Coating structure, sheet-like product and its use.
Patent Information
- Application Number
- BR112022022695
- Authority / Receiving Office
- BR · BR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-06-17
- Filing Date
- 2021-06-14
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2041-06-14
AI Technical Summary
Existing coatings for packaging materials, particularly those used in food and consumable liquids, face challenges in providing effective grease barriers that are resistant to cracking and bending, while also being environmentally sustainable, recyclable, and free from petroleum-based chemicals.
A two-layer coating structure comprising a water-soluble cellulose derivative and a plasticizer, applied directly onto a substrate without intermediate layers, enhances grease barrier properties, reduces cracking, and ensures biodegradability and recyclability, using bio-based components from non-food sources.
The coating structure effectively prevents grease leakage, maintains flexibility, and is easily repulped, offering improved converting properties and environmental sustainability without the need for petroleum-based polymers.
Abstract
Description
[0001] The present invention relates to a coating structure, a sheet-like product, and its use in accordance with the preambles of the independent claims included.
[0002] Various coatings can be applied to the surface of paper or cardboard in order to improve its properties. Grease barrier properties are particularly important for paper and cardboard used in products for packaging purposes. Coatings applied to the surface of paper or cardboard must provide an effective barrier against leakage of the packaged items and / or protect the packaged items from contamination and / or contact with surroundings. Barrier requirements are especially stringent for packaging materials used for food and consumable liquids.
[0003] Coatings for packaging purposes must have good resistance to wrinkling and folding. The coating must not crack when the paper or cardboard is folded into a box or wrapped around the product. Cracking can diminish or even completely destroy the barrier properties of the coating.
[0004] Synthetic petroleum-based polymers or fluorine chemical compounds have been conventionally used in coating compositions to provide desired barrier properties with simultaneous crack resistance. For environmental reasons, it may be desirable to find effective alternatives to these petroleum-based chemical compounds. Alternatives should be sustainable and based on bio-based sources. Conventional bio-based components used in coating formulations, such as starch, often do not perform well in re Petition 870220103522, dated 08 / 11 / 2022, page 7 / 42 2 / 25 barrier coatings. They often make the coating brittle or stiff, leading to cracking of the coating during folding. Furthermore, the bio-based component should preferably originate from non-food chain sources, a requirement not met by starch and starch derivatives. Consequently, there is a need for new alternatives that can solve the problems currently encountered.
[0005] In addition, barrier coatings used for packaging must also meet recyclability requirements. Paper and cardboard packaging is ideally collected for recycling and repulp formation. Many traditional barrier coatings are problematic for repulp formation and / or require special process arrangements in repulp formation. Coatings applied to paper and cardboard must meet recycling requirements and, for example, they must not disrupt the repulp formation process.
[0006] One objective of this invention is to minimize or even possibly eliminate the disadvantages existing in the prior art.
[0007] Another objective of the present invention is to provide a coating structure and a sheet-like product that are based on renewable raw materials and that are readily biodegradable and / or re-pulped.
[0008] Yet another objective of the present invention is to provide a coating structure and a sheet-like product that provide good grease barrier properties.
[0009] Yet another objective of the present invention is to provide a barrier coating structure, which can be used to create a coating that withstands cracking when wrinkled and / or folded.
[0010] These objectives are achieved with the invention having the characteristics presented below in the characterization sections of the invention. Petition 870220103522, dated 08 / 11 / 2022, p. 8 / 42 3 / 25 Independent claims. Some preferred embodiments of the invention are presented in the dependent claims.
[0011] The embodiments mentioned in this text refer, where applicable, to all aspects of the invention, even if this is not always separately mentioned.
[0012] A typical coating structure according to the present invention for a sheet-like substrate comprising cellulosic and / or lignocellulosic fibers comprises at least a first coating layer and a second coating layer, wherein the second coating layer is disposed in direct contact with the first coating layer, and at least the first coating layer or the second coating layer is a barrier coating layer comprising
[0013] - at least one water-soluble cellulose derivative selected from alkyl celluloses, hydroxy alkyl alkyl celluloses, hydroxy alkyl cellulose and any mixtures thereof, and
[0014] - a plasticizer.
[0015] A typical use of a coating structure according to the present invention is to provide a grease barrier when applied over a sheet-like product comprising cellulosic and / or lignocellulosic fibers.
[0016] A typical sheet-like product according to the present invention comprises
[0017] - a substrate comprising cellulosic and / or lignocellulosic fibers, and having a first large surface and a second large surface, which are parallel to each other, and
[0018] - a coating structure according to the present invention applied at least to the first or second large surface of the substrate.
[0019] A typical use of a sheet-like product according Petition 870220103522, dated 08 / 11 / 2022, page 9 / 42 4 / 25 with the present invention is for the manufacture of a food service packaging.
