A PERC-based double-sided solar cell back conductive structure and manufacturing method
By designing gradient linear laser grooved zones and fitting points on the back of PERC+ double-sided solar cells, and combining screen printing technology, the precise nesting of the back conductive structure is achieved, solving the problem of insufficient photogenerated carrier conduction capability. It improves the photoelectric conversion efficiency and filling factor of solar cells, and is suitable for large-scale production.
Patent Information
- Application Number
- CN201810265056.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-03-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2038-03-28
AI Technical Summary
The back conductive structure of PERC+ double-sided solar cells leads to a decrease in the conduction capacity of photogenerated carriers, affecting the photoelectric conversion efficiency and filling factor of the battery, and the back laser groove design is difficult to expand to improve efficiency.
The gradient linear laser grooved zone and fitting point design is adopted, combined with screen printing technology, silver grid lines and aluminum grid lines are printed layer by layer to ensure accurate nesting and conductive structures and improve the conductivity of the back passivation film layer.
The photoelectric conversion efficiency and filling factor product of solar cells are improved, the series resistance is reduced, and the large-scale production control capability of the battery is enhanced.
Smart Images

Figure CN108365026B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of crystalline silicon solar cell manufacturing, and specifically relates to a PERC-based double-sided solar cell back conductive structure and a manufacturing method. Background Art
[0002] Passivated emitter rear contact (PERC) solar cells are a new generation of high-efficiency cell devices. Compared with traditional aluminum back field solar cells, PERC cells can significantly improve the photoelectric conversion efficiency of cells. Based on the PERC cell process, a PERC+ bifacial solar cell is derived by printing partial aluminum grid lines instead of full aluminum printing in the screen printing process. PERC+ bifacial solar cells can reduce the use of aluminum paste, improve the warping stress of the cell, and reduce the fragmentation rate caused by warping stress in the welding process of the battery packaging component. Since PERC+ bifacial solar cells can be packaged into double-glass solar modules, compared with traditional photovoltaic modules, the back side can absorb scattered light and secondary reflected light from the ground, and an additional 20%-30% of power generation is generated, while increasing the terminal application channels of solar modules.
[0003] Since the PERC+ bifacial solar cell uses a partial aluminum grid line on the back side instead of the full aluminum back field, the metal conduction area is reduced, which inevitably causes the conduction capacity of photogenerated carriers to decrease, resulting in a partial loss of the front efficiency of the cell due to the increase in series resistance. In addition, only the local aluminum grid line area on the back side in contact with the back passivation film can be connected to the silicon wafer substrate after laser grooving to form LBSF, while the insulating back passivation film layer in other areas plays the role of light transmission and protection of the silicon wafer substrate and cannot act on the laser. This limits the increase in the back grooving area to improve the fill factor and the adjustable grooving ratio to balance the back passivation to ensure that the open circuit voltage does not decrease. Since the photovoltaic conversion efficiency of the solar cell is proportional to the product of the open circuit voltage and the fill factor, the increase in series resistance will cause the fill factor to decrease nonlinearly. Therefore, the back conductive electrode structure and laser grooving design of the PERC+ bifacial solar cell are extremely important for the balanced improvement of the photovoltaic conversion efficiency of the front and back sides of this type of bifacial cell. On the other hand, after the local grid lines on the back are refined, they need to be accurately nested and printed in the laser grooved area on the back. Therefore, it is necessary to design a special three-layer nested printing structure of back silver grid lines, aluminum grid lines and laser grooves to ensure precise nested printing layer by layer, so that the grooved back passivation film layer area can fully bear the conduction requirements of photogenerated carriers, thereby maximizing the efficiency of batch cells and facilitating large-scale production process control of such bifacial solar cells. Summary of the invention
[0004] The purpose of the present invention is to solve the problem of low photoelectric conversion efficiency of the front and back sides of a bifacial cell and to provide a PERC-based bifacial solar cell back side conductive structure and a manufacturing method.
[0005] The technical solution adopted by the present invention is as follows:
[0006] A PERC-based back conductive structure of a bifacial solar cell comprises a back passivation film layer, a back silver main grid electrode is arranged on the back passivation film layer, laser grooved areas are arranged on both sides of the back silver main grid electrode, and the width of the laser grooved areas gradually narrows towards the direction away from the back silver main grid electrode.
[0007] Furthermore, the line width of the laser grooved area is 12-160 um, the line length is 9-32 mm, and the distance between the laser grooved area and the back silver main gate electrode is greater than 0 and less than or equal to 1 mm.
