Filler taking distillers grains waste as raw material, preparation method therefor, and use thereof

By processing the distiller's grain waste and mixing it with modified montmorillonite and diatomaceous earth, the deficiencies in strength and waterproof and oil-proof performance of the pulp molding filler are solved, the comprehensive performance and resource utilization rate of the product are improved, and the environmental impact is reduced. pollute.

WO2024221752A1PCT designated stage expired Publication Date: 2024-10-31DONGGUAN ZHONGZHIDA BIOLOGICAL NEW MATERIALS CO LTD

Patent Information

Application Number
PCT/CN2023/124396
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2023-10-13
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing pulp molding fillers are deficient in improving the strength and waterproof and oil-proof properties of pulp molded products, and the retention rate and density problems of the fillers lead to uneven strength of the products, and some fillers are not effective in waterproofing and oil-proofing after modification. Obviously, the distiller's grain waste has not been effectively utilized, resulting in resource waste and environmental pollution.

Method used

The distiller's grain waste is used as raw material, and its porosity and hydrophobicity are increased through treatment. It is mixed with modified montmorillonite and diatomite, and materials such as attapulgite, calcium carbonate and sepiolite are added to improve the comprehensive performance of the filler. Specific steps include vacuum drying and oxidation activation of the distiller's grain powder, and introducing hydrophobic groups, followed by reaction with modified montmorillonite and diatomaceous earth, and adding dispersants to improve the hydrophobicity and mechanical properties of the filler.

Benefits of technology

It improves the hydrophobicity, waterproof and moisture-proof performance and mechanical strength of pulp molded products, reduces the precipitation of fillers, improves the processing performance and resource utilization rate of the products, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

A filler taking distillers grains waste as a raw material, a preparation method therefor, and a use thereof. The filler comprises the following raw materials in parts by weight: 40-60 parts of distillers grains waste powder, 30-40 parts of modified diatomite, 10-20 parts of attapulgite, 10-20 parts of calcium carbonate, 5-10 parts of sepiolite, 0.5-3 parts of a dispersant, and 10-20 parts of modified montmorillonite. The filler takes distillers grains waste as a raw material; by treating distillers grains, pores in the surface thereof are increased, thereby improving the overall porosity; then, distillers grains are subjected to oxidation activation, reactive groups on the surface of distillers grains powder are increased, and hydrophobic groups are introduced to improve the hydrophobicity of the distillers grains powder; and then, modified montmorillonite and modified diatomite are mixed and react with the distillers grains powder, and attapulgite, calcium carbonate, sepiolite, and dispersant are added, thereby improving the comprehensive performance of the filler.
Need to check novelty before this filing date? Find Prior Art

Description

A filler using distiller's grains waste as raw material, and its preparation method and application Technical Field

[0001] The invention belongs to the technical field of pulp molded packaging products, and particularly relates to a filler using distiller's grains waste as a raw material, and a preparation method and application thereof. Background Art

[0002] Pulp molding uses a certain concentration of primary or secondary fiber pulp and an appropriate amount of chemical additives as raw materials. Using a special mold under appropriate pressure (negative or positive), temperature, and time, the fibers are evenly distributed on the mold surface. After dehydration, the wet paper blank is formed into a specific geometric shape. Further dehydration, demolding, drying, and shaping are then performed to create an integrated, environmentally friendly packaging product. This product, with its abundant raw material sources and pollution-free production and use, is lightweight, has high compressive strength, excellent cushioning properties, and is easily recyclable. It is a classic green packaging product, and pulp molding, as an alternative to PE plastic, is gaining increasing attention both domestically and internationally.

[0003] Due to the wide range of applications for pulp molded products, the performance requirements vary. These relatively specific requirements can be met by varying the formulations of pulp additives and fillers. Currently, fillers primarily enhance product strength and impact resistance, improve moisture and mildew resistance, and impart water and oil resistance. Depending on the product's intended use, more than one filler may be required to achieve the desired product.

[0004] Most fillers are inorganic, which generally reduce the physical strength of pulp molded products. The total filler retention rate is around 40%. Furthermore, due to their high density, fillers tend to settle to the bottom after being added to the pulp, resulting in uneven strength of the pulp molded products. Furthermore, a large amount of filler is lost with the whitewater and deposited in the whitewater pool, causing serious problems with whitewater purification and waste disposal. Filler modification can effectively increase filler retention and, to a certain extent, improve the strength properties of the filled pulp molded products. Traditional filler modification methods often use polymer materials such as starch, polyvinyl alcohol, polyacrylamide, and modified cellulose to physically coat the filler particles to increase their size, change the charge and adsorption properties of the filler surface, and improve filler retention. However, physically modified fillers still suffer from poor shear resistance and unsatisfactory reinforcement effects. Furthermore, some modified fillers are not significantly effective in improving the waterproof, oil-proof, moisture-proof, and mildew-proof properties of pulp molded products.

