RFID antenna, RFID tag, and RFID antenna manufacturing method
By using nickel slurry and low-temperature sintering technology, the problem of high cost of ceramic RFID tag antennas is solved, cost reduction and performance improvement are achieved, which is in line with the development direction of energy conservation and emission reduction.
Patent Information
- Application Number
- CN201810289018.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2038-03-30
AI Technical Summary
Existing ceramic RFID tag antennas use precious metal silver conductive paste, which results in high costs, and the sintering process requires high temperatures, which affects energy conservation and emission reduction.
Nickel paste is used as the conductive material, the viscosity is between 85Pa·s-115Pa·s, the linear resolution is less than 200μm, the resistivity is less than 80mΩ/Sq, the adhesion is greater than or equal to 625N/cm2, and it is on a 96% alumina ceramic substrate Low-temperature sintering is performed, and the design includes a T-matching network to reduce cost and size.
It reduces the material cost by more than 35%, improves the soldering resistance and conductivity, achieves energy saving and emission reduction through low-temperature sintering, and does not require additional protective layer printing and drying processes, and improves the current, voltage and magnetic loss performance of the antenna. .
Smart Images

Figure CN108550977B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of antennas, and more specifically, to an RFID antenna, an RFID tag and a method for manufacturing the RFID antenna. Background Art
[0002] Radio Frequency Identification (RFID) is an advanced form of automatic identification technology. As an advanced automatic identification technology, RFID has the characteristics of large storage capacity, read and write, long identification distance, fast identification speed, long service life, good environmental adaptability and simultaneous identification of multiple tags. It can be widely used in supply chain management, transportation management, industrial production management, animal identification management, access control, anti-counterfeiting, anti-theft, logistics, sports timing and other occasions.
[0003] With the rapid development of the global Internet of Things, the annual demand for RFID tags will be in the billions. The low cost of RFID tags has become an inevitable requirement for the rapid popularization and development of the Internet of Things, especially for ceramic RFID tags used in vehicle management system projects. At present, ceramic RFID tag antennas are basically made by thick film printing of precious metal silver conductive paste, in which silver paste is used as the conductive paste, and the cost of the conductive paste accounts for more than 70% of the entire RFID tag, making the entire RFID antenna cost relatively high. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide an RFID antenna, an RFID tag and a method for manufacturing the RFID antenna in view of the above-mentioned defects of the prior art.
[0005] The technical solution adopted by the present invention to solve the technical problem is: construct an RFID antenna, the slurry of which is nickel slurry, wherein the nickel slurry satisfies: viscosity between 85Pa·s-115Pa·s, linear resolution less than 200μm, resistivity less than 80mΩ / Sq, adhesion greater than or equal to 625N / cm 2 .
[0006] Preferably, the ceramic substrate used for printing the nickel paste comprises a ceramic substrate having an aluminum oxide content of 96%.
[0007] Preferably, the RFID antenna operates in a frequency range of 840 MHz to 845 MHz.
[0008] Preferably, the RFID antenna comprises a T-type matching network for impedance matching.
[0009] Preferably, the RFID antenna comprises:
[0010] Feed point for signal input;
[0011] Two L-shaped transmission lines connecting the feeding point and mirroring each other relative to the feeding point;
[0012] A straight-line transmission line connecting one end of the two L-shaped transmission lines away from the feeding point;
[0013] A matching line parallel to one end of the two L-shaped transmission lines connected to the feeding point;
[0014] Two radiating arms are respectively connected to two ends of the straight-line transmission line, and the two radiating arms are mirror images of each other relative to the feeding point.
[0015] The present invention also constructs an RFID tag, comprising any one of the above-mentioned RFID antennas.
[0016] Preferably, the ceramic substrate of the RFID antenna is connected to the housing via double-sided tape.
[0017] The present invention also relates to a method for manufacturing an RFID antenna, the method comprising: configuring a viscosity between 85Pa·s-115Pa·s, a linear resolution less than 200μm, a resistivity less than 80mΩ / Sq, and an adhesion greater than or equal to 625N / cm 2 The nickel paste is printed on a ceramic substrate and sintered.
[0018] Preferably, the ceramic substrate is a ceramic substrate with an aluminum oxide content of 96%.
[0019] Preferably, the sintering includes sintering using a low temperature sintering technology with a sintering temperature of 700°C±20°C.
