Anti-stress thin floor and processing technology

By designing multiple transverse back grooves and moisture-proof film layers on the thin floor, combined with heat treatment and process parameter optimization, the problem of insufficient resistance to deformation of the thin floor is solved, the service life and yield are improved, and the stability and moisture content are ensured optimization.

CN108952070BActive Publication Date: 2024-10-18JIUSHENG WOOD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN201811093426.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-09-19
Publication Date
2024-10-18
Estimated Expiration
2038-09-19

AI Technical Summary

Technical Problem

Thin flooring has reduced resistance to deformation due to changes in thickness, and is prone to moisture expansion, dry shrinkage, and warping due to external environmental stress, which affects the use effect and lifespan. It also has poor processing stability and low yield.

Method used

A stress-resistant thin floor with a thickness of 10 to 16 mm is used. Multiple vertical and horizontal back grooves are distributed on the back of the board body, and a moisture-proof film layer is set up outside the back groove. It is combined with heat treatment and optimization of specific process parameters, including the size and moisture content control of the wood board base material. , use moisture-proof membrane layers and back grooves to reduce warpage and dimensional changes.

Benefits of technology

It effectively improves the service life and yield of thin flooring, reduces the warpage rate during wet expansion and dry shrinkage, maintains moisture content stability, delays dimensional changes, and improves processing and use stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN108952070B_ABST
    Figure CN108952070B_ABST
Patent Text Reader

Abstract

The invention discloses an anti-stress thin floor, comprising a plate body (1), the plate body (1) having a thickness of 10 to 17 mm, a plurality of transverse back grooves (2) perpendicular to the length direction of the plate body (1) being evenly distributed on the back of the plate body (1), a moisture-proof film layer (3) located on the back of the plate body (1) and on both long sides is arranged outside the transverse back grooves (2), the transverse back grooves (2) having a thickness of 2 mm, a depth of the transverse back grooves (2) being one third of the thickness of the plate body (1), the spacing between adjacent transverse back grooves (2) being the same, and the spacing between the short side wall of the plate body (1) and the transverse back grooves (2) being the same as the spacing between adjacent transverse back grooves (2). The invention has the characteristics of long service life, high yield rate and good stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a thin floor and a manufacturing method thereof, in particular to an anti-stress thin floor and a processing technology thereof. Background Art

[0002] Thin floor is a pure solid wood floor processed by a new technology to ensure the stability of the floor. Its thickness is less than the 18mm to 22mm thickness of conventional floor on the market. Compared with traditional solid wood floor, thin floor can directly replace the original 8-15mm thick laminate floor or solid wood composite floor in the second renovation of fine decoration. And because of its advantages of saving raw materials and reducing costs, it is more and more widely used in solid wood floor in different occasions. However, compared with traditional solid wood floor, the thin floor will reduce its anti-deformation ability due to the change of thickness, which makes the thin floor susceptible to stress generated by the external environment during production and use, causing different degrees of wet expansion and shrinkage of the thin floor to form warping, thus affecting the user's use effect and reducing its service life. And because the thin floor is more susceptible to its own moisture content and raw material warping during the processing process than the conventional floor, the stability of the thin floor is poor during the processing, and the external dimensions change greatly after the processing, thereby reducing the yield rate of the thin floor and reducing the processing effect of each process on the thin floor, resulting in further reduction of its performance and service life. Therefore, the existing thin floor has the problems of short service life, low yield and poor stability. Summary of the invention

[0003] The purpose of the present invention is to provide a stress-resistant thin floor and a processing technology, which has the characteristics of long service life, high yield rate and good stability.

[0004] The technical solution of the present invention is as follows: a stress-resistant thin floor comprises a board body, the thickness of the board body is 10 to 16 mm, a plurality of transverse back grooves perpendicular to the length direction of the board body are evenly distributed on the back side of the board body, a moisture-proof film layer is arranged on the back side and the long sides of the board body on the outside of the transverse back grooves, the thickness of the transverse back grooves is 2 mm, the depth of the transverse back grooves is one third of the thickness of the board body, the spacing between adjacent transverse back grooves is the same, and the spacing between the short side wall of the board body and the transverse back groove is the same as the spacing between adjacent transverse back grooves.