[0005] Wine lees are usually used for traditional anaerobic biogas fermentation and livestock feed in rural areas, or even packaged and sold directly, with low added economic value. Wine lees are widely available, inexpensive, and have a simple production process. Moreover, as a by-product of grain processing, wine lees are safe and reliable. In recent years, they have also been widely used to produce other chemical products. White wine lees are rich in fiber fermentation residues, rice husks, protein, starch and other by-products, which can be comprehensively utilized in many aspects. These biomass residues are prone to corrosion and deterioration due to their high moisture content and high acidity. If large quantities of white wine lees cannot be processed in time, it will not only result in a waste of resources, but also easily rot and deteriorate, causing environmental pollution. In this context, research on the comprehensive utilization of white wine lees is of great significance to improving resource utilization and protecting the ecological environment. Summary of the Invention

[0006] In view of the deficiencies in the prior art, the object of the present invention is to provide a filler using distiller's grains waste as raw material, and a preparation method and application thereof. The filler uses distiller's grains waste as raw material, and the lees are treated to increase the pores on their surface and improve the overall looseness. The lees are then oxidized and activated to increase the reactive groups on the surface of the distiller's grains powder, and hydrophobic groups are introduced to improve their hydrophobicity. Modified montmorillonite and modified diatomaceous earth are then mixed and reacted with the filler, and attapulgite, calcium carbonate, sepiolite and a dispersant are added to improve the comprehensive performance of the filler.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] A filler made from distiller's grains waste, comprising the following raw materials in parts by weight:

[0009] 40-60 parts of vinasse waste powder, 30-40 parts of modified diatomaceous earth, 10-20 parts of attapulgite, 10-20 parts of calcium carbonate, 5-10 parts of sepiolite, 0.5-3 parts of dispersant, and 10-20 parts of modified montmorillonite.

[0010] Preferably, the vinasse waste powder is pre-treated, and the processing steps are as follows:

[0011] (1) The white wine lees were air-dried and vacuum-dried at 60°C for 6-12 hours, and then crushed and passed through a 40-60 mesh sieve to obtain wine lees powder;

[0012] (2) adding the vinasse powder obtained in step (1) to a sodium hydroxide solution with a concentration of 20 g / L, stirring and reacting at 50-60° C. under microwave conditions for 30-50 min, filtering, washing, and drying after the reaction is completed to obtain oxidized vinasse powder;

[0013] (3) The oxidized vinasse powder obtained in step (2) is added to deionized water, followed by the addition of maleic anhydride, sodium lignin sulfonate, and dodecafluoroheptylpropyltrimethoxysilane, and the mixture is reacted at 60-80° C. for 3-5 hours. After the reaction is completed, the mixture is filtered, dried, and crushed through an 80-120 mesh sieve to obtain the vinasse waste powder.

[0014] Preferably, the microwave power in step (2) is 200-300 W; and the mass ratio of the oxidized vinasse powder, maleic anhydride, sodium lignin sulfonate, and dodecafluoroheptylpropyltrimethoxysilane in step (3) is 100:5-8:3-6:2-4.

[0015] Preferably, the preparation method of the modified diatomaceous earth comprises the following steps:

[0016] The diatomaceous earth is calcined at 300-500° C. for 2-3 hours, and after the calcination is completed, it is added to a hydrochloric acid solution with a mass concentration of 15% and immersed for 1-2 hours. After the immersion is completed, it is filtered, washed, and dried to obtain pretreated diatomaceous earth; the pretreated diatomaceous earth is added to deionized water, and then starch and stearic acid are added, and the reaction is carried out at 50-70° C. for 2-4 hours. After the reaction is completed, it is filtered, washed, and dried to obtain the modified diatomaceous earth.

[0017] Preferably, the mass ratio of the pretreated diatomaceous earth, starch and stearic acid is 30:20-30:5-10.

[0018] Preferably, the preparation method of the modified montmorillonite comprises the following steps:

[0019] (a) adding montmorillonite to deionized water, stirring at 50-70°C for 2-4 hours, then adding hexadecyldimethylbenzyl ammonium chloride, and continuing to stir for 4-6 hours. After the reaction is complete, filtering, washing, and drying to obtain an organic montmorillonite;

[0020] (b) adding the organic montmorillonite obtained in step (a) to deionized water, followed by adding chitosan acetic acid solution and epichlorohydrin, stirring and reacting at 70-90° C. for 3-5 hours, and filtering, washing, and drying after the reaction to obtain chitosan / organic montmorillonite;

[0021] (c) adding the chitosan / organic montmorillonite obtained in step (b) to anhydrous ethanol, followed by adding γ-glycidyloxypropyltrimethoxysilane, stirring and reacting at 60-70° C. for 2-5 hours. After the reaction is completed, filtering and drying to obtain the modified montmorillonite.

[0022] Preferably, the mass ratio of montmorillonite to hexadecyldimethylbenzyl ammonium chloride in step (a) is 100:10-15; the mass ratio of the organic montmorillonite, chitosan acetic acid solution, and epichlorohydrin in step (b) is 20:60-80:2-4, the mass concentration of chitosan in the chitosan acetic acid solution is 5%, and the mass concentration of acetic acid is 15%; and the mass ratio of chitosan / organic montmorillonite to γ-glycidyloxypropyltrimethoxysilane in step (c) is 50:3-6.

[0023] Preferably, the dispersant is one or more of carboxymethyl cellulose, sodium hexamethyl phosphate, and sodium dodecylbenzene sulfonate.

[0024] The present invention also protects a method for preparing the filler using distiller's grains waste as raw material, comprising the following steps:

[0025] The raw materials are weighed according to the formula, and the vinasse waste powder is added to deionized water, followed by the addition of modified diatomaceous earth and calcium carbonate, and stirred at 50-60°C for 1-2 hours. Then, modified montmorillonite, attapulgite, sepiolite, and dispersant are added, and stirring is continued for 0.5-1 hour. The mixture is then filtered, dried, and crushed to 80-120 mesh to obtain the filler made from vinasse waste.