[0020] The RFID antenna, RFID tag and RFID antenna manufacturing method of the present invention have the following beneficial effects:
[0021] 1. Compared with the most widely used silver precious metal conductive paste, nickel conductive paste can reduce material costs by more than 35%, which is in line with the company's business philosophy of reducing costs through scale;
[0022] 2. Nickel has good stability, solder resistance, electrical conductivity and thermal conductivity, meeting the requirements of low impedance, solder resistance, no ion migration and screen printing compatibility of electronic tag antenna materials;
[0023] 3. The oxidation-resistant nickel conductive paste can be sintered in the air without any modification to the original thick film sintering equipment;
[0024] 4. Compared with silver conductive paste that needs to be sintered at above 850°C, nickel conductive paste can be sintered at low temperature, which has obvious advantages in energy saving and emission reduction;
[0025] 5. Nickel is a cathode inert material that is highly resistant to current and voltage bombardment and is not prone to drift;
[0026] 6. The performance of antennas printed with nickel conductive paste is improved in terms of solder resistance, magnetic loss, etc. compared with silver conductive paste.
[0027] 7. Compared with the silver conductive paste which needs to print a sintering protective layer (glass glaze) on the sintered silver layer, the anti-oxidation nickel conductive paste does not need to print a sintering protective layer, which directly reduces the three steps of printing, drying and sintering of the protective layer (glass glaze).
[0028] Therefore, replacing precious metal silver conductive paste with nickel conductive paste not only has a clear market demand and is in line with the national development direction of industrial energy conservation and emission reduction, but also has huge economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The present invention will be further described below with reference to the accompanying drawings and embodiments, in which:
[0030] Figure 1 It is a structural schematic diagram of an embodiment of an RFID antenna of the present invention;
[0031] Figure 2 is a dimensional diagram of an embodiment of an RFID antenna of the present invention;
[0032] Figure 3 It is a schematic structural diagram of an embodiment of an RFID tag of the present invention;
[0033] Figure 4 yes Figure 1 The S11 parameter simulation results of the embodiment;
[0034] Figure 5 yes Figure 1 The Smith chart simulation result of the embodiment;
[0035] Figure 6 yes Figure 2 Sensitivity test results of the embodiment;
[0036] Figure 7 yes Figure 2 The recognition distance test results of the embodiment;
[0037] Figure 8 yes Figure 2 The reflected power test results of the embodiment. DETAILED DESCRIPTION
[0038] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described in detail with reference to the accompanying drawings.
[0039] The RFID antenna of the present invention has a nickel paste, wherein the nickel paste satisfies the following requirements: viscosity between 85Pa·s and 115Pa·s, linear resolution less than 200μm, resistivity less than 80mΩ / Sq, and adhesion greater than or equal to 625N / cm 2 . Specifically, the existing RFID antenna is usually made by printing a conductive paste on a substrate. The RFID antenna in the present invention is made by printing a nickel paste that meets the requirements on a ceramic substrate (the nickel paste constitutes the antenna body), and then sintering it. Different proportions of nickel can be selected here to debug a suitable nickel paste. Compared with the silver conductive paste that needs to print a sintered protective layer (glass glaze) on the sintered silver layer, the antioxidant nickel conductive paste does not need to print a sintered protective layer, which directly reduces the three steps of printing, drying and sintering of the protective layer (glass glaze). The main components of the nickel paste here include NixB@Ni composite powder, glass powder, organic thickener, etc., and the above effect can be achieved by mixing different proportions of various materials.
[0040] Furthermore, the ceramic substrate for printing nickel paste includes a ceramic substrate with an aluminum oxide content of 96%. Specifically, the nickel paste can be printed on a 96 aluminum oxide ceramic substrate, that is, a ceramic substrate with an aluminum oxide content of 96%. The dielectric constant of this material is 9.4, which can meet the antenna performance requirements, and is fragile and can prevent disassembly, while having the advantage of low cost.
[0041] Furthermore, the frequency range of the RFID antenna includes 840MHz-845MHz. Specifically, since the conductivity of nickel conductive paste is weaker than that of silver conductive paste, the center frequency of the antenna made of nickel paste is usually higher than the center frequency of the silver paste tag.
[0042] Furthermore, the RFID antenna includes a T-type matching network for impedance matching. Specifically, in order to achieve matching between the antenna and the chip, a matching network is often used in the design and application of RFID antennas. The additional matching network will undoubtedly increase the cost of the antenna and increase the size of the antenna. Therefore, many RFID antennas often design the matching network together with the antenna, which not only can achieve good matching between the antenna and the chip, but also reduces the cost and size of the antenna. Currently, the commonly used RFID antenna feeding networks include: T-type matching network, slot coupling feeding network, slot nested feeding network, etc. In the embodiment here, the following is used: Figure 1 The T-type matching network B1 shown in the figure has a simple structure and is easy to adjust the antenna impedance and is commonly used in the design of RFID antennas.