[0008] Furthermore, an aluminum grid line is arranged at the laser grooved area on the back passivation film layer, and a silver grid line is arranged on the aluminum grid line, and the laser grooved area, the aluminum grid line and the silver grid line overlap in sequence from bottom to top and are symmetrical about the center line of the laser grooved area; the width of the aluminum grid line is always greater than the width of the laser grooved area at its location, and the width of the silver grid line is always less than the width of the aluminum grid line at its location.
[0009] Furthermore, the silver grid lines adopt a gradual linear structure or a uniform straight line structure, and the aluminum grid lines adopt a gradual linear structure.
[0010] Furthermore, the aluminum grid line is located in the aluminum grid layer, the silver grid line and the back silver main grid electrode are located in the silver grid layer, and concentric alignment points with gradually decreasing areas are arranged at the same positions of the back passivation film layer, the aluminum grid layer and the silver grid layer to align the back passivation film layer, the aluminum grid layer and the silver grid layer.
[0011] Furthermore, the connection length between the aluminum grid line and the edge of the back silver main grid electrode is greater than 100um.
[0012] A method for manufacturing a back conductive structure of a bifacial solar cell based on PERC, comprising the following steps:
[0013] S1: reserve a silver main gate electrode area on the back passivation film layer, and set a laser groove area and alignment and insertion points.
[0014] Among them, the back passivation film layer includes but is not limited to back single-layer passivation film layers or back stacked passivation film layers such as silicon oxide, aluminum oxide, silicon carbide, silicon nitride and amorphous silicon grown and deposited by dry / wet oxygen, APCVD, ALD, PECVD, PVD and sputtering, and the back single-layer passivation film layer or the back stacked passivation film layer with a thickness of 90-140nm is selected for groove opening.
[0015] First, 5-16 parallel silver main gate electrode areas for printing the main gate electrode are reserved on the back passivation film layer. The structure of the silver main gate electrode area adopts a segmented structure or a connected structure. Then, a laser with a wavelength of 400-1200nm is used to open holes in the silver main gate electrode area and the area outside the epitaxial distance of 0-1mm, and the laser hole opening spot must completely penetrate the back passivation film layer, that is, the hole opening spot depth must be greater than 90nm. A single laser hole opening spot is a circular spot with a diameter of 12-60um. The circular spots overlap to form a gradient linear laser slot area perpendicular to the silver main gate electrode area, that is, the slot line diameter close to the silver main gate electrode area is thicker than the slot line diameter away from the silver main gate electrode area, and the slot line width is 12-160um. The slot line length depends on the number of silver main gate electrode areas, and the slot line length is 9-32mm. At the same time, laser holes are opened on the edge of the back passivation film layer to form multiple laser slotting alignment points for alignment. The laser slotting alignment points can be selected in any pattern such as circle, rectangle, cross, etc., and their positions are preferably 4 concentric circles or squares located within the silver main gate electrode area and its extension line area, and their size is 0.1-1mm.
[0016] Then, the screen printing alignment points of the same pattern are marked on the corresponding positions of the screen, so that the screen printer CCD and process personnel can fine-tune the printing position by offsetting the laser slotting alignment points and the screen printing alignment points to ensure accurate overprinting.
[0017] S2: Using the alignment points, printing aluminum grid lines on the laser grooved areas.
[0018] First, the aluminum paste printing alignment points of the same pattern are marked on the corresponding positions of the aluminum grid line screen where the aluminum grid line is set, and the screen printer captures the laser groove alignment points marked by the laser, and then the center of the aluminum paste printing alignment points is aligned with the center of the laser groove alignment points and the screen printing alignment points, and then the aluminum grid line is screen-printed on the laser groove area at the corresponding position, and then the aluminum paste is dried at 150-350°C. Among them, in order to match the gradient linear laser groove area formed by the laser opening, the aluminum grid line adopts a similar gradient linear structure, that is, the aluminum grid line line diameter close to the silver main grid electrode area is thicker than the aluminum grid line line diameter away from the silver main grid electrode area, and the aluminum grid line width is always greater than the laser groove area width at the said position. The line width of the aluminum grid line is 20-200um, the line length of the aluminum grid line is 9-32mm, and the connection section between the aluminum grid line and the edge of the silver main grid electrode area is greater than 100um.