[0026] The present invention also protects a use of the filler using distiller's grains waste as raw material in pulp molding, which comprises at least the following steps:

[0027] Step 1: soak the waste corrugated cardboard in water, then introduce it into a pulper barrel for beating for 20-30 minutes to prepare a pulp suspension with a solid content of 9-13%;

[0028] Step 2: Add the filler to the pulp suspension prepared in step 1 in an amount of 10-15% of the mass of the corrugated board, and stir at 60-70° C. and 500-700 rpm for 40-50 minutes to obtain a mixture A;

[0029] Step 3: Add Span-80 and polyvinyl alcohol to the mixture A in step 2, and stir for 30-40 minutes to obtain a mixture B; the amount of Span-80 added is 0.5-2% by weight of the corrugated board, and the amount of polyvinyl alcohol added is 0.5-1% by weight of the corrugated board;

[0030] Step 4: Mixture B is introduced into a mold, dried and dehydrated, pressed and formed, and cut to obtain a pulp molded product.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] (1) The filler prepared by the present invention using wine lees waste as raw material is first air-dried to remove a large amount of water, and then placed in a sodium hydroxide solution for oxidation activation, so that a large number of hydroxyl groups and phenolic hydroxyl groups are exposed on the surface of the cellulose in the wine lees, and then sodium lignin sulfonate and dodecafluoroheptylpropyltrimethoxysilane are added to react. The sodium lignin sulfonate and dodecafluoroheptylpropyltrimethoxysilane can increase the spatial steric hindrance of the cellulose in the wine lees and improve the dispersion performance, thereby making it have better looseness, which is conducive to the subsequent filling of inorganic small molecules such as modified diatomaceous earth and modified montmorillonite, so that the overall density of the filler is moderate, and it is not easy to settle to the bottom of the reaction tank when preparing pulp molded products, thereby improving the processing performance of the pulp molded products; at the same time, the fluorine-containing group in the introduced dodecafluoroheptylpropyltrimethoxysilane has good hydrophobicity, which can improve the hydrophobicity of wine lees powder, so that the prepared pulp molded products have good hydrophobicity.

[0033] (2) The filler prepared by the present invention with wine lees waste as raw material is calcined by diatomaceous earth to remove decomposable impurities such as carbonate minerals, organic matter and iron oxide minerals, and then impregnated with hydrochloric acid to increase the specific surface area of ​​diatomaceous earth and increase the porosity, which is conducive to the subsequent adsorption of large molecules by diatomaceous earth. Then, it is reacted with starch and stearic acid to composite-coat the diatomaceous earth particles to improve the adhesion between diatomaceous earth particles and pulp fibers, thereby making the pulp molded products have better mechanical strength; montmorillonite is added to water for heating and swelling to increase its interlayer spacing, and then hexadecyl dimethyl benzyl ammonium chloride is used to perform intercalation modification on montmorillonite, which can increase the adhesion between montmorillonite and pulp fibers. The compatibility between pulp fibers can also be improved. On the other hand, the interlayer spacing of montmorillonite can be increased to improve the degree of exfoliation of montmorillonite in pulp fibers. The increased interlayer spacing can be beneficial to the subsequent reaction. It is then intercalated with chitosan to give the montmorillonite a larger surface area and a complex internal structure, which increases the propagation path of water vapor. When used in pulp molded products, it can effectively improve the water barrier properties of the products. The montmorillonite is then modified for the second time by a silane coupling agent to form a multi-molecular covering film on the surface of the montmorillonite layer, thereby further changing the inherent hydrophilic properties of chitosan, making the surface of the montmorillonite layer have better hydrophobicity and improving the hydrophobicity of pulp molded products.

[0034] (3) The filler prepared by the present invention with wine lees waste as raw material is prepared by treating wine lees to increase the pores on its surface and improve the overall looseness. It is then oxidized and activated to increase the reactive groups on the surface of wine lees powder and introduce hydrophobic groups to improve its hydrophobicity. Modified montmorillonite and modified diatomaceous earth are then mixed and reacted with it. The hydrophobicity of wine lees waste powder and the water barrier property of modified montmorillonite synergistically improve the waterproof and moisture-proof properties of pulp molded products. Wine lees waste powder itself is rich in cellulose, hemicellulose, protein, starch and other substances and has good compatibility with pulp. It synergistically acts with modified diatomaceous earth to improve the mechanical strength of pulp molded products. In addition, the added attapulgite, calcium carbonate, sepiolite and dispersant can improve the comprehensive performance of the filler. DETAILED DESCRIPTION

[0035] The technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0036] The diatomite was purchased from Shengzhou Xinglong Diatomite Development Products Co., Ltd. with a mesh size of 325 mesh; the attapulgite was purchased from Mingguang Hongjiu Environmental Protection Materials Co., Ltd. with a mesh size of 325 mesh; the calcium carbonate was purchased from Jinan Tenghuida Chemical Co., Ltd. with a mesh size of 325 mesh; the sepiolite was purchased from Hebei Kexu Building Materials Co., Ltd. with a mesh size of 325 mesh; the montmorillonite was purchased from Nanyang Zhongrun Bentonite Technology Co., Ltd. with a mesh size of 325 mesh. Example

[0037] A filler using distiller's grains waste as raw material, comprising the following raw materials:

[0038] 6kg of vinasse waste powder, 4kg of modified diatomaceous earth, 2kg of attapulgite, 2kg of calcium carbonate, 1kg of sepiolite, 0.3kg of sodium dodecylbenzenesulfonate, and 2kg of modified montmorillonite.

