Vacuum bag film, and preparation method therefor and use thereof
By using PA6 and PA66 isolation layers, ethylene-tetrafluoroethylene copolymer functional layer and adhesive in vacuum bag film, the temperature resistance and mold releaseability of vacuum bag films in the high temperature environment in the prior art is solved. The problem of high temperature resistance of 230°C and good airtightness and mold release properties are achieved.
Patent Information
- Application Number
- PCT/CN2023/138694
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-05
- Filing Date
- 2023-12-14
- Publication Date
- 2024-11-14
AI Technical Summary
The existing vacuum bag films are insufficient in high temperature environments and are prone to mold release, making it difficult to meet the needs of composite materials in the aerospace field.
The isolation layer is prepared by PA6 and PA66, and the functional layer is prepared by ethylene-tetrafluoroethylene copolymer and adhesive. By blending copolymer and functional bonding fluororesin, the effective bonding of the isolation layer and the release layer is achieved, and the film is lifted. heat resistance and easy release.
It realizes the high temperature resistance of vacuum bag films in a 230℃ environment for a long time, ensures the airtightness and easy release of composite materials, and meets the strength, modulus, temperature resistance and release in the aerospace field. Sexual requirements.
Smart Images

Figure CN2023138694_14112024_PF_FP_ABST
Abstract
Description
A vacuum bag film and its preparation method and application Technical Field
[0001] The present application belongs to the technical field of thin film materials, and specifically relates to a vacuum bag film and a preparation method and application thereof. Background Art
[0002] Vacuum bagging film is a vacuum-assisting material used in the production of composite parts. Its quality plays a crucial role in composite manufacturing, particularly in the aerospace sector. The development and use of high-temperature resins and prepregs has placed higher demands on the temperature resistance and versatility of vacuum bagging film, a vacuum-assisting material that traditional nylon composite films cannot meet.
[0003] CN112874097A discloses a high-temperature, high-efficiency release Teflon and nylon multilayer composite material. The composite material has a three-layer or five-layer structure. In the three-layer structure, the first layer is Teflon, the second layer is an adhesive resin, and the third layer is PA6 or PA66. In the five-layer structure, the first layer is Teflon, the second layer is an adhesive resin, the third layer is PA6 or PA66, the fourth layer is an adhesive resin, and the fifth layer is Teflon. This technical solution utilizes a multilayer structure combining Teflon and nylon, which significantly improves the film's high-temperature resistance and tensile strength, achieving a maximum temperature resistance of 220°C. However, Teflon, despite its excellent non-stick properties, is prone to delamination, and its temperature resistance still needs to be further improved.
[0004] CN103692708A discloses a vacuum bag with a separator effect, comprising an inner layer, a middle layer, and an outer layer, which are co-extruded and laminated in sequence. The inner and outer layers are made of a mixture of nylon and a fluorinated material, and the middle layer is made of nylon. This technical solution provides a vacuum bag that is airtight in a vacuum state, but is incompatible with composite materials. Even after the composite material has cured, it is easily peeled off. No mention is made of improvements to heat resistance.
[0005] CN106189200A discloses a high-temperature-resistant vacuum bagging film (LVF200G) and its preparation method. The film is blown and molded by mixing the following raw materials in parts by weight: 10-25 parts homonylon, 70-90 parts copolymer nylon, 1-10 parts elastomer, 1-4 parts heat stabilizer, and 0.2-2 parts masterbatch. This high-temperature-resistant vacuum bagging film has a maximum operating temperature of 205°C, but the nylon material can be difficult to demold, and its temperature resistance needs to be further improved.
[0006] Therefore, it is necessary to develop a vacuum bag film that is resistant to high temperatures, easy to demould, and has good barrier properties.
[0007] Summary of the Invention
[0008] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0009] In view of the deficiencies in the prior art, the purpose of this application is to provide a vacuum bag film and its preparation method and application, wherein the vacuum bag film has the characteristics of single-sided isolation, high temperature resistance, easy demoulding and good barrier properties.
[0010] To achieve this goal, this application adopts the following technical solutions:
[0011] In a first aspect, the present application provides a vacuum bag film, wherein the vacuum bag film comprises an isolation layer, a functional layer, and a release layer stacked in sequence.
[0012] The raw materials for preparing the isolation layer include PA6 and PA66, the raw materials for preparing the functional layer include ethylene-tetrafluoroethylene copolymer and adhesive, and the raw materials for preparing the release layer include ethylene-tetrafluoroethylene copolymer (ETFE).
