Ice phobic coating compositions with robust Anti-icing and de-icing properties
A two-phase ice-phobic coating with crosslinked soft particles and a hydrophilic gel phase effectively addresses the challenge of simultaneous anti-icing and de-icing, providing durable and cost-effective performance over multiple freezing cycles by delaying frost formation and reducing ice adhesion stress.
Patent Information
- Application Number
- PCT/IB2024/055519
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-09
- Filing Date
- 2024-06-06
- Publication Date
- 2024-12-12
AI Technical Summary
Current ice-phobic coatings fail to simultaneously provide effective anti-icing and de-icing properties over multiple freezing cycles, with existing solutions either being durable but not cost-effective or vice versa, and often losing effectiveness due to ice damage or removal of infused materials.
A two-phase ice-phobic coating composition featuring crosslinked soft particles swollen with a solvent that depresses the freezing point, dispersed in an elastomeric higher modulus phase, where the hydrophilic gel phase encapsulates freezing point depressants like DMSO or ethylene glycol, ensuring slow release and mechanical stability.
The coating significantly delays frost formation and reduces ice adhesion stress, maintaining performance for numerous frosting cycles with improved durability and cost-effectiveness compared to existing technologies.
Smart Images

Figure IMGF000020_0001 
Figure IMGF000020_0002 
Figure IMGF000021_0001
Abstract
Description
[0001] ICE PHOBIC COATING COMPOSITIONS WITH ROBUST ANTI-ICING AND DE-ICING PROPERTIES
[0002] FIELD OF THE INVENTION:
[0003] The present invention relates to ice-phobic coatings that are simultaneously anti- icing and deicing that retain their performance over multiple freezing cycles. The present invention more particularly relates to ice-phobic coatings comprising hydrophilic phase with a freezing point depressant in gel form, dispersed in hydrophobic phase. The said coatings are effective for anti-icing and de-icing and are durable (over several frosting cycles) and cost-effective.
[0004] BACKGROUND OF THE INVENTION:
[0005] It is of interest to prevent the formation of ice on (anti-icing) and to increase ease of ice removal from (de-icing) a variety of surfaces. This is of enormous practical interest - for example, ice formation on aircraft necessitates time-consuming and expensive de-icing before the plane can be operated. Similarly, the ice deposition on power lines in cold regions can result in power outages. Approaches for anti- icing and de-icing include passive solutions, such as coatings, as well as active solutions, such as example, heating power lines to prevent ice formation and accumulation or mechanical methods for removal of ice or, spraying with chemicals to melt and remove ice accretion. Given the importance of this problem to a wide variety of areas, there is continuing interest in developing cost-effective and long-lasting anti-icing and de-icing technologies.
[0006] From a use perspective, it is technologically attractive to consider passive coatings. These should ideally exhibit both anti-icing and de-icing properties and also be durable / long lasting over many cycles of frosting. Recently, the use of superhydrophobic surfaces or liquid infused slippery surfaces for icephobicity has been extensively researched. Superhydrophobic surfaces are those where the contact angle of a drop of water placed on the surface exceeds 150°. Such surfaces are created by generating roughness at multiple length scales (micron and nanometer scales) and by rendering the surface hydrophobic (for example, using an organosilane coating). However, such surfaces have been demonstrated to be compromised by frost formation. Further, such surfaces are not durable since the formation of ice damages the surface, altering the roughness. Liquid-infused slippery surfaces have been proposed as effective ice-phobic surfaces. However, while these are effective for anti-icing, successive freezing cycles result in the removal of the low surface energy liquids that are infused into the surface, rendering them ineffective. Anti-icing surfaces that use freezing point depressants as chemical coatings also suffer from loss of effectiveness as these agents are removed over freezing cycles. Also, such coatings are not effective in de-icing. Researchers have also proposed the use of stress-localized surfaces for de-icing. Here, a low modulus coating is applied on a surface and affords easy removal of deposited ice. However, as such coatings are not mechanically robust, a blend morphology is employed with a continuous matrix of a stiffer and tougher material, into which a majority phase of the low modulus material is embedded. While such materials show robust de-icing, they are entirely ineffective as anti- icing materials. Therefore, the development of coatings that are effective for anti- icing and de-icing and that are durable (mechanically and over several frosting cycles) as well as cost-effective, remains a very challenging and important problem.
[0007] ES2677444B1 teaches a use of phase change material to slow the formation of ice or produce de-icing in wind turbines. This invention focuses on preventing ice formation on the surface of wind turbines by use of a phase change material as a coating. Coatings based on such phase change materials are not necessarily freezing point depressants and this does not teach the gelation of such phase change materials. Whereas the present invention relates to a general icephobic coating, which not only prevents or delays ice formation but also facilitates easy ice removal once it is formed. US10167413B2 describes the formulation of an icephobic coating consisting of an elastomer, filler particles, and a cryoprotectant. Here, the elastomer is added to provide mechanical durability to the coating, the filler nanoparticles provide erosion resistance, and the cryoprotectant delays the ice formation on these coatings.
