Method for producing low-arsenic gold concentrate

LAP923AUndetermined Publication Date: 2026-03-27NITTETABU MINING CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
LAP923
Authority / Receiving Office
LA · LA
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-02-25
Filing Date
2022-02-25
Publication Date
2026-03-27

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

In the production of a gold concentrate by flotation in which the gold ore is separated from the arsenic ore by using a mercuric oxoacid and an oxidizing agent, the arsenic in the gold concentrate is reduced in a simple way. In the production of a gold concentrate by flotation in which the arsenic-containing gold ore is a raw material, a mercuric oxoacid and a hydroperoxide as an oxidizing agent are used together as additional reducing agents, and are added in this order.
Need to check novelty before this filing date? Find Prior Art

Description

Manufacturing method for low-arsenic copper concentrate

[0001] The present invention relates to a method for producing copper concentrate by flotation using arsenic-containing copper ore as a raw material, characterized in that a sulfur oxoacid and hydrogen peroxide are used in combination as additives.

[0002] There are two main methods for smelting copper. The first is a dry process in which copper concentrate is produced by concentrating copper sulfide from ore containing naturally occurring copper sulfide, mainly through flotation, and this copper concentrate is then thermally decomposed in a flash smelting furnace or bath furnace to obtain metallic copper. The second is a wet process in which copper is leached from ore containing naturally occurring copper oxide, copper carbonate, copper sulfate, etc., mainly using sulfuric acid, and metallic copper is then electrochemically deposited from this leachate. The former method is particularly important, accounting for more than half of global copper production.

[0003] Copper concentrate, the raw material for dry copper smelting, is a concentrated form of sulfides, primarily chalcopyrite, including bornite, chalcocite, and covellite. Flotation is a widely used concentration method. Flotation involves introducing air into a slurry of crushed ore, allowing the target mineral to adhere to the air bubbles and rise to the surface, allowing it to be recovered. Generally, copper sulfide minerals have hydrophobic surfaces, making them more stable when attached to air bubbles in a slurry than when dispersed in the liquid. This method is widely used in metal mines around the world to recover metal sulfide minerals, not just copper minerals.

[0004] While copper concentrate naturally requires minimal impurities, a certain level of impurity is often tolerated because impurities are removed during the subsequent dry smelting process. Chalcopyrite, the primary mineral in copper concentrate, has the chemical formula CuFeS2 and contains iron and sulfur in addition to copper. As for these non-copper components, iron is separated as slag during the smelting process, while sulfur becomes a heat source through oxidation and is discharged as sulfur oxide, which is then recovered as sulfuric acid. Additionally, silicate components such as quartz and feldspar, which are contained as impurities in copper concentrate, are separated as slag, and some metal components such as zinc and lead volatilize in the smelting furnace and are separated from the copper.

[0005] However, the impurity content of copper concentrate has been increasing year by year, raising concerns that it may cause problems in the copper smelting process (Non-Patent Document 1). In particular, among the impurities, arsenic, if present in a certain amount or less, is distributed in the slag during the copper smelting process, where it is immobilized and insoluble, i.e., rendered non-toxic. However, if copper concentrate containing arsenic exceeding this allowable amount is subjected to copper refining, the immobilization of arsenic in the slag becomes insufficient, and it has been pointed out that there is a risk of the arsenic leaching into the environment or being released as dust.

[0006] In this situation, research and development into the separation of arsenic minerals has been actively conducted in recent years in the copper concentrate manufacturing process, i.e., the process of concentrating copper sulfide from copper ore by flotation to produce copper concentrate.

[0007] For example, Patent Document 1 discloses a method for separating arsenic minerals from copper-bearing materials by adding a flotation agent containing an inhibitor, a foaming agent, and a collector to a slurry of copper-bearing materials containing arsenic, and then blowing air into the slurry to float the copper concentrate, thereby separating arsenic minerals from copper-bearing materials, characterized in that sodium thiosulfate is used as the inhibitor.

[0008] Patent Document 2 discloses a method for separating arsenic minerals from copper-bearing materials by adding water to the copper-bearing material containing arsenic minerals to form a slurry, adjusting the pH of the slurry to 8 to 12, and then flotation the slurry to separate the arsenic minerals from the copper-bearing material. The method includes at least one of a soluble copper removal step in which the copper-bearing material is treated with a chelating agent such as triethylenetetramine or ethylenediaminetetraacetic acid that forms a chelate with copper ions, and an oxidation step in which the arsenic minerals are oxidized using an oxidizing agent such as air or oxygen.