[0013] In the present application, the isolation layer is made of PA6 and PA66, and has the functions of isolation and improving heat resistance; the functional layer is made of ethylene-tetrafluoroethylene copolymer and adhesive. The ethylene-tetrafluoroethylene copolymer has low surface tension and is easy to delaminate. The functional layer made of ethylene-tetrafluoroethylene copolymer and adhesive is used to bond the isolation layer and the release layer, which effectively solves the problem of easy delamination. The functional layer plays a supporting role in the structure; the release layer is made of ethylene-tetrafluoroethylene copolymer, and has the functions of improving heat resistance and achieving single-sided release.
[0014] In this application, the high temperature resistance means that it can be used normally for more than 6 hours at an ambient temperature of 230°C.
[0015] In one embodiment, the melt index of PA6 and PA66 is each independently 3-10 g / 10 min (190° C. / 2.16 kg). For example, at 190° C. and a pressure of 2.16 kg, the melt index of the ethylene-tetrafluoroethylene copolymer can be 3 g / 10 min, 4 g / 10 min, 5 g / 10 min, 6 g / 10 min, 7 g / 10 min, 8 g / 10 min, 9 g / 10 min or 10 g / 10 min, etc.
[0016] In one embodiment, the relative viscosities of PA6 and PA66 are independently 2.2-4.5, for example, 2.2, 2.4, 2.5, 2.7, 3, 3.5, 3.8, 4, 4.2 or 4.5.
[0017] In one embodiment, the raw materials for preparing the isolation layer further include a heat stabilizer.
[0018] In this application, PA6, PA66 and heat stabilizers are used as raw materials for the isolation layer, and PA6 and PA66 are made into nylon alloys, which can improve impact resistance and solubility resistance, and maintain strong strength and rigidity at higher temperatures. Adding heat stabilizers helps to improve temperature resistance.
[0019] In one embodiment, the thermal stabilizer comprises a copper salt thermal stabilizer.
[0020] In one embodiment, the thermal stabilizer comprises copper iodide.
[0021] In one embodiment, the melt index of the ethylene-tetrafluoroethylene copolymer is 5-20 g / 10 min (370° C. / 5 kg). For example, at 370° C. and a pressure of 5 kg, the melt index of the ethylene-tetrafluoroethylene copolymer can be 5 g / 10 min, 8 g / 10 min, 10 g / 10 min, 12 g / 10 min, 14 g / 10 min, 16 g / 10 min, 18 g / 10 min or 20 g / 10 min, etc.
[0022] In one embodiment, the adhesive comprises a functional bonding fluororesin.
[0023] In one embodiment, the melt index of the functional adhesive fluororesin is 15-30 g / 10 min (370° C. / 5 kg). For example, at 370° C. and a pressure of 5 kg, the melt index of the functional adhesive fluororesin can be 15 g / 10 min, 16 g / 10 min, 18 g / 10 min, 20 g / 10 min, 12 g / 10 min, 14 g / 10 min, 26 g / 10 min, 28 g / 10 min or 30 g / 10 min, etc.
[0024] In one embodiment, the functional adhesive fluororesin includes any one of LM730AP, LM740AP, AH2000, AH3000, or AH5000, or a combination of at least two thereof.
[0025] In one embodiment, the raw materials for preparing the functional layer further include masterbatch.
[0026] In one embodiment, based on the total mass of the raw materials for preparing the vacuum bag film as 100 parts, the raw materials for preparing the isolation layer include the following components in parts by weight: 10-55 parts (e.g., 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts or 55 parts, etc.) PA6, 10-30 parts (e.g., 10 parts, 12 parts, 15 parts, 18 parts, 20 parts, 22 parts, 25 parts, 28 parts or 30 parts, etc.) PA66 and 0-5 parts of a heat stabilizer.
[0027] In one embodiment, the raw materials of the functional layer include the following components in parts by weight: 30-55 parts (for example, 30 parts, 32 parts, 35 parts, 38 parts, 40 parts, 42 parts, 45 parts, 50 parts, 52 parts or 55 parts, etc.) of ethylene-tetrafluoroethylene copolymer, 10-30 parts (for example, 10 parts, 12 parts, 15 parts, 18 parts, 20 parts, 22 parts, 25 parts, 28 parts or 30 parts, etc.) of adhesive and 0.1-2 parts (for example, 0.1 parts, 0.5 parts, 0.8 parts, 1 part, 1.2 parts, 1.5 parts, 1.8 parts, 1.9 parts or 2 parts, etc.) of masterbatch.
[0028] Exemplarily, the masterbatch includes Kolan 342.42 and / or FRDG1-B.