[0005] In the aforementioned anti-stress thin floor, the two long sides of the plate body are respectively provided with a first female groove and a first male groove that match each other, and the two short sides of the plate body are respectively provided with a second female groove and a second male groove that match each other.

[0006] In the aforementioned anti-stress thin floor, the moisture-proof film layer includes a first moisture-proof film layer, a second moisture-proof film layer and a third moisture-proof film layer which are connected to each other, the first moisture-proof film layer is pressed on the side wall of the board body close to the first male groove, the second moisture-proof film layer is pressed on the back side of the board body, and the third moisture-proof film layer is pressed on the side wall of the board body between the first female groove and the back side.

[0007] In the aforementioned anti-stress thin floor, the side walls around the board body are provided with a first wear-resistant paint layer, the front and back sides of the board body are provided with a second wear-resistant paint layer, and the moisture-proof film layer is arranged outside the first wear-resistant paint layer and the second wear-resistant paint layer.

[0008] In the aforementioned anti-stress thin floor, the moisture-proof film layer is a PE moisture-proof film layer, and the thickness of the moisture-proof film layer is 0.07-0.08 mm.

[0009] In the aforementioned anti-stress thin floor, when the length of the board body is not more than 600mm, the number of transverse back grooves is two; when the length of the board body exceeds 600mm and is not more than 900mm, the number of transverse back grooves is three; when the length of the board body exceeds 900mm and is not more than 1200mm, the number of transverse back grooves is four; when the length of the board body exceeds 1200mm, the number of transverse back grooves increases by one for every 300mm extension of the length of the board body.

[0010] The aforementioned processing technology of the anti-stress thin floor comprises the following steps:

[0011] ① Set the required length of the finished plain board to a, the width of the finished plain board to b, and the thickness of the finished plain board to c; select a board with a length of a+10~15mm, a width of b+10~15mm, a thickness of c+1.0~1.5mm, and a moisture content of 12~15% as the board substrate; obtain board A;

[0012] ② Heat-treat plate A at 130-145°C to make the moisture content of plate A 7-9% after heat treatment, and obtain plate B;

[0013] ③Put plate B in a drying kiln at 35-45℃ and let it stand for 20-30 hours, then open the exhaust hole of the drying kiln, let it stand for another 18-25 days and then take it out of the kiln to obtain plate C;

[0014] ④ Slot the four side walls of the C plate respectively, and then make a transverse back groove on one side of the C plate to obtain the D plate;

[0015] ⑤Paint the D board and cover it with moisture-proof film in turn to obtain the finished floor.

[0016] In the aforementioned processing technology of the stress-resistant thin floor, the humidity of the drying kiln during drying in step ③ is 35-45%.

[0017] In the aforementioned processing technology of the stress-resistant thin floor, the specific steps of step ⑤ are: first spray water-based paint on the four side walls of the D board, then apply UV paint on the front and back of the D board, and finally press a PE moisture-proof film layer on one side of the horizontal back groove and the long side walls on both sides of the D board; and obtain a finished board.

[0018] In the aforementioned processing technology of the stress-resistant thin floor, the pressure of the PE moisture-proof film layer during pressing in step ⑤ is 500-700N.

[0019] In the aforementioned processing technology of stress-resistant thin floor, in the step ①, the convex warping of the wooden board substrate in the length direction is not greater than 6‰ of the length of the wooden board substrate, the concave warping of the wooden board substrate in the length direction is not greater than 3‰ of the length of the wooden board substrate, the convex warping of the wooden board substrate in the width direction is not greater than 2‰ of the width of the wooden board substrate, and the concave warping of the wooden board substrate in the width direction is not greater than 1.5‰ of the width of the wooden board substrate.

[0020] In the aforementioned processing technology of the stress-resistant thin floor, the air-dry density of the wood substrate is 0.7-1.0 g / cm 3 The compressive strength of the wood board substrate along the grain is above 50MPa, the flexural strength of the wood board substrate is above 100MPa, and the flexural elastic modulus of the wood board substrate is above 12000MPa.

[0021] Compared with the prior art, the present invention can effectively reduce the warping rate and single-piece warping of the board body during wet expansion and dry shrinkage and reduce the moisture content change range of the board body during use through the cooperation of the moisture-proof film layer and multiple transverse back grooves, so as to make the present invention have a good service life and yield rate, and after the moisture content change range is reduced, the present invention can maintain the optimal value of its own moisture content performance in different external environments, thereby further improving the service life of the present invention; the transverse back grooves and moisture-proof film layer can also reduce the dimensional change rate of the floor during processing and use, thereby facilitating manufacturers to control the size of the finished floor during processing and saving the cost of the wood board substrate, and enabling the finished floor to delay its own dimensional changes after being affected by external factors when in use, thereby improving the stability of the present invention during operation.

