A color-changing lens and its preparation method and application

By setting a gradient layer in the color-changing lens and using fading liquid processing technology, the gradient effect of different color-changing depths under sunlight is achieved, which solves the problem that existing lenses cannot meet the needs of different environments and color depth mutations, and improves the sensitivity to strong light and UV protective effect.

CN110596911BActive Publication Date: 2024-10-29SHANGHAI CONANT OPTICS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN201910980261.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-10-15
Publication Date
2024-10-29
Estimated Expiration
2039-10-15

AI Technical Summary

Technical Problem

Existing photochromic lenses can only show one color-changing depth in a completely color-changing state, which cannot meet the user's needs for different color-changing depths when viewing near and far outdoors. Moreover, the sudden change in color depth caused by changes in light intensity brings serious problems to users. Dizziness or the discomfort of being unable to see for a moment.

Method used

A color-changing lens is designed. By setting up a first photochromic gradient layer and a second photochromic gradient layer, and using a fading liquid immersion process, the lens shows different color-changing depths when activated by sunlight, achieving a gradient effect and avoiding sudden changes in color depth.

Benefits of technology

It realizes the gradient of the light transmittance of the lens from more than 10% to less than 70% under sunlight activation, meeting the depth of discoloration requirements in different environments, avoiding user discomfort, and improving the protection effect against strong light and ultraviolet rays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110596911B_ABST
    Figure CN110596911B_ABST
Patent Text Reader

Abstract

The present invention provides a photochromic lens and a preparation method and application thereof, wherein the photochromic lens comprises a substrate, a first photochromic gradient layer, a second photochromic gradient layer, a first hard reinforcing layer and a second hard reinforcing layer. The first photochromic gradient layer and the second photochromic gradient layer firstly give the photochromic lens the property of being colorless and transparent under indoor light intensity and changing to a dark color when activated by outdoor sunlight; secondly, through a fading treatment process, the photochromic lens presents different color change depths when activated by sunlight, and the transition between different color change depths realizes the gradient effect of the photochromic lens, meets the user's demand for different color change depths when looking near and far outdoors, and avoids the discomfort caused to the user by sudden changes in color depth. The photochromic lens can be obtained by a layer-by-layer dipping, pulling and curing method, and the preparation process is simple, with broad industrialization prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of eyeglass lenses, and in particular relates to a photochromic lens and a preparation method and application thereof. Background Art

[0002] The ultraviolet rays in sunlight can be divided into three categories according to their wavelengths: UVA, UVB and UVC. UVC is absorbed when it passes through the atmosphere, so the ultraviolet rays that affect the human eye are mainly UVA and UVB. When light enters the eye, only about 4% is lost through reflection on the surface of the cornea. The vast majority of the light is refracted into the eye and is absorbed by the cornea, aqueous humor, lens and nitrite in turn, including ultraviolet rays that can damage the eyes. Studies have shown that ultraviolet damage to the eyes is cumulative. Long-term exposure to ultraviolet rays can cause damage to the cornea, conjunctiva and lens, and increase the risk of conjunctivitis, keratitis, cataracts and macular degeneration. Therefore, it is necessary for outdoor activities to wear photochromic glasses as a preventive measure against ultraviolet rays.

[0003] The color of the photochromic lenses in photochromic glasses can change with the changes in external light. Under strong sunlight, the lenses can quickly turn dark, greatly reducing the light transmittance of the lenses, thereby protecting the eyes from light stimulation; after entering the room and the light weakens, the color of the lenses gradually becomes lighter and returns to a colorless and transparent state. At present, the more mature photochromic lens preparation processes include incorporation and film-layer types. Among them, the film-layer type is to compound a layer of photochromic resin material on ordinary resin lenses, so that ordinary resin lenses have photochromic properties on the basis of maintaining their original properties. It has the characteristics of uniform color change, fast reaction and no specification restrictions on lens types, so it has a broader application prospect.