[0029] In this application, by blending ethylene-tetrafluoroethylene copolymer and a functional adhesive fluororesin to form a functional layer, the barrier layer and release layer are bonded, thus resolving the problem of composite materials being prone to delamination and simultaneously improving the heat resistance of vacuum bag films. The functional adhesive fluororesin is highly compatible with nylon materials and can be used in any proportion, resulting in good adhesion between the functional layer and the barrier layer. The addition of ethylene-tetrafluoroethylene copolymer to the functional layer resolves the problem of the ethylene-tetrafluoroethylene copolymer's release layer having low surface tension and poor adhesion to other layers, which can easily lead to delamination.
[0030] In one embodiment, the vacuum bag film has a thickness of 50-300 μm, for example, 50 μm, 80 μm, 100 μm, 120 μm, 150 μm, 200 μm, 220 μm, 250 μm, 280 μm or 300 μm.
[0031] In one embodiment, based on the total thickness of the vacuum bag film being 100%, the thickness of the isolation layer accounts for 20-35%, the thickness of the functional layer accounts for 30-60%, and the thickness of the release layer accounts for 20-35%.
[0032] In the present application, the thickness of the isolation layer accounts for 20-35%. The reason is that if the thickness of the isolation layer is too low, it will affect the barrier properties of the vacuum bag film, while if it is too high, it will affect the overall processing stability of the vacuum bag film.
[0033] In a second aspect, the present application provides a method for preparing a vacuum bag film as described in the first aspect, the preparation method comprising the following steps: mixing and extruding PA6 and / or PA66 to obtain an isolation layer, mixing and extruding an ethylene-tetrafluoroethylene copolymer and an adhesive to obtain a functional layer, extruding an ethylene-tetrafluoroethylene copolymer to obtain a release layer, and co-extruding or blow-molding the isolation layer, functional layer and release layer stacked in sequence to obtain the vacuum bag film.
[0034] In one embodiment, the preparation method comprises the following steps: mixing PA6, PA66 and a heat stabilizer and adding them to the hopper of extruder A, mixing ethylene-tetrafluoroethylene copolymer, an adhesive and a masterbatch and adding them to the hopper of extruder B, adding ethylene-tetrafluoroethylene copolymer to the hopper of extruder C, and sequentially stacking and extruding the extruders A, B and C to the die head of an extruder or a film blowing machine, and performing co-extrusion molding or inflation molding to obtain the vacuum bag film.
[0035] In one embodiment, the vacuum bag film prepared by blow molding has a thickness of 50-150 μm, for example, 50 μm, 60 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm or 150 μm.
[0036] In one embodiment, the vacuum bag film prepared by extrusion molding has a thickness of 150-300 μm, for example, 160 μm, 180 μm, 200 μm, 210 μm, 220 μm, 240 μm, 250 μm, 280 μm or 300 μm.
[0037] In a third aspect, the present application provides a vacuum bag, which is made from the vacuum bag film as described in the first aspect.
[0038] Compared with the prior art, this application has the following beneficial effects:
[0039] This application uses PA6 and PA66 to form an isolation layer, ethylene-tetrafluoroethylene copolymer and adhesive to form a functional layer, and ethylene-tetrafluoroethylene copolymer to form a release layer, so that the vacuum bag film has the characteristics of single-sided isolation, high temperature resistance, easy demolding, and good barrier properties. The maximum operating temperature of the vacuum bag film can reach 230°C, and it can be kept warm for several hours without leakage. After the composite material part is completed, it can be easily demolded, which improves the problem of traditional nylon composite film being difficult to demold. It can meet the strength, modulus, temperature resistance and release requirements of vacuum bag film in the production process of composite materials in the aerospace field, and ensure the airtightness requirements of the vacuum bag.
[0040] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.
[0042] FIG1 is a schematic structural diagram of the vacuum bag film according to Example 1;
[0043] Among them, 1-isolating layer; 2-functional layer; 3-release layer. DETAILED DESCRIPTION
[0044] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.
[0045] Example 1
[0046] This embodiment provides a vacuum bag film and a preparation method thereof. The vacuum bag film has a thickness of 60 μm and includes an isolation layer, a functional layer and a release layer stacked in sequence. As shown in FIG1 , the thickness of the isolation layer accounts for 30%, the thickness of the functional layer accounts for 40%, and the thickness of the release layer accounts for 30%.