[0019] S3: Using the alignment and embedding points, print the back silver main grid electrode and silver grid lines on the aluminum grid layer.
[0020] The method of printing the back silver main grid electrode and the silver grid line on the aluminum grid layer includes:
[0021] 1) first printing the back silver main grid electrode in the silver main grid electrode area, and then printing the silver grid lines in the laser groove area and the location of the aluminum grid lines;
[0022] 2) First connect the back silver main grid electrode and the silver grid line, and then print the back silver main grid electrode and the silver grid line on the aluminum grid line together.
[0023] If method 1) is adopted to print the back silver main grid electrode and silver grid line on the aluminum grid line, then the silver paste printing alignment and interlocking points of the same pattern are marked on the corresponding positions of the silver main grid electrode screen provided with the back silver main grid electrode and the silver grid line screen provided with the silver grid line, respectively, the screen printer captures the aluminum paste printing alignment and interlocking points marked by the aluminum paste printer, and then aligns the center of the silver paste printing alignment and interlocking points with the center of the aluminum paste printing alignment and interlocking points, and then screen prints the back silver main grid electrode and silver grid line in sequence. The back silver main grid electrode on the silver main grid electrode screen is printed on the silver main grid electrode area at the corresponding position, and then the silver paste is dried at 160-380℃. Then the silver grid line on the silver grid line screen is printed on the aluminum grid line at the corresponding position, and then the silver paste is dried at 160-380℃. The silver grid line can adopt a gradient linear structure or a uniform straight line structure, and the width of the silver grid line is always smaller than the width of the aluminum grid line at the location, and the line width is 16-180um and the line length is 9-32mm to ensure the center overprinting. The back silver main grid electrode and the silver grid line are printed separately, and the printing can be completed by using silver pastes with different characteristics.
[0024] If method 2) is adopted to print the back silver main grid electrode and silver grid line on the aluminum grid line, the back silver main grid electrode and the silver grid line are first connected, and the connected back silver main grid electrode and the silver grid line are set on the same silver grid screen, and then the silver paste printing alignment points of the same pattern are marked on the corresponding positions of the silver grid screen. Then, the screen printer captures the aluminum paste printing alignment points marked by the aluminum paste printer, aligns the center of the silver paste printing alignment points with the center of the aluminum paste printing alignment points, and then screen prints the back silver main grid electrode and the silver grid line on the silver grid screen on the aluminum grid line at the corresponding position, and then dries the silver paste at 160-380°C. Among them, the silver grid line can adopt a gradual linear structure or a uniform straight line structure, and the width of the silver grid line is always smaller than the width of the aluminum grid line at the position, and its line width is 16-180um, and the line length is 9-32mm to ensure centered overprinting. When printing the silver main grid electrode and the silver grid line on the back side at the same time, the printing is completed using a silver paste with the same properties.
[0025] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0026] 1. In the present invention, by opening holes on the back passivation film layer to form a gradient linear laser slotted area, the passivation effect of the back passivation film and the requirements for the conduction of photogenerated carriers can be balanced, and a variety of back passivation film slot ratio combinations can be achieved in a limited back grid line contact area, thereby taking into account the product matching of the cell open circuit voltage and the fill factor, so that the photoelectric conversion efficiency of the solar cell is improved. At the same time, the gradually widened gradient structure improves the ability of the back photogenerated carriers to be exported along the local grid line, reduces the heat loss and power loss during the export process, and thus improves the photoelectric conversion efficiency of the front and back sides of the PERC+ bifacial solar cell.
[0027] 2. In the present invention, laser is used to open holes in the back passivation film layer to form laser groove alignment interlocking points, and interlocking point patterns are designed in the screen printing and laser groove processes to ensure that the refined back aluminum grid lines can be accurately nested and printed in the laser groove area, and to ensure that the silver grid lines can be accurately nested and printed in the aluminum grid line printed area, thereby solving the alignment problem of the refined silver grid lines, aluminum grid lines and laser grooves, and facilitating large-scale production process control of double-sided solar cells.
[0028] 3. In the present invention, in a limited local aluminum gate line area on the back side, by adjusting the LBSF area at different areas away from the silver main gate electrode on the back side, the ability of the aluminum gate line to extract photogenerated carriers from the silicon substrate is improved, the requirements of the back passivation effect and the conduction of photogenerated carriers are balanced, and the adjustable range of the open circuit voltage and the fill factor product matching is increased.
