Flame-retardant modified urea-formaldehyde glue and application thereof
A technology for modifying urea-formaldehyde and urea-formaldehyde adhesives, used in adhesives, aldehyde/ketone condensation polymer adhesives, adhesive types, etc., can solve the problems of poor flame retardancy, poor stability of urea-formaldehyde adhesives, and short storage time. Improve flame retardant performance, save work efficiency, and improve the effect of initial viscosity
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Publication Date
- 2015-02-04
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
technical field
[0001] The invention relates to a modified urea-formaldehyde glue and its application. Background technique
[0002] At present, the main raw materials of urea-formaldehyde glue used in wood processing industry are formaldehyde and urea. Among them, the content of formaldehyde is very high, and formaldehyde has the characteristics of strong volatility. The volatile gas is highly irritating to people and harmful to human health. Therefore, the study of low-toxicity urea-formaldehyde glue has become an urgent problem to be solved. In recent years, there have been related reports and researches. The use of a new type of modified urea-formaldehyde glue can reduce the free formaldehyde content to less than 0.5%. Low, thereby increasing the labor intensity, which is not conducive to the improvement of work efficiency, and the existing urea-formaldehyde glue has the danger of curing during the glue mixing process. For example, when the pH is lower than 4.6 when mi...
Examples
specific Embodiment approach 1
[0018] Specific embodiment 1: A flame-retardant modified urea-formaldehyde glue of this embodiment is composed of 600-700 parts by weight of 37% formaldehyde, 300-400 parts of urea, 35-45 3-7 parts of melamine, 6-14 parts of 4-bromophenol, 3-7 parts of cellulose sodium, 3-7 parts of ammonia water with a mass percentage of 25%-28% and 3-7 parts of polyvinyl alcohol. become.
[0019] In this embodiment, the wood-based panel is prepared by adding urea-formaldehyde glue formed by 4-bromophenol, which can further improve the flame-retardant performance of the wood-based panel, and can make the wood-based panel achieve the flame-retardant effect.
[0020] The ammonia water added in the urea-formaldehyde glue of this embodiment can further reduce the formaldehyde content, and the added 4-bromophenol can further increase the hot water property of the glue and reduce the free formaldehyde content to a very low value. In the urea-formaldehyde glue of this embodiment Free formaldehyde c...
specific Embodiment approach 2
[0022] Specific embodiment two: the difference between this embodiment and specific embodiment one is that the urea-formaldehyde glue is 37% formaldehyde, 333 parts of urea, 40 parts of melamine, 10 parts of urea-formaldehyde glue in parts by weight. 4-bromophenol, 5 parts of sodium cellulose, 5 parts of ammonia water with a mass percentage of 25% to 28% and 5 parts of polyvinyl alcohol. Others are the same as in the first embodiment.
specific Embodiment approach 3
[0023] Embodiment 3: A modified urea-formaldehyde glue of this embodiment is used as a flame retardant material for the preparation of wood-based panels.
[0024] In this embodiment, the wood-based panel is prepared by adding urea-formaldehyde glue formed by 4-bromophenol, which can further improve the flame-retardant performance of the wood-based panel, and can make the wood-based panel achieve the flame-retardant effect.
[0025] The ammonia water added in the urea-formaldehyde glue of this embodiment can further reduce the formaldehyde content, and the added 4-bromophenol can further increase the hot water property of the glue and reduce the free formaldehyde content to a very low value. In the urea-formaldehyde glue of this embodiment Free formaldehyde content is less than 0.1%.
[0026] The cellulose sodium in the urea-formaldehyde glue of the present embodiment can improve the initial viscosity of the glue, improve the water solubility of the glue, and improve the stabil...