[0043] Furthermore, in Figure 1 The RFID antenna 100 shown (wherein the substrate is not shown) includes: a feeding point A1 for signal input; two L-shaped transmission lines B11 and B12 connected to the feeding point A1 and mirrored to each other relative to the feeding point A1; a straight-line transmission line B13 connecting the two L-shaped transmission lines B11 and B12 at one end away from the feeding point A1; a matching line B14 parallel to the end of the two L-shaped transmission lines B11 and B12 connected to the feeding point A1; two radiating arms C1 and C2 respectively connected to the two ends of the straight-line transmission line B13, and the two radiating arms C1 and C2 are mirrored to each other relative to the feeding point A1. Specifically, the feeding point A1 is used to connect the RFID chip, to receive the chip's signal input, and to output the signal. There is a gap between the matching line B14 and the short arms of the L-shaped transmission lines B11 and B12, and the gap can be adjusted as needed. Here, the entire RFID antenna adopts a symmetrical layout design, and its matching network includes L-shaped transmission lines B11 and B12 for matching, a straight-line transmission line B13, and radiation arms C1 and C2 for radio frequency radiation. Of course, other structural designs can also be adopted in some embodiments.
[0044] In addition, if Figure 2 The RFID antenna 100 shown (with the substrate not shown) provides a reference for the antenna size (mainly the antenna body made of nickel paste) when the above structure is designed, and the antenna size unit here is mm (millimeter). Typical sizes here are such as the size of the radiation arms C1 and C2, which are 24mmx48mm rectangles, and the distance between the two radiation arms C1 and C2 is 34mm, which is also the length of the straight transmission line B13. The width of the straight transmission line B13 is 3mm, and the long arm of the L-shaped transmission lines B11 and B12 connecting the straight transmission line B13 is 12.1mm in length, and the gap between its short arms is 2mm (which can also be understood as the size of the feeding point).
[0045] In order to reduce the design cycle and design cost, the electromagnetic field simulation software HFSS and HFSS-High Frequency Structure three-dimensional electromagnetic simulation software are used. The simulation results of the RFID antenna of the present invention can be obtained here. Figure 4 , Figure 5 Note that according to the conductivity of nickel paste material, the center frequency used in the simulation is higher than the center frequency of the actual RFID antenna product to be designed, so as to ensure that the actual product meets the design requirements.
[0046] In addition, the RFID tag 200 of the present invention comprises the above-mentioned RFID antenna 100, and the ceramic substrate 102 of the RFID antenna 100 is connected to the housing 201 by a double-sided adhesive 202. Specifically, as Figure 3In the illustrated embodiment, the structure of the nickel conductive paste RFID tag 200 includes, in sequence, a housing 201, an RFID antenna 100 (including an antenna body 101 made of nickel paste and a ceramic substrate 102 on which the antenna body 101 is printed), and in some embodiments, a release paper 204. The RFID chip 206 is connected to the RFID antenna feeding point A1 to transmit signals between the chip 206 and the RFID antenna 100. The housing 201 and the ceramic substrate 102 of the RFID antenna 100 are connected on one side on which the antenna body 101 is printed by a double-sided adhesive tape 202, and the other side of the ceramic substrate 102 is connected to the release paper 204 by a double-sided adhesive tape 203. The ceramic substrate 102 is made of 96% alumina ceramic, which meets the requirements of GB / T14619. The antenna body 101 on the ceramic substrate 102 is printed with nickel conductive paste and sintered at low temperature. The double-sided adhesives 202 and 203 are made of acrylic foam substrate, which is colorless and transparent, and the adhesive strength is greater than or equal to 0.28N / mm 2 The positive tensile bonding strength is not less than 7kgf / cm2, and the dynamic shear strength is not less than 4kgf / cm 2 , operating temperature range is -40℃~+85℃.
[0047] In order to quickly and accurately debug the various performances of the RFID tag 200 of the present invention to achieve the design goal, the Tagformance test system is used for debugging and testing. After repeated debugging and testing, the RFID tag is determined. The test results of the RFID tag made of the finalized nickel conductive paste tested by the Tagformance test system are as follows: Figure 6-8 It can be seen that the center frequency of the nickel paste RFID tag is between 840MHz and 845MHz, and the sensitivity is ≤-16dBm, the identification distance can reach 28m, and the reflected power is greater than or equal to -36dBm.
