Stainless steel alloys and turbocharger kinematic components formed of stainless steel alloys
By using stainless steel alloys of specific components, the turbocharger kinematic components reduce friction and wear at high temperatures and extend service life, solving the problem of vulnerability of components in the prior art.
Patent Information
- Application Number
- CN201810547630.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-05-31
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2038-05-31
AI Technical Summary
Kinematic components in turbochargers are susceptible to friction and wear at high temperatures, resulting in reduced service life.
Turbocharged alloys using sintering process using stainless steel alloys containing 20% to 35% chromium, 10% to 15% nickel, 10% to 15% cobalt, 2.0% to 4.0% carbon, 0.4% to 2.5% silicon and balanced iron Pressure kinematic components to reduce friction and improve wear resistance.
The friction and wear of kinematic components is significantly reduced under high temperature conditions, extends the service life of the components, and improves the efficiency of the turbocharger.
Smart Images

Figure CN109385565B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates generally to iron-based alloys, such as stainless steel alloys, and articles formed therefrom. More particularly, the present disclosure relates to stainless steel alloys used, for example, in sintering applications, such as turbine and turbocharger kinematic components, wherein such kinematic components exhibit reduced friction and increased wear resistance at elevated (turbocharger operating) temperatures. Background Art
[0002] In the context of a turbine engine, a turbocharger uses the heat and volume flow of the engine exhaust to pressurize or boost the intake air flow entering the combustion chamber. Specifically, the exhaust from the engine is routed into the turbine housing of the turbocharger. The turbine is mounted inside the housing, and the exhaust flow causes the turbine to rotate. The turbine is mounted on one end of a shaft that has a radial air compressor mounted on its opposite end. Therefore, the rotational action of the turbine also causes the air compressor to rotate. The rotational action of the air compressor causes intake air to enter the compressor housing and be pressurized or boosted before the intake air is mixed with fuel and burned in the engine combustion chamber.
[0003] Various systems within a turbocharger include tribological interfaces, i.e., surfaces of components that interact with each other and move relative to each other when the turbocharger is in operation. Such components, which are often referred to as kinematic components, are susceptible to friction and wear, especially at elevated temperatures, which reduces their useful life. Examples of turbocharger systems that may include kinematic components include wastegate systems, which divert exhaust away from the turbine to adjust the air flow to the turbine, and variable geometry systems, which include a row of movable inlet vanes to achieve the same purpose. These systems typically include various components, such as shafts, bushings, valves, etc., which are kinematic components and are therefore subject to friction and wear because they interact with each other and move relative to each other.
[0004] Accordingly, it is desirable to provide materials suitable for use in the manufacture of kinematic components for turbine engines that exhibit reduced friction during relative motion with each other and resist wear during operation at elevated temperatures. Additionally, other desirable features and characteristics of the inventive subject matter will become apparent from the subsequent detailed description of the inventive subject matter and the appended claims, taken in conjunction with the accompanying drawings and this background of the inventive subject matter. Summary of the invention
[0005] Stainless steel alloys and turbocharger kinematic components made from the alloys (eg, by sintering) are provided.
[0006] In an embodiment, by way of example only, the stainless steel alloy includes, by weight: about 20% to about 35% chromium; about 10% to about 15% nickel; about 10% to about 15% cobalt; about 10% to about 15% molybdenum; about 2.0% to about 4.0% carbon; about 0.4% to about 2.5% silicon; about 0.0% to about 1.0% niobium; and the balance iron and other necessary / unavoidable impurities.
[0007] In another embodiment, by way of example only, a turbocharger kinematic component is made of an alloy comprising a stainless steel alloy, which itself comprises, by weight: about 20% to about 35% chromium; about 10% to about 15% nickel; about 10% to about 15% cobalt; about 10% to about 15% molybdenum; about 2.0% to about 4.0% carbon; about 0.4% to about 2.5% silicon; about 0.0% to about 1.0% niobium; and the balance iron and other necessary / unavoidable impurities.