[0004] CN109752866A discloses a photochromic ophthalmic lens and a preparation method thereof. The lens comprises a body and a photochromic layer formed on the body, wherein the photochromic layer is obtained by immersing the body in a photochromic coating solution and then curing by heating or ultraviolet radiation, wherein the photochromic coating solution comprises a photochromic compound-cyclodextrin inclusion complex, a crosslinking agent and a solvent, wherein the photochromic compound is at least one of spiropyran, spirodiol, diarylethene, hexaarylbiimidazole, fulgide, azobenzene and chroman, the cyclodextrin is methacrylic acid-modified cyclodextrin, and the crosslinking agent comprises methacrylic resin, a silane coupling agent grafted with methacrylic resin and an initiator; under heating or ultraviolet radiation, the crosslinking agent and the photochromic compound-cyclodextrin inclusion complex undergo a polymerization reaction and are connected to the lens body through the silane coupling agent to obtain a stable photochromic ophthalmic lens. CN107099230A discloses a method for preparing a photochromic lens and the prepared photochromic lens, wherein the preparation method comprises: coating a photochromic coating on a substrate, curing and irradiating the substrate with ultraviolet light, thereby forming a photochromic layer on the upper surface of the substrate, coating the photochromic layer with a hardening layer, and sequentially depositing an anti-reflection layer, a radiation protection layer and a waterproof superhard layer on the hardening layer by vacuum sputtering; wherein the photochromic coating is a mixture of polyacrylate, a multifunctional acrylate monomer and a photochromic dye. The preparation method avoids the phenomenon that the photochromic compound is easily decomposed by high-temperature baking and curing, thereby improving the quality of the photochromic lens. CN105892093A discloses a color-changing process for resin lenses, the main steps of which include: (1) lens pretreatment: including KOH etching, ultrasonic cleaning, dichloromethane cleaning and ultrasonic pure water cleaning; (2) preparing spiropyran color-changing and hardening liquid and adding plasticizer; (3) spin-coating the color-changing liquid on the lens surface and UV curing; (4) coating with anti-reflection film and super waterproof film; (5) quality inspection. This process completes the hardening and color-changing of the lens in one step, so that the lens changes color evenly, has a long service life, and effectively reduces costs; at the same time, the color-changing powder and plasticizer are dispersed in the hardening layer in the form of microparticles, which can effectively improve the impact resistance of the lens.

[0005] However, the existing photochromic lenses, when fully discolored, have only one degree of discoloration depth, corresponding to a certain light transmittance value, which cannot meet the needs of some users for different discoloration depths when looking at near and far objects outdoors. Moreover, the photochromic lenses in the prior art rapidly change color depth under changes in light intensity, and this sudden change in depth can cause discomfort to the user, such as dizziness or loss of vision for a moment.

[0006] Therefore, developing a photochromic lens that can present different color change depths and avoid sudden changes in color depth is an urgent problem to be solved by those skilled in the art. Summary of the invention

[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a photochromic lens and a preparation method and application thereof. The photochromic lens is provided with a first photochromic gradient layer and a second photochromic gradient layer so that a photochromic lens presents different color change depths when activated by sunlight. The transition between different color change depths realizes the gradient effect of the photochromic lens, which can prevent strong light from causing damage to the eyes, and at the same time meet the user's needs for different color change depths when looking near and far outdoors, and avoid the discomfort caused to the user by sudden changes in color depth.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a photochromic lens, comprising a substrate (1), a first photochromic gradient layer (2-1), a second photochromic gradient layer (2-2), a first hard reinforcing layer (3-1) and a second hard reinforcing layer (3-2).

[0010] The first photochromic gradient layer (2-1) and the second photochromic gradient layer (2-2) are respectively arranged on two sides of the substrate (1); the first hard reinforcing layer (3-1) is arranged on the surface of the first photochromic gradient layer (2-1); and the second hard reinforcing layer (3-2) is arranged on the surface of the second photochromic layer (2-2).

[0011] In the photochromic lens provided by the present invention, a first photochromic gradient layer (2-1) and a second photochromic gradient layer (2-2) are specially designed. Firstly, the first photochromic gradient layer (2-1) and the second photochromic gradient layer (2-2) give the photochromic lens the property of being colorless and transparent under indoor light intensity and changing to a dark color when activated by outdoor sunlight; secondly, the first photochromic gradient layer (2-1) and the second photochromic gradient layer (2-2) are obtained by a process of soaking the photochromic coating in a fading liquid, and by setting the soaking time and speed, the first photochromic gradient layer (2-1) and the second photochromic gradient layer (2-2) have a specific content of color-changing substances, thereby realizing that the photochromic lens changes color when activated by sunlight. Different color change depths are presented, and the transition between different color change depths realizes the gradual effect of the photochromic lens, so that the transmittance of a photochromic lens under sunlight activation can gradually increase from more than 10% (10-26%) to less than 70% (21-65%). The difference between the maximum transmittance and the minimum transmittance of a photochromic lens under sunlight activation is 1-50%, which can protect the eyes from strong light damage, and at the same time meet the user's needs for different color change depths when looking near and far outdoors, and avoid the dizziness or instantaneous inability to see caused by sudden changes in color depth.