[0008] EP3115421B1 teaches an anti-icing coating containing an anti-icing agent reservoir embedded in a UV-curable matrix material. The matrix phase used in this invention is photopolymerizable or cured using UV radiation.
[0009] US6702953B2 teaches a coating which includes a glassy matrix formed by crosslinking a mixture of a functionally-terminated silicone and an alkoxyfunctionalized siloxane to provide an interpenetrating polymer network of glass and silicone; at least two materials capable of microphase separation, at least one of which is graftable to the glassy matrix; and a freezing point depression agent.
[0010] Therefore there is a need to develop passive ice-phobic coatings that are simultaneously anti-icing and deicing that retain their performance over multiple freezing cycles.
[0011] The present inventors have developed coating composition comprising crosslinked soft particles swollen with a solvent that depresses the freezing point of ice and dispersed in an elastomeric higher modulus phase possess anti-icing and de-icing properties. A critical aspect of the present invention is the use of crosslinked soft particles that allow slow release of the small molecule freezing point depressant, and the dispersion of a high volume fraction of these hydrophilic soft particles in a hydrophobic crosslinkable medium.
[0012] The present inventors have found that separately formulating the DMSO or ethylene glycol phase as a gel and dispersing these gel particles in the incompatible hydrophobic matrix followed by adjusting the modulus of the gel phase and its volume fraction ensures that the matrix exhibits de-icing properties so that anti-icing and de-icing properties are observed over many repeated cycles of frosting.
[0013] In the present invention, tough matrix phase used in the coating is thermally cured, preferably at room temperature, and the organogel phase, which encapsulates the freezing point depressant, is crosslinked using a crosslinker such as glutaraldehyde, oligoethylene glycol diglycidyl ether, or N-hydroxy succinimide esters. Preferably glutaraldehyde.
[0014] The present is focused on a two phase structure with a curable hydrophobic polymer matrix phase in which water-soluble and hygroscopic freezing point depressants such as small molecule Triethylene glycol, Diethylene Glycol, Dimethyl Acetamide (DMAc), Dimethyl Formamide (DMF), Acetonitrile, dimethyl sulphoxide DMSO or ethylene glycol are embedded as gelled particles.
[0015] It is particularly important that the freezing point depressant is in a gel form. The present invention provide data to show that when the DMSO is not gelled, then the anti-icing effect is observed only for a couple of cycles of frosting. Therefore, a key enabling feature of the present invention is to separately formulate the DMSO or ethylene glycol phase as a gel and to disperse these gel particles in the incompatible hydrophobic matrix. Further, there is a need to adjust the modulus of the gel phase and its volume fraction to ensure that the matrix exhibits de-icing properties. In particular, anti-icing and de-icing properties are observed over many repeated cycles of frosting. Therefore the present invention provide significant improvement over the prior arts coatings.
[0016] OBJECTS OF THE INVENTION:
[0017] It is an object of the present invention to provide an ice-phobic coatings composition that are simultaneously anti-icing and deicing that retain their performance over multiple freezing cycles. It is another object of the present invention to provide a coating composition comprising crosslinked soft particles that allow slow release of the small molecule freezing point depressant, and the dispersion of a high volume fraction of these hydrophilic soft particles in a gel form into a hydrophobic crosslinkable medium.
[0018] It is another object of the present invention to provide a coating composition that comprises crosslinked soft particles swollen with a solvent that depresses the freezing point of ice and is dispersed in an elastomeric higher modulus phase.
[0019] It is another object of the present invention to provide a blended coating that comprises a majority included phase that slowly releases a freezing point depressant (for example, Triethylene glycol, Diethylene Glycol, Dimethyl Acetamide (DMAc), Dimethyl Formamide (DMF), Acetonitrile, dimethyl sulphoxide, DMSO or ethylene glycol, EG) and simultaneously decreases the modulus. The minority matrix phase provides mechanical stability to the coating.
[0020] SUMMARY OF THE INVENTION:
[0021] According to an aspect of the present invention there is provided an ice-phobic coating composition comprising: i. Hydrophilic phase comprising organogel phase encapsulating the freezing point depressant; and ii. Hydrophobic phase.
[0022] According to another aspect of the present invention there is provided a process for the preparation of ice-phobic coating composition comprising the steps of: i. preparing hydrophobic phase containing silicone elastomer; ii preparing hydrophilic phase comprising organogel phase encapsulating hygroscopic freezing point depressant; wherein a crosslinker is added in step (i) or (ii); iii. adding hydrophilic phase of step (ii) to the hydrophobic phase of step (i) to obtain the ice-phobic coating; iv. curing the obtained ice-phobic coating of step (iii) under UV irradiation or room temperature.
[0023] According to yet another aspect of the present invention there is provided a process for the preparation of gel based ice-phobic coating composition comprising the steps of: i. preparing hydrophobic phase containing silicone elastomer; ii. preparing hydrophilic phase comprising organogel phase encapsulating hygroscopic freezing point depressant in presence of crosslinker; iii. soaking hydrophilic phase of step (ii) in the benzophenone in solvent solution; iv. adding the benzophenone-soaked hydrophilic phase of step (iii) into the hydrophobic phase of step (i), to obtain the icephobic coating; v. curing the obtained ice-phobic coating of step (iv) under UV irradiation at room temperature.