[0020] It has now been surprisingly verified that a two-layer coating structure, comprising at least one barrier layer formed of a specific water-soluble cellulose derivative and a plasticizer, is capable of functioning effectively as a grease barrier, especially against liquid grease or oil, and sometimes even as a barrier to mineral oil. The use of the water-soluble cellulose derivative makes the coating structure easy for re-pulp formation and reduces the need for components from non-renewable sources. The water-soluble cellulose derivative is a bio-based component but originates from renewable non-food sources, which is advantageous. Furthermore, it has been verified that the simultaneous use of the specific water-soluble cellulose derivative and the plasticizer unexpectedly improves the properties of the coating structure, making it less sticky and reducing the risk of blockage.Also, the tendency for cracking of the coating structure is significantly reduced, which improves the conversion properties of the resulting coating structure.
[0021] The coating structure according to the present invention comprises at least a first coating layer and a second coating layer. The first coating layer is applied directly to the surface of a sheet-like substrate comprising cellulosic and / or lignocellulosic fibers. This means that the coating structure is preferably free of pre-coating and top coating layers and consists solely of the first coating layer and second coating layer, where the first coating layer is in contact with the substrate surface and the second coating layer forms the outer surface of the coating layer and Petition 870220103522, dated 08 / 11 / 2022, page 10 / 42 5 / 25 subsequently the outer surface of the substrate. In some embodiments, the surface of the sheet-like substrate may be surface-bonded, for example, with a layer of hydrophobic surface adhesive, prior to application of the first coating layer, but preferably the first coating layer is applied directly onto the surface of a sheet-like substrate that is free of any pre-existing treatment layers, such as surface adhesive layers. The sheet-like substrate may comprise an internal adhesive. The first coating layer and the second coating layer may be applied to the substrate surface using any conventional adhesive or surface coating techniques, or combinations thereof.For example, the first coating layer can be applied using a surface adhesive device, and the second coating layer can be applied using a coating device, such as a blade or stick coating device.
[0022] The second coating layer is placed in direct contact with the first coating layer, meaning that it is applied directly to the surface of the first coating layer, in immediate and intimate contact with it. The coating structure is thus free of any intermediate layers between the first coating layer and the second coating layer.
[0023] The coating structure may comprise two or more first coating layers and / or two or more second coating layers. Preferably, if the coating structure comprises a plurality of first coating layers and / or a plurality of second coating layers, the first coating layers are preferably chemically Petition 870220103522, dated 08 / 11 / 2022, page 11 / 42 6 / 25 identical to each other and the second coating layers are preferably chemically identical to each other. Chemically identical means that the coating layers are manufactured from the same components in identical quantities, i.e., coating layers are manufactured using identical coating formulation. The coating weight within a plurality of first coating layers and / or a plurality of second coating layers may vary.
[0024] According to a preferred embodiment, the first and second layers are identical to each other and both are barrier coating layers. The use of two identical coating layers can allow the use of lower coating weights per individual layer while achieving the desired barrier effect. Furthermore, the risk of coating defects can be minimized when the coating structure comprises two or more identical coating layers.
[0025] According to one embodiment, the first coating layer and the second coating layer are different from each other. For example, the first coating layer may comprise a different water-soluble cellulose derivative and / or plasticizer than the second coating layer. In this way, it is possible to tailor the properties of the coating structure to meet even very specific needs, for example, with regard to barrier properties to be obtained.
[0026] The coating weight of the first coating layer and the second coating layer can be freely chosen depending on the desired end use and desired barrier properties. According to one embodiment of the invention, the first coating layer can have a coating weight of 2-30 g / m2, preferably 3-20 g / m2, more preferably 5-15 g / m2, and the second Petition 870220103522, dated 08 / 11 / 2022, page 12 / 42 7 / 25 of the coating layer may have a coating weight of 0.520 g / m2, preferably 0.5-15 g / m2, more preferably 0.5-10 g / m2. Typically, the first coating layer may have a higher coating weight than the second coating layer.
[0027] The coating structure of the present invention comprises at least one barrier coating layer. This means that the coating structure comprises at least two coating layers, of which at least one is a barrier coating layer. At least the first coating layer or the second coating layer in the coating structure is a barrier coating layer. It is possible that the first coating layer is the barrier coating layer or that the second coating layer is the barrier coating layer according to the present invention. It is also possible that both the first coating layer and the second coating layer are barrier coating layers according to the present invention.The present invention provides possibilities for optimizing the barrier properties of the coating structure by selecting the number and location of barrier layers in the coating structure.