[0022] During processing, the present invention can further reduce the variation range of moisture content and size of the floor through heat treatment, thereby further improving the stability of the floor during processing and use; and the present invention also sets the corresponding substrate size and moisture content according to the size parameters of the required finished floor product; and optimizes the process parameters of various processes, thereby further improving the stability of the wood board substrate during processing and enabling the wood board substrate to reach the size and moisture content required by the user after processing, with high yield rate and good processing and working stability. Therefore, the present invention has the characteristics of long service life, high yield rate and good stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is a bottom view of the present invention;

[0024] Figure 2 yes Figure 1 A-direction sectional view;

[0025] Figure 3 yes Figure 1 B-direction cross-sectional view.

[0026] The markings in the accompanying drawings are: 1-plate body, 2-lateral back groove, 3-moisture-proof film layer, 4-first female groove, 5-first male groove, 6-second female groove, 7-second male groove, 8-first wear-resistant paint layer, 9-second wear-resistant paint layer, 301-first moisture-proof film layer, 302-second moisture-proof film layer, 303-third moisture-proof film layer. DETAILED DESCRIPTION

[0027] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but they are not intended to limit the present invention.

[0028] Embodiment 1. A stress-resistant thin floor, comprising: Figure 1 As shown, it includes a plate body 1, the thickness of the plate body 1 is 10 to 16 mm, a plurality of transverse back grooves 2 perpendicular to the length direction of the plate body 1 are evenly distributed on the back side of the plate body 1, the width of the transverse back grooves 2 is 2 mm, and a moisture-proof film layer 3 is provided on the back side and the long sides of the plate body 1 on the outside of the transverse back grooves 2, the depth of the transverse back grooves 2 is one third of the thickness of the plate body 1, the spacing between adjacent transverse back grooves 2 is the same, and the spacing between the short side wall of the plate body 1 and the transverse back grooves 2 is the same as the spacing between adjacent transverse back grooves 2.

[0029] The two long sides of the plate body 1 are respectively provided with a first female groove 4 and a first male groove 5 that match each other, and the two short sides of the plate body 1 are respectively provided with a second female groove 6 and a second male groove 7 that match each other.

[0030] The moisture-proof film layer 3 includes a first moisture-proof film layer 301, a second moisture-proof film layer 302 and a third moisture-proof film layer 303 that are interconnected. The first moisture-proof film layer 301 is pressed onto the side wall of the plate body 1 close to the first male groove 5, the second moisture-proof film layer 302 is pressed onto the back of the plate body 1, and the third moisture-proof film layer 303 is pressed onto the side wall of the plate body 1 between the first female groove 4 and the back.

[0031] In the aforementioned anti-stress thin floor, the side walls of the plate body 1 are provided with a first wear-resistant paint layer 8, the front and back sides of the plate body are provided with a second wear-resistant paint layer 9, and the moisture-proof film layer 3 is arranged on the outside of the first wear-resistant paint layer 8 and the second wear-resistant paint layer 9; the first wear-resistant paint layer 8 is a water-based paint layer, and the second wear-resistant paint layer 9 is a UV paint layer.

[0032] The moisture-proof film layer 3 is a PE moisture-proof film layer, and the thickness of the moisture-proof film layer 3 is 0.07-0.08 mm.

[0033] When the length of the plate body 1 is not more than 600mm, the number of the transverse back grooves 2 is two; when the length of the plate body 1 exceeds 600mm and is not more than 900mm, the number of the transverse back grooves 2 is three; when the length of the plate body 1 exceeds 900mm and is not more than 1200mm, the number of the transverse back grooves 2 is four; when the length of the plate body 1 exceeds 1200mm, the number of the transverse back grooves 2 increases by one for every 300mm extension of the length of the plate body 1.