[0047] The raw materials for preparing the isolation layer include 13 parts of PA6 (melt index of 3g / 10min, 190℃ / 2.16kg), 13 parts of PA66 (melt index of 3g / 10min, 190℃ / 2.16kg) and 4 parts of heat stabilizer (copper iodide); the raw materials for preparing the functional layer include 14 parts of ethylene-tetrafluoroethylene copolymer (melt index of 18g / 10min, 370℃ / 5kg), 25 parts of adhesive (AH5000) and 1 part of masterbatch (Kolan 342.42); the raw materials for preparing the release layer include 30 parts of ethylene-tetrafluoroethylene copolymer (melt index of 18g / 10min, 370℃ / 5kg).
[0048] The preparation method is as follows:
[0049] PA6, PA66 and a heat stabilizer are mixed and added to the hopper of a spiral plastic extruder A; an ethylene-tetrafluoroethylene copolymer, an adhesive and a masterbatch are mixed and added to the hopper of a spiral plastic extruder B; and the ethylene-tetrafluoroethylene copolymer is added to the hopper of a spiral plastic extruder C. The mixture is plasticized and melted by the spiral plastic extruders A, B and C. Under the action of the internal pressure of the barrel of the spiral plastic extruder and the forward thrust of its screw, the molten raw materials are conveyed to the die head of a three-layer film blowing machine. The raw materials for the isolation layer, the functional layer and the release layer are sequentially stacked and extruded at the die head of the three-layer film blowing machine, and are blown to obtain the tubular vacuum bag film.
[0050] The screw temperatures of the A screw plastic extruder, the B screw plastic extruder and the C screw plastic extruder are 270°C, the speed of the A screw plastic extruder is 30rpm, the speed of the B screw plastic extruder is 40rpm; the speed of the C screw plastic extruder is 30rpm, the temperature of the die head of the three-layer film blowing machine is 285°C, the blow-up ratio is 1.5, and the curling speed is 7m / min.
[0051] Example 2
[0052] This embodiment provides a vacuum bag film and a preparation method thereof. The vacuum bag film has a thickness of 100 μm and includes an isolation layer, a functional layer and a release layer stacked in sequence. The thickness of the isolation layer accounts for 25%, the thickness of the functional layer accounts for 45%, and the thickness of the release layer accounts for 30%.
[0053] The raw materials for preparing the isolation layer include 11 parts of PA6 (melt index of 5g / 10min, 190℃ / 2.16kg), 11 parts of PA66 (melt index of 5g / 10min, 190℃ / 2.16kg) and 3 parts of heat stabilizer (copper iodide); the raw materials for preparing the functional layer include 19 parts of ethylene-tetrafluoroethylene copolymer (melt index of 5g / 10min, 370℃ / 5kg), 25 parts of adhesive (LM730AP) and 1 part of masterbatch (FRDG1-B, purchased from Taizhou Jianlong Technology Co., Ltd.); the raw materials for preparing the release layer include 30 parts of ethylene-tetrafluoroethylene copolymer (melt index of 5g / 10min, 370℃ / 5kg).
[0054] The preparation method is as follows:
[0055] PA6, PA66 and a heat stabilizer are mixed and added to the hopper of a spiral plastic extruder A; an ethylene-tetrafluoroethylene copolymer, an adhesive and a masterbatch are mixed and added to the hopper of a spiral plastic extruder B; and the ethylene-tetrafluoroethylene copolymer is added to the hopper of a spiral plastic extruder C. The mixture is plasticized and melted by the spiral plastic extruders A, B and C. Under the action of the internal pressure of the barrel of the spiral plastic extruder and the forward thrust of its screw, the molten raw materials are conveyed to the die head of a three-layer film blowing machine. The raw materials for the isolation layer, the functional layer and the release layer are sequentially stacked and extruded at the die head of the three-layer film blowing machine, and are blown to obtain the tubular vacuum bag film.
[0056] The screw temperatures of the A screw plastic extruder, the B screw plastic extruder and the C screw plastic extruder are 270°C, the speed of the A screw plastic extruder is 25rpm, the speed of the B screw plastic extruder is 45rpm; the speed of the C screw plastic extruder is 30rpm, the temperature of the die head of the three-layer film blowing machine is 265°C, the blow-up ratio is 1.5, and the curling speed is 7m / min.
[0057] Example 3
[0058] This embodiment provides a vacuum bag film and a preparation method thereof. The vacuum bag film has a thickness of 50 μm and includes an isolation layer, a functional layer and a release layer stacked in sequence. The thickness of the isolation layer accounts for 20%, the thickness of the functional layer accounts for 60%, and the thickness of the release layer accounts for 20%.
[0059] The raw materials for preparing the isolation layer include 9 parts of PA6 (melt index of 10g / 10min, 190℃ / 2.16kg), 9 parts of PA66 (melt index of 10g / 10min, 190℃ / 2.16kg) and 2 parts of heat stabilizer (copper iodide); the raw materials for preparing the functional layer include 28 parts of ethylene-tetrafluoroethylene copolymer (melt index of 20g / 10min, 370℃ / 5kg), 30 parts of adhesive (LM740AP) and 2 parts of masterbatch (Kolan 342.42); the raw materials for preparing the release layer include 20 parts of ethylene-tetrafluoroethylene copolymer (melt index of 20g / 10min, 370℃ / 5kg).
[0060] The preparation method is as follows:
[0061] PA6, PA66 and a heat stabilizer are mixed and added to the hopper of a spiral plastic extruder A; an ethylene-tetrafluoroethylene copolymer, an adhesive and a masterbatch are mixed and added to the hopper of a spiral plastic extruder B; and the ethylene-tetrafluoroethylene copolymer is added to the hopper of a spiral plastic extruder C. The raw materials are plasticized and melted in the spiral plastic extruders A, B and C. Under the action of the internal pressure of the barrel of the spiral plastic extruder and the forward thrust of the screw, the molten raw materials are conveyed to the die head of a three-layer film blowing machine. The raw materials for the isolation layer, the functional layer and the release layer are sequentially stacked and extruded in the die head of the three-layer film blowing machine, and are blown to obtain the tubular vacuum bag film.
[0062] The screw temperatures of the A screw plastic extruder, the B screw plastic extruder and the C screw plastic extruder are 270°C, the speed of the A screw plastic extruder is 20rpm, the speed of the B screw plastic extruder is 60rpm; the speed of the C screw plastic extruder is 20rpm, the temperature of the die head of the three-layer film blowing machine is 280°C, the blow-up ratio is 1.5, and the curling speed is 7m / min.
[0063] Example 4
[0064] This embodiment provides a vacuum bag film and a preparation method thereof. The vacuum bag film has a thickness of 200 μm and includes an isolation layer, a functional layer and a release layer stacked in sequence. The thickness of the isolation layer accounts for 20%, the thickness of the functional layer accounts for 60%, and the thickness of the release layer accounts for 20%.
[0065] The raw materials for preparing the isolation layer include 10 parts of PA6 (melt index of 10g / 10min, 190℃ / 2.16kg) and 10 parts of PA66 (melt index of 10g / 10min, 190℃ / 2.16kg), the raw materials for preparing the functional layer include 8 parts of ethylene-tetrafluoroethylene copolymer (melt index 18g / 10min, 370℃ / 5kg), 50 parts of adhesive (AH5000) and 2 parts of masterbatch (Kolan 342.42), and the raw materials for preparing the release layer include 20 parts of ethylene-tetrafluoroethylene copolymer (melt index 18g / 10min, 370℃ / 5kg).
[0066] The preparation method is as follows:
[0067] PA6 and PA66 are mixed and added to the hopper of spiral plastic extruder A, ethylene-tetrafluoroethylene copolymer, adhesive and masterbatch are mixed and added to the hopper of spiral plastic extruder B, and ethylene-tetrafluoroethylene copolymer is added to the hopper of spiral plastic extruder C. After being plasticized and melted by spiral plastic extruders A, B and C, the molten raw materials are transported to the extruder die head under the internal pressure of the barrel of the spiral plastic extruder and the forward thrust of the screw to obtain the vacuum bag film.
[0068] The screw temperatures of the A screw plastic extruder, the B screw plastic extruder and the C screw plastic extruder are 270°C, the speed of the A screw plastic extruder is 20rpm, the speed of the B screw plastic extruder is 60rpm; the speed of the C screw plastic extruder is 20rpm, the temperature of the die head of the three-layer extruder is 280°C, and the pulling speed is 2m / min.
[0069] Example 5
[0070] This embodiment provides a vacuum bag film and a preparation method thereof. The vacuum bag film has a thickness of 300 μm and includes an isolation layer, a functional layer and a release layer stacked in sequence. The thickness of the isolation layer accounts for 35%, the thickness of the functional layer accounts for 30%, and the thickness of the release layer accounts for 35%.