[0024] According to another aspect of the present invention there is provided a process for the preparation of emulsion-based ice-phobic coating composition comprising the steps of: i. preparing hydrophobic phase containing silicone elastomer; ii. preparing hydrophilic phase comprising organogel phase encapsulating hygroscopic freezing point depressant; iii. adding the hydrophilic phase of step (ii) into the hydrophobic phase in step (i) in the presence of a surface-active agent and a crosslinker to the emulsion based icephobic coating; iv. curing the obtained icephobic coating in step (iii) at room temperature. BRIEF DESCRIPTION OF FIGURES:
[0025] Figure 1: Anti-icing performance of various coatings: G-ICE (present invention), E-ICE (present invention), SLS, SHS / SLIPS and aluminium.
[0026] Figure 2: Anti-icing Performance of Pure DMSO-gel (DG) under multiple freezethaw cycles.
[0027] Figure 3: (A) Anti-icing Performance of E-ICEwg coating under multiple freeze - thaw cycles. (B) Formation of cracks in the coating due to diffusion of DMSO while curing.
[0028] Figure 4: Anti-icing Performance of E-ICE coating developed in this invention under multiple freeze-thaw cycles.
[0029] Figure 5: Ice adhesion stress values for various surfaces with the number of icing cycles.
[0030] Figure 6: SEM Images of SHS before (A, C) and after (B, D) 10 icing cycles. (A, B) microscale roughness (100 um, x50 magnification), (C, D) Nanoscale roughness (100 nm, x30,000 magnification)
[0031] DETAILED DESCRIPTION OF THE INVENTION
[0032] The following description with reference to the accompanying drawings is provided to assist in a comprehensive understanding of exemplary embodiments of the invention. It includes various specific details to assist in that understanding but these are to be regarded as merely exemplary.
[0033] Accordingly, those of ordinary skill in the art will recognize that various changes and modifications of the embodiments described herein can be made without departing from the scope of the invention. In addition, descriptions of well-known functions and constructions are omitted for clarity and conciseness.
[0034] The terms and words used in the following description and claims are not limited to the bibliographical meanings, but, are merely used by the inventor to enable a clear and consistent understanding of the invention. Accordingly, it should be apparent to those skilled in the art that the following description of exemplary embodiments of the present invention are provided for illustration purpose only and not for the purpose of limiting the scope of the invention as defined by the appended claims and their equivalents.
[0035] It is to be understood that the singular forms “a,” “an,” and “the” include plural referents unless the context clearly dictates otherwise.
[0036] Features that are described and / or illustrated with respect to one embodiment may be used in the same way or in a similar way in one or more other embodiments and / or in combination with or instead of the features of the other embodiments.
[0037] It should be emphasized that the term “comprises / comprising” when used in this specification is taken to specify the presence of stated features, steps or components but does not preclude the presence or addition of one or more other features, steps, components or groups thereof.
[0038] The present invention relates to ice-phobic coatings that are simultaneously anti- icing and deicing that retain their performance over multiple freezing cycles. The present invention more particularly relates to ice-phobic coatings that are effective for anti-icing and de-icing and that are durable over several frosting cycles) and cost-effective.
[0039] The coating of the present invention provides an unprecedented combination of anti-icing, de-icing, and robust ability to retain performance over many cycles of frosting. It is capable of significantly delaying frost formation on a test aluminum substrate as well as decreasing the force required to shear off the ice that is formed on the surface.
[0040] The blended coating comprises a majority included phase that slowly releases a freezing point depressant (for example, dimethyl sulphoxide, DMSO or ethylene glycol, EG) and simultaneously decreases the modulus. The minority matrix phase provides mechanical stability to the coating.
[0041] In an embodiment of the present invention there is provided an ice-phobic coating composition comprises: i. Hydrophilic phase comprising organogel phase encapsulating the freezing point depressant; and ii. Hydrophobic phase.
[0042] In another embodiment of the present invention there is provided a process for the preparation of ice-phobic coating composition comprising the steps of: i. preparing hydrophobic phase containing silicone elastomer; ii preparing hydrophilic phase comprising organogel phase encapsulating hygroscopic freezing point depressant; wherein a crosslinker is added in step (i) or (ii); iii. adding hydrophilic phase of step (ii) to the hydrophobic phase of step (i) to obtain the ice-phobic coating; iv. curing the obtained ice-phobic coating of step (iii) under UV irradiation or room temperature.
[0043] In another embodiment of the present invention hydrophilic phase comprises crosslinked soft particles that allow slow release of the small molecule freezing point depressant.
[0044] In another embodiment of the present invention the crosslinked soft particles is swollen with a solvent. In preferred embodiment of the present invention there is provided as gel-based and emulsion-based coating composition.
[0045] In another embodiment of the present invention there is provided a process for the preparation of gel based ice-phobic coating composition comprising the steps of: i. preparing hydrophobic phase containing silicone elastomer; ii. preparing hydrophilic phase comprising organogel phase encapsulating hygroscopic freezing point depressant in presence of crosslinker; iii. soaking hydrophilic phase of step (ii) in the benzophenone in solvent solution iv. adding the benzophenone-soaked hydrophilic phase of step (iii) into the hydrophobic phase of step (i), to obtain the icephobic coating; v. curing the obtained ice-phobic coating of step (iv) under UV irradiation at room temperature.
[0046] In yet another embodiment of the present invention there is provided a process for the preparation of emulsion-based ice-phobic coating composition comprising the steps of: i. preparing hydrophobic phase containing silicone elastomer; ii. preparing hydrophilic phase comprising organogel phase encapsulating hygroscopic freezing point depressant; iii. adding the hydrophilic phase of step (ii) into the hydrophobic phase in step (i) in the presence of a surface-active agent and a crosslinker to the emulsion based icephobic coating; iv. curing the obtained icephobic coating in step (iii) at room temperature.
[0047] In another embodiment of the present invention hydrophobic phase is an elastomeric higher modulus phase. In another embodiment of the present invention the hydrophobic phase comprises of hydrophobic crosslinkable medium.
[0048] In another embodiment of the present invention the high volume fraction of hydrophilic crosslinked soft particles is dispersed in a hydrophobic crosslinkable medium.
[0049] In another embodiment of the present invention the freezing point depressant is selected from Triethylene glycol, Diethylene Glycol, Dimethyl Acetamide (DMAc), Dimethyl Formamide (DMF), Acetonitrile, dimethyl sulphoxide (DMSO) or ethylene glycol (EG). Preferably dimethyl sulphoxide (DMSO) or ethylene glycol.
[0050] In preferred embodiment of the present invention there is provided a coating comprising a low shear modulus organogel phase (G’ less than 10000 Pa, preferably between 100 Pa and 4000 Pa) containing a hygroscopic freezing point depressant in the form of a slow release gel, dispersed in a tough, high modulus hydrophobic phase.
[0051] The low modulus organogel phase is the majority phase with a volume fraction of greater than 50%, and less than 95%, while the continuous phase is t high modulus hydrophobic matrix.
[0052] In an embodiment the coating of the present invention comprises a tough modulus hydrophobic phase containing silicone elastomer cured thermally. The said coating comprising of a soft organogel gel phase encapsulating the hygroscopic freezing point depressant, which is crosslinked.
[0053] In an embodiment of the coating of the present invention, the gel of hydrophilic soft phase is crosslinked in situ in the hard silicone phase. In UV-initiated free radical curing, the gel phase is crosslinked before adding it to the silicone matrix.
[0054] In emulsion-based coating, the soft gel phase is crosslinked in situ with the silicone phase.
[0055] In an embodiment of the coating composition of the present invention, the silicone elastomer is dissolved in a solvent selected from xylene, n-hexane, toluene, Cyclohexane, or n-heptane. Preferably xylene and n-hexane.
[0056] In an embodiment, the coating composition of the present invention comprises gelling agent selected from gelatin, kappa carrageenan, chitosan, alginate, synthetic smectite clay (Laponite®), or synthetic block copolymers (Pluronic®).
[0057] In an embodiment the coating composition of the present invention comprises of crosslinkers / crosslinking agents selected from glutaraldehyde, oligoethylene glycol diglycidyl ether, or N-hydroxy succinimide esters.
[0058] In an embodiment the coating composition of the present invention comprises of surface active agent selected from sodium bis(2-ethylhexyl) sulfosuccinate (AOT), polysorbate, sorbitan monooleate, or sodium dodecyl sulphate. Preferably sodium bis(2-ethylhexyl) sulfosuccinate (AOT).
[0059] The coating of the present invention comprised of a hydrophobic tough phase and a hydrophilic soft phase, which are made compatible with each other using UV- initiated free-radical curing or using an emulsion-based system stabilized by surface active agents.
[0060] The coating of the present invention can be applied to various substrates, including metal substrates, such as aluminium. ANTI-ICING PERFORMANCE OF THE COATINGS
[0061] The frost formation on a surface was observed using a homemade setup. A Peltier module was used to cool the surface to -20°C while the atmosphere was at room temperature (28°C and 70% relative humidity). A microscopic camera (Dino lite) captured the frosting phenomena on the surfaces. The prepared coating was tested and compared against a superhydrophobic coating (SHS), slippery liquid infused surface (SLIPS), stress localized surface (SLS), and an uncoated aluminium surface. The area covered by the frost formed was qualitatively observed over some time.
[0062] The coating of the present invention outperforms all other surfaces, as shown in Fig 1. Both uncoated aluminium and stress localized surface (SLS) are frosted completely within 5 mins, whereas the superhydrophobic surface and SLIPS can delay the frost formation for 12 and 20 minutes, respectively. The presence of air pockets in the case of SHS and lubricant in the case of SLIPS provides thermal resistance and delays the frost formation, whereas in the case of hydrophilic aluminium, absence of such entities leads to shorter frosting times.
[0063] The better performance of SLIPS in comparison with SHS is due to the smooth surface offered by SLIPS, which has significantly fewer heterogeneous sites than SHS, which increases the energy barrier for heterogenous nucleation on SLIPS (Kim et al. 2012 (https: / / doi.org / 10.1021 / nn302310q). Whereas in the case of SHS, the presence of heterogeneities results in a greater number of pinning sites, which further aids the heterogeneous nucleation of frost. As shown in Fig 1, the coatings of the present invention, both the gel-based (G-ICE) and emulsion-based (E-ICE), perform significantly better than their counterparts, preventing frost formation for more than 90 minutes.
[0064] The robustness of this anti-icing coating is tested by performing repeated frosting runs of 1 hour each at the conditions mentioned above. In this test, the coating prepared in this invention was compared with a pure DMSO-gel-coated aluminium surface (Comparative example 4) and a coating prepared without using the gelling agent (Comparative example 5). The pure DMSO-based gel showed superior anti-icing performance than the coating of the present invention initially, but the durability of the coating was limited. When the frosting experiment was repeated several times, the efficacy decreased dramatically after even just a single cycle, as shown in Fig 2.
[0065] Similarly, the coating E-ICEwg was excellent in preventing frost formation in the first cycle; however, the whole surface got covered up in frost in the second cycle just after 20 mins, as shown in Fig 3 (A). The rapid diffusion of DMSO out of the coating occurs even during the curing period, which is evident from the cracks formed in the coating (yellow markings), as shown in Fig 3 (B). In the case of coating of the present invention, the structural design results in controlled diffusion of the freezing point depressant without affecting the integrity of the coating, which leads to highly robust performance. The coating of the present invention can withstand more repeated cycles of frosting, providing excellent anti- icing performance even under the extremely harsh conditions tested, as shown in Fig 4.
[0066] DE-ICING PERFORMANCE OF THE COATINGS
[0067] De-icing performance of the coating is measured in terms of ice adhesion stress, which is defined as the force per unit area required to remove the block of ice frozen on the surface of the coating. Ice adhesion is measured using a self-made experimental setup, as shown in Fig 2.
[0068] A load cell is attached to the X-axis moving arm of the 3D printer, and it is connected to the Arduino microcontroller board. The load sensor is calibrated using known weights before performing the stress measurement experiments. A plastic cuvette is filled with water and placed upside down onto the substrate. The substrate is cooled down to -20°C using the Peltier module. After the water inside the cuvette is frozen completely, the Y-axis arm of the 3D printer is moved at a speed of 1 mm / s. The force required to detach the cuvette of ice completely is measured using the load cell. This experiment is repeated 3 times, and the average of the force values is taken. Finally, the force obtained is divided by the surface area of the cuvette to get the ice adhesion stress. The above experiment was performed on SHS, SLIPS, SLS, uncoated aluminium, and an aluminium surface coated with coatings (G-ICE and E-ICE) of the present invention. The durability of the surfaces with icing cycles is tested by performing the above experiment repeatedly for 10 cycles, and the ice adhesion values are noted for each time and reported in Fig 5.
[0069] Fig 5 depicts the results of ice adhesion stress analysis. Since there are no standard techniques to find the Ice adhesion stress values (IAS), different ways of measurement may lead to different absolute values of IAS (Dhyani et al. 2022 (https: / / doi.org / 10.1016Zj.matt.2022.04.012)). Hence in this experiment, more prominence is given to relative values of adhesion stress among the different coatings tested rather than the absolute IAS values on each coating. The above figure shows that all the surfaces have a comparable value of IAS initially. However, as the number of cycles increases, the IAS values increase for SHS and SLIPS, indicating the poor durability of these coatings. Whereas, in the case of stress localized surface (SLS) and the coating in this invention, the IAS values do not vary much, with the number of cycles indicating better coating durability. However, we note that the stress-localized surface showed poor anti-icing performance (as shown in Fig 1).
[0070] The main reason for the short durability of SHS is that, under highly humid conditions, condensation occurs in the microscale roughness. This results in the penetration of water droplets into the asperities of the superhydrophobic surfaces, thereby increasing the liquid to the solid contact area. Also, once frozen, these condensed water molecules expand to form ice which exerts stress on these asperities and ultimately leads to the permanent destruction of the protrusions. Softening or de-roughening of the surfaces increases the ice adhesion stress. Fig 6 depicts the decrease in the roughness of SHS in the microscale and the complete absence of roughness in the nanoscale after the icing cycles.
[0071] The loss of icephobicity in the case of SLIPS is due to the gradual depletion of the lubricant layer from the surface. The formation of a ridge occurs when a water droplet is in contact with a SLIPS surface. A four-phase contact line is formed between the water droplet, the lubricant, the air, and the textured solid. Frosting nucleates the formation of nano icicles on the surface of condensed water and ice droplets. Due to the positive difference in the surface tension of the ice-solid interface and lubricant-solid interface, the lubricant migrates into this nano-icicle from the lubricant-water ridge through capillary action, leaving the solid surface open for direct water contact.
[0072] As elucidated by Chaudhury et al. in their work (Chaudhury and Kim 2007 (https: / / doi.org / 10.1140 / epje / i2007-10171-x), the critical adhesive stress on an elastomeric coating is directly proportional to the material's shear modulus. Hence, as we reduce the value of the coating shear modulus, the stress required for adhesive fracture also decreases. However, a very low value of shear modulus can drastically decrease the mechanical durability of the surface, and the surface is susceptible to excessive mechanical abrasion and wear. In stress-localized surfaces, this conundrum is solved by introducing a two-coating system comprising of a rigid minority phase and a soft gel majority phase.
[0073] Stress-localized surfaces (SLS) induce adhesive fracture by creating artificial stress localization on specific points on the surface. Ice is sheared off the SLS easily due to the interfacial cavitations that develop cracks and propagate them through the ice-solid interface when a force is applied slightly above the interface.
[0074] Through extensive experimentation, the inventors of the present invention have designed a coating where the low-modulus elastomeric phase is an organogel. This organogel contributes not only to the de-icing performance as in the case of SLS but also helps in achieving excellent anti-icing performance. Similar to SLS, the coating prepared in this invention also comprises a soft gel phase and a rigid matrix phase. Unlike the organogel of PDMS prepared for SLS, the soft gel, in this case, is prepared using a gelling agent / substance and a freezing point depressant such as DMSO. This achieves the objective of reducing the ice adhesion stress on the coating. From Fig 5, it is clear that the ice adhesion stress values of coating (G-ICE) of the present invention are comparable to the SLS coating. Even after 10 cycles of frosting, the performance of this coating is still significantly better than the uncoated aluminium, which has an IAS of around 1000 kPa. The other coating developed in the present invention (E-ICE) performs even better than G-ICE, as seen in Fig 5. It shows an IAS reduction of almost 99% (~10 kPa) compared to the uncoated aluminium substrate. Like G-ICE and SLS, it can maintain the de-icing performance even after 10 freezing and thawing cycles.
[0075] EXAMPLES
[0076] The following examples are meant to illustrate the present invention. The examples are representative illustration and are not to be considered as limiting to the scope of the invention.
[0077] Comparative Example 1: Preparation of superhydrophobic surfaces (SHS)
[0078] As received Aluminium sheets were cut into 4cm x 4cm pieces and were cleaned with acetone, di-isopropyl alcohol, and water. The sheets were sonicated in each of these solvents for 10 mins each. After which, the sheets were sonicated with 1 wt.% sodium hydroxide (NaOH) solution for 10 mins. This process is essential to remove the oxides present on the aluminium surface. After cleaning, the aluminium sheets are etched with IM FeC13 at 25°C for 45 minutes to form the microscale roughness (Sharma et al. 2017 (https: / / doi.org / 10.1021 / acsnano.6b07471)). The nanoscale roughness is obtained by etching the sample in boiling water for 10 mins at 95°C. After creating hierarchical roughness, the samples are thoroughly dried to remove the traces of moisture. These dried samples are immersed in a solution of 200 pL 1H, 1H, 2H, 2H. perflourooctyltriethoxy silane in 25 mL of ethanol for 4 hrs. at ambient temperature conditions. The samples after the silanization are baked at 120°C for 45 mins to evaporate the residual solvent present on the surface.
[0079] Comparative Example 2: Preparation of Slippery Infused Porous surfaces (SLIPS):
[0080] The SLIPS surfaces are prepared from the superhydrophobic surfaces by infusing a lubricant into the porous surface. The SHS samples are fabricated as mentioned above, after which spin coating of silicone oil is performed on this surface at 2000 RPM for 60 secs. Then the samples are placed in an inclined position overnight to drain the excess lubricant present.
[0081] Comparative Example 3: Preparation of Stress localized Surfaces (SLS)
[0082] Stress-localized surfaces are prepared by mixing a hard, rigid elastomeric phase and soft organogel. The soft gel is prepared as follows, firstly, 5 mL of Sylgard 184 base and 0.5 mL of Sylgard 184 curing agent are mixed, then 50 mL of Xylene is added to the above mixture and stirred vigorously to obtain a homogenous solution. The mixture is cured at 100°C for 4 hrs. in a hot air oven. Thus, obtained soft gel is crushed in the presence of xylene to avoid aggregation of gel particles. These organogel particles, after filtering excess xylene, are added to an elastomeric solution (Room-Temperature- Vulcanizing (RTV-1) silicone) of pre-defined concentration. The viscosity of the mixture was adjusted using xylene solvent. The obtained solution was coated onto the aluminium substrates to get stress-localized surfaces.
[0083] Comparative Example 4: Preparation of DMSO-gel-based coating (DG)
[0084] A 30 mL solution of 8.3% w / v of gelling substance such as gelatin is prepared in a 90:10 v / v solution of DMSO and water by slight heating and vigorous stirring. lOOpL of the glutaraldehyde (GT A) crosslinker is added to the mixture, which is immediately coated onto the aluminium substrate. The coating is allowed to cure at room temperature for 2hrs. Comparative Example 5: Preparation of Emulsion based Icephobic coating without the gelating agent (E-ICEwg)
[0085] A coating comprised of two phases, in which a freezing point depressant (Phase II) is embedded into a tough matrix of an elastomer (Phase I). :
[0086] A 10 mL solution of 20% w / v of RTV-1 silicone in n-hexane is prepared by continuous stirring. Then a predetermined amount of sodium bis(2-ethylhexyl) sulfosuccinate (AOT) surfactant (% 4 w / v) is added to this solution, and the stirring is continued until a homogenous solution is obtained.