[0012] Preferably, the first photochromic gradient layer (2-1) and the second photochromic gradient layer (2-2) are coatings formed by soaking a photochromic coating in a fading liquid and then drying it.

[0013] Preferably, the fading liquid is an organic solvent.

[0014] Preferably, the organic solvent is selected from any one or a combination of at least two of methanol, ethanol, isopropanol, propylene glycol methyl ether, cyclohexanone, tetrahydrofuran or methyl pyrrolidone.

[0015] Preferably, the thickness of the first photochromic gradient layer (2-1) and the second photochromic gradient layer (2-2) is independently 5 to 15 μm, for example, 5.2 μm, 5.4 μm, 5.6 μm, 5.8 μm, 6.0 μm, 6.5 μm, 7.0 μm, 7.5 μm, 8.0 μm, 8.5 μm, 9.0 μm, 9.5 μm, 10.0 μm, 10.5 μm, 11.0 μm, 11.5 μm, 12.0 μm, 12.5 μm, 13.0 μm, 13.5 μm, 14.0 μm or 14.5 μm, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0016] Preferably, the photochromic coating is a mixed coating of polymer and photochromic powder.

[0017] Preferably, the polymer is polyurethane and / or polyacrylate.

[0018] Preferably, the color-changing powder is selected from any one or a combination of at least two of spiropyran compounds, diarylethene compounds or spiroidine compounds.

[0019] Preferably, the first hard reinforcement layer (3-1) and the second hard reinforcement layer (3-2) are organic silicon compound coatings.

[0020] Preferably, the thickness of the first hard strengthening layer (3-1) and the second hard strengthening layer (3-2) are independently 1 to 5 μm, for example, 1.2 μm, 1.5 μm, 1.7 μm, 2.0 μm, 2.2 μm, 2.5 μm, 2.7 μm, 3.0 μm, 3.3 μm, 3.5 μm, 3.7 μm, 4.0 μm, 4.2 μm, 4.5 μm, 4.7 μm or 4.9 μm, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0021] Preferably, the substrate (1) is made of an optically transparent polymer material.

[0022] Preferably, the refractive index of the optical transparent polymer material is 1.50-1.74, for example, 1.52, 1.54, 1.56, 1.58, 1.60, 1.62, 1.64, 1.66, 1.68, 1.70, 1.72 or 1.73.

[0023] The substrate of the photochromic lens of the present invention is preferably an optical transparent polymer material with a refractive index of 1.50 to 1.74. Specific materials include polycarbonates, polymethyl methacrylates, and polymer alloys. The present invention does not specifically limit the specific material.

[0024] Preferably, the difference between the maximum transmittance and the minimum transmittance of the photochromic lens under sunlight activation is 1-50%, for example 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, 30%, 32%, 35%, 38%, 40%, 42%, 45%, 47% or 49%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively enumerates the specific point values ​​included in the said range, and it is further preferably 3-40%.

[0025] In another aspect, the present invention provides a method for preparing the photochromic lens as described above, the method comprising the following steps:

[0026] (1) placing a substrate in a photochromic coating liquid, dipping, pulling out, drying, and curing to obtain a photochromic layer substrate I;

[0027] (2) treating and washing the photochromic layer substrate I obtained in step (1) in an alkali solution to obtain a photochromic layer substrate II;

[0028] (3) dipping the photochromic layer substrate II obtained in step (2) in a fading solution, pulling it out, and drying it to obtain a photochromic gradient layer substrate;

[0029] (4) placing the photochromic gradient layer substrate obtained in step (3) in a hard strengthening coating liquid for dipping, pulling out, drying, and curing to obtain the photochromic lens.

[0030] Preferably, the substrate in step (1) is a pretreated substrate.

[0031] Preferably, the pretreatment method is: placing the substrate in an alkali solution for ultrasonic treatment, washing, and drying.

[0032] Preferably, the treatment time is 12 to 18 minutes, for example, 13 minutes, 14 minutes, 15 minutes, 16 minutes or 17 minutes.

[0033] Preferably, the treatment temperature is 55-60°C, for example, 55.5°C, 56°C, 56.5°C, 57°C, 57.5°C, 58°C, 58.5°C, 59°C or 59.5°C.