[0029] 4. In the present invention, the gradient lower aluminum grid line and upper silver grid line are combined to conduct current to the back silver main grid electrode, which solves the problem of large series resistance of the back photogenerated carriers of the PERC-based bifacial solar cell along the aluminum grid line to the back silver main grid electrode, and ensures the lower Al-BSF field passivation mechanism. By screen printing the gradient aluminum grid line electrode structure and nesting the overprinted silver fine grid lines, the power loss of the back grid line conducting current to the back silver main grid electrode can be reduced, thereby reducing the battery series resistance.
[0030] 5. In the present invention, a silver paste with high conductivity is used for silver grid line nesting printing, which improves the conductivity of the back grid line and increases the transmission cross-sectional area of electrons at the local grid line end. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a layered side view of the back conductive structure of the PERC+ bifacial solar cell in the present invention.
[0032] Figure 2 This is a microstructure diagram of the laser grooving in the present invention.
[0033] Figure 3 It is a schematic diagram of the structure of the laser grooved layer in the present invention.
[0034] Figure 4 It is a schematic diagram of the structure of the aluminum grid layer in the present invention.
[0035] Figure 5 It is a schematic diagram of the structure of the silver grid layer in the present invention.
[0036] Figure 6 It is a top view of the superposition of the laser grooved layer, the aluminum grid layer and the silver grid layer in the present invention.
[0037] Markings in the figure: 1-back laminated passivation film layer, 2-silver main gate electrode area, 3-gradient linear laser groove area, 4-laser groove alignment and embedding point, 5-aluminum paste printing alignment and embedding point, 6-aluminum grid line, 7-silver paste printing alignment and embedding point, 8-back silver main gate electrode, 9-silver grid line. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0039] Example 1
[0040] The manufacturing process of the PERC-based conjoined five-busbar bifacial solar cell is as follows:
[0041] 1) P-type single crystal silicon wafers are cleaned to remove impurities and surface defects, and double-sided texturing is performed to form a 2-6um random pyramid texture surface.
[0042] 2) Back-to-back diffusion, diffusing the phosphorus source under negative pressure on the front side of the silicon wafer to prepare a 0.3um deep PN junction.
[0043] 3) Remove PSG on the front side and the extra diffused PN junction at the side boundary, and polish the back side appropriately to correct the velvet surface by 2-4um.
[0044] 4) Double-sided oxidation and annealing to form a 3-7nm silicon dioxide film layer.
[0045] 5) ALD reaction deposits an Al2O3 film with a thickness of 4-6nm on the back surface.
[0046] 6) Double-sided PECVD reaction deposition of Si3N4 film, 75-90nm silicon nitride anti-reflection passivation protective film deposited on the front PN junction area, and 100nm silicon nitride transparent passivation protective film deposited on the back.
[0047] 7) Five parallel silver main gate electrode regions 2 adapted to the main gate electrode with a length of 155.5 mm and a width of 0.8 mm are reserved on the above-mentioned back laminated passivation film layer 1. Laser drilling is performed outside the silver main gate electrode region 2 and its extension at a distance of 0.3 mm. The drilling spot depth is 120 nm, the spot diameter is 35 um, and the spot radius overlaps one by one to form a gradient linear laser slotted region 3. The width of the gradient linear laser slotted region 3 close to the silver main gate electrode region 2 is 120 um, the width away from the silver main gate electrode region 2 is 70 um, and the slotted line length is 14.8 mm. At the same time, holes are drilled in the 20×20 mm area at the four corners of the back laminated passivation film layer 1 to form laser slotted alignment and interlocking points 4. The laser slotted alignment and interlocking points 4 are designed as concentric circles with a diameter of 0.5 mm.
[0048] 8) Aluminum paste printing alignment points 5 with the same pattern and a diameter of 0.4 mm are marked on the corresponding positions of the aluminum grid line screen with aluminum grid lines 6, and the centers of the laser slotting alignment points 4 and the aluminum paste printing alignment points 5 are concentric, and the center of the aluminum paste printing alignment points 5 is located on the extended area of the silver main grid electrode area 2. The aluminum paste printer captures the laser slotting alignment points 4 marked by the laser, and the CCD camera of the aluminum paste printer adjusts the X, Y and angle of the aluminum grid line screen to align the laser slotting alignment points 4 and the screen printing alignment points, and then nests and prints the aluminum grid lines 6 on the corresponding positions of the gradual laser slotting areas 3, and then dries the aluminum paste at 150-350°C. The aluminum grid line 6 near the silver main grid electrode area 2 has a line width of 150um, the aluminum grid line 6 far from the silver main grid electrode area 2 has a line width of 100um, the aluminum grid line 6 has a line length of 15.2mm, and the length of the connecting section between the aluminum grid line 6 and the edge of the silver main grid electrode area 2 is 100um. In a pattern-to-pattern manner, the aluminum grid line 6 is ensured to be accurately nested and printed in the gradient laser slotted area 3, thereby achieving precise printing alignment and ensuring that photogenerated carriers are drawn out of the silicon wafer.