[0034] The processing technology of the anti-stress thin floor comprises the following steps:

[0035] ① Set the length of the required finished plain board (the finished plain board is the size of the floor raw material after slotting in step ④) to a, the width of the finished plain board to b, and the thickness of the finished plain board to c; select a wooden board with a length of a+10~15mm, a width of b+10~15mm, a thickness of c+1.0~1.5mm, and a moisture content of 12~15% as the wooden board substrate; the convex curvature of the wooden board substrate in the length direction is not greater than 6‰ of the length of the wooden board substrate, the concave curvature of the wooden board substrate in the length direction is not greater than 3‰ of the length of the wooden board substrate, the convex curvature of the wooden board substrate in the width direction is not greater than 2‰ of the width of the wooden board substrate, and the concave curvature of the wooden board substrate in the width direction is not greater than 1.5‰ of the width of the wooden board substrate; obtain board A;

[0036] ② Heat-treat plate A at 130-145°C to make the moisture content of plate A 7-9% after heat treatment, and obtain plate B;

[0037] ③Put plate B in a drying kiln at 35-45℃ and let it stand for 20-30 hours, then open the exhaust hole of the drying kiln to exhaust, and then let it stand for 18-25 days before taking it out of the kiln. The humidity of the drying kiln during drying is 35-45%, and plate C is obtained;

[0038] ④ Slot the four side walls of the C plate respectively, and then make a transverse back groove on one side of the C plate to obtain the D plate;

[0039] ⑤ First spray water-based paint on the side walls around the D board, then apply UV paint on the front and back of the D board, and finally press PE moisture-proof film layer on one side of the horizontal back groove and the long side walls on both sides of the D board. The pressure of the PE moisture-proof film layer during pressing is 500-700N; the finished board is obtained.

[0040] Embodiment 2. The processing technology of the anti-stress thin floor comprises the following steps:

[0041] ① Set the required length of the finished board to a, the width of the finished board to b, and the thickness of the finished board to c; select the length of the board to be a+10mm (where the length of the board substrate with a better straightness is a+10mm, and the length of the board substrate with a worse straightness is a+15mm; when the angle between the long side and the short side of the board's top view is 85-95°, the board has a better straightness; when the angle between the long side and the short side of the board's top view is 75-85° or 95-105°, the board has a worse straightness, and the angle between the long side and the short side of the board's top view is less than 75° or greater than 105° The wood board is an unqualified blank and cannot be used), the wood board width is b+10mm, the wood board thickness is c+1mm, and the wood board with a moisture content of 12-15% is the wood board substrate; the convex curvature of the wood board substrate in the length direction is not greater than 6‰ of the length of the wood board substrate, the concave curvature of the wood board substrate in the length direction is not greater than 3‰ of the length of the wood board substrate, the convex curvature of the wood board substrate in the width direction is not greater than 2‰ of the width of the wood board substrate, the concave curvature of the wood board substrate in the width direction is not greater than 1.5‰ of the width of the wood board substrate, and the air-dry density of the wood board substrate is 0.9g / cm 3 , the compressive strength of the wood substrate along the grain is above 50MPa, the flexural strength of the wood substrate is above 100MPa, and the flexural elastic modulus of the wood substrate is above 12000MPa; A board is obtained;

[0042] ② Heat-treat plate A at 140°C, so that the moisture content of plate A after heat treatment is 7-9%, the width of plate A after heat treatment is b+7mm, and the length and thickness of plate A after heat treatment change slightly and can be ignored, thus obtaining plate B;

[0043] ③Put plate B in a drying kiln at 40℃ and let it stand for 24 hours, then open one of the exhaust holes of the drying kiln to exhaust the air, and then let it stand for another 20 days before taking it out of the kiln. The humidity of the drying kiln during drying is 39%, and plate C is obtained;

[0044] ④ Slot the four side walls of the C plate respectively, and then make a transverse back groove on one side of the C plate to obtain the D plate;

[0045] ⑤ First spray water-based paint on the side walls around the D board, then apply UV paint on the front and back of the D board, and finally press PE moisture-proof film layer on one side of the horizontal back groove and the long side walls on both sides of the D board. The pressure of the PE moisture-proof film layer during pressing is 600N, and the finished floor is obtained.

[0046] This embodiment optimizes the corresponding process parameters and the performance parameters required by the wood board substrate, thereby further improving the yield and structural stability of the floor after processing.