[0034] Preferably, the mass percentage of the solute in the alkali solution is 12-18%, for example, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 15.5%, 16%, 16.5%, 17% or 17.5%, etc.

[0035] In the present invention, the substrate is placed in an alkali solution for ultrasonic pretreatment, which is to fully clean the substrate on the one hand, and on the other hand, the alkali solution has an etching effect on the substrate in the ultrasonic environment, so that a micro-nano scale rough surface is formed on the substrate, which is beneficial to improve the adhesion between the substrate and the photochromic layer.

[0036] Preferably, the photochromic coating liquid in step (1) is a mixed solution of polyurethane and spiropyran-based color-changing powder.

[0037] Preferably, the mass percentage of polyurethane in the photochromic coating liquid in step (1) is 40-60%, for example, 42%, 44%, 46%, 48%, 50%, 52%, 54%, 56%, 58% or 59%, etc.

[0038] Preferably, the polyurethane is hexamethylene diisocyanate.

[0039] Preferably, the mass percentage of the spiropyran color-changing powder in the photochromic coating liquid of step (1) is 5-15%, for example, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13% or 14%, etc., and more preferably 8-12%.

[0040] Preferably, the hard strengthening coating liquid in step (4) is a glycidoxytrimethoxysilane solution.

[0041] Preferably, the mass percentage of glycidoxytrimethoxysilane in the hard strengthening coating liquid in step (4) is 20-50%, for example, 22%, 24%, 26%, 28%, 30%, 33%, 35%, 38%, 40%, 43%, 45%, 47% or 49%, etc., and more preferably 30-40%.

[0042] Preferably, the dipping time of step (1), step (3) and step (4) is each independently 5 to 15 s, for example, 5.5 s, 6 s, 6.5 s, 7 s, 7.5 s, 8 s, 8.5 s, 9 s, 9.5 s, 10 s, 10.5 s, 11 s, 11.5 s, 12 s, 12.5 s, 13 s, 13.5 s, 14 s or 14.5 s, etc.

[0043] Preferably, the dipping temperatures in step (1), step (3) and step (4) are each independently 12 to 18°C, for example, 12.5°C, 13°C, 13.5°C, 14°C, 14.5°C, 15°C, 15.5°C, 16°C, 16.5°C, 17°C or 17.5°C, etc.

[0044] Preferably, the pulling speeds in step (1) and step (4) are independently 0.8 to 1.2 mm / s, for example, 0.85 mm / s, 0.9 mm / s, 0.95 mm / s, 1.0 mm / s, 1.05 mm / s, 1.1 mm / s, 1.15 mm / s or 1.18 mm / s, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0045] Preferably, the drying temperatures in step (1), step (3) and step (4) are each independently 80-90°C, for example, 80.5°C, 81°C, 81.5°C, 82°C, 82.5°C, 83°C, 83.5°C, 84°C, 84.5°C, 85°C, 85.5°C, 86°C, 86.5°C, 87°C, 87.5°C, 88°C, 88.5°C, 89°C or 89.5°C, etc.

[0046] Preferably, the drying time in step (1), step (3) and step (4) is each independently 15 to 20 min, for example, 15.5 min, 16 min, 16.5 min, 17 min, 17.5 min, 18 min, 18.5 min, 19 min or 19.5 min, etc.

[0047] Preferably, the curing temperature in step (1) and step (4) is independently 110-120°C, for example, 110.5°C, 111°C, 111.5°C, 112°C, 112.5°C, 113°C, 113.5°C, 114°C, 114.5°C, 115°C, 115.5°C, 116°C, 116.5°C, 117°C, 117.5°C, 118°C, 118.5°C, 119°C or 119.5°C, etc.

[0048] Preferably, the curing time of step (1) and step (4) is each independently 60 to 120 min, for example, 62 min, 65 min, 67 min, 70 min, 72 min, 75 min, 77 min, 80 min, 82 min, 85 min, 87 min, 90 min, 93 min, 95 min, 98 min, 100 min, 102 min, 105 min, 107 min, 110 min, 112 min, 115 min, 117 min or 119 min, etc.

[0049] Preferably, the treatment method in step (2) is ultrasonic treatment.

[0050] Preferably, the treatment time in step (2) is 12 to 18 minutes, for example, 13 minutes, 14 minutes, 15 minutes, 16 minutes or 17 minutes.