[0071] The raw materials for preparing the isolation layer include 10 parts of PA6 (melt index of 10g / 10min, 190℃ / 2.16kg), 24 parts of PA66 (melt index of 10g / 10min, 190℃ / 2.16kg) and 1 part of heat stabilizer (copper iodide); the raw materials for preparing the functional layer include 20 parts of ethylene-tetrafluoroethylene copolymer (melt index of 18g / 10min, 370℃ / 5kg), 10 parts of adhesive (AH5000) and 0.1 part of masterbatch (Kolan 342.42); the raw materials for preparing the release layer include 34.9 parts of ethylene-tetrafluoroethylene copolymer (melt index of 18g / 10min, 370℃ / 5kg).
[0072] The preparation method is as follows:
[0073] PA6, PA66 and a heat stabilizer are mixed and added to the hopper of a spiral plastic extruder A; an ethylene-tetrafluoroethylene copolymer, an adhesive and a masterbatch are mixed and added to the hopper of a spiral plastic extruder B; and the ethylene-tetrafluoroethylene copolymer is added to the hopper of a spiral plastic extruder C. After being plasticized and melted by the spiral plastic extruders A, B and C, the molten raw materials are transported to the extruder die head under the internal pressure of the barrel of the spiral plastic extruder and the forward thrust of the screw thereof to obtain the vacuum bag film.
[0074] The screw temperatures of the A screw plastic extruder, the B screw plastic extruder and the C screw plastic extruder are 270°C, the speed of the A screw plastic extruder is 35rpm, the speed of the B screw plastic extruder is 30rpm; the speed of the C screw plastic extruder is 35rpm, the temperature of the die head of the three-layer extruder is 280°C, and the pulling speed is 2m / min.
[0075] Example 6
[0076] This embodiment provides a vacuum bag film and a preparation method thereof. The vacuum bag film has a thickness of 150 μm and includes an isolation layer, a functional layer and a release layer stacked in sequence. The thickness of the isolation layer accounts for 37%, the thickness of the functional layer accounts for 43%, and the thickness of the release layer accounts for 20%.
[0077] The raw materials for preparing the isolation layer include 16 parts of PA6 (melt index of 10g / 10min, 190℃ / 2.16kg), 16 parts of PA66 (melt index of 10g / 10min, 190℃ / 2.16kg) and 5 parts of thermal stabilizer (copper iodide); the raw materials for preparing the functional layer include 23 parts of ethylene-tetrafluoroethylene copolymer (melt index of 18g / 10min, 370℃ / 5kg) and 20 parts of adhesive (AH5000); the raw materials for preparing the release layer include 20 parts of ethylene-tetrafluoroethylene copolymer (melt index of 18g / 10min, 370℃ / 5kg).
[0078] The preparation method is as follows:
[0079] PA6, PA66 and a heat stabilizer are mixed and added to the hopper of a spiral plastic extruder A, an ethylene-tetrafluoroethylene copolymer and an adhesive are mixed and added to the hopper of a spiral plastic extruder B, and the ethylene-tetrafluoroethylene copolymer is added to the hopper of a spiral plastic extruder C. After being plasticized and melted by the spiral plastic extruders A, B and C, the molten raw materials are transported to the extruder die head under the internal pressure of the barrel of the spiral plastic extruder and the forward thrust of the screw to obtain the vacuum bag film.
[0080] The screw temperatures of the A screw plastic extruder, the B screw plastic extruder and the C screw plastic extruder are 270°C, the speed of the A screw plastic extruder is 37rpm, the speed of the B screw plastic extruder is 43rpm; the speed of the C screw plastic extruder is 20rpm, the temperature of the die head of the three-layer extruder is 280°C, and the pulling speed is 2m / min.
[0081] Comparative Example 1
[0082] This comparative example provides a vacuum bag film and a preparation method thereof. The only difference between the comparative example and Example 1 is that the raw materials for preparing the isolation layer do not include PA66, the mass fraction of PA6 is 26 parts, and the other raw materials, amounts and preparation methods are the same as those in Example 1.
[0083] Comparative Example 2
[0084] This comparative example provides a vacuum bag film and a preparation method thereof. The only difference between the comparative example and Example 1 is that the raw materials for preparing the isolation layer do not include PA6, and the mass fraction of PA66 is 26 parts. Other raw materials, amounts and preparation methods are the same as those in Example 1.
[0085] Comparative Example 3
[0086] This comparative example provides a vacuum bag film and a preparation method thereof. The only difference between it and Example 1 is that the raw materials for preparing the functional layer do not include ethylene-tetrafluoroethylene copolymer, the mass fraction of the adhesive is 39 parts, and the other raw materials, amounts and preparation methods are the same as those in Example 1.
[0087] Comparative Example 4
[0088] This comparative example provides a vacuum bag film and a preparation method thereof. The only difference between it and Example 1 is that the adhesive in the preparation raw materials of the functional layer is replaced by nylon adhesive CT2018 of the same mass, and the other raw materials, amounts and preparation methods are the same as those in Example 1.