[0039] Wherein, the vinasse waste powder is pre-treated, and the processing steps are as follows:

[0040] (1) The white wine lees were air-dried and vacuum-dried at 60°C for 12 h, and then crushed and passed through a 60-mesh sieve to obtain wine lees powder;

[0041] (2) adding 1 kg of the vinasse powder obtained in step (1) into 10 L of a sodium hydroxide solution having a concentration of 20 g / L, stirring and reacting for 30 min at a microwave power of 300 W and a temperature of 60° C. After the reaction is completed, filtering, washing, and drying to obtain oxidized vinasse powder;

[0042] (3) The oxidized vinasse powder (1 kg) obtained in step (2) was added to 10 L of deionized water, followed by the addition of 80 g of maleic anhydride, 60 g of sodium lignin sulfonate, and 40 g of dodecafluoroheptylpropyltrimethoxysilane. The mixture was reacted at 80 °C for 3 h. After the reaction was completed, the mixture was filtered, dried, and crushed through a 120-mesh sieve to obtain the vinasse waste powder.

[0043] The preparation method of the modified diatomaceous earth comprises the following steps:

[0044] 300 g of diatomaceous earth was calcined at 500° C. for 2 h. After the calcination, 2 L of the solution was added to a 15% hydrochloric acid solution and immersed for 2 h. After the immersion, the solution was filtered, washed, and dried to obtain pretreated diatomaceous earth. 300 g of the pretreated diatomaceous earth was added to 2 L of deionized water, followed by the addition of 300 g of starch and 100 g of stearic acid, and the mixture was reacted at 70° C. for 2 h. After the reaction was completed, the solution was filtered, washed, and dried to obtain the modified diatomaceous earth.

[0045] The preparation method of the modified montmorillonite comprises the following steps:

[0046] (a) 100 g of montmorillonite was added to 800 mL of deionized water and stirred at 70°C for 2 h. Subsequently, 15 g of hexadecyldimethylbenzylammonium chloride was added and stirring was continued for 4 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain an organic montmorillonite.

[0047] (b) adding 100 g of the organic montmorillonite obtained in step (a) to 800 mL of deionized water, followed by adding 400 g of chitosan acetic acid solution and 20 g of epichlorohydrin, and stirring at 90° C. for 3 h. After the reaction is completed, filtering, washing, and drying to obtain chitosan / organic montmorillonite, wherein the chitosan acetic acid solution has a chitosan mass concentration of 5% and an acetic acid mass concentration of 15%;

[0048] (c) The chitosan / organic montmorillonite (50 g) obtained in step (b) was added to 400 mL of anhydrous ethanol, followed by the addition of 6 g of γ-glycidyloxypropyltrimethoxysilane. The mixture was stirred at 70° C. for 2 h. After the reaction was completed, the mixture was filtered and dried to obtain the modified montmorillonite.

[0049] A method for preparing a filler using distiller's grains waste as raw material comprises the following steps:

[0050] The raw materials were weighed according to the formula, and the vinasse waste powder was added to deionized water, followed by the addition of modified diatomaceous earth and calcium carbonate, and stirred at 60°C for 2 hours. Then, modified montmorillonite, attapulgite, sepiolite, and sodium dodecylbenzenesulfonate were added, and stirring was continued for 1 hour. The mixture was then filtered, dried, and crushed to 120 mesh to obtain the filler made from vinasse waste. Example

[0051] A filler using distiller's grains waste as raw material, comprising the following raw materials:

[0052] 5 kg of vinasse waste powder, 3.5 kg of modified diatomaceous earth, 1.5 kg of attapulgite, 1.5 kg of calcium carbonate, 0.8 kg of sepiolite, 0.2 kg of carboxymethyl cellulose, and 1.5 kg of modified montmorillonite.

[0053] Wherein, the vinasse waste powder is pre-treated, and the processing steps are as follows:

[0054] (1) The white wine lees were air-dried and vacuum-dried at 60°C for 9 h, crushed and passed through a 60-mesh sieve to obtain wine lees powder;

[0055] (2) adding 1 kg of the vinasse powder obtained in step (1) into 10 L of a sodium hydroxide solution having a concentration of 20 g / L, stirring and reacting for 40 min at a microwave power of 250 W and a temperature of 55° C., filtering, washing, and drying after the reaction is completed to obtain oxidized vinasse powder;

[0056] (3) The oxidized vinasse powder (1 kg) obtained in step (2) was added to 10 L of deionized water, followed by the addition of 60 g of maleic anhydride, 50 g of sodium lignin sulfonate, and 30 g of dodecafluoroheptylpropyltrimethoxysilane. The mixture was reacted at 70 °C for 4 h. After the reaction was completed, the mixture was filtered, dried, and crushed through a 100-mesh sieve to obtain the vinasse waste powder.

[0057] The preparation method of the modified diatomaceous earth comprises the following steps:

[0058] 300 g of diatomaceous earth was calcined at 400° C. for 3 h. After the calcination, 2 L of the solution was added to a 15% hydrochloric acid solution and immersed for 2 h. After the immersion, the solution was filtered, washed, and dried to obtain pretreated diatomaceous earth. 300 g of the pretreated diatomaceous earth was added to 2 L of deionized water, followed by the addition of 250 g of starch and 80 g of stearic acid, and the mixture was reacted at 60° C. for 3 h. After the reaction was completed, the solution was filtered, washed, and dried to obtain the modified diatomaceous earth.

[0059] The preparation method of the modified montmorillonite comprises the following steps:

[0060] (a) 100 g of montmorillonite was added to 800 mL of deionized water and stirred at 60°C for 3 h. Subsequently, 13 g of hexadecyldimethylbenzylammonium chloride was added and stirred for 5 h. After the reaction was complete, the mixture was filtered, washed, and dried to obtain an organic montmorillonite.