[0087] Preparation of the emulsion-based coating:
[0088] Phase II consisting of a freezing point depressant such as DMSO solution (without any gelling agent) is slowly added dropwise into the phase I solution in 70:30 v / v ratio. Care must be taken to avoid phase separation between the hydrophobic and hydrophilic phases. Hence, dropwise addition and vigorous stirring of the solution are critical to obtain a mini emulsion of phase II in phase I. The emulsion obtained is coated onto the aluminium substrate and cured at room temperature overnight.
[0089] Example 1: Preparation of ice-phobic coating of the present invention comprising gelled phase (G-ICE):
[0090] The prepared coating is comprised of two phases. Phase II (hydrophobic phase) is a rigid elastomeric material, whereas phase 211 (hydrophilic phase) is a soft gel that slowly releases the freezing point depressant. Preparation of each of these phases is as follows,
[0091] Preparation of Phase (Hydrophilic phase):
[0092] A 30 mL solution of 8.3% w / v of a gelling substance such as gelatin is prepared in a 90:10 v / v solution of DMSO and water by slight heating and vigorous stirring. lOOpL of the glutaraldehyde (GT A) crosslinker is added to the mixture, which is immediately transferred to a petri-dish and cured at room temperature. Thus, the obtained gel is used as the phase 2 material for the icephobic coating prepared.
[0093] Preparation of Phase (Hydrophobic phase):
[0094] A 15 mL solution of 20% w / v of room-temperature- vulcanizing silicone (RTV-1 silicone) and xylene is prepared by vigorous stirring. This solution is the phase 1 matrix used for the icephobic coating.
[0095] Preparation of the coating:
[0096] Hydrophilic phase II (soft gel) is added / soaked in to 20 mL of 10% w / v solution of benzophenone in ethanol. Then it is crushed into micron-sized particles using an ultra-blender. The particles are filtered from the benzophenone solution and added to the phase I solution in a 70:30 w / w ratio of phase II and phase I, respectively. After vigorous stirring, the coating is applied onto the aluminium substrate and cured overnight under UV irradiation.
[0097] Example 2: Preparation of novel emulsion-based coating described in this invention (E-ICE)
[0098] Similar to example 1, this coating also comprises a two-phase system with a hard rigid phase and a soft organogel phase. Unlike the previous example, this example has better and easy coating properties. In this coating, the gel is crosslinked in situ in the hard silicone phase and is stabilized using a surface-active agent such as AOT instead of the UV-radiated curing in the previous case. (Hydrophilic phase):
[0099] A 10 mL solution of 8.3 % w / v of gelating substance such as gelatin in a 50:50 (v / v) ethyleneEthylene glycol-water solution is prepared by slight heating and vigorous stirring. Preparation of Phase I:
[0100] A 10 mL solution of 20% w / v solution of RTV-1 silicone in n-hexane is prepared. . Then a predetermined amount of AOT surfactant (4 % w / v) is added to this solution, and the stirring is continued until a homogenous solution is obtained. A lOpL of glutaraldehyde solution is added as the crosslinker into this solution.
[0101] Preparation of the emulsion-based coating:
[0102] The phase II solution is added dropwise into the phase I solution in a 70:30 (v / v) ratio. Care must be taken to avoid phase separation between the hydrophobic and hydrophilic phases. Hence, dropwise addition and vigorous stirring of the solution are primal to obtain a mini emulsion of phase II in phase I. The emulsion obtained is coated onto the aluminium substrate and cured at room temperature overnight. During this period, both the rigid elastomer and soft gel phases are cured simultaneously, and we obtained a two-phase icephobic coating with excellent anti-icing and de-icing properties.
[0103] The coating of the present invention shows excellent anti-icing performance and can delay frosting for over 90 minutes at a surface temperature of -20°C, while the environment is maintained at room temperature conditions (28°C and 70% RH) and de-icing performance, with ice adhesion stress of less than 10% of uncoated aluminium substrate.
[0104] The coating of the present invention is robust in retaining the anti-icing performance for over 3 cycles of 1 hr. each under extremely harsh conditions (low temperature and high humidity ratio). The deicing performance of the coating is unchanged to within 10% even after 20 repeat cycles of frosting and thawing at - 20°C.
[0105] It is to be understood that the present invention is susceptible to modifications, changes and adaptations by those skilled in the art. Such modifications, changes, adaptations are intended to be within the scope of the present invention.
Claims
CLAIMS:
1. An ice-phobic coating composition comprising: i. Hydrophilic phase comprising organogel phase encapsulating the freezing point depressant; and ii. Hydrophobic phase.
2. The ice-phobic coating composition as claimed in claim 1, wherein in the hydrophilic phase (i), the freezing point depressant is encapsulated in a gel form.