[0089] Comparative Example 5
[0090] This comparative example provides a vacuum bag film and a preparation method thereof. The vacuum bag film has a thickness of 60 μm and is a single-layer structure.
[0091] The raw materials for preparing the isolation layer include 13 parts of PA6, 13 parts of PA66, 4 parts of heat stabilizer (copper iodide), 25 parts of adhesive (AH5000), 1 part of masterbatch (Kolan 342.42) and 44 parts of ethylene-tetrafluoroethylene copolymer.
[0092] The preparation method is as follows:
[0093] PA6, PA66, heat stabilizer, adhesive, masterbatch and ethylene-tetrafluoroethylene copolymer are added to the hopper of a screw plastic extruder, plasticized and melted by the screw plastic extruder, and under the action of the internal pressure of the barrel of the screw plastic extruder and the forward thrust of the screw, the molten raw materials are transported to the die head of the single-layer film blowing machine, and are blown to obtain the single-layer vacuum bag film.
[0094] The screw temperature of the screw plastic extruder is 270° C., the speed of screw plastic extruder A is 40 rpm, the temperature of the die head of the three-layer film blowing machine is 285° C., the blow-up ratio is 1.5, and the curling speed is 7 m / min.
[0095] The vacuum bag films provided in the examples and comparative examples were subjected to the following performance tests:
[0096] (1) Tensile strength and elastic modulus: Tensile strength and elastic modulus tests were performed according to GB / T 1040.3-2006.
[0097] (2) Peel strength: Peel strength test was performed according to GB / T 8808-1988.
[0098] (3) Temperature resistance and barrier property test: The vacuum bag films provided in the examples and comparative examples are used as vacuum auxiliary materials for composite material production tests. The test is a hot press vacuum tank test at a temperature of 230°C, a pressure of 0.6 MPa, and a time of 6 hours. The temperature resistance test is performed to observe whether the vacuum degree is less than -0.7 MPa. If it is less than -0.7 MPa, the temperature resistance and barrier property are good.
[0099] (4) Release property: If the vacuum bag film can be easily separated from the upper and lower surfaces of the workpiece, the release performance is good.
[0100] The test results are shown in Table 1.
[0101] Table 1
[0102] In Table 1, “MD direction” means the mechanical stretching direction parallel to the vacuum bag film during preparation; “TD direction” means the mechanical stretching direction perpendicular to the vacuum bag film during preparation; and “ / ” means that the test was not performed.
[0103] According to the test results in Table 1, the vacuum bag film provided in the present application has the characteristics of single-sided release, high temperature resistance, easy demoulding, and good barrier properties. It can be seen from Examples 1 to 6 that the tensile strength of the vacuum bag film in the MD direction is 60-67 MPa, the elongation at break is 350-380%, the elastic modulus is 600-700 MPa, and the peel strength is 28-43 KN / m; the tensile strength in the TD direction is 55-60 MPa, the elongation at break is 400-440%, the elastic modulus is 500-650 MPa, and the peel strength is 30-39 KN / m; the heat resistance temperature is 230°C, and it has good release properties.
[0104] Compared with Example 1, if the raw materials for preparing the isolation layer do not include PA66 and the mass fraction of PA6 is 40 parts (Comparative Example 1), the vacuum degree increases, and the temperature resistance and barrier properties decrease.
[0105] Compared with Example 1, if the raw materials for preparing the isolation layer do not include PA6 and the mass fraction of PA66 is 40 parts (Comparative Example 2), the tensile strength is slightly reduced and holes are easily generated at the fold tips.
[0106] Compared with Example 1, if the raw materials for preparing the functional layer do not include ethylene-tetrafluoroethylene copolymer and the mass fraction of the adhesive is 55 parts (Comparative Example 3), the interlayer peel strength is low, the interlayer adhesion is low, and delamination is easy.
[0107] Compared with Example 1, if the adhesive in the raw materials for preparing the functional layer is replaced with nylon adhesive CT2018 of the same mass (Comparative Example 4), the peel strength between the layers is low, the interlayer adhesion is low, and delamination is easy.
[0108] Compared with Example 1, if the vacuum bag film is a single-layer structure, and other preparation raw materials and amounts are the same as Example 1 (Comparative Example 5), the vacuum degree of the product is -0.03Mpa, which is greater than -0.7Mpa, the temperature resistance and barrier properties are reduced, and the release performance is poor.