[0047] Embodiment 3. The processing technology of the mangosteen thin floor (910*118*15mm) comprises the following steps:

[0048] ① Select a board with a length of 920mm, a width of 129mm, a thickness of 16mm, and a moisture content of 15% as the board substrate (the right angle of the board substrate is better), and the air-dry density of the board substrate is 0.6g / cm 3 , the compressive strength of the wood substrate along the grain is 50MPa, the flexural strength of the wood substrate is 102.8MPa, and the flexural elastic modulus of the wood substrate is 12069MPa; A board is obtained;

[0049] ② Heat-treat plate A at 135°C, so that the moisture content of plate A after heat treatment is 8%, and the width of plate A after heat treatment is 126.23 mm, thereby obtaining plate B;

[0050] ③Put plate B in a drying kiln at 35℃ and let it stand for 30 hours, then open one of the exhaust holes of the drying kiln to exhaust the air, and then let it stand for 25 days before taking it out of the kiln. The humidity of the drying kiln during drying is 35%, and plate C is obtained;

[0051] ④ Slot the four side walls of the C plate respectively, and then make a transverse back groove on one side of the C plate. The number of transverse back grooves is 4, and the D plate is obtained;

[0052] ⑤ First spray water-based paint on the side walls around the D board, then apply UV paint on the front and back of the D board, and finally press PE moisture-proof film layer on one side of the horizontal back groove and the long side walls on both sides of the D board. The pressure of the PE moisture-proof film layer during pressing is 500N, and the finished floor is obtained.

[0053] The present invention sets the corresponding size parameters of the wood board substrate according to the material of the mangosteen, so that the floor can maintain good size parameters and performance after processing.

[0054] Embodiment 4. The processing technology of the thin oak floor (800*125*12mm) comprises the following steps:

[0055] ① Select a board with a length of 815mm, a width of 140mm, a thickness of 13.5mm, and a moisture content of 12% as the board substrate (the right angle of the board substrate is poor), and the air-dry density of the board substrate is 0.76g / cm 3 , the compressive strength along the grain of the wood substrate is 54MPa, the flexural strength of the wood substrate is 106MPa, and the flexural elastic modulus of the wood substrate is 12273MPa; A board is obtained;

[0056] ② Heat-treat plate A at 145°C, so that the moisture content of plate A after heat treatment is 7%, and the width of plate A after heat treatment is 137.8 mm, thereby obtaining plate B;

[0057] ③Put plate B in a drying kiln at 45℃ and let it stand for 20 hours, then open one of the exhaust holes of the drying kiln to exhaust the air, and then let it stand for 18 days before taking it out of the kiln. The humidity of the drying kiln during drying is 45%, and plate C is obtained;

[0058] ④ Slot the four side walls of the C plate respectively, and then make a transverse back groove on one side of the C plate. The number of transverse back grooves is 3, and the D plate is obtained;

[0059] ⑤ First spray water-based paint on the side walls around the D board, then apply UV paint on the front and back of the D board, and finally press PE moisture-proof film layer on one side of the horizontal back groove and the long side walls on both sides of the D board. The pressure of the PE moisture-proof film layer during pressing is 600N, and the finished floor is obtained.

[0060] The present invention sets the corresponding size parameters of the wood board substrate according to the material of the oak, so that the floor can maintain good size parameters and performance after processing.

[0061] Embodiment 5. The processing technology of the round bean thin floor (600*60*16mm) comprises the following steps:

[0062] ① Select a board with a length of 612mm, a width of 70mm, a thickness of 17mm, and a moisture content of 12% as the board substrate. The air-dry density of the board substrate is 1.07g / cm 3 , the compressive strength of the wood substrate along the grain is 76MPa, the flexural strength of the wood substrate is 128.9MPa, and the flexural elastic modulus of the wood substrate is 19448MPa; A board is obtained;

[0063] ② Heat-treat plate A at 135°C, so that the moisture content of plate A after heat treatment is 9% and the width of plate A after heat treatment is 69.2 mm, thereby obtaining plate B;

[0064] ③Put plate B in a drying kiln at 45℃ and let it stand for 30 hours, then open one of the exhaust holes of the drying kiln to exhaust the air, and then let it stand for 25 days before taking it out of the kiln. The humidity of the drying kiln during drying is 35%, and plate C is obtained;

[0065] ④ Slot the four side walls of the C plate respectively, and then make two transverse back grooves on one side of the C plate, and obtain the D plate;

[0066] ⑤ First spray water-based paint on the side walls around the D board, then apply UV paint on the front and back of the D board, and finally press PE moisture-proof film layer on one side of the horizontal back groove and the long side walls on both sides of the D board. The pressure of the PE moisture-proof film layer during pressing is 700N, and the finished floor is obtained.