[0008] This summary is provided to introduce a series of concepts in a simplified form, which are further described below in the detailed description. This summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used as an aid in determining the scope of the claimed subject matter. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] The inventive subject matter will hereinafter be described in conjunction with the following drawings, wherein like reference numerals indicate like elements, and wherein:
[0010] Figure 1 is a system view of an embodiment of an internal combustion engine of a turbocharger according to the present disclosure;
[0011] Figure 2 yes Figure 1 a cross-sectional view of an internal combustion engine of a turbocharger; and
[0012] Figure 3 is a system diagram of a turbocharger including a wastegate system according to the present disclosure. DETAILED DESCRIPTION
[0013] The following detailed description is merely exemplary in nature and is not intended to limit the invention or the present application and the use of the invention. As used herein, the word "exemplary" means "serving as an example, instance or illustration". Therefore, any embodiment described as "exemplary" in this article is not necessarily interpreted as being preferred or advantageous over other embodiments. As used herein, numerical ordinals such as "first", "second", "third", etc., such as first, second and third components, only represent different singles in a plurality, unless specifically limited by the language in the attached claims. In addition, as used herein, the term "about" means, in one embodiment, an absolute change of + / -5% of the stated value, while in other embodiments, the term "about" can be omitted and the exact value (as stated) is adopted. All percentages herein are given by weight of the total alloy.
[0014] All stainless steel alloys described herein may be understood as: (1) "comprising" the recited elements in varying percentages of the recited elements in an open context; or (2) "consisting of" the recited elements in varying percentages in a closed context. Alternatively, the stainless steel alloys described herein may be understood as: (3) "consisting essentially of" the recited elements in varying percentages thereof, with other elements being present in amounts that do not affect the novel / unobvious properties of the alloy. Therefore, as used herein, the terms "comprising," "consisting of," and "consisting essentially of" should be understood to apply to all ranges of alloy compositions disclosed herein.
[0015] All embodiments and implementations of the stainless steel alloy, turbocharger kinematic components, and methods for manufacturing the same described herein are exemplary embodiments, which are provided to enable those skilled in the art to make or use the present invention, and do not limit the scope of the present invention as defined by the claims. Of course, the described embodiments should not be considered to be limited to such components, but rather may be considered to be applicable to any product in which an iron alloy or a stainless steel alloy may be used. In addition, it is not intended to be limited by any representation or implied theory presented in the aforementioned technical field, background technology, summary of the invention, or the following specific embodiments.
[0016] As noted above, the present disclosure relates to stainless steel alloys used in kinematic components of turbochargers for the purpose of reducing friction and wear associated with the use and implementation of said kinematic components. As further noted above, variable geometry turbochargers (and possibly other turbocharger systems) employ such kinematic components. Accordingly, for completeness of description, Figure 1A portion of a variable geometry turbocharger (VGT) 10 is illustrated, which includes a turbine housing 12 having a standard inlet 14 for receiving an exhaust gas flow and an outlet 16 for directing the exhaust gas to the exhaust system of the engine. A volute is connected to the exhaust inlet, and an integral outer nozzle wall is included in the turbine housing cast adjacent to the volute. A turbine wheel 17 and a shaft assembly 18 are supported within the turbine housing 12. Exhaust gas or other high energy gas supplying the turbocharger enters the turbine housing through the inlet 14 and is distributed in the turbine housing by the volute for generally radial transmission to the turbine wheel through a circumferential nozzle inlet 20.
[0017] A plurality of vanes 22 are mounted to a nozzle wall 24, which is machined into the turbine housing, with shafts 26 protruding vertically outward from the vanes. The shafts 26 are rotationally engaged within corresponding openings 28 in the nozzle wall. The vanes each include an actuation tab 30, which protrudes from the side opposite the shaft and is engaged by a corresponding groove 32 in a unison ring 34, which acts as a second nozzle wall. The tabs 30, grooves 32, and other described components move relative to each other, and thus, for tribological purposes, it would be desirable to reduce friction between them.
