ternary cathode material according to claim 1, wherein M' comprises one or more selected from Al and Zr, Ti, Y, Sr, W, and Mg, and preferably M' comprises Al and Zr.

5. Chemical composition Li a (Ni x Co y M 1-x-y ) 1-b M' b O 2-c A c 2. The ternary cathode material of claim 1, wherein c=0.

6. Particle diameter D when the particle size distribution reaches 50% cumulatively v50 2μm≦D v50 The ternary cathode material according to claim 1, characterized in that it satisfies ≦5 μm.

7. Step S1: thoroughly mixing a ternary positive electrode precursor containing Ni, Co, Mn or Ni, Co, Al with a lithium source to form a mixture I; Step S2 of heating the mixture I in an air or oxygen atmosphere, holding it at 700-1100° C. for 4-15 hours, and rolling and grinding the mixture to obtain an intermediate product II; Step S3 of thoroughly mixing the intermediate product II, the aluminum-containing solid powder, and the Co-containing solid powder to form a mixture III; Mixture III is heated in an air or oxygen atmosphere, held at 700-1000°C for 4-15 hours, and then rolled and crushed to obtain α-NaFeO 2 and a step S4 of obtaining a ternary cathode material having the structure, However, when the element M' in the ternary positive electrode material contains one or more elements selected from Zr, Ti, Y, Sr, W, and Mg, a compound containing one or more elements selected from Zr, Ti, Y, Sr, W, and Mg is added in the process of forming the mixture I and / or the process of forming the mixture III; 7. The method for producing a ternary cathode material according to claim 1, wherein when the ternary cathode material contains element A, a compound containing element A is added in the process of forming mixture I and / or the process of forming mixture III.

8. 8. The method for producing a ternary cathode material according to claim 7, wherein in step S1, the lithium source is one or more selected from the group consisting of lithium carbonate and lithium hydroxide.

9. 8. The method for preparing the ternary cathode material according to claim 7, characterized in that in step S1, the element M' in the ternary cathode material comprises Zr element, and a Zr-containing compound is added in the process of forming mixture I.

10. In step S3, the aluminum-containing solid powder is an aluminum oxide powder, and the particle diameter of the aluminum-containing solid powder is 100 nm≦D 酸化アルミニウム 8. The method of claim 7, wherein the thickness of the ternary cathode material is less than or equal to 1000 nm.

11. In step S3, the Co-containing solid powder is 3 O 4 , CoO, Co(OH) 2 , CoOOH, CoCO 3 The method for producing a ternary positive electrode material according to claim 7, characterized in that the ternary positive electrode material is any one or more selected from the following:

12. 8. The method for producing a ternary cathode material according to claim 7, wherein in step S3, the molar ratio of Co element in the Co-containing solid powder to the intermediate product II is (1-3):100, and / or the mass ratio of Al element in the aluminum-containing solid powder to the intermediate product II is (0.02-1.5):

100.

13. A positive electrode plate, characterized in that it comprises the ternary positive electrode material according to any one of claims 1 to 6.

14. A lithium ion battery comprising the positive plate of claim 13.

Citation Information

Patent Citations

  • Low-gas-production high-capacity ternary positive electrode material

    CN112151775A

  • Positive electrode material, preparation method thereof, positive electrode comprising positive electrode material and lithium ion battery

    CN113851607A

  • Cathode Powders of Lithium Nickel Manganese Cobalt Oxide for High Voltage Lithium Ion Batteries

    JP2018510450A

  • Method for manufacturing a positive electrode active material for a lithium secondary battery, a positive electrode active material for a lithium secondary battery, a positive electrode for a lithium secondary battery including the same, and a lithium secondary battery

    JP2021516434A

  • Positive electrode active material, method for producing the same, and lithium secondary battery including a positive electrode containing the same

    JP2023523667A