[0061] (b) adding 100 g of the organic montmorillonite obtained in step (a) to 800 mL of deionized water, followed by adding 350 g of a chitosan acetic acid solution and 15 g of epichlorohydrin, and stirring the mixture at 80° C. for 4 h. After the reaction is completed, filtering, washing, and drying to obtain a chitosan / organic montmorillonite solution, wherein the chitosan mass concentration in the chitosan acetic acid solution is 5% and the mass concentration of the acetic acid is 15%;

[0062] (c) The chitosan / organic montmorillonite (50 g) obtained in step (b) was added to 400 mL of anhydrous ethanol, followed by the addition of 5 g of γ-glycidyloxypropyltrimethoxysilane. The mixture was stirred at 65° C. for 4 h. After the reaction was complete, the mixture was filtered and dried to obtain the modified montmorillonite.

[0063] A method for preparing a filler using distiller's grains waste as raw material comprises the following steps:

[0064] The raw materials were weighed according to the formula, and the vinasse waste powder was added to deionized water. Subsequently, modified diatomaceous earth and calcium carbonate were added, and the mixture was stirred at 55°C for 2 hours. Then, modified montmorillonite, attapulgite, sepiolite, and carboxymethyl cellulose were added, and the mixture was stirred for 0.5 hours. The mixture was then filtered, dried, and crushed to 100 mesh to obtain the filler made from vinasse waste. Example

[0065] A filler using distiller's grains waste as raw material, comprising the following raw materials:

[0066] 4 kg of vinasse waste powder, 3 kg of modified diatomaceous earth, 1 kg of attapulgite, 1 kg of calcium carbonate, 0.5 kg of sepiolite, 0.05 kg of sodium hexamethylphosphate, and 1 kg of modified montmorillonite.

[0067] Wherein, the vinasse waste powder is pre-treated, and the processing steps are as follows:

[0068] (1) The white wine lees were air-dried and vacuum-dried at 60°C for 6 h, crushed and passed through a 40-mesh sieve to obtain wine lees powder;

[0069] (2) adding 1 kg of the vinasse powder obtained in step (1) into 10 L of a sodium hydroxide solution having a concentration of 20 g / L, stirring and reacting for 50 min at a microwave power of 200 W and a temperature of 50° C. After the reaction is completed, filtering, washing, and drying to obtain oxidized vinasse powder;

[0070] (3) The oxidized vinasse powder (1 kg) obtained in step (2) was added to 10 L of deionized water, followed by the addition of 50 g of maleic anhydride, 30 g of sodium lignin sulfonate, and 20 g of dodecafluoroheptylpropyltrimethoxysilane. The mixture was reacted at 60 °C for 5 h. After the reaction was completed, the mixture was filtered, dried, and crushed through an 80-mesh sieve to obtain the vinasse waste powder.

[0071] The preparation method of the modified diatomaceous earth comprises the following steps:

[0072] 300 g of diatomaceous earth was calcined at 300° C. for 3 h. After the calcination was completed, 2 L of the solution was added to a hydrochloric acid solution with a mass concentration of 15% and immersed for 1 h. After the immersion was completed, the solution was filtered, washed, and dried to obtain pretreated diatomaceous earth. 300 g of the pretreated diatomaceous earth was added to 2 L of deionized water, followed by the addition of 200 g of starch and 50 g of stearic acid, and the mixture was reacted at 50° C. for 4 h. After the reaction was completed, the solution was filtered, washed, and dried to obtain the modified diatomaceous earth.

[0073] The preparation method of the modified montmorillonite comprises the following steps:

[0074] (a) 100 g of montmorillonite was added to 800 mL of deionized water and stirred at 50°C for 4 h. Subsequently, 10 g of hexadecyldimethylbenzylammonium chloride was added and stirred for another 4 h. After the reaction was complete, the mixture was filtered, washed, and dried to obtain an organic montmorillonite.

[0075] (b) adding 100 g of the organic montmorillonite obtained in step (a) to 800 mL of deionized water, followed by adding 300 g of chitosan acetic acid solution and 10 g of epichlorohydrin, and stirring at 70° C. for 5 h. After the reaction is completed, filtering, washing, and drying to obtain chitosan / organic montmorillonite, wherein the chitosan acetic acid solution has a chitosan mass concentration of 5% and an acetic acid mass concentration of 15%;

[0076] (c) The chitosan / organic montmorillonite (50 g) obtained in step (b) was added to 400 mL of anhydrous ethanol, followed by the addition of 3 g of γ-glycidyloxypropyltrimethoxysilane. The mixture was stirred at 60° C. for 5 h. After the reaction was complete, the mixture was filtered and dried to obtain the modified montmorillonite.

[0077] A method for preparing a filler using distiller's grains waste as raw material comprises the following steps:

[0078] The raw materials were weighed according to the formula, and the vinasse waste powder was added to deionized water. Subsequently, modified diatomaceous earth and calcium carbonate were added, and the mixture was stirred at 50°C for 2 hours. Then, modified montmorillonite, attapulgite, sepiolite, and sodium hexamethyl phosphate were added, and the mixture was stirred for 0.5 hours. The mixture was then filtered, dried, and crushed to 80 mesh to obtain the filler made from vinasse waste.

[0079] A filler using distiller's grains waste as raw material, comprising the following raw materials:

[0080] 6kg of wine lees powder, 4kg of modified diatomaceous earth, 2kg of attapulgite, 2kg of calcium carbonate, 1kg of sepiolite, 0.3kg of sodium dodecylbenzenesulfonate, and 2kg of modified montmorillonite.

[0081] The processing steps of the vinasse powder are as follows: air-dry the white vinasse and vacuum-dry it at 60° C. for 12 hours, grind it and pass it through a 60-mesh sieve to obtain the vinasse powder.