[0049] 9) Connect the back silver main grid electrode 8 and the silver grid line 9, and set the connected back silver main grid electrode 8 and the silver grid line 9 on the silver grid screen, and then mark the silver paste printing alignment embedding point 7 with the same pattern and a diameter of 0.3mm on the corresponding position of the silver grid screen, and make the center of the silver paste printing alignment embedding point 7 and the aluminum paste printing alignment embedding point 5 concentric, and the center of the silver paste printing alignment embedding point 7 is located on the extended area not covered by the silver main grid electrode area 2. Then, the silver paste printer captures the aluminum paste printing alignment embedding point 5 marked by the aluminum paste printer, and the CCD camera of the silver paste printer adjusts the X, Y and angle of the screen to align the center of the silver paste printing alignment embedding point 7 with the center of the aluminum paste printing alignment embedding point 5, and then screen prints the back silver main grid electrode 8 and the silver grid line 9 on the silver grid screen on the aluminum grid line 6 at the corresponding position, and then dries the silver paste at 160-380℃. The silver grid line 9 adopts a uniform straight line structure, with a line width of 60um and a line length of 15.1mm. In a pattern-to-pattern manner, the silver grid line 9 and the back silver main grid electrode 8 are accurately superimposed on the aluminum grid line 6 area, thereby achieving precise superposition and overprinting, ensuring that the resistivity of the back conductive grid line is reduced and the transmission cross-sectional area is increased.
[0050] 10) Turn over the battery cell, screen print the front electrode according to the conventional process, dry at 300-820℃, co-sinter the front paste and the back paste, and penetrate the laminated passivation film to form a good ohmic contact.
[0051] 11) Bifacial IV characteristics are measured to characterize the performance of PERC-based bifacial solar cells and classify them.
[0052] Example 2
[0053] On the basis of Example 1, a silver paste printing alignment embedding point 1 with the same pattern and a diameter of 0.3 mm is marked on the corresponding position of the silver main grid electrode screen with a back silver main grid electrode 8 with a length of 155.5 mm and a width of 0.8 mm, and the center of the silver paste printing alignment embedding point 1 and the aluminum paste printing alignment embedding point 5 are concentric, and the center of the silver paste printing alignment embedding point 1 is located on the extended area not covered by the silver main grid electrode area 2. Then, the silver paste printer captures the aluminum paste printing alignment embedding point 5 marked by the aluminum paste printer, and the CCD camera of the silver paste printer adjusts the X, Y and angle of the screen to align the center of the silver paste printing alignment embedding point 1 with the center of the aluminum paste printing alignment embedding point 5, and then screen prints the back silver main grid electrode 8 on the silver main grid electrode screen on the silver main grid electrode area 2 at the corresponding position, and then dries the silver paste at 160-380°C.
[0054] Mark the silver paste printing alignment embedding point 2 with the same pattern and a diameter of 0.25mm on the corresponding position of the silver grid line screen with silver grid lines, and make the center of the silver paste printing alignment embedding point 2 and the center of the silver paste printing alignment embedding point 1 concentric, and the center of the silver paste printing alignment embedding point 2 is located on the extended area not covered by the silver main grid electrode area 2. Then, the silver paste printer captures the marked silver paste printing alignment embedding point 1, and the CCD camera of the silver paste printer adjusts the X, Y and angle of the screen to align the center of the silver paste printing alignment embedding point 2 with the center of the silver paste printing alignment embedding point 1, and then screen prints the silver grid lines on the silver grid line screen on the corresponding positions of the gradient laser slotted area 3 and the gradient aluminum grid line 6, and then dries the silver paste at 160-380℃. The silver grid line 9 adopts a gradient linear structure, the line width of the silver grid line 9 close to the silver main grid electrode area 2 is 100um, the line width of the silver grid line 9 far away from the silver main grid electrode area 2 is 50um, and the line length of the silver grid line 9 is 15.0mm. In a pattern-to-pattern manner, the silver grid line 9 and the back silver main grid electrode 8 are accurately superimposed on the aluminum grid line 6 area, thereby achieving precise superposition and overprinting, ensuring that the resistivity of the back conductive grid line is reduced and the transmission cross-sectional area is increased.