[0018] Figure 2 The general movement pattern of a conventional vane 36 used in a VGT as described and illustrated above when actuated by the synchro ring 34 is illustrated. Each vane tab 42 is disposed within a corresponding elongated slot 38 of the synchro ring 40. In the closed position "A", the vane tab 42 is located adjacent to the first end 44 of the slot 38. This position is referred to as a closed position because the vanes are not radially spread outward, thereby serving to restrict the flow of exhaust gas to the turbine. At the intermediate position "B", the synchro ring 40 has been rotated a sufficient amount such that the vane tab 42 moves within the slot 38 away from the first slot end 44 (as opposed to the second slot end 46) toward the intermediate position of the slot. Likewise, as components of the vane 36 move relative to components of the synchro ring 40, it will be desirable to reduce friction for tribological purposes.
[0019] Additionally, as noted above, the wastegate system may also include tribological components, and thus, for completeness of disclosure, Figure 3 An exemplary wastegate system is illustrated. Specifically, Figure 3A cross-sectional view of an example of an assembly 300 is shown, the assembly 300 including a turbine housing component 320 and a wastegate 380. In the assembly 300, the turbine housing component 320 includes an opening 340, for example, as defined by a surface 332 of a generally cylindrical wall portion 330 of the turbine housing component 320. As shown, the wall 332 extends to an edge (e.g., defining the opening 340) and then flattens to join a relatively flat surface 334, which may be referred to as a wastegate seat. Figure 3 In the example of , the surface 332 defines, for example, a relatively short channel having an axis (e.g., the z-axis), and the surface 332 is arranged at a radial distance therefrom (e.g., the r-axis). The seat 334 extends away from the opening 340 and descends along another surface 336 (e.g., of the generally cylindrical wall portion 330) to a floor 348 of an exhaust chamber, which is partially formed by the turbine housing component 320, for example, in combination with the wall surface 346. Figure 3 As shown in FIG. , the wall surface 346 of the turbine housing component 320 rises to the edge of the opening 349 that defines the exhaust chamber and then extends outward to a relatively flat surface 328, which may include one or more apertures, such as aperture 325, for example to enable another component to be attached to the turbine housing component 320.
[0020] exist Figure 3 In the example of , the wastegate 380 includes a plug portion 382 connected to a wastegate arm 390. The plug portion 382 includes a lower surface 381, a rod 383 extending upward to an upper end 385 of the plug portion 382, and an edge surface 384 (e.g., disposed at a radius around the rod 383 and having an axial height). As shown, the rod 383 is received by a hole 393 of the wastegate arm 390, wherein the hole 393 extends between the lower surface 391 and the upper surface 395 of the wastegate arm 390. Figure 3 In the example of FIG. 3 , the clamping washer 387 clamps to the rod 383 of the plug portion 382 to thereby prevent the rod 383 from sliding through the hole 393 of the wastegate arm 390. Accordingly, when the wastegate arm 390 pivots, the lower surface 381 of the plug portion 382 is positioned relative to the seat 334 of the turbine housing component 320 for opening and closing the wastegate 380.
[0021] Typical embodiments of the present disclosure are in motor vehicles equipped with a gasoline or diesel powered internal combustion engine and a turbocharger. The turbocharger is equipped with a unique combination of features that can provide efficiency benefits in various embodiments by relatively limiting the amount (and kinetic energy) of secondary flows in the turbine and / or compressor compared to comparable unmodified systems. The stainless steel alloys used in the turbocharger can have an operating temperature of up to about 1050°C (or up to about 1100°C) or greater. Some embodiments of the present disclosure are directed to stainless steel alloys including iron alloyed with various alloying elements, as described in more detail below in weight percentages based on the total weight of the alloy.