[0067] The present invention sets the size parameters of the corresponding wood board substrate according to the material of the round bean, so that the floor can maintain good size parameters and performance after processing.

[0068] Example 6. The processing technology of the New Dundou thin floor (1200*120*15mm) comprises the following steps:

[0069] ① Select a board with a length of 1210mm, a width of 131mm, a thickness of 16mm, and a moisture content of 11% as the board substrate. The air-dry density of the board substrate is 0.81g / cm 3 , the compressive strength of the wood substrate along the grain is 62MPa, the flexural strength of the wood substrate is 114MPa, and the flexural elastic modulus of the wood substrate is 14200MPa; A board is obtained;

[0070] ② Heat-treat plate A at 145°C, so that the moisture content of plate A after heat treatment is 9% and the width of plate A after heat treatment is 130 mm, thereby obtaining plate B;

[0071] ③Put plate B in a drying kiln at 35℃ and let it stand for 20 hours, then open one of the exhaust holes of the drying kiln to exhaust the air, and then let it stand for 18 days before taking it out of the kiln. The humidity of the drying kiln during drying is 45%, and plate C is obtained;

[0072] ④ Slot the four side walls of the C plate respectively, and then make a transverse back groove on one side of the C plate. The number of transverse back grooves is 4, and the D plate is obtained;

[0073] ⑤ First spray water-based paint on the side walls around the D board, then apply UV paint on the front and back of the D board, and finally press PE moisture-proof film layer on one side of the horizontal back groove and the long side walls on both sides of the D board. The pressure of the PE moisture-proof film layer during pressing is 800N, and the finished floor is obtained.

[0074] The present invention sets the corresponding size parameters of the wood board substrate according to the material of the wood, so that the floor can maintain good size parameters and performance after processing.

[0075] Experimental example: In the present invention, a group of comparative experimental groups is formed by using 48 pieces of mangosteen material and a size of 910*118*15mm on a wooden board, and a total of 8 comparative experimental groups are set up; then, as shown in Table 1, different process treatments are performed on each comparative experimental group, and then wet swelling or dry shrinkage treatment is performed on it. The experimental time is 6 months, and the experimental results are measured after the treatment.

[0076] Table 1 Processing and treatment processes of different experimental groups

[0077]

[0078]

[0079] The heat treatment is the process treatment described in step ② of the present invention, the stress groove is the transverse back groove opened on one side of the wooden board in step ④ of the present invention, and the coating is the PE moisture-proof film layer pressed on one side of the transverse back groove and the long side walls on both sides of the wooden board in step ⑤ of the present invention.

[0080] The influence of different processes on board shape: The present invention detects the warpage of different comparative experimental groups according to the detection method described in "GB / T 15036.2-2009 Solid Wood Flooring Part 2 Detection Method". And according to the detection standard in "GB / T 15036.1-2009 Solid Wood Flooring Part 1 Technical Requirements" (convex warpage in width direction ≤ 0.2%, concave warpage ≤ 0.15; convex warpage in length direction ≤ 1%, concave warpage ≤ 0.5%); the convex warpage in the width direction of the floor ≤ 0.2%, concave warpage ≤ 0.15%, the convex warpage of a single piece in the length direction ≤ 0.5%, concave warpage ≤ 0.25% is the standard value, and if only one of them is reached, it is considered that the board shape is warped.

[0081] The test results are shown in Table 2 and Table 3: The warping rate is the ratio of the number of warped wood boards in each comparison test group to the total number (48 pieces). The wet expansion warping rate of the heat-treated floor decreased by 12.50%, the performance optimization range was 54.55%, the single-piece warping decreased by 0.1%, and the performance optimization range was 31.25%. The dry shrinkage warping rate decreased by 12.5%, the performance optimization range was 60%, the single-piece warping decreased by 0.09%, and the performance optimization range was 32.14%.

[0082] After the stress grooves were opened, the floor's wet expansion warping rate decreased by 8.33%, the performance optimization range was 44.44%, the single piece warping decreased by 0.08%, the performance optimization range was 26.67%. The dry shrinkage warping rate decreased by 6.25%, the performance optimization range was 42.86%, the single piece warping decreased by 0.07%, the performance optimization range was 26.92%.

[0083] After coating, the wet expansion warping rate of the floor decreased by 20.83%, the performance optimization range was 66.67%, the single piece warping decreased by 0.13%, the performance optimization range was 37.14%. The dry shrinkage warping rate decreased by 10.42%, the performance optimization range was 55.56%, the single piece warping decreased by 0.14%, the performance optimization range was 42.42%.

[0084] The experimental results show that the present invention can effectively improve the yield and processing stability of the finished floor after heat treatment of the wood substrate, opening horizontal back grooves and pressing a moisture-proof film layer, and make the finished floor have good working stability and service life when in use.

[0085] Table 2 Comparison of warpage rate and single piece warpage of different comparative experimental groups after wet swelling treatment

[0086]

[0087] Table 3 Comparison of warpage rate and single piece warpage of different comparative experimental groups after shrinkage treatment

[0088]

[0089] Effect of different processes on moisture content and dimensional change: The present invention tests the size and moisture content of each comparative experimental group after wet expansion or shrinkage, and the test results are shown in Tables 4 and 5: Wet expansion or shrinkage stability coefficient = size change rate / moisture content change*100%. The increase in moisture content of the heat-treated floor after wet expansion treatment decreased by 0.1%, and the performance optimization range was 3.57%; the size change range decreased by 0.26%, and the performance optimization range was 23.21%; the wet expansion stability coefficient increased by 0.08, and the performance optimization range was 20.37%.

[0090] The moisture content of the floor after heat treatment decreased by 0.97% after shrinkage treatment, and the performance was optimized by 30.11%; the size change decreased by 0.52%, and the performance was optimized by 43.33%; the shrinkage stability coefficient increased by 0.07, and the performance was optimized by 18.92%. The experimental results show that the heat treatment in step ② of the present invention can effectively reduce the size change and moisture content change of the floor during the working process, so that the present invention can have good working stability and service life in different environments.

[0091] After the horizontal back groove was opened, the moisture content of the floor after wet swelling treatment decreased by 0.3%, and the performance optimization range was 10% (during the six-month experiment, the highest value was 15.01%); the dimensional change range decreased by 0.16%, and the performance optimization range was 15.69% (the highest value was 26.31%); the wet swelling stability coefficient increased by 0.02, and the performance optimization range was 6.32%.

[0092] The moisture content of the floor with horizontal back grooves after shrinkage treatment decreased by 0.03%, and the performance optimization was 1.43% (the highest value was 8.61%); the size change decreased by 0.08%, and the performance optimization was 10.53% (the highest value was 20.41%); the shrinkage stability coefficient increased by 0.03, and the performance optimization was 9.09%. On the 110th-125th day of the experiment, the size change rate and moisture content performance of the floor with horizontal back grooves reached the maximum value compared with the floor without horizontal back grooves, and then began to decline and basically stabilized after 150 days. The experimental results show that the horizontal back groove has little effect on the stability coefficient of the floor, but can effectively delay the size change of the floor during the working process, thereby improving the working stability of the floor.

[0093] The moisture content of the floor covered with a moisture-proof film layer after wet swelling treatment decreased by 1.36%, and the performance was optimized by 33.42%; the size change decreased by 0.6%, and the performance was optimized by 41.10%; the wet swelling stability coefficient increased by 0.04, and the performance was optimized by 11.52%.

[0094] The moisture content of the floor covered with the moisture-proof film layer after shrinkage treatment decreased by 1%, and the performance optimization range was 30.64%; the size change range decreased by 0.4%, and the performance optimization range was 37.04%; the shrinkage stability coefficient increased by 0.03, and the performance optimization range was 9.09%. The experimental results show that the floor can effectively slow down the size change range and moisture content change range of the floor during the working process after the moisture-proof film layer is pressed, thereby improving the working stability of the present invention.