[0028] The barrier coating layer according to the present invention comprises at least one water-soluble cellulose derivative selected from the group consisting of alkyl celluloses, hydroxy alkyl celluloses, hydroxy alkyl celluloses and any mixtures thereof. The water-soluble cellulose derivative may preferably be selected from the group consisting of methyl cellulose, hydroxy methyl cellulose, hydroxy ethyl cellulose, hydroxy propyl cellulose, (hydroxy ethyl) methyl cellulose, and (hydroxy propyl) methyl cellulose and any mixtures thereof. Preferably the water-soluble cellulose derivative is methyl cellulose, (hydroxy propyl) methyl cellulose or hydroxy ethyl cellulose, plus Petition 870220103522, dated 08 / 11 / 2022, page 13 / 42 8 / 25 preferably hydroxyethyl cellulose. It has been observed that when one of the specified water-soluble cellulose derivatives is present in the barrier coating layer, the layer is more flexible and does not crack as easily in wrinkling or folding. Furthermore, the specified cellulose derivatives provide increased dry solids content to the coating formulation, making it easier to apply to the surface of the substrate to be coated and providing better film-forming properties.
[0029] In particular, the use of (hydroxypropyl) methyl cellulose can provide a coating that exhibits mineral oil barrier properties and may therefore also be suitable for technical applications.
[0030] The cellulose derivatives suitable for the present invention are soluble in water at least at room temperature (+21°C). In the present context, the term "water-soluble cellulose derivative" represents cellulose derivatives that dissolve in water without gel formation. An unsaturated (in water) solution of the water-soluble cellulose derivative at +21°C is free of solid particles and is filterable through a filter with 100 micron openings. Methyl cellulose and (hydroxypropyl) methyl cellulose become insoluble in hot water (about +75°C), but they are still suitable for use in the present invention and may even provide limited water barrier properties, especially against hot liquids, for the coating layer in addition to grease barrier properties.
[0031] The barrier coating layer comprising a water-soluble cellulose derivative, i.e., the first coating layer and / or the second coating layer, is preferably formed without the use of organic solvents. Typically, the barrier coating layer is formed using an aqueous solution. Petition 870220103522, dated 08 / 11 / 2022, page 14 / 42 9 / 25 sa of water-soluble cellulose derivative that is free of organic solvents.
[0032] The first coating layer and the second coating layer may both be barrier coating layers comprising water-soluble cellulose derivatives that are chemically identical. Alternatively, the first coating layer and the second coating layer may both be barrier coating layers wherein the first barrier coating layer comprises a first water-soluble cellulose derivative and the second barrier layer comprises a second water-soluble cellulose derivative. The first and second water-soluble cellulose derivatives are different from each other and selected from the group of alkyl celluloses, hydroxy alkyl celluloses, hydroxy alkyl celluloses and any mixtures thereof.
[0033] The barrier coating layer, that is, the first and / or second coating layer, may comprise water-soluble cellulose derivative in an amount of 50-99% by weight, preferably 60-97% by weight, more preferably 70-95% by weight or 80-95% by weight, calculated from the total solids content of the barrier coating layer. With the present invention it is possible to produce coating structures where the content of bio-based components is high while maintaining the essential barrier properties and crack resistance at least at an acceptable level.
[0034] In addition to the water-soluble cellulose derivative, the barrier coating layer comprises a plasticizer. The plasticizer is incorporated into the barrier coating layer between the water-soluble cellulose derivative chains, where it spaces them apart and controls their mobility within the barrier coating layer. The selected plasticizer is preferably suitable for food packaging purposes, meaning, for example, Petition 870220103522, dated 08 / 11 / 2022, page 15 / 42 10 / 25 example, phthalate esters are excluded. The plasticizer may be selected from a group comprising polyols, such as sorbitol, mannitol, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, or polyethylene glycol; fatty acids; monosaccharides, ethanolamine, triethanolamine; alkyl citrates, urea; lecithin and glycerol. According to a preferred embodiment, the plasticizer may be selected from sorbitol, polyethylene glycol, or glycerol. Frequently, the incorporation of a plasticizer into a barrier coating layer makes the barrier coating layer very sticky, which can easily lead to blockage problems. Now, it has been unexpectedly observed that the stickiness of the barrier coating layer comprising plasticizer is significantly decreased when the barrier coating layer comprises water-soluble cellulose derivative.This means that it is possible to obtain a coating layer where the blocking and cracking resistance properties can be balanced with flexibility in order to obtain a coating structure with optimal properties for the desired purpose.
[0035] The barrier coating layer may comprise plasticizer in an amount of 1-50% by weight, preferably 3-40% by weight, more preferably 5-30% by weight or 5-20% by weight, calculated from the total solids content of the barrier coating layer.
[0036] According to a preferred embodiment of the present invention, at least the barrier coating layer may still comprise inorganic pigment particles. The inorganic mineral pigment may be selected from kaolin, talc, calcium carbonate, or any mixture thereof, preferably calcium carbonate, such as ground calcium carbonate or precipitated calcium carbonate. The particle size D50 of the inorganic pigment particles Petition 870220103522, dated 08 / 11 / 2022, page 16 / 42 11 / 25 nico can be < 5 micrometers. According to one embodiment, the barrier coating layer may comprise inorganic mineral particles, where at least 45% of the inorganic mineral particles have a particle size < 2 micrometers. Addition of inorganic mineral pigment can further enhance the barrier properties obtained. It was unexpectedly observed that water-soluble cellulose derivatives increase the flexibility of the barrier coating layer in a way that allows incorporation of high quantities of inorganic pigment particles into the barrier coating layer. This can not only enhance the barrier properties but also make the coating structure more economical to produce.