[0009] Patent Document 3 discloses a method in which a copper-containing material containing arsenic is crushed, water is added to form a slurry, a flotation agent consisting of an inhibitor, a foaming agent, and a collector is added to the resulting slurry, and air is blown in to perform flotation, in which a chelating agent such as polyethyleneamines is used as an inhibitor.

[0010] Patent Document 4 discloses a method in which copper concentrate containing arsenic is heat-treated at 90 to 120°C, repulped, and then preferably 10 to 15 kg of yellow prussate is added per ton of the copper concentrate, followed by flotation to remove arsenic minerals by flotation and recover copper concentrate with a low arsenic content as a sink.

[0011] Patent Document 5 discloses an ore dressing method including a flotation step in which potassium amylxanthogenate is added to a mineral slurry containing a raw material, and flotation is carried out to separate the resulting mixture into a sink ore containing a higher grade of arsenic-free sulfide minerals than the raw material, and a float ore containing a higher grade of arsenic-containing sulfide minerals than the raw material.

[0012] Patent Document 6 discloses a method for selecting arsenic-containing minerals using peptides having specific amino acid sequences.

[0013] However, although these prior art methods are effective for specific ores, they are not sufficient for separating arsenic efficiently and easily from ores with a wide range of properties.Furthermore, they have problems such as the need to use expensive chemicals or to add large amounts of chemicals.

[0014] Japanese Patent No. 4450108, Japanese Patent Application Laid-Open No. 2012-241249, Japanese Patent Application Laid-Open No. 2011-156521, Japanese Patent Application Laid-Open No. 2006-239553, Japanese Patent Application Laid-Open No. 2020-104095, Japanese Patent Application Laid-Open No. 2020-65485

[0015] JOGMEC Metal Resources Report 19-06-vol49 "Technological development regarding impurities in copper raw materials"

[0016] In view of the above-mentioned problems of the prior art, an object of the present invention is to provide a technology for efficiently separating arsenic minerals from arsenic-containing copper ore and producing a low-arsenic copper concentrate that can be suitably used in copper smelting.

[0017] In order to solve the above problems, the present invention proposes the following methods. [1] A method for producing low-arsenic copper concentrate, characterized in that when producing copper concentrate by flotation using arsenic-bearing copper ore as a raw material, sulfur oxoacids and hydrogen peroxide are used in combination as additive chemicals. [2] A method for producing low-arsenic copper concentrate as set forth in [1], characterized in that the sulfur oxoacids are thiosulfates or sulfites. [3] A method for producing low-arsenic copper concentrate as set forth in [1] or [2], characterized in that the amount of sulfur oxoacids added is 0.1 to 3 kg per ton of arsenic-bearing copper ore. [4] A method for producing low-arsenic copper concentrate as set forth in any one of [1] to [3], characterized in that the amount of hydrogen peroxide added is 0.1 to 5 kg per ton of arsenic-bearing copper ore. [5] The method for producing low-arsenic copper concentrate according to any one of [1] to [4], characterized in that the order of adding the chemicals is sulfur oxoacids followed by hydrogen peroxide. [6] The method for producing low-arsenic copper concentrate according to any one of [1] to [5], characterized in that the arsenic minerals contained in the arsenic-bearing copper ore are enargite and tetrahedrite.

[0018] According to the present invention, in the process of producing copper concentrate by flotation, it is possible to effectively separate arsenic minerals from copper concentrate by a simple method of using sulfur oxoacids and hydrogen peroxide in combination as additive agents, and it is also possible to produce low-arsenic copper concentrate that is suitable for copper smelting even from arsenic-containing copper ore.

[0019] 1A and 1B are schematic flow diagrams of the production of low-arsenic copper concentrate by direct and integrated preferential flotation, respectively;

[0020] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The embodiments for carrying out the present invention will be described in detail below.

[0021] In the present invention, when copper concentrate is produced by flotation using arsenic-containing copper ore as the raw material, a low-arsenic copper concentrate is produced by using a sulfur oxoacid and hydrogen peroxide in combination as additives.

[0022] First, there are no particular restrictions on the arsenic-containing copper ore used as the raw material, and copper ores containing copper sulfide produced from porphyry copper deposits, sedimentary copper deposits, skarn deposits, massive sulfide deposits, iron oxide-bearing gold-copper deposits, etc., which are found all over the world, can be used. In addition, intermediate products of other mineral dressing processes and even copper concentrates can also be used.

[0023] The arsenic content in ore varies greatly depending on the type of ore deposit and occurrence. Generally, the copper content in copper ore is about 0.2 to 3 wt%, but the arsenic content can range from several tens of ppm to even exceeding 1%. When producing copper concentrate by flotation, if no arsenic separation measures are taken, copper and arsenic are usually concentrated in similar ratios. This is due to the fact that both copper sulfide minerals and arsenic minerals have hydrophobic surfaces, as mentioned above.

[0024] The method for producing low-arsenic copper concentrate of the present invention aims to produce copper concentrate with a reduced arsenic content by separating at least a portion of the arsenic minerals contained in the copper concentrate in a general flotation process in which no measures for arsenic reduction are taken.

[0025] For example, if one example of copper ore from a porphyry copper deposit has a copper content of 2.5 wt% and an arsenic content of 0.10 wt%, when this ore is processed by a typical flotation method, the copper concentrate will have a copper content of 25 wt% (a concentration rate of 10 times) and an arsenic content of 1.0 wt% (also a concentration rate of 10 times). In this case, the arsenic content can be reduced to less than 1.0 wt%.

[0026] The arsenic content in the low-arsenic copper concentrate produced by the present invention is sufficient as long as it is reduced to the arsenic content required for the copper concentrate to be used in copper smelting. The upper limit of the arsenic content required for the copper concentrate cannot be determined in general terms because it varies depending on the copper smelting method, the blend ratio with other copper concentrates, etc., but generally, it is desirable for it to be 0.2 wt% or less.

[0027] The copper minerals contained in arsenic-containing copper ore include chalcopyrite (CuFeS2), bornite (Cu5FeS4), chalcocite (Cu2S), covellite (CuS), etc., and the present invention can be carried out without any particular restrictions.

[0028] Arsenic minerals include enargite (Cu3AsS4) and tetrahedrite (Cu, Fe, Zn) 12 (Sb,As)4S 13 ), arsenopyrite (FeAsS), realgar (AsS), and oropite (AsS), etc., can be used in the present invention without any particular restrictions, but arsenopyrite and tetrahedrite are particularly suitable arsenic minerals because they can more effectively reduce arsenic in the production method of the present invention. As the names suggest, arsenopyrite and tetrahedrite are also copper minerals that contain copper, but in this specification, these copper-containing arsenic minerals will also be referred to simply as "arsenic minerals," and the above copper minerals that do not contain arsenic will be referred to as "copper minerals."

[0029] Arsenic-containing copper ore mined in a mine is subjected to a dry crushing process, a wet grinding process, and then a flotation process. In the method for producing low-arsenic copper concentrate of the present invention, a sulfur oxoacid and hydrogen peroxide are used in combination as additives in the wet grinding process and / or the flotation process to produce low-arsenic copper concentrate.

[0030] The sulfur oxoacids to be added can be appropriately selected from industrially available chemicals, but among them, thiosulfates or sulfites are preferred in terms of the ease of separating arsenic minerals. More specifically, sodium thiosulfate, potassium thiosulfate, and ammonium thiosulfate can be used as thiosulfates, and sodium sulfite, sodium hydrogensulfite, potassium sulfite, and ammonium sulfite, as well as hydrates thereof, can be used as sulfites.

[0031] When added, it may be in the form of a powder or an aqueous solution.

[0032] The amount of addition can be adjusted as appropriate depending on the type and content of copper minerals contained in the arsenic-containing copper ore, and the type and content of arsenic minerals. Specifically, a flotation test is conducted each time, and the amount of sulfur oxoacids added is selected so that the copper mineral recovery rate and arsenic mineral separation are desired, but more preferably, it is 0.1 to 3 kg per ton of arsenic-containing copper ore. If the amount is less than 0.1 kg, the copper mineral recovery rate tends to be low, and conversely, adding more than 3 kg does not have a significant effect on the flotation results compared to adding 3 kg or less, and may have the disadvantage of increasing chemical costs.

[0033] Hydrogen peroxide is preferably added as aqueous hydrogen peroxide.

[0034] The amount of hydrogen peroxide added, like the amount of sulfur oxoacid added, can be adjusted as appropriate depending on the type and content of copper minerals contained in the arsenic-containing copper ore, and the type and content of arsenic minerals. Specifically, a flotation test is conducted each time, and the amount of hydrogen peroxide added is selected so that the recovery rate of copper minerals and the separation rate of arsenic minerals are desired. More preferably, the amount is 0.1 to 5 kg per ton of arsenic-containing copper ore. If the amount is less than 0.1 kg, the arsenic minerals tend to be easily recovered as float together with the copper minerals, and a low-arsenic copper concentrate may not be obtained. Conversely, if more than 5 kg is added, the recovery rate of copper minerals tends to decrease, and economical copper concentrate production may not be achieved.

[0035] In the wet grinding process, a ball mill or a rod mill is used, and in order to obtain the target particle size, a classification operation using a wet cyclone, a screen, etc. is appropriately combined. Regarding the target particle size of grinding, it is preferable that the copper mineral and the arsenic mineral are in a liberated state from the viewpoint of separation efficiency in the subsequent flotation process.

[0036] In flotation, various chemicals are used, such as collectors to improve adhesion between the metallic ore to be recovered and air bubbles, foaming agents to improve foaming when air is introduced, activators to improve the function of the collectors, inhibitors to prevent unwanted minerals from adhering to the air bubbles, and pH adjusters to adjust the solution state so that the effects of each of the above chemicals are exerted. These are often added in the wet milling process, and the sulfur oxoacids and hydrogen peroxide that are the added chemicals in this invention can also be added in the wet milling process.

[0037] In the wet crushing process, the ore is crushed to a particle size suitable for the subsequent flotation step to prepare a slurry, which is then sent to the flotation step.

[0038] In the flotation process, various chemicals are added to the ore slurry and it is treated in a conditioning tank to stabilize the added chemicals. Then, in a flotation machine where air is introduced into the ore slurry, the ore is separated into float, which adheres to the air bubbles, and sink, which does not adhere to the air bubbles and remains in the slurry. Various types of flotation machines can be used in the present invention, such as a self-priming flotation machine, a forced air flotation machine, and a column flotation machine.

[0039] The sulfur oxoacids and hydrogen peroxide added in the present invention can be added at various locations in the wet grinding process, as well as in the conditioning tank or flotation machine in the flotation process, or in the pipes or cushion tank connecting the various devices. The location of addition does not need to be limited to one location, and they may be added at multiple locations in the wet grinding process and the flotation process.

[0040] Here, the order of addition of sulfur oxoacids and hydrogen peroxide in the present invention is not particularly limited, but it is more preferable to add sulfur oxoacids first, followed by hydrogen peroxide. For example, there is a method in which sulfur oxoacids are added in a liquid cyclone in the wet grinding process and hydrogen peroxide is added in a conditioning tank in the flotation process, or a method in which sulfur oxoacids are added in the conditioning tank and then hydrogen peroxide is added in a flotation machine. By using this addition order, it is possible to retain the arsenic mineral to be separated in the sink while maintaining a high recovery rate of the copper mineral as float.

[0041] In the flotation process, a flotation circuit is formed by combining multiple flotation machines to recover and concentrate the copper minerals to be recovered, and separate out the unwanted minerals. The flotation circuit that can be suitably applied to the present invention is described below.

[0042] First, there is direct preferential flotation. In this circuit, copper minerals are first recovered as float in a process called rough sorting, and then the recovered material is processed into a copper concentrate with a copper content of, for example, 25% in a concentration process called refinement.

[0043] When the present invention is applied to a direct preferential flotation circuit, sulfur oxoacids and hydrogen peroxide are added in the roughing stage. As a result, arsenic minerals can be separated into the sink and copper minerals into the float. Since the roughing stage usually cannot concentrate the copper to the level required for copper smelting, the rougher flotation is concentrated in the subsequent purification step.

[0044] In the refining stage, if arsenic is sufficiently separated in the rough sorting stage, it is not necessary to add sulfur oxoacids and hydrogen peroxide. However, if arsenic is not sufficiently separated in the rough sorting stage, sulfur oxoacids and hydrogen peroxide are further added to produce a low-arsenic copper concentrate having the specified copper and arsenic contents.

[0045] When applied to direct preferential flotation, the arsenic in copper ore remains intact in the coarsely filtered sinks, and therefore there is an advantage that no highly concentrated arsenic-containing material is produced in the flotation process, making this a suitable method for treating the coarsely filtered sinks.

[0046] Next, we will discuss comprehensive preferential flotation. In this circuit, neither sulfur oxoacids nor hydrogen peroxide are added in the roughing stage, and both copper and arsenic minerals are recovered as rougher flotation. In the next stage of flotation, sulfur oxoacids and hydrogen peroxide are added to this rougher flotation, and the copper minerals are recovered as float, while the arsenic minerals remain as sink.

[0047] In this method, the amount of ore processed is reduced in the rough sorting stage, and then chemicals are added in the next stage, flotation, which reduces the amount of chemicals used.

[0048] On the other hand, since the resulting ore has a relatively high arsenic content, care must be taken in its treatment. However, in the case of arsenic minerals containing copper, such as enargite and tetrahedrite, they can be subjected to smelting that can appropriately treat both copper and arsenic, so it is possible to produce two types of copper concentrate: one made from arsenic-free copper minerals, and the other made from arsenic minerals containing copper.

[0049] In addition, if the copper recovery rate in the rough sorting or refinement stage is low, a scavenging step can be added in the subsequent stage to recover any remaining copper ore, or if the copper content in the float does not increase in the refinement stage, a wet crushing step can be added again to promote separation of the impurities adhering to the copper ore. There is no problem with appropriately combining processes that are applied to ordinary flotation circuits.

[0050] Since the properties of arsenic-bearing copper ore vary greatly depending on the type of deposit and the occurrence, it goes without saying that it is desirable to appropriately select the flotation circuit and circuit configuration that are best suited to each ore.

[0051] The details of why the combined use of sulfur oxoacids and hydrogen peroxide in the present invention makes it possible to reduce the arsenic content so effectively are not clear, but it is presumed that the oxidizing action of hydrogen peroxide oxidizes both copper minerals and arsenic minerals, weakening their surface hydrophobicity and making it impossible to recover either mineral by flotation; however, the effect of sulfur oxoacids maintains the surface hydrophobicity of only the copper minerals, and as a result, copper minerals are selectively recovered by flotation while reducing the recovery of arsenic minerals.

[0052] Patent Document 1 describes that sodium thiosulfate, a sulfur oxoacid, acts as an inhibitor for arsenic minerals, and Patent Document 2 proposes a technology for oxidizing arsenic minerals by oxidation treatment using an oxidizing agent such as air or oxygen, and separating them from copper minerals by flotation. Both documents aim to inhibit the arsenic minerals, but in the present invention, hydrogen peroxide, which has an oxidizing effect, effectively changes the arsenic minerals to a state that makes them difficult to recover by flotation, and it is presumed that sulfur oxoacids such as thiosulfate play a role in maintaining the surface hydrophobicity of copper minerals rather than acting as inhibitors as in the past, which can be said to be a newly discovered mechanism in the present invention.

[0053] The low-arsenic copper concentrate produced in this manner has a lower arsenic content than copper concentrate produced by flotation without any measures for arsenic separation, and is therefore suitable for use in copper smelting.

[0054] The present invention will be described in more detail with reference to the following examples and comparative examples, but it goes without saying that the present invention is not limited to these examples and is defined by the claims.

[0055] Examples 1 to 3, Comparative Examples 1 and 2 Using arsenic-containing copper ore A from Chile having the composition shown in Table 1 as a raw material, flotation tests were carried out.

[0056]

[0057] First, arsenic-containing copper ore A was crushed to -1.7 mm using a jaw crusher, and 500 g of the ore was taken and ground using a wet rod mill and a ball mill to prepare an arsenic-containing copper ore slurry with a particle size of 180 μm (80% passing diameter). Water was added to this slurry to adjust the solids concentration to 37 wt %, and then, in the conditioning step prior to flotation, various chemicals shown in Table 2 were added. Furthermore, 10 g / t of AP3477 (a dithiophosphate-based product, manufactured by Solvay) was added as a collector, and 20 g / t of MIBC (manufactured by Junsei Chemical Co., Ltd.) was added as a foaming agent. Then, flotation was carried out using an Agitair-type tester. The float was collected for 16 minutes after the start of flotation, and the float and tailings were each chemically analyzed. The copper and arsenic recovery rates were calculated from the weight of the collected float and its chemical analysis values.