[0022] In an embodiment, the stainless steel alloy of the present disclosure includes from about 20% to about 35% chromium (Cr), for example, from about 22% to about 33% Cr, such as about 24% to about 31% Cr, for example, about 26% to about 29% Cr. Specific embodiments may employ about 27.5% Cr. It is also possible to range from about 20% to about 22% Cr, about 22% to about 24% Cr, about 24% to about 26% Cr, about 26% to about 28% Cr, about 28% to about 30% Cr, about 30% to about 32% Cr, about 32% to about 35% Cr. It has been found that if Cr is excessively added, coarse primary carbides of Cr are formed, resulting in extreme brittleness. Thus, the Cr content is preferably limited to a maximum of about 35% in order to maintain an appropriate volume fraction for corrosion resistance in the stainless steel.
[0023] In an embodiment, the stainless steel alloy of the present disclosure includes nickel (Ni) from about 10% to about 15%, such as about 11% to about 14% Ni, such as about 12% to about 13% Ni. Specific embodiments may use about 12.5% Ni. It is also possible to range from about 10% to about 11.5% Ni, about 11.5% to about 13% Ni, and about 13% to about 15% Ni. Ni, together with optional nitrogen (which is described in more detail below), is an element that stabilizes the austenite phase. In order to reduce manufacturing costs, if the content of expensive Ni is reduced, the reduction of Ni can be replaced by increasing the content of optional nitrogen that forms the austenite phase. However, if the content of Ni is excessively reduced, the optional nitrogen will be excessively required, thereby deteriorating corrosion resistance and hot forming properties. Therefore, the content of Ni preferably ranges from about 10% to about 15%.
[0024] In an embodiment, the stainless steel alloy of the present disclosure includes from about 10% to about 15% molybdenum (Mo), such as about 11% to about 14% Mo, for example about 12% to about 13% Mo. Specific embodiments may utilize about 12.5% Mo. It is also possible to range from about 10% to about 11.5% Mo, about 11.5% to about 13% Mo, and about 13% to about 15% Mo. Since molybdenum also increases the risk of forming intermetallic phases, the level should be up to 15%, and preferably less than 14%. If the content of Mo is too much, Mo may form σ phase when it is annealed, thereby deteriorating corrosion resistance and impact resistance, which is harmful to the tribological performance of the kinematic components of the turbocharger described herein.
[0025] In an embodiment, the stainless steel alloy of the present disclosure includes from about 10% to about 15% cobalt (Co), such as about 11% to about 14% Co, such as about 12% to about 13% Co. Specific embodiments may employ about 12.5% Co. It is also possible to range from about 10% to about 11.5% Co, about 11.5% to about 13% Co, and about 13% to about 15% Co. As found herein, the presence of Co in an amount greater than about 10% in stainless steel improves the durability and hardness of stainless steel at higher temperatures, and is therefore included herein in an amount of 10% or more. However, stainless steel with an amount of Co greater than about 15% has a slightly greater decarburization tendency and is more sensitive to cracking when exposed to abrupt temperature changes, and thus, the present disclosure is limited to Co in an amount of about 15% or less.
[0026] Compared to stainless steel alloys known in the prior art, it should be understood that the stainless steel alloys disclosed herein generally include a relatively low amount of Ni and a relatively low amount of Co, and a relatively high amount of Mo. Therefore, as between Ni, Co and Mo, specific embodiments may employ an amount of Ni including an amount / range of 13% or less, such as an amount / range of 12.5% or less; these embodiments may also employ an amount of Co including an amount / range of 13% or less, such as an amount / range of 12.5% or less; in addition, these embodiments may also employ an amount of Mo including an amount / range of 12% or more, such as an amount / range of 12.5% or more.
[0027] In an embodiment, the stainless steel alloy of the present disclosure includes from about 2.0% to about 4.0% carbon (C), for example, about 2.5% to about 3.5% C. Specific embodiments may use about 3.0% C. C has the function of improving the sintering ability of the alloy. When present in a relatively high disclosed range, C also forms eutectic carbides with niobium (as discussed in more detail below, which may also be included in the alloy), which improves wear resistance. In order to effectively exhibit such a function, the amount of C should be 2.0% or more. In addition, C is effective for strengthening the material by solid solution strengthening (solid solution strengthening). In order to maximize corrosion resistance, the content of C is reduced to about 4.0% and below.