[0082] The preparation method of the modified diatomaceous earth comprises the following steps:

[0083] 300 g of diatomaceous earth was calcined at 500° C. for 2 h. After the calcination, 2 L of the solution was added to a 15% hydrochloric acid solution and immersed for 2 h. After the immersion, the solution was filtered, washed, and dried to obtain pretreated diatomaceous earth. 300 g of the pretreated diatomaceous earth was added to 2 L of deionized water, followed by the addition of 300 g of starch and 100 g of stearic acid, and the mixture was reacted at 70° C. for 2 h. After the reaction was completed, the solution was filtered, washed, and dried to obtain the modified diatomaceous earth.

[0084] The preparation method of the modified montmorillonite comprises the following steps:

[0085] (a) 100 g of montmorillonite was added to 800 mL of deionized water and stirred at 70°C for 2 h. Subsequently, 15 g of hexadecyldimethylbenzylammonium chloride was added and stirring was continued for 4 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain an organic montmorillonite.

[0086] (b) adding 100 g of the organic montmorillonite obtained in step (a) to 800 mL of deionized water, followed by adding 400 g of chitosan acetic acid solution and 20 g of epichlorohydrin, and stirring at 90° C. for 3 h. After the reaction is completed, filtering, washing, and drying to obtain chitosan / organic montmorillonite, wherein the chitosan acetic acid solution has a chitosan mass concentration of 5% and an acetic acid mass concentration of 15%;

[0087] (c) The chitosan / organic montmorillonite (50 g) obtained in step (b) was added to 400 mL of anhydrous ethanol, followed by the addition of 6 g of γ-glycidyloxypropyltrimethoxysilane. The mixture was stirred at 70° C. for 2 h. After the reaction was completed, the mixture was filtered and dried to obtain the modified montmorillonite.

[0088] A method for preparing a filler using distiller's grains waste as raw material comprises the following steps:

[0089] The raw materials were weighed according to the formula, and the vinasse powder was added to deionized water, followed by the addition of modified diatomaceous earth and calcium carbonate, and stirred at 60°C for 2 hours. Then, modified montmorillonite, attapulgite, sepiolite, and sodium dodecylbenzenesulfonate were added, and stirring was continued for 1 hour. The mixture was then filtered, dried, and crushed to 120 mesh to obtain the filler made from vinasse waste.

[0090] A filler using distiller's grains waste as raw material, comprising the following raw materials:

[0091] 6 kg of vinasse waste powder, 4 kg of diatomaceous earth, 2 kg of attapulgite, 2 kg of calcium carbonate, 1 kg of sepiolite, 0.3 kg of sodium dodecylbenzenesulfonate, and 2 kg of modified montmorillonite.

[0092] Wherein, the vinasse waste powder is pre-treated, and the processing steps are as follows:

[0093] (1) The white wine lees were air-dried and vacuum-dried at 60°C for 12 h, and then crushed and passed through a 60-mesh sieve to obtain wine lees powder;

[0094] (2) adding 1 kg of the vinasse powder obtained in step (1) into 10 L of a sodium hydroxide solution having a concentration of 20 g / L, stirring and reacting for 30 min at a microwave power of 300 W and a temperature of 60° C. After the reaction is completed, filtering, washing, and drying to obtain oxidized vinasse powder;

[0095] (3) The oxidized vinasse powder (1 kg) obtained in step (2) was added to 10 L of deionized water, followed by the addition of 80 g of maleic anhydride, 60 g of sodium lignin sulfonate, and 40 g of dodecafluoroheptylpropyltrimethoxysilane. The mixture was reacted at 80 °C for 3 h. After the reaction was completed, the mixture was filtered, dried, and crushed through a 120-mesh sieve to obtain the vinasse waste powder.

[0096] The preparation method of the modified montmorillonite comprises the following steps:

[0097] (a) 100 g of montmorillonite was added to 800 mL of deionized water and stirred at 70°C for 2 h. Subsequently, 15 g of hexadecyldimethylbenzylammonium chloride was added and stirring was continued for 4 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain an organic montmorillonite.

[0098] (b) adding 100 g of the organic montmorillonite obtained in step (a) to 800 mL of deionized water, followed by adding 400 g of chitosan acetic acid solution and 20 g of epichlorohydrin, and stirring at 90° C. for 3 h. After the reaction is completed, filtering, washing, and drying to obtain chitosan / organic montmorillonite, wherein the chitosan acetic acid solution has a chitosan mass concentration of 5% and an acetic acid mass concentration of 15%;

[0099] (c) The chitosan / organic montmorillonite (50 g) obtained in step (b) was added to 400 mL of anhydrous ethanol, followed by the addition of 6 g of γ-glycidyloxypropyltrimethoxysilane. The mixture was stirred at 70° C. for 2 h. After the reaction was completed, the mixture was filtered and dried to obtain the modified montmorillonite.

[0100] A method for preparing a filler using distiller's grains waste as raw material comprises the following steps:

[0101] The raw materials were weighed according to the formula, and the vinasse waste powder was added to deionized water, followed by the addition of diatomaceous earth and calcium carbonate, and stirred at 60°C for 2 hours. Then, modified montmorillonite, attapulgite, sepiolite, and sodium dodecylbenzenesulfonate were added, and stirring was continued for 1 hour. The mixture was then filtered, dried, and crushed to 120 mesh to obtain the filler made from vinasse waste.

[0102] A filler using distiller's grains waste as raw material, comprising the following raw materials:

[0103] 6kg of vinasse waste powder, 4kg of modified diatomaceous earth, 2kg of attapulgite, 2kg of calcium carbonate, 1kg of sepiolite, 0.3kg of sodium dodecylbenzenesulfonate, and 2kg of montmorillonite.