[0051] Preferably, the treatment temperature in step (2) is 55-60°C, for example, 55.5°C, 56°C, 56.5°C, 57°C, 57.5°C, 58°C, 58.5°C, 59°C or 59.5°C, etc.

[0052] Preferably, the alkali solution in step (2) is an aqueous sodium hydroxide solution and / or an aqueous potassium hydroxide solution.

[0053] Preferably, the mass percentage of the solute in the alkali solution in step (2) is 12-18%, for example, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 15.5%, 16%, 16.5%, 17% or 17.5%, etc.

[0054] Preferably, the cleaning in step (2) is cleaning with pure water.

[0055] The alkali solution ultrasonic cleaning process in step (2) of the present invention can, on the one hand, wash away the components and impurities that are not completely cross-linked on the photochromic layer substrate I obtained in step (1); on the other hand, the alkali solution can be used to etch the photochromic layer substrate I under an ultrasonic environment to form a micro-nano scale rough surface, which is beneficial to improving the adhesion between the photochromic gradient layer and the hard strengthening layer.

[0056] Preferably, the pulling speed in step (3) is 0.2-5.0 mm / s, for example, 0.25 mm / s, 0.3 mm / s, 0.35 mm / s, 0.4 mm / s, 0.45 mm / s, 0.5 mm / s, 0.55 mm / s, 0.6 mm / s, 0.65 mm / s, 0.7 mm / s, 0.8 mm / s, 0.9 mm / s, 1.0 mm / s, 1.2 mm / s, 1.4 mm / s, 1. 6mm / s, 1.8mm / s, 2.0mm / s, 2.3mm / s, 2.5mm / s, 2.8mm / s, 3.0mm / s, 3.2mm / s, 3.5mm / s, 3.8mm / s, 4.0mm / s, 4.2mm / s, 4.5mm / s or 4.8mm / s, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0057] Preferably, the pulling in step (3) is uniform speed pulling or variable speed pulling.

[0058] Preferably, the speed change interval of the speed change pull is fixed or not fixed.

[0059] In the preparation process of the photochromic lens of the present invention, on the basis of a lens provided with a photochromic coating, a first photochromic gradient layer (2-1) and a second photochromic gradient layer (2-2) are obtained by immersing the photochromic coating in a fading liquid for fading. First, the photochromic layer substrate II is immersed in the fading liquid for 5 to 15 seconds, and then pulled. In the process of pulling the lens from top to bottom, different positions of the lens have different immersion times in the fading liquid, thereby achieving different fading effects, and finally achieving a gradient effect with different color change depths under sunlight activation.

[0060] In addition, the pulling in step (3) can be uniform pulling or variable pulling, and the rate of uniform pulling or variable pulling can be controlled by a computer program. Uniform linear gradient effect of the lens can be achieved in the process of uniform pulling; variable speed pulling can achieve a wider range of curved gradient effect.

[0061] In the preparation method of the photochromic lens of the present invention, the process parameters such as the immersion time and the pulling speed of the fading liquid treatment process in step (3) are within the above-defined range, and the obtained photochromic lens has an appropriate transmittance gradient range under sunlight activation. If the immersion time of the fading liquid is too short and the speed is too fast, the transmittance gradient range of the photochromic lens under sunlight activation will be extremely small, that is, the transmittance of each part of the photochromic lens is basically the same under strong light, and there is no effect of gradual transmittance change; if the immersion time of the fading liquid is too long and the speed is too slow, the photochromic coating in the photochromic lens will fade excessively, the color depth of the photochromic lens under strong light is low, and the function of blocking strong light and ultraviolet rays cannot be effectively exerted.

[0062] Preferably, the preparation method comprises the following specific steps:

[0063] (1) placing a substrate that has been ultrasonically treated with 12-18% alkali solution at 55-60° C. for 12-18 min, washed with pure water, dried, and cooled to room temperature in a photochromic coating liquid, dip-coated at 12-18° C. for 5-15 s, pulled out at a speed of 0.8-1.2 mm / s, dried at 80-90° C. for 15-20 min, cured at 110-120° C. for 60-120 min, and cooled to room temperature to obtain a photochromic layer substrate I.

[0064] (2) placing the photochromic layer substrate I obtained in step (1) in a 12-18% alkali solution, ultrasonically treating it at 55-60° C. for 12-18 min, washing it with pure water, drying it, and cooling it to room temperature to obtain a photochromic layer substrate II.