[0028] In an embodiment, the stainless steel alloy of the present disclosure includes from about 0.4% to about 2.5% silicon (Si), for example, about 1.0% to about 2.0% Si. Specific embodiments may use about 1.5% Si. Si has the effect of increasing the structural stability of the alloy metal and its oxidation resistance. In addition, when present in an amount greater than about 0.4%, Si has the function of a deoxidizer and is also effective for improving castability and reducing pinholes in the resulting sintered product. If the content of Si is too much, Si deteriorates the mechanical properties of the stainless steel, such as impact toughness. Therefore, the content of Si is preferably limited to about 2.5% and below.
[0029] In an embodiment, the stainless steel alloy of the present disclosure includes from about 0.0% to about 1.0% niobium (Nb), such as from about 0.3% to about 0.7% Nb. It has been found that high castability, as well as high strength and ductility are provided to the friction-resistant and wear-resistant stainless steel of the present disclosure by forming eutectic carbides of Nb, and thus, in an embodiment, Nb is present in an amount of about 0.5%. However, as indicated by the lower range end of 0.0%, embodiments are contemplated in which Nb is absent.
[0030] Certain necessary / unavoidable impurities may also be present in the stainless steel alloys of the present disclosure, for example, as described below with respect to phosphorus, sulfur, and nitrogen (the amounts of such impurities (and others) should be minimized as far as practicable).
[0031] In an embodiment, phosphorus (P) may be present in the alloy, but is minimized to about 0.03% or less. P is scattered in grain boundaries or interfaces and may deteriorate corrosion resistance and toughness. Therefore, the content of P is reduced as much as possible. Preferably, considering the efficiency of the refining process, the upper limit content of P is limited to 0.03%. The content of harmful impurities such as P should be as small as possible. However, due to cost considerations associated with removing these impurities, the P content is limited to 0.03%.
[0032] In an embodiment, sulfur (S) may be present in the alloy, but is minimized to about 0.03% or less. S in steel degrades hot workability and may form sulfide inclusions that adversely affect pitting corrosion resistance. Therefore, it should be limited to less than 0.03%. S degrades hot workability, thereby degrading corrosion resistance. Therefore, the content of S is reduced as much as possible. The content of harmful impurities such as S (sulfur) should be as small as possible. However, due to cost considerations associated with removing these impurities, the S content is limited to about 0.03%.
[0033] Nitrogen (N) is an element that can improve high temperature strength and thermal fatigue resistance like C, and such effects can be achieved when the amount of N is 0.01% or more. However, N is optional and does not need to be included in any amount. On the other hand, in order to ensure production stability and avoid brittleness caused by precipitation of nitrides of Cr, the upper limit of N should be about 0.03%. N, together with Ni, is one of the elements that contribute to the stability of the austenite phase. As the content of N increases, corrosion resistance and high strengthening are achieved. However, when the content of N is too high, the hot formability of the steel deteriorates, thereby reducing its product yield. Therefore, the preferred range of the content of N is up to a maximum of about 0.03%, although it does not need to be included at all.
[0034] Additionally, it should be understood that although entirely optional, boron (B), calcium (Ca), and cerium (Ce) may be added / (present) in the disclosed steels in very small amounts to improve hot workability. For B, Ca, and Ce, if included, the preferred levels are less than about 0.005% each individually.
[0035] Other elements that may be included in some stainless steels known in the prior art may be specifically excluded (or substantially excluded and / or effectively excluded) from the stainless steel alloys of the present disclosure. These excluded elements include, for example, one or more of the following: manganese (Mn), tungsten (W) and / or vanadium (V).
[0036] The disclosed alloys, i.e., stainless steel alloys, also include a balance of iron (Fe). As used herein, the term "balance" refers to the amount remaining to achieve 100% of the total alloy in terms of weight. It should be understood that in the case of a balance with Fe, if an embodiment "comprises" the element, "consists of" the element, or "consists essentially of" the element, the amount will be different.