[0037] The first coating layer and the second coating layer may both contain inorganic mineral particles, regardless of whether they are both barrier coating layers according to the present invention or not. The inorganic mineral particles, their type and / or quantity, in the first coating layer and the second coating layer may be the same or different. Preferably, the first coating layer and the second coating layer comprise identical inorganic mineral particles, even if their quantity may be different in the first and second coating layers.
[0038] According to a preferred embodiment, at least the second coating layer, which is directly applied over the first coating layer(s), may be a barrier coating layer comprising inorganic pigment particles, preferably calcium carbonate particles. In this case, the first coating layer may function as a sealant layer, which reduces or prevents the penetration of the barrier coating layer into the surface of the substrate to be coated. Petition 870220103522, dated 08 / 11 / 2022, p. 17 / 42 12 / 25
[0039] According to one embodiment of the present invention, the water-soluble cellulose derivative can be selected from alkyl celluloses, such as methyl cellulose, where the barrier coating layer can comprise inorganic pigment particles in an amount of 5-20% by weight, preferably 7-17% by weight, more preferably 7-15% by weight, calculated from the total solids content of the barrier coating layer. For example, the barrier coating layer may comprise 50-90% by weight, preferably 60-90% by weight, or 75-87% by weight of alkyl cellulose, such as methyl cellulose, 5-20% by weight, preferably 7-17% by weight or preferably 7-15% by weight of inorganic pigment particles, and 5-30% by weight, preferably 5-25% by weight or 5-20% by weight of plasticizer, calculated from the total dry solids content of the barrier coating layer, the total amount of components added to 100%.
[0040] According to another embodiment of the present invention, the water-soluble cellulose derivative is preferably selected from hydroxy alkyl celluloses or hydroxy alkyl alkyl celluloses, such as hydroxy ethyl cellulose or (hydroxy propyl) methyl cellulose, wherein the barrier coating layer may comprise inorganic pigment particles in an amount of 20-60% by weight, preferably 30-55% by weight, more preferably 40-50% by weight, calculated from the total dry solids content of the barrier coating layer.For example, the barrier coating layer may comprise 20-60% by weight, preferably 30-55% by weight or 40-50% by weight of hydroxy alkyl celluloses, such as hydroxy ethyl cellulose or (hydroxy propyl) methyl cellulose, 20-50% by weight, preferably 30-50% by weight or 30-50% by weight of inorganic pigment particles, and 5-30% by weight, preferably 10-30% by weight or 15-26% by weight of plasticizer, calculated from the total dry solids content of approx. Petition 870220103522, dated 08 / 11 / 2022, page 18 / 42 13 / 25 barrier coating layer, the total quantity of components added to 100%. The use of hydroxyalkyl cellulose or hydroxyalkyl alkyl cellulose allows the use of high levels of inorganic pigment particles in the barrier coating layer without deterioration of the coating layer properties, such as crack resistance.
[0041] Starch can increase the brittleness of the coating structure and reduce the resistance of coating structures to cracking. Therefore, the amount of starch in the coating structure according to the present invention is preferably minimized. More preferably, the first and second coating layers of the coating structure are starch-free.
[0042] According to one embodiment of the invention, the first coating layer of the coating structure may comprise carboxymethyl cellulose provided that the second coating layer is a barrier coating layer according to the present invention and free of carboxymethyl cellulose. According to another preferred embodiment of the invention, both the first coating layer and the second coating layer of the coating structure are completely free of carboxymethyl cellulose.
[0043] According to one embodiment of the invention, at least the barrier coating layer may still comprise an additional coating binder, preferably polyvinyl alcohol. The weight-average molecular weight of the polyvinyl alcohol may be < 100,000 g / mol, preferably < 90,000 g / mol. Polyvinyl alcohol that is particularly suitable for use as an additional coating binder may have a weight-average molecular weight of <70,000 g / mol, preferably 13,000–70,000 g / mol. Polyvinyl alcohol may be at least partially hydrolyzed. Polyvinyl alcohol, when used co Petition 870220103522, dated 08 / 11 / 2022, page 19 / 42 14 / 25 mo an additional coating binder can improve film formation and both the barrier properties to mineral oil and water vapor of the coating layer. Polyvinyl alcohol can also reduce the tendency of the coating structure to become blocked. According to one embodiment, the first and / or second coating layer is free of polyvinyl alcohol.
[0044] According to one embodiment, the coating layer may comprise one or more of the following additives: thickener(s), crosslinker(s), lubricant(s), alkyl ketene dimer(s), alkenyl succinic anhydride(s), and dispersing agent(s). Preferably, the first and second coating layers are free of animal-based additives and / or components, such as chitosan or animal-based gelatin. Exclusion of animal-based additives makes the coating structure suitable for food service packaging products intended for all consumer groups, regardless of their religion or ideology.
[0045] The coating structure may further comprise one or more additional coating layers that are applied over the surface of the second coating layer. The additional coating layer(s) may be different from the second coating layer.
[0046] According to a preferred embodiment, the coating structure is free of additive agents that are synthetic polymers. In particular, the coating structure may be free of styrene-based synthetic polymers, such as styrene-butadiene latex or styrene-acrylate. Exclusion of synthetic polymers may improve the biodegradability and / or compostability of the coating structure and make it more environmentally friendly, even if disposed of improperly by the end consumer. Exclusion of styrene-based polymers also makes the structure... Petition 870220103522, dated 08 / 11 / 2022, page 20 / 42 15 / 25 safe coating structure for production. Specifically, according to one embodiment of the present invention, the coating structure is free of any layers of laminated polymer films. This improves the ability of the coating structure to produce new pulp and compostability.
[0047] The substrate for the coating structure according to the present invention may comprise cellulosic and / or lignocellulosic fibers. The cellulosic or lignocellulosic fibers may have been obtained through any conventional pulping process, including chemical, mechanical, chemo-mechanical pulping processes. The substrate may also comprise or consist of recycled fibers. The substrate has a first and a second large surface, parallel to each other, and it is usually in the form of a fibrous mesh. The substrate may have a basis weight of 25-800 g / m2, preferably 30-700 g / m2, more preferably 40-500 g / m2.The coating structure can be applied to at least the first and / or second large surface of the substrate through the use of any conventional surface bonding techniques or coating techniques, such as stick coating, sheet coating, spray coating or curtain coating.
[0048] According to a preferred embodiment, the sheet-like product obtained coated with the coating structure may have a TAPPI 559 KIT test value of at least 8, preferably at least 10, more preferably at least 12. The KIT test value measures the repellency of the coating to oil and grease, and the measurements are performed in accordance with the TAPPI T-559 pm-96 standard method.
[0049] According to a preferred embodiment, the sheet-like product obtained is coated with the coating structure po Petition 870220103522, dated 08 / 11 / 2022, page 21 / 42 16 / 25 of having a mineral oil barrier HVTR value < 100 g / m² / d. The hexane vapor transmission rate (HVTR) value used is obtained through the use of a test method developed by BASF. In the test, hexane is placed in a measuring cup covered by a barrier sample, and the evaporation of hexane through a known area is measured. The test method is commonly known to those skilled in the art.
[0050] According to a preferred embodiment, the sheet-like product obtained coated with the coating structure may have a water vapor barrier at 23°C and 50% relative humidity, WVTR value < 100 g / m² / d. WVTR value may be measured using standard methods of ASTM F-1249, ISO 15105-2, ISO 15106-3, DIN 53122-2.
[0051] The foil-like product coated with the coating structure can be used for manufacturing food service packaging or for packaging liquids. Typical examples of food service packaging are packaging for light meals, ready-to-eat meals, sandwiches, bakery products such as biscuits, cookies or the like.
[0052] In the present context, unless otherwise stated, all % by weight values given for the various components are calculated from the total dry solids content of the coating layer. Experimental
[0053] Some embodiments of the invention are described in the following non-limiting examples. Preparation of Cellulose Derivative Solutions
[0054] Used cellulose derivatives were dissolved in water. Cellulose derivatives were dissolved to maximum solids content, which produced a cellulose derivative solution with a viscosity... Petition 870220103522, dated 08 / 11 / 2022, page 22 / 42 17 / 25 Brookfield density below 1000 mPas at room temperature. The dissolution procedures are described below and the cellulose derivatives used and properties of the cellulose derivative solutions obtained are described in Table 1.
[0055] Methyl cellulose (MEC); (hydroxypropyl) methyl cellulose (HPMC): One-third of the total amount of water used was heated to boiling temperature, and powdered cellulose derivative was added while mixing to prevent lump formation. The resulting suspension was placed in an ice bath, and mixing continued until the powdered cellulose derivative had dissolved. The remaining amount of water was then added while mixing.
[0056] Hydroxyethyl cellulose (HEC): Powdered cellulose derivative was added to water under mixing and the resulting suspension was heated to 60°C and maintained at this temperature until the derivative was completely dissolved. Table 1 Properties of the cellulose derivative solutions obtained Cellulose derivative Solids content [% by weight] Viscosity Br100* [mPas] Methyl cellulose MEC 6.5 410 (+19°C) (Hydroxypropyl) methyl cellulose HPMC 4.6 758 (+21°C) 2-hydroxyethyl cellulose HEC 10 911 (+22°C) *Viscosity measurement temperature given in parentheses. Coating Layer Preparation and Measurement
[0057] Coating formulations used in the examples were prepared using Diaf solvents for mixing.