[0095] Table 4 Comparison of size change rate and moisture content of different comparative experimental groups after wet swelling treatment

[0096]

[0097]

[0098] Table 5 Comparison of dimensional change rate and moisture content of different comparative experimental groups after shrinkage treatment

[0099]

[0100] It can be seen from the above experiments that the present invention can effectively reduce the size change rate, warping rate, warping amplitude and moisture content change amplitude of the floor in different environments through the cooperation of heat treatment, transverse back groove and moisture-proof film layer, so that the present invention has good structural stability and anti-deformation ability when working, and the moisture content in the floor can be maintained in the optimal range for a long time, with good working stability and long service life.

Claims

1. A processing technology for anti-stress thin floor, characterized in that: The following steps are involved: ① Set the required length of the finished plain board to a, the width of the finished plain board to b, and the thickness of the finished plain board to c; select a board with a length of a+10~15mm, a width of b+10~15mm, a thickness of c+1.0~1.5mm, and a moisture content of 12~15% as the board substrate; obtain board A; ② Heat-treat plate A at 130-145°C to make the moisture content of plate A 7-9% after heat treatment, and obtain plate B; ③Put plate B in a drying kiln at 35-45℃ and let it stand for 20-30 hours, then open the exhaust hole of the drying kiln, let it stand for another 18-25 days and then take it out of the kiln to obtain plate C; ④ Slot the four side walls of the C plate respectively, and then make a transverse back groove on one side of the C plate to obtain the D plate; ⑤ Paint and apply moisture-proof film to the D board in sequence to obtain the finished floor; In step ③, the humidity of the drying kiln during drying is 35-45%; The specific steps of step ⑤ are: first spray water-based paint on the side walls around the D board, then apply UV paint on the front and back of the D board, and finally press PE moisture-proof film layer on one side of the horizontal back groove and the long side walls on both sides of the D board to obtain a finished board; In step ⑤, the pressure of the PE moisture-proof film layer during lamination is 500-700N; In the step ①, the convex curvature of the wood substrate in the length direction is not greater than 6‰ of the length of the wood substrate, the concave curvature of the wood substrate in the length direction is not greater than 3‰ of the length of the wood substrate, the convex curvature of the wood substrate in the width direction is not greater than 2‰ of the width of the wood substrate, and the concave curvature of the wood substrate in the width direction is not greater than 1.5‰ of the width of the wood substrate; The stress-resistant thin floor is obtained by processing according to the processing technology of the stress-resistant thin floor, comprising a board body (1), the thickness of the board body (1) is 10-16 mm, a plurality of transverse back grooves (2) perpendicular to the length direction of the board body (1) are evenly distributed on the back side of the board body (1), a moisture-proof film layer (3) is provided on the outside of the transverse back grooves (2) and located on the back side and the long sides of the board body (1), the thickness of the transverse back grooves (2) is 2 mm, the depth of the transverse back grooves (2) is one third of the thickness of the board body (1), the spacing between adjacent transverse back grooves (2) is the same, and the spacing between the short side wall of the board body (1) and the transverse back groove (2) is the same as the spacing between adjacent transverse back grooves (2); The two long sides of the plate body (1) are respectively provided with a first female groove (4) and a first male groove (5) that cooperate with each other, and the two short sides of the plate body (1) are respectively provided with a second female groove (6) and a second male groove (7) that cooperate with each other; The moisture-proof film layer (3) comprises a first moisture-proof film layer (301), a second moisture-proof film layer (302) and a third moisture-proof film layer (303) which are connected to each other, the first moisture-proof film layer (301) being pressed onto the side wall of the plate body (1) close to the first male groove (5), the second moisture-proof film layer (302) being pressed onto the back side of the plate body (1), and the third moisture-proof film layer (303) being pressed onto the side wall of the plate body (1) between the first female groove (4) and the back side; The moisture-proof film layer (3) is a PE moisture-proof film layer, and the thickness of the moisture-proof film layer (3) is 0.07-0.08 mm; When the length of the plate body (1) is not greater than 600 mm, the number of the transverse back grooves (2) is two; when the length of the plate body (1) exceeds 600 mm and is not greater than 900 mm, the number of the transverse back grooves (2) is three; when the length of the plate body (1) exceeds 900 mm and is not greater than 1200 mm, the number of the transverse back grooves (2) is four; when the length of the plate body (1) exceeds 1200 mm, the number of the transverse back grooves (2) increases by one for every 300 mm increase in the length of the plate body (1).

Citation Information

Patent Citations

  • Method for manufacturing solid wood multilayer composite floor

    CN103496023A

  • Solid wood floor

    CN107795096A