[0037] The articles described herein, such as kinematic components of a turbocharger made using the stainless steel alloy described above, can be formed using a sintering process. For example, as known in the art, sintering refers to a process in which a solid block of material is compacted and formed by heat and / or pressure without melting the material to a liquefaction point.
[0038] Thus, embodiments of the present disclosure provide materials suitable for use in the manufacture of kinematic components for turbine engines that exhibit reduced friction during relative motion with respect to one another and resist wear during operation at elevated temperatures. As noted above, examples of kinematic components that may be included for turbocharger systems include wastegate systems and variable geometry systems. Of course, the described embodiments should not be considered limited to such components, but rather may be considered applicable to any article in which an iron alloy or stainless steel alloy may be employed.
[0039] Although at least one exemplary embodiment is given in the above detailed description of the inventive subject matter, it should be understood that there are many variations. It should also be understood that the exemplary embodiment or multiple exemplary embodiments are only examples and are not intended to limit the scope, applicability or configuration of the inventive subject matter in any way. More specifically, the above detailed description will provide a convenient roadmap for implementing the exemplary embodiments of the inventive subject matter to those skilled in the art. It should be understood that various changes can be made in the functions and arrangement structures of the elements described in the exemplary embodiments without departing from the scope of the inventive subject matter as stated in the appended claims.
Claims
1. An iron-based alloy comprising, by weight: 20% to 35% chromium; 10% to 15% nickel; 10% to 15% cobalt; 10% to 15% molybdenum; 2.0% to 4.0% carbon; 0.4% to 2.5% silicon; 0.0% to 1.0% niobium; and A balance of iron and necessary / unavoidable impurities, in which elemental manganese is excluded from the iron-based alloy.
2. The iron-based alloy of claim 1, comprising 22% to 33% chromium.
3. The iron-based alloy of claim 1 comprising 24% to 31% chromium.
4. The iron-based alloy of claim 1 comprising 26% to 29% chromium.
5. The iron-based alloy of claim 1 comprising 11% to 14% nickel.
6. The iron-based alloy of claim 1 comprising 12% to 13% nickel.
7. The iron-based alloy of claim 1 comprising 11% to 14% cobalt.
8. The iron-based alloy of claim 1 comprising 12% to 13% cobalt.
9. The iron-based alloy of claim 1 comprising 11% to 14% molybdenum.
10. The iron-based alloy of claim 1 comprising 12% to 13% molybdenum.
11. The iron-based alloy of claim 1 comprising 1.0% to 2.0% silicon.
12. The iron-based alloy of claim 1 comprising 2.5% to 3.5% carbon.
13. The iron-based alloy of claim 1 comprising 0.3% to 0.7% niobium.
14. A turbocharger kinematic component, comprising: A sintered iron-based alloy, wherein the sintered iron-based alloy comprises, by weight: 20% to 35% chromium; 10% to 15% nickel; 10% to 15% cobalt; 10% to 15% molybdenum; 2.0% to 4.0% carbon; 0.4% to 2.5% silicon; 0.0% to 1.0% niobium; and A balance of iron and necessary / unavoidable impurities, in which elemental manganese is excluded from the iron-based alloy.
15. The turbocharger kinematic component of claim 14 comprising 26% to 29% chromium.
16. The turbocharger kinematic component of claim 14 comprising 12% to 13% nickel.
17. The turbocharger kinematic component of claim 14 comprising 12% to 13% cobalt.
18. The turbocharger kinematic component of claim 14 comprising 12% to 13% molybdenum.
19. The turbocharger kinematic component of claim 14 comprising 1.0% to 2.0% silicon.
20. The turbocharger kinematic component of claim 14 comprising 2.5% to 3.5% carbon.
Citation Information
Patent Citations
Fe base alloy for cladding by welding
JP1994297188A
Wastegate valve and method for installing a wastegate valve into the turbine housing of an exhaust-gas turbocharger
US20150292395A1