[0058]

[0059] The analytical results of the flotation test products are shown in Tables 3 and 4. As is clear from Tables 3 and 4, under normal flotation conditions (Comparative Example 1) in which neither sulfur oxoacid nor hydrogen peroxide was added, both copper and arsenic were recovered in the float at approximately the same recovery rates. In contrast, in Examples 1 to 3 of the present invention, the arsenic recovery rate was kept low relative to the copper recovery rate. Furthermore, the arsenic / copper ratio in the float was lower than that in the sink, demonstrating that the arsenic grade was effectively reduced. Furthermore, Example 3, which is a more preferred embodiment of the present invention, in which sulfur oxoacid was added first and then hydrogen peroxide was added, enabled even more effective arsenic reduction. It can also be seen that the hydrogen peroxide of the present invention is superior to the method of using oxygen as an oxidizing agent shown in the prior art (Patent Document 2).

[0060]

[0061]

[0062] [Examples 4 and 5, Comparative Examples 3 to 5] Using arsenic-containing copper ore B from Chile having the composition shown in Table 5 as a raw material, flotation tests were carried out.

[0063]

[0064] First, arsenic-containing copper ore B was crushed to -1.7 mm using a jaw crusher, and 480 g of the ore was removed and ground using a wet rod mill and a ball mill to prepare an arsenic-containing copper ore slurry with a particle size of 70 μm (80% passing diameter). Water was added to this slurry to adjust the solids concentration to 37 wt %, and then, in the conditioning step prior to flotation, various chemicals shown in Table 6 were added. Furthermore, 50 g / t of AP3477 (a dithiophosphate-based product, manufactured by Solvay) was added as a collector, and 24 g / t of MIBC (manufactured by Junsei Chemical Co., Ltd.) was added as a foaming agent. Then, flotation was carried out using an Agitair-type tester. The float was collected for 16 minutes after the start of flotation, and the float and sink were each chemically analyzed. The recovery rates of copper and arsenic were calculated from the weight of the collected float and its chemical analysis values.

[0065]

[0066] The analytical results of the flotation test products are shown in Tables 7 and 8. As is clear from Tables 7 and 8, under normal flotation conditions (Comparative Example 3) in which neither sulfur oxoacid nor hydrogen peroxide was added, both copper and arsenic were recovered in the float at approximately the same recovery rate. In contrast, in Examples 4 and 5 of the present invention, the arsenic recovery rate was kept low relative to the copper recovery rate. Furthermore, the arsenic / copper ratio in the float was lower than that in the sink, demonstrating that the arsenic grade was effectively reduced. In Comparative Example 4, in which only hydrogen peroxide was used, both copper and arsenic were equally suppressed, resulting in ineffective separation. Furthermore, in Comparative Example 5, which uses only sodium thiosulfate as shown in the prior art (Patent Document 1), the effect of arsenic reduction was limited. Examples 4 and 5 demonstrate more effective arsenic reduction. In other words, it is shown that by using both a sulfur oxoacid and hydrogen peroxide as in the present invention, a low-arsenic copper concentrate in which the arsenic content is effectively reduced can be produced.

[0067]

[0068]

Claims

1. A method for producing low-arsenic copper concentrate, characterized in that when producing copper concentrate by flotation using arsenic-containing copper ore as a raw material, thioacids of sulfur and hydrogen peroxide are used in combination as additives.

2. The method for producing low-arsenic copper concentrate according to claim 1, characterized in that the thioacids of sulfur are thiosulfate or sulfite.

3. The method for producing low-arsenic copper concentrate according to claim 1 or 2, characterized in that the addition amount of the thioacids of sulfur is 0.1 to 3 kg per 1 t of arsenic-containing copper ore.

4. The method for producing low-arsenic copper concentrate according to any one of claims 1 to 3, characterized in that the addition amount of hydrogen peroxide is 0.1 to 5 kg per 1 t of arsenic-containing copper ore.

5. The method for producing low-arsenic copper concentrate according to any one of claims 1 to 4, characterized in that as the addition order of the additives, thioacids of sulfur are added first, followed by hydrogen peroxide.

6. The method for producing low-arsenic copper concentrate according to any one of claims 1 to 5, characterized in that the arsenic minerals contained in the arsenic-containing copper ore are enargite and tennantite.