[0058] A Brookfield DV-E viscometer (Brookfield GmbH, Lorch, (Germany) was used for measuring the volume viscosity of the coating formulation immediately after its preparation. Different Petition 870220103522, dated 08 / 11 / 2022, page 23 / 42 18 / 25 rods were used according to the viscosity range of the respective sample. Measurements were performed at 100 rpm.
[0059] Laboratory coating tests were performed using a K pull-coating control coater (RK Print Coat Instruments, Litlington, UK) with different coating speeds and rolling rods. Samples were dried using an IR InfraRR dryer for 60 seconds. All samples were double-coated. The substrate used in coating tests was virgin fiber-based cardboard, base weight 295 g / m2. Barrier coating layers were applied to the uncoated underside of the substrate.
[0060] Coating weight of a coated substrate was determined by weighing a coated sample and uncoated base paper, and coating weight was obtained by the difference in weights. Simple conversion testing was performed on the samples, including sample wrinkling using a punching unit and a Cyklos COM 450 wrinkling machine. Wrinkling and folding were performed in the machine direction and transversely. Staining testing was performed on the wrinkled samples using methyl red dissolved in ethanol. For folding, a Cobb roller was used to yield uniform bending pressure.
[0061] The water resistance of the coated substrate was tested using the Cobb60 test, in accordance with ISO 535 standard.
[0062] Water vapor barrier properties, WVTR, of the coated substrate were measured using a Systech Permeation Analyzers M7002 instrument.
[0063] The vapor transmission rate of hexane from the coated substrate was determined using a cup method. 20 grams of hexane were placed in a metal cup. The coated substrate was placed on top of the cup between two gaskets, coated side to side. Petition 870220103522, dated 08 / 11 / 2022, page 24 / 42 19 / 25 xo. A metal frame was used to clamp the sample to the cup. Weight loss was recorded for 24 hours.
[0064] Grease barrier properties of coated substrates are given as KIT values.
[0065] Blocking tests were performed at a temperature of 40°C and a pressure of 150 bar for 4 hours. The coated sample is coated with a barrier coating on one side and with a top-side coating on the other side. The barrier-coated sample was placed against the top-side coating in the test. The scale used for blocking test results is shown in Table 2. Table 2 Blocking test scale used in Examples Result Explanation 1 Samples do not adhere together 2 There is a noise when pulling the samples apart 3 Coating defect <50% of the surface area 4 Coating defect > 50% of the surface area 5 Delamination of base paper Example 1: Impact of different plasticizers on coating layer properties
[0066] The impact of different plasticizers was tested with low molecular weight hydroxypropyl methylcellulose, HPMC. Glycerol, sorbitol, and polyethylene glycol were selected as plasticizers. Coating formulations comprised 20% by weight of plasticizer and 80% by weight of HPMC. All samples were double-coated.
[0067] Coating weights obtained and barrier properties are shown in Table 3. Good film formation was obtained with all plasticizers tested. Petition 870220103522, dated 08 / 11 / 2022, page 25 / 42 20 / 25 Table 3. Coating weights and barrier properties for Example 1 samples Sample Plasticizer Coating Weight [g / m2] KIT 1-1 Glycerol 10.0 12 1-2 Sorbitol 8.6 12 1-3 PEG300 7.6 12
[0068] It can be seen from Table 3 that all coating layers with different plasticizers showed good barrier properties for grease. Example 2: Impact of adding inorganic pigment on coating layer properties
[0069] The impact of adding inorganic pigment was tested for the following cellulose derivatives: hydroxypropyl methylcellulose (HPMC), methyl cellulose (MEC), and hydroxyethyl cellulose (HEC). Ground calcium carbonate (HydroCarb 60, Omya) was used as an inorganic pigment. All coating formulations comprised 20% by weight of plasticizer. In coating formulations comprising HPMC or HEC, the plasticizer was PEG300; in coating formulations comprising MEC, the plasticizer was d-sorbitol. The amount of cellulose derivative and inorganic pigment in the coating formulations is shown in Table 4. All samples were double-coated.