[0048] In addition, a method for manufacturing an RFID antenna of the present invention comprises: configuring a viscosity between 85Pa·s-115Pa·s, a linear resolution less than 200μm, a resistivity less than 80mΩ / Sq, and an adhesion greater than or equal to 625N / cm 2 The nickel paste is printed on a ceramic substrate and sintered.
[0049] Specifically, according to the requirements of thick film process and electronic tag performance, the viscosity is selected to be between 85Pa·s-115Pa·s, the linear resolution is less than 200μm, the resistivity is less than 80mΩ / Sq, and the adhesion is greater than or equal to 625N / cm 2 The nickel paste, wherein the main components of the nickel paste are NixB@Ni composite powder, glass powder, organic thickener, etc., can achieve the above effect by mixing different proportions of various materials. In some embodiments, the oxidation resistance of the nickel paste can also be considered.
[0050] Furthermore, the ceramic substrate uses a ceramic substrate with an aluminum oxide content of 96%. Specifically, the nickel paste can be printed on a 96 aluminum oxide ceramic substrate, that is, a ceramic substrate made of a ceramic with an aluminum oxide content of 96%. The dielectric constant of this material is 9.4, which can meet the antenna performance requirements, and it is fragile and can play an anti-disassembly effect, and it also has the advantage of low cost.
[0051] Furthermore, the sintering includes sintering using a low-temperature sintering technology with a sintering temperature of 700°C ± 20°C. Specifically, during the sintering process of the nickel paste, the sintering temperature cannot be too high, otherwise the nickel paste film layer will be burned, and the sintering temperature cannot be too low, otherwise the nickel paste film layer will easily fall off. The optimal temperature is around 700°C. For example, the structure of the above-mentioned RFID antenna can be used to make a screen for printing the nickel paste RFID antenna structure from a film pattern, and the nickel paste is printed on a 96% alumina ceramic of 85.6mmx54mmx0.635mm. After drying and low-temperature sintering, the nickel paste RFID antenna is completed.
[0052] It can be understood that the above embodiments only express the preferred implementation modes of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the patent scope of the present invention. It should be pointed out that, for ordinary technicians in this field, the above technical features can be freely combined without departing from the concept of the present invention, and several deformations and improvements can be made, which all belong to the protection scope of the present invention. Therefore, all equivalent changes and modifications made to the scope of the claims of the present invention should belong to the coverage of the claims of the present invention.
Claims
1. An RFID antenna, characterized in that: The slurry is nickel slurry, and the components of the nickel slurry include NixB@Ni composite powder, glass powder, and organic thickener, and the nickel slurry meets the following requirements: viscosity between 85Pa·s-115Pa·s, linear resolution less than 200μm, resistivity less than 80mΩ / Sq, and adhesion greater than or equal to 625N / cm 2 ; Wherein, the operating frequency range of the RFID antenna includes 840MHz-845MHz.
2. The RFID antenna according to claim 1, characterized in that: The ceramic substrate used for printing the nickel paste includes a ceramic substrate with an aluminum oxide content of 96%.
3. The RFID antenna according to claim 1, characterized in that: The RFID antenna includes a T-type matching network for impedance matching.
4. The RFID antenna according to claim 3, characterized in that: The RFID antenna comprises: Feed point for signal input; Two L-shaped transmission lines connecting the feeding point and mirroring each other relative to the feeding point; A straight-line transmission line connecting one end of the two L-shaped transmission lines away from the feeding point; A matching line parallel to one end of the two L-shaped transmission lines connected to the feeding point; Two radiating arms are respectively connected to two ends of the straight-line transmission line, and the two radiating arms are mirror images of each other relative to the feeding point.
5. An RFID tag, characterized in that: The RFID antenna comprises the RFID antenna described in any one of claims 1 to 3.
6. The RFID tag according to claim 5, characterized in that: The ceramic substrate of the RFID antenna is connected to the shell through double-sided adhesive.
7. A method for manufacturing an RFID antenna, characterized in that: The method comprises: The configuration viscosity is between 85Pa·s -115Pa·s, the linear resolution is less than 200μm, the resistivity is less than 80mΩ / Sq, and the adhesion is greater than or equal to 625N / cm 2 The nickel paste is printed on a ceramic substrate and sintered; the nickel paste comprises NixB@Ni composite powder, glass powder, and an organic thickener, wherein the operating frequency range of the RFID antenna includes 840 MHz-845 MHz.
8. The method for manufacturing an RFID antenna according to claim 7, characterized in that: The ceramic substrate is a ceramic substrate with an aluminum oxide content of 96%.
9. The method for manufacturing an RFID antenna according to claim 8, characterized in that: The sintering includes sintering using a low temperature sintering technology with a sintering temperature of 700°C±20°C.