[0055] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A PERC-based bifacial solar cell back conductive structure, comprising a back passivation film layer (1), a back silver main grid electrode (8) being arranged on the back passivation film layer (1), and laser grooved areas being arranged on both sides of the back silver main grid electrode (8), characterized in that: The width of the laser grooved area gradually narrows toward the direction away from the back silver main grid electrode (8); The line width of the laser grooved area is 12-160 μm, the line length is 9-32 mm, and the distance between the laser grooved area and the back silver main grid electrode (8) is greater than 0 and less than or equal to 1 mm; An aluminum grid line (6) is arranged at the laser slotted area on the back passivation film layer (1), and a silver grid line (9) is arranged on the aluminum grid line (6), and the laser slotted area, the aluminum grid line (6) and the silver grid line (9) overlap in sequence from bottom to top and are symmetrical about the center line of the laser slotted area; the width of the aluminum grid line (6) is always greater than the width of the laser slotted area at the location, and the width of the silver grid line (9) is always less than the width of the aluminum grid line (6) at the location; The silver grid lines (9) adopt a gradual linear structure or a uniform straight line structure, and the aluminum grid lines (6) adopt a gradual linear structure.
2. A PERC-based double-sided solar cell back conductive structure according to claim 1, characterized in that: The aluminum grid lines (6) are located in the aluminum grid layer, the silver grid lines (9) and the back silver main grid electrode (8) are located in the silver grid layer, and concentric alignment points with gradually decreasing areas are arranged at the same positions of the back passivation film layer (1), the aluminum grid layer and the silver grid layer, so that the back passivation film layer (1), the aluminum grid layer and the silver grid layer are aligned.
3. The PERC-based double-sided solar cell back conductive structure according to claim 1, characterized in that: The edge connection length between the aluminum grid line (6) and the back silver main grid electrode (8) is greater than 100 μm.
4. A method for manufacturing a back conductive structure of a bifacial solar cell based on PERC, characterized in that: The following steps are involved: S1: a silver main gate electrode region (2) is reserved on the back passivation film layer (1), and a laser slotting region and an alignment and insertion point are provided; the width of the laser slotting region gradually narrows in a direction away from the back silver main gate electrode region (2); the line width of the laser slotting region is 12-160 μm, and the line length is 9-32 mm; S2: using the alignment points, printing the aluminum grid lines (6) on the laser slotted areas; the aluminum grid lines (6) adopt a gradient linear structure; S3: Using the alignment points, the back silver main grid electrode (8) and the silver grid line (9) are printed on the aluminum grid layer; the distance between the laser slotted area and the back silver main grid electrode (8) is greater than 0 and less than or equal to 1 mm; the silver grid line (9) is arranged on the aluminum grid line (6), and the laser slotted area, the aluminum grid line (6) and the silver grid line (9) overlap in sequence from bottom to top and are symmetrical about the center line of the laser slotted area; the width of the aluminum grid line (6) is always greater than the width of the laser slotted area at the location, and the width of the silver grid line (9) is always less than the width of the aluminum grid line (6) at the location.
5. The method for manufacturing a back conductive structure of a PERC-based bifacial solar cell according to claim 4, characterized in that: In the step S3, the method of printing the back silver main grid electrode (8) and the silver grid line (9) on the aluminum grid layer includes: 1) first printing a back silver main grid electrode (8) on the silver main grid electrode area (2), and then printing silver grid lines (9) on the laser grooved area and the location of the aluminum grid lines (6); 2) Firstly, the back silver main grid electrode (8) and the silver grid line (9) are connected, and then the back silver main grid electrode (8) and the silver grid line (9) are printed together on the aluminum grid line (6).
Citation Information
Patent Citations
Preparation method for solar battery electrode
CN103633191A
Improved P-type PERC (Passivated Emitter Rear Contact) two-sided solar cell and preparation method thereof
CN106876499A
P-type PERC double-sided solar cell and module, system and preparation method thereof
CN106887476A
Double -faced solar cell back conducting structure based on PERC
CN207938619U
Photoelectric converter and fabrication thereof
JP1994053531A