[0070] Coating weights obtained and barrier properties are shown in Table 4. Petition 870220103522, dated 08 / 11 / 2022, page 26 / 42 21 / 25 Table 4. Coating formulations, coating weights obtained, and barrier properties for samples from Example 2. Sample Cellulose derivative Cellulose derivative, -% by weight Inorganic pigment weight -% Coating weight, g / m2 KIT (flat) Blocking 2-1 HPMC 70 10 9.6 12 - 2-3 HPMC 70 10 8.9 - - 2-4 HPMC 70 10 9.7 - 1 2-5 HPMC 60 20 10.9 12 - 2-6 HPMC 60 20 11.5 - - 2-7 HPMC 60 20 11.1 - 1 2-8 HPMC 50 30 12.9 12 - 2-9 HPMC 50 30 11.8 - - 2-10 HPMC 50 30 12.2 - 1 2-11 MEC 70 10 5.2 9 - 2-12 MEC 70 10 10.5 8 1 2-13 MEC 60 20 5.3 8 - 2-14 MEC 60 20 9.7 8 - 2-15 MEC 50 30 6.7 9 - 2-16 MEC 50 30 10.8 7 - 2-17 HEC 70 10 6.1 4 - 2-18 HEC 70 10 7.3 12 - 2-19 HEC 70 10 13.5 12 2 2-20 HEC 60 20 6.9 3 - 2-21 HEC 60 20 9.5 12 - 2-22 HEC 60 20 14.8 12 2 2-23 HEC 50 30 6.5 4 - 2-24 HEC 50 30 10.8 12 - 2-25 HEC 50 30 18.7 12 2 Petition 870220103522, dated 08 / 11 / 2022, p. 27 / 42 22 / 25
[0071] It can be seen from Table 4 that none of the HPMC or HEC samples tested showed wrinkling cracking up to a pigment content of 30% by weight. KIT values of 12 were obtained for all pigment addition levels for coating structures double-coated with HPMC and HEC. HPMC and HEC samples showed good grease barrier properties.
[0072] MEC samples comprising 10% by weight of inorganic pigment show no wrinkling cracking, while MEC samples with higher inorganic pigment content showed some wrinkling cracking. KIT values 7-8 were obtained for all pigment addition levels for double-coated MEC coating structures. Example 3: Coating structure with a high amount of inorganic pigment and an additional binder.
[0073] A higher pigment content in the coating structure was tested with hydroxyethyl cellulose and hydroxypropyl methyl cellulose coating formulations. Ground calcium carbonate GCC (HydroCarb 60, Omya) was used as an inorganic pigment. The impact of the presence of an additional binder in the coating layer was also tested. Coating formulations for manufacturing coating layers are presented in Table 5. Table 5 Coating formulations used in Example 3 Coating Component Coating Formulation HEC A HEC B HPMC A HPMC B Hydroxyethyl cellulose 55 40 Hydroxypropyl methyl cellulose 50 50 GCC 35 40 35 30 PEG-300 10 20 15 10 Additional binder, polyvinyl alcohol 10 Petition 870220103522, dated 08 / 11 / 2022, page 28 / 42 23 / 25
[0074] Coating weights obtained and barrier properties for double-coated samples are shown in Table 6. HVTR values < 100 g / m2 are considered to indicate good barrier properties against mineral oil. Table 6 Coating formulations, coating weights obtained, and barrier properties for samples from Example 3 Coating Formulation Coating Weight g / m2 KIT (Flat) WVT R g / m2 / d Block 0 HVTR g / m2* d HPMC A 12.4 12 143 - - HPMC A 11.5 12 - - 22 HPMC A 11.7 12 - 1 - HPMC B 11.8 12 133 1 - HPMC B 12.0 12 - - 92 HEC A 4.9 5 - - - HEC A 6.8 12 - - 3 HEC A 6.9 12 - 1 - HEC B 5.4 5 - - - HEC B 9.4 12 107 - 11 HEC B 10.5 12 - 1 -
[0075] It can be seen from the results in Table 6 that both HPMC and HEC yield good grease barrier properties as well as mineral oil barrier properties. Furthermore, the blocking results are good, and the coatings do not crack during wrinkling. Example 4: Coating structure with a high amount of inorganic pigment
[0076] An inorganic pigment content of up to 50% by weight in Petition 870220103522, dated 08 / 11 / 2022, page 29 / 42 24 / 25 coating structure was tested with hydroxyethyl cellulose and hydroxypropyl methyl cellulose coating formulations. Ground calcium carbonate GCC (HydroCarb 60, Omya) was used as an inorganic pigment. The impact of the presence of an additional binder in the coating layer was also tested. Coating formulations for manufacturing coating layers are presented in Table 7. Table 7 Coating formulations used in Example 4 Coating Component Coating Formulation HEC C HEC D HPMC C HPMC D HPMC E HPMC F Hydroxyethyl cellulose 40 45 Hydroxypropyl methyl cellulose 45 35 40 30 GCC 50 45 40 50 40 50 PEG-300 10 10 15 15 10 10 Additional binder, polyvinyl alcohol 10 10
[0077] Coating weights obtained and barrier properties for double-coated samples are shown in Table 8.
[0078] It can be seen from the results in Table 8 that the coating formulations had good grease barrier properties as well as mineral barrier properties. In addition, the blocking results are good. Petition 870220103522, dated 08 / 11 / 2022, pages 30 / 42 25 / 25 Table 8 Coating formulations, coating weights obtained, and barrier properties for samples from Example 4 Coating Formulation Coating Weight g / m2 KIT (flat) WVTR g / m2 / d Blocking HVTR g / m2*d HEC C 7.0 5 - - - HEC C 11.5 12 105 - 13 HEC C 11.5 12 - 1 - HEC D 5.4 4 - - - HEC D 9.9 12 111 - 11 HEC D 9.9 12 - 1 - HPMC C 10.9 12 143 - 24 HPMC C 11.4 12 - 1 - HPMC C 9.6 12 - - - HPMC D 14.7 12 153 - 30 HPMC D 11.8 12 - 1 - HPMC D 10.3 12 - - - HPMC E 13.7 12 133 - 142 HPMC E 11.3 12 - 1 - HPMC E 10.7 10 - - - HPMC F 15.9 12 - - - HPMC F 14.9 12 138 - 253 HPMC F 12.4 12 - 1 -
[0079] Even though the invention has been described with reference to what at present appear to be the most practical and preferred embodiments, it is appreciated that the invention should not be limited to the embodiments described above, but the invention is intended to also cover different modifications and equivalent technical solutions within the scope of the enclosed claims.
Claims
1. Coating structure for a sheet-like substrate comprising cellulosic and / or lignocellulosic fibers, characterized in that it comprises at least a first coating layer and a second coating layer, wherein the second coating layer is arranged in direct contact with the first coating layer and at least the first coating layer or the second coating layer is a barrier coating layer comprising - at least one water-soluble cellulose derivative selected from alkyl celluloses, hydroxy alkyl celluloses, hydroxy alkyl celluloses and any mixtures thereof, and - a plasticizer.
2. Coating structure according to claim 1, characterized in that the water-soluble cellulose derivative is selected from the group consisting of methyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, (hydroxyethyl) methyl cellulose and (hydroxypropyl) methyl cellulose and any mixtures thereof.
3. Coating structure according to claim 1 or 2, characterized in that the barrier coating layer comprises water-soluble cellulose derivative in an amount of 50-99% by weight, preferably 60-97% by weight, more preferably 70-95% by weight, calculated from the total solids content of the barrier coating layer.
4. Coating structure according to claim 1, 2 or 3, characterized in that the plasticizer of the barrier coating layer is selected from a group comprising polyols, such as sorbitol, mannitol, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, or polyethylene glycol; fatty acids; monosaccharides, ethanolamine; triethanolamine; urea; lecithin and glycerol.
5. Coating structure according to any one of claims 1 to 4, characterized in that the barrier coating layer comprises plasticizer in an amount of 150% by weight, preferably 3-40% by weight, more preferably 5-30% by weight or 5-20% by weight, calculated from the total solids content of the barrier coating layer.
6. Coating structure according to any one of claims 1 to 5, characterized in that at least the barrier coating layer still comprises inorganic pigment particles.
7. Coating structure according to claim 6, characterized in that the water-soluble cellulose derivative is selected from alkyl celluloses, such as methyl cellulose, wherein the barrier coating layer comprises inorganic pigment particles in an amount of 5-20% by weight, preferably 7-17% by weight, more preferably 7-15% by weight, calculated from the total dry solids content of the barrier coating layer.
8. Coating structure according to claim 6, characterized in that the water-soluble cellulose derivative is selected from hydroxyalkyl celluloses or hydroxyalkyl alkyl celluloses, wherein the barrier coating layer comprises inorganic pigment particles in an amount of 20-60% by weight, preferably 30-55% by weight, more preferably 40-50% by weight, calculated from the total dry solids content of the barrier coating layer.
9. Coating structure according to any one of claims 1 to 8, characterized in that the first coating layer and the second coating layer are barrier coating layers.
10. Coating structure according to any one of claims 1 to 9, characterized in that the first coating layer has a coating weight of 2-30 g / cm2, preferably 3-20 g / m2, more preferably 5-15 g / m2, and the second coating layer has a coating weight of 0.5-20 g / m2, preferably 0.5-15 g / m2, more preferably 0.5-10 g / m2.
11. Use of a coating structure as defined in any one of claims 1 to 10, characterized in that it provides a barrier to grease when applied over a sheet-like product comprising cellulosic and / or lignocellulosic fibers.
12. Sheet-like product, characterized in that it comprises: - a substrate comprising cellulosic and / or lignocellulosic fibers, having a first large surface and a second large surface, which are parallel to each other, and - a coating structure as defined in any one of claims 1 to 10, applied over at least the first or second large surface of the substrate.
13. Product according to claim 12, characterized in that the substrate has a basis weight of 25-800 g / m2, preferably 30-700 g / m2, more preferably 40-500 g / m2.
14. Product according to claim 12 or 13, characterized in that the product has a KIT test value of at least 8, and / or a mineral oil barrier HVTR value < 100 g / m2 / d.
15. Use of a sheet-like product as defined in any one of claims 12 to 14, characterized in that it is for the manufacture of a food service packaging.