3. The ice-phobic coating composition as claimed in claim 1, wherein the hydrophilic phase comprises organogel phase encapsulating a hygroscopic freezing point depressant in the form of a slow release gel dispersed in a tough, high modulus hydrophobic phase.
4. The ice-phobic coating composition as claimed in claim 1, wherein the organogel phase comprises gelling substance selected from gelatin, kappa carrageenan, chitosan, alginate, synthetic smectite clay, or synthetic block copolymers.
5. The ice-phobic coating composition as claimed in claim 1, wherein the organogel phase that encapsulates the hygroscopic freezing point depressant, is crosslinked using a crosslinker selected from glutaraldehyde, oligoethylene glycol diglycidyl ether or N -hydroxy succinimide esters.
6. The ice-phobic coating composition as claimed in claim 1, wherein the freezing point depressant is selected from Triethylene glycol, Diethylene Glycol, Dimethyl Acetamide (DMAc), Dimethyl Formamide (DMF), Acetonitrile, dimethyl sulphoxide (DMSO) or ethylene glycol (EG).
7. The ice-phobic coating composition as claimed in claim 1, wherein the hydrophobic phase comprises silicone elastomer.
8. The ice-phobic coating composition as claimed in claim 1, wherein the hydrophobic phase comprising silicone elastomer is cured thermally.
9. The ice-phobic coating composition as claimed in claim 1, wherein the organogel phase is the majority phase with a volume fraction of greater than 50%, and less than 95%, while the continuous phase is the hydrophobic phase.
10. The ice-phobic coating composition as claimed in claim 9, wherein the low shear modulus of organogel (G’) is in the range of 100 Pa to 10,000 Pa.
11. A process of preparation of ice-phobic coating composition comprising the steps of: i. preparing hydrophobic phase containing silicone elastomer; ii preparing hydrophilic phase comprising organogel phase encapsulating hygroscopic freezing point depressant; wherein a crosslinker is added in step (i) or (ii); iii. adding hydrophilic phase of step (ii) to the hydrophobic phase of step (i) to obtain the ice-phobic coating; iv. curing the obtained ice-phobic coating of step (iii) under UV irradiation or room temperature.
12. The process of preparation of ice-phobic coating composition as claimed in claim 11 wherein the hydrophobic phase further comprises a surface active agent selected from sodium bis(2-ethylhexyl) sulfosuccinate (AOT), polysorbate, sorbitan monooleate, or sodium dodecyl sulphate.
13. The ice-phobic coating composition as claimed in claim 1 is a gel -based or an emulsion-based coating.
14. A process for preparation of gel based ice-phobic coating composition comprising the steps of: i. preparing hydrophobic phase containing silicone elastomer; ii. preparing hydrophilic phase comprising organogel phase encapsulating hygroscopic freezing point depressant in presence of crosslinker; iii. soaking hydrophilic phase of step (ii) in the benzophenone in solvent solution; iv. adding the benzophenone-soaked hydrophilic phase of step (iii) into the hydrophobic phase of step (i), to obtain the icephobic coating; v. curing the obtained ice-phobic coating of step (iv) under UV irradiation at room temperature.
15. The process for the preparation of ice-phobic coating composition as claimed in claim 14, wherein step (i) comprises dissolving silicone elastomer in a solvent selected from xylene, n-hexane, toluene, cyclohexane, or n-heptane.
16. The process for the preparation of ice-phobic coating composition as claimed in claim 14, wherein in the benzophenone-soaked hydrophilic phase of step (iv) is crushed into micron-sized particles and dispersed in hydrophobic phase to obtain gel-based coating.
17. A process for the preparation of emulsion-based ice-phobic coating composition comprising the steps of: i. preparing hydrophobic phase containing silicone elastomer; ii. preparing hydrophilic phase comprising organogel phase encapsulating hygroscopic freezing point depressant;iii. adding the hydrophilic phase of step (ii) into the hydrophobic phase in step (i) in the presence of a surface-active agent and a crosslinker to the emulsion based icephobic coating; iv. curing the obtained icephobic coating in step (iii) at room temperature.
18. The process for the preparation of ice-phobic coating composition as claimed in claim 17, wherein step (i) comprises dissolving silicone elastomer in a solvent selected from xylene, n-hexane, toluene, alkanes, or aromatic solvents.
19. The process for the preparation of ice-phobic coating composition as claimed in claim 17, wherein step (i) further comprises adding surface active agents under stirring to obtain a homogeneous solution followed by addition of crosslinker solution to the hydrophobic phase.
20. The process for the preparation of ice-phobic coating composition as claimed in claim 17 wherein the surface active agent is selected from sodium bis(2- ethylhexyl) sulfo succinate (AOT), polysorbate, sorbitan monooleate or sodium docecyl sulphate.
Citation Information
Patent Citations
Durable icephobic surfaces
EP3289039A1
Transparent hydrophobic and icephobic compositions, coatings, and methods
US20210032477A1
Anti-icing composition
US6702953B2
Methods and compositions for inhibiting surface icing
WO2008137147A2
Cited By
Preparation method of cable box anti-condensation nano modified coating
CN120988553A