[0104] Wherein, the vinasse waste powder is pre-treated, and the processing steps are as follows:

[0105] (1) The white wine lees were air-dried and vacuum-dried at 60°C for 12 h, and then crushed and passed through a 60-mesh sieve to obtain wine lees powder;

[0106] (2) adding 1 kg of the vinasse powder obtained in step (1) into 10 L of a sodium hydroxide solution having a concentration of 20 g / L, stirring and reacting for 30 min at a microwave power of 300 W and a temperature of 60° C. After the reaction is completed, filtering, washing, and drying to obtain oxidized vinasse powder;

[0107] (3) The oxidized vinasse powder (1 kg) obtained in step (2) was added to 10 L of deionized water, followed by the addition of 80 g of maleic anhydride, 60 g of sodium lignin sulfonate, and 40 g of dodecafluoroheptylpropyltrimethoxysilane. The mixture was reacted at 80 °C for 3 h. After the reaction was completed, the mixture was filtered, dried, and crushed through a 120-mesh sieve to obtain the vinasse waste powder.

[0108] The preparation method of the modified diatomaceous earth comprises the following steps:

[0109] 300 g of diatomaceous earth was calcined at 500° C. for 2 h. After the calcination, 2 L of the solution was added to a 15% hydrochloric acid solution and immersed for 2 h. After the immersion, the solution was filtered, washed, and dried to obtain pretreated diatomaceous earth. 300 g of the pretreated diatomaceous earth was added to 2 L of deionized water, followed by the addition of 300 g of starch and 100 g of stearic acid, and the mixture was reacted at 70° C. for 2 h. After the reaction was completed, the solution was filtered, washed, and dried to obtain the modified diatomaceous earth.

[0110] A method for preparing a filler using distiller's grains waste as raw material comprises the following steps:

[0111] The raw materials were weighed according to the formula, and the vinasse waste powder was added to deionized water, followed by the addition of modified diatomaceous earth and calcium carbonate, and stirred at 60°C for 2 hours. Then, montmorillonite, attapulgite, sepiolite, and sodium dodecylbenzenesulfonate were added, and stirring was continued for 1 hour. The mixture was then filtered, dried, and crushed to 120 mesh to obtain the filler made from vinasse waste.

[0112] The fillers prepared in Examples 1-3 and Comparative Examples 1-3 using wine lees waste as raw materials were applied to pulp molded products. The specific preparation method is as follows:

[0113] Step 1: 250 g of waste corrugated cardboard was soaked in 2 L of water, and then introduced into a pulper barrel for beating for 30 minutes to prepare a pulp suspension;

[0114] Step 2: adding 25 g of filler made from distiller's grains waste to the pulp suspension prepared in step 1, in an amount of 10-15% of the mass of the corrugated board, and stirring at 60° C. and 600 rpm for 50 min to obtain a mixture A;

[0115] Step 3: Add 2.5 g of Span-80 and 2 g of polyvinyl alcohol to the mixture A in step 2 and stir for 40 min to obtain a mixture B;

[0116] Step 4: Mixture B is introduced into the mold and dehydrated to obtain a wet blank with a water content of 50%. The wet blank is then placed in a drying oven and dried at 80°C for 2 hours. It is then transferred to a flat vulcanizer and hot-pressed at 120°C and 4 MPa for 3 minutes to obtain a pulp molded product.

[0117] The pulp molded products of Examples 1-3 and Comparative Examples 1-3 were subjected to performance tests. The dry tensile strength was tested according to GB / T 12914-2018 "Paper and paperboard - Determination of tensile strength - Constant rate of tension method". The sampling direction was longitudinal, the sample size was 250 mm × 15 mm, the tensile speed was 20 mm / min, and the samples were placed in an environment with a temperature of 23 ° C and a relative humidity of 50% for 24 h before the test. The wet tensile strength was tested according to GB / T 465.2-2008 "Determination of the tensile strength of paper and paperboard after immersion in water" was tested at a temperature of 23°C for 2 hours. Water absorption was determined by placing a 50mm x 50mm sample in a 50°C oven for 24 hours, removing it and weighing its mass m1. The sample was then immersed in pre-prepared 30°C tap water for 24 hours, removed, and allowed to dry naturally. The water on the bottom of the sample was then gently wiped with filter paper and weighed m2. The water absorption was calculated as (m2 - m1) / m1 × 100%. The test results are shown in Table 1 below:

[0118] Table 1

[0119] It can be seen from the above test data that the filler prepared by the present invention using distiller's grains waste as raw material can improve the tensile strength and water resistance of pulp molded products after being used in pulp molded products, and has broad application prospects.

[0120] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.

Claims

1. A filler made from distiller's grains waste, characterized in that: By weight, it includes the following raw materials: 40-60 parts of vinasse waste powder, 30-40 parts of modified diatomaceous earth, 10-20 parts of attapulgite, 10-20 parts of calcium carbonate, 5-10 parts of sepiolite, 0.5-3 parts of dispersant, and 10-20 parts of modified montmorillonite; Wherein, the vinasse waste powder is pre-treated, and the processing steps are as follows: (1) air-drying the white wine lees, vacuum drying at 60°C for 6-12h, crushing and passing through a 40-60 mesh sieve to obtain wine lees powder; (2) adding the vinasse powder obtained in step (1) into a sodium hydroxide solution with a concentration of 20 g / L, stirring and reacting at 50-60° C. for 30-50 min under microwave conditions, and filtering, washing and drying after the reaction is completed to obtain oxidized vinasse powder; (3) adding the oxidized distiller's grains powder obtained in step (2) into deionized water, and then adding maleic anhydride, sodium lignin sulfonate, and dodecafluoroheptylpropyltrimethoxysilane, and reacting at 60-80° C. for 3-5 hours. After the reaction is completed, filtering, drying, and crushing through an 80-120 mesh sieve to obtain the distiller's grains waste powder; The preparation method of the modified diatomite comprises the following steps: The diatomite is calcined at 300-500°C for 2-3h, and after the calcination is completed, it is added to a hydrochloric acid solution with a mass concentration of 15% and immersed for 1-2h. After the immersion is completed, it is filtered, washed, and dried to obtain pretreated diatomite; the pretreated diatomite is added to deionized water, and then starch and stearic acid are added, and the reaction is carried out at 50-70°C for 2-4h. After the reaction is completed, it is filtered, washed, and dried to obtain the modified diatomite; The preparation method of the modified montmorillonite comprises the following steps: (a) adding montmorillonite to deionized water, stirring at 50-70° C. for 2-4 hours, then adding hexadecyl dimethyl benzyl ammonium chloride, and continuing to stir for 4-6 hours. After the reaction is completed, filtering, washing, and drying to obtain organic montmorillonite; (b) adding the organic montmorillonite obtained in step (a) into deionized water, and then adding chitosan acetic acid solution and epichlorohydrin, stirring and reacting at 70-90° C. for 3-5 hours, filtering, washing and drying after the reaction is completed to obtain chitosan / organic montmorillonite; (c) adding the chitosan / organic montmorillonite obtained in step (b) into anhydrous ethanol, and then adding γ-glycidyloxypropyltrimethoxysilane, stirring and reacting at 60-70° C. for 2-5 hours, filtering and drying after the reaction is completed, thereby obtaining the modified montmorillonite.

2. A filler made of wine lees waste as raw material according to claim 1, characterized in that: The microwave power in step (2) is 200-300 W; the mass ratio of the oxidized vinasse powder, maleic anhydride, sodium lignin sulfonate and dodecafluoroheptylpropyltrimethoxysilane in step (3) is 100:5-8:3-6:2-4.

3. The filler made of wine lees waste as raw material according to claim 1, characterized in that: The mass ratio of the pretreated diatomaceous earth, starch and stearic acid is 30:20-30:5-10.

4. The filler made of wine lees waste as raw material according to claim 1, characterized in that: The mass ratio of montmorillonite to hexadecyldimethylbenzyl ammonium chloride in step (a) is 100:10-15; the mass ratio of organic montmorillonite, chitosan acetic acid solution and epichlorohydrin in step (b) is 20:60-80:2-4, the mass concentration of chitosan in the chitosan acetic acid solution is 5%, and the mass concentration of acetic acid is 15%; the mass ratio of chitosan / organic montmorillonite to γ-glycidyloxypropyltrimethoxysilane in step (c) is 50:3-6.

5. The filler made of wine lees waste as raw material according to claim 1, characterized in that: The dispersant is one or more of carboxymethyl cellulose, sodium hexamethyl phosphate, and sodium dodecylbenzene sulfonate.

6. A method for preparing a filler using wine lees waste as raw material as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: The raw materials are weighed according to the formula, and the vinasse waste powder is added to deionized water, followed by the addition of modified diatomaceous earth and calcium carbonate, and stirred at 50-60°C for 1-2h, and then the modified montmorillonite, attapulgite, sepiolite and dispersant are added, and stirring is continued for 0.5-1h, followed by filtering, drying and crushing to 80-120 meshes to obtain the filler using vinasse waste as raw material.

7. Use of the filler made of wine lees waste as raw material in pulp molding according to any one of claims 1 to 5, characterized in that: The steps include at least: Step 1: soak the waste corrugated cardboard in water, and then introduce it into a pulper barrel for pulping for 20-30 minutes to prepare a pulp suspension with a solid content of 9-13%; Step 2: Add filler to the pulp suspension in step 1 in an amount of 10-15% of the mass of the corrugated board, stir at 60-70° C. and 500-700 r / min for 40-50 min to obtain mixture A; Step 3, adding Span-80 and polyvinyl alcohol to the mixture A in step 2, stirring for 30-40 minutes, to obtain a mixture B; the amount of Span-80 added is 0.5-2% of the mass of the corrugated board, and the amount of polyvinyl alcohol added is 0.5-1% of the mass of the corrugated board; Step 4: Mixture B is introduced into a mold, dried and dehydrated, pressed, formed, and cut to obtain a pulp molded product.

Citation Information

Patent Citations

  • Method for producing degradable material with manioc waste and wine stillage

    CN101302734A

  • Method for producing corrugated paper and textile spool paper by manioc slag and wine stillage slag

    CN101413225A

  • Method for producing sodium humate and by-product paper pulp by using cassava dregs as raw materials

    CN101666051A

  • Vinasse-reinforced modified phenolic resin foam material and preparation methods thereof

    CN104945842A

  • Manufacturing method of bobbin paper

    CN106555360A

Cited By

  • High-strength heat-resistant polylactic acid DTY (Draw Textured Yarn) filament and preparation method thereof

    CN119900105A

  • Hard rock tunneling muck recycling improvement process construction method

    CN120172687A

  • Process for treating acidic sewage in smelting industry

    CN120247289A

  • Carbon-silicon intercalation composite clay material for biogas slurry additive, preparation method and application

    CN120515387A

  • Self-drying acrylic enamel paint and preparation method thereof

    CN120944442A