Fabrication process of blended yarn of wool with rabbit hair

A production process and blended yarn technology, which is applied in yarn, textile, papermaking, biochemical fiber treatment, etc., can solve the problems of low strength, poor wear resistance, rough hand feeling, etc., and achieve simplified production steps, optimized production process, and better hand feel. good effect

CN102747476AInactive Publication Date: 2012-10-24TAICANG MINGLIU GARMENT
4 Cites 3 Cited by

Patent Information

Authority / Receiving Office
CN · China
Current Assignee / Owner
Publication Date
2012-10-24
Estimated Expiration
Not applicable · inactive patent
Patent Text Reader

Abstract

The invention discloses a fabrication process of a blended yarn of wool with rabbit hair. The process comprises steps of matching raw materials, opening, cotton carding, drawing, roving, spinning, enzyme treatment, washing, softening treatment, quality control and packaging. According to the fabrication process, the production process is optimized through simplification of the production steps, the production efficiency is improved while the product quality is guaranteed, the increase of market competitiveness is facilitated, and simultaneously, appearances and handle feels of products are better due to the additional steps such as enzyme treatment and softening treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field

[0001] The invention relates to a manufacturing process of yarn, in particular to a manufacturing process of a sheep and rabbit wool blended yarn. Background technique

[0002] Rabbit hair is a precious natural protein fiber. In recent years, it has been widely used in woolen products. It and wool blended fabric with short and smooth wool coats are elegant and smooth, good drape, bright, natural, and warm. Good features, and moderate prices, are favored by consumers. However, due to the limitation of the material of rabbit fur and wool, most of its products have the disadvantages of low strength, poor wear resistance and rough hand feeling. Summary of the invention

[0003] Objective of the invention: The objective of the present invention is to overcome the shortcomings of the prior art and provide a process for producing a sheep and rabbit wool blended yarn with high strength and comfortable hand feeling.

[0004] Technical Solution: In order to solve the above t...

Examples

Embodiment 1

[0019] (a) Proportioning raw materials: prepare raw materials, including 25% wool, 25% rabbit hair, 35% cotton, and 15% chemical fiber;

[0020] (b) Opening process: use FA106 type opening machine to mix the raw materials, in which the speed of the needle roller is 510r / min, the speed of the beater is 750r / min, and the distance between the beater and the roller is 10mm;

[0021] (c) Carding process: FX256 combing machine is used to comb the raw materials, the speed is 190m / min, 170 tongs / min;

[0022] (d) Drawing process: draw frame FA322 is used to draw the yarn, and the speed is 250m / min;

[0023] (e) Coarse sanding process: roving the blended yarn with the roving frame RF4a;

[0024] (f) Spinning process: use spinning frame B583 to subdivide the blended yarn;

[0025] (g) Enzyme treatment step: 1398 protease is used to remove the gum on the blended yarn, the concentration is 6% owf, the bath ratio is 1:20, the pH value is 6.5, and the treatment temperature is 45°C. Processing time is...

Embodiment 2

[0031] (a) Proportioning raw materials: prepare raw materials, including 25% wool, 25% rabbit hair, 35% cotton, and 15% chemical fiber;

[0032] (b) Opening process: use FA106 type opening machine to mix the raw materials, in which the speed of the needle roller is 550r / min, the speed of the beater is 800r / min, and the distance between the beater and the roller is 10mm;

[0033] (c) Carding process: use FX256 combing machine to comb the raw materials, the speed is 250m / min, 250 tongs / min;

[0034] (d) Drawing process: draw frame FA322 is used to draw the yarn, and the speed is 400m / min;

[0035] (e) Coarse sanding process: roving the blended yarn with the roving frame RF4a;

[0036] (f) Spinning process: use spinning frame B583 to subdivide the blended yarn;

[0037] (g) Enzyme treatment process: using 1398 protease to remove the gum on the blended yarn, the concentration is 10% owf, the bath ratio is 1:30, the pH value is 7.5, and the treatment temperature is 55°C. Processing time is 3...

Embodiment 3

[0043] (a) Proportioning raw materials: prepare raw materials, including 25% wool, 25% rabbit hair, 35% cotton, and 15% chemical fiber;

[0044] (b) Opening process: The FA106 type opening machine is used to mix the raw materials. The speed of the needle roller is 530r / min, the speed of the beater is 780r / min, and the distance between the beater and the roller is 10mm;

[0045] (c) Carding process: use FX256 combing machine to comb the raw materials, the speed is 220m / min, 190 tongs / min;

[0046] (d) Drawing process: draw frame FA322 is used to draw the yarn, and the speed is 320m / min;

[0047] (e) Coarse sanding process: roving the blended yarn with the roving frame RF4a;

[0048] (f) Spinning process: use spinning frame B583 to subdivide the blended yarn;

[0049] (g) Enzyme treatment process: using 1398 protease to remove the gum on the blended yarn, the concentration is 8% owf, the bath ratio is 1:25, the pH value is 7, and the treatment temperature is 48°C. Processing time is 2.5h;...