[0109] The applicant declares that while the above-mentioned embodiments are used to illustrate the process of the present application, the present application is not limited to the above-mentioned process steps, which does not mean that the present application must rely on the above-mentioned process steps in order to be implemented. Those skilled in the art should understand that any improvements to the present application, equivalent replacements for the raw materials used in the present application, addition of auxiliary components, and selection of specific methods, etc., fall within the scope of protection and disclosure of the present application.
Claims
1. A vacuum bag film, comprising an isolation layer, a functional layer and a release layer stacked in sequence; The raw materials for preparing the isolation layer include PA6 and PA66, the raw materials for preparing the functional layer include ethylene-tetrafluoroethylene copolymer and adhesive, and the raw materials for preparing the release layer include ethylene-tetrafluoroethylene copolymer.
2. The vacuum bag film according to claim 1, wherein: The melt index of the PA6 and PA66 is independently 3-10 g / 10 min.
3. The vacuum bag film according to claim 1 or 2, wherein: The raw materials for preparing the isolation layer also include a heat stabilizer.
4. The vacuum bag film according to claim 3, wherein: The heat stabilizer includes a copper salt heat stabilizer; Optionally, the thermal stabilizer comprises copper iodide.
5. The vacuum bag film according to any one of claims 1 to 4, wherein: The melt index of the ethylene-tetrafluoroethylene copolymer is 5-20 g / 10 min; Optionally, the adhesive comprises a functional bonding fluororesin; Optionally, the functional adhesive fluororesin has a melt index of 15-30 g / 10 min.
6. The vacuum bag film according to any one of claims 1 to 5, wherein: The raw materials for preparing the functional layer also include masterbatches.
7. The vacuum bag film according to any one of claims 1 to 6, wherein: Based on 100 parts of the total weight of the raw materials for preparing the vacuum bag film, the raw materials for preparing the isolation layer include the following components in parts by weight: 10-55 parts of PA6, 10-30 parts of PA66 and 0-5 parts of a heat stabilizer; Optionally, the raw materials for preparing the functional layer include the following components in parts by weight: 10-30 parts of ethylene-tetrafluoroethylene copolymer, 10-30 parts of adhesive and 0.1-2 parts of masterbatch; Optionally, the raw materials for preparing the release layer include the following components in parts by weight: 20-35 parts of ethylene-tetrafluoroethylene copolymer.
8. The vacuum bag film according to any one of claims 1 to 7, wherein: The thickness of the vacuum bag film is 50-300 μm.
9. The vacuum bag film according to any one of claims 1 to 8, wherein: Taking the total thickness of the vacuum bag film as 100%, the thickness of the isolation layer accounts for 20-35%, the thickness of the functional layer accounts for 30-60%, and the thickness of the release layer accounts for 20-35%.
10. The method for preparing a vacuum bag film according to any one of claims 1 to 9, wherein: The preparation method comprises the following steps: mixing and extruding PA6 and PA66 to obtain an isolation layer, mixing and extruding an ethylene-tetrafluoroethylene copolymer and an adhesive to obtain a functional layer, extruding the ethylene-tetrafluoroethylene copolymer to obtain a release layer, and co-extruding or inflation molding the isolation layer, the functional layer and the release layer stacked in sequence to obtain the vacuum bag film.
11. The method for preparing a vacuum bag film according to claim 10, wherein: The preparation method comprises the following steps: mixing PA6, PA66 and a heat stabilizer and adding them to the hopper of an extruder A, mixing ethylene-tetrafluoroethylene copolymer, an adhesive and a masterbatch and adding them to the hopper of an extruder B, adding ethylene-tetrafluoroethylene copolymer to the hopper of an extruder C, sequentially stacking and extruding the extruders A, B and C to a die head of a three-layer extruder or a film blowing machine, and co-extruding or inflation molding to obtain the vacuum bag film; Optionally, the vacuum bag film prepared by blow molding has a thickness of 50-150 μm; Optionally, the vacuum bag film prepared by extrusion molding has a thickness of 150-300 μm.
12. A vacuum bag made from the vacuum bag film according to any one of claims 1 to 9.
Citation Information
Patent Citations
Vacuum bag film with double-sided release function and preparation method thereof
CN110481128A
Functional multi-layer co-extruded fluororesin composite film and preparation method thereof
CN114274626A
Vacuum bag film and preparation method and application thereof
CN116533616A
Multifunctional vacuum film
DE102016124718A1
Release film
JP2008183738A
Cited By
Vacuum bag film and preparation method thereof
CN120424495A
Vacuum bag film and preparation method
CN120424495B