[0065] (3) placing the photochromic layer substrate II obtained in step (2) in a fading solution, dipping for 5 to 15 seconds at 12 to 18° C., pulling out at a constant speed or variable speed of 0.2 to 5.0 mm / s, drying at 80 to 90° C. for 15 to 20 minutes, and cooling to room temperature to obtain a photochromic gradient layer substrate.

[0066] (4) placing the photochromic gradient layer substrate obtained in step (3) in a hard strengthening coating liquid, dipping it at 12-18° C. for 5-15 s, pulling it out at a speed of 0.8-1.2 mm / s, drying it at 80-90° C. for 15-20 min, curing it at 110-120° C. for 60-120 min, and cooling it to room temperature to obtain the photochromic lens.

[0067] In the preparation method of the present invention, the photochromic coating liquid is exemplarily a mixed solution of hexamethylene diisocyanate and spiropyran color-changing powder, and the solvent is a ketone ether organic solvent (for example, any one of acetone, cyclohexanone, methyl pyrrolidone or propylene glycol methyl ether or a combination of at least two); the hard strengthening coating liquid is exemplarily a glycidoxytrimethoxysilane solution, and the solvent is an alcohol solvent (for example, any one of methanol, ethanol or isopropanol or a combination of at least two) or a mixed solvent of an alcohol solvent and water. The preparation method of the photochromic coating and the hard strengthening coating liquid is carried out with reference to the prior art, for example, with reference to CN100575448 or US4753827.

[0068] In another aspect, the present invention provides a photochromic spectacles comprising the photochromic lenses as described above.

[0069] Compared with the prior art, the present invention has the following beneficial effects:

[0070] The photochromic lens provided by the present invention comprises a substrate, a first photochromic gradient layer, a second photochromic gradient layer, a first hard reinforcing layer and a second hard reinforcing layer. Among them, the first photochromic gradient layer and the second photochromic gradient layer firstly give the photochromic lens the property of being colorless and transparent under indoor light intensity and changing to a dark color under outdoor sunlight activation; secondly, through the fading treatment process, the photochromic lens presents different color change depths under sunlight activation, and the transition between different color change depths realizes the gradient effect of the photochromic lens, so that the light transmittance of a photochromic lens under sunlight activation can be gradually increased from 10 to 26% to 21 to 70%, which can protect the eyes from strong light damage, and at the same time can meet the user's needs for different color change depths when looking near and far outdoors, and avoid the discomfort such as dizziness or instantaneous inability to see caused by sudden changes in color depth. The photochromic lens can be obtained by a layer-by-layer dipping, pulling, and curing method, and the preparation process is simple, easy to operate, and has broad industrialization prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0071] Figure 1 This is a schematic structural diagram of the photochromic lens provided by the present invention, wherein 1 is a substrate, 2-1 is a first photochromic gradient layer, 2-2 is a second photochromic gradient layer, 3-1 is a first hard reinforcing layer, and 3-2 is a second hard reinforcing layer. DETAILED DESCRIPTION

[0072] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0073] The experimental materials used in the following examples of the present invention are as follows:

[0074] The substrate is a polycarbonate material with a refractive index of 1.50, 1.60, 1.67, and 1.74, respectively, purchased from Shanghai Connet Optics Co., Ltd. NaOH, KOH, methyl pyrrolidone, propylene glycol methyl ether, cyclohexanone, tetrahydrofuran, methanol, ethanol, and isopropanol were purchased from Shanghai Lingfeng Chemical Reagent Co., Ltd. The photochromic coating liquid is a mixed solution of hexamethylene diisocyanate and spiropyran color-changing powder, wherein the mass percentage of hexamethylene diisocyanate is 50%, the mass percentage of spiropyran color-changing powder is 10%, and the solvent is a mixed solvent of cyclohexanone and propylene glycol methyl ether (volume ratio 1:1); hexamethylene diisocyanate and spiropyran color-changing powder were purchased from Guangzhou Chongyu Industrial Materials Technology Co., Ltd. The hard strengthening coating liquid is a 35% glycidoxytrimethoxysilane solution, the brand is VH series products, purchased from Duen Optics Co., Ltd.

[0075] Example 1

[0076] The present embodiment provides a photochromic lens, which comprises a substrate (1), a first photochromic gradient layer (2-1), a second photochromic gradient layer (2-2), a first hard reinforcing layer (3-1) and a second hard reinforcing layer (3-2); the first photochromic gradient layer (2-1) and the second photochromic gradient layer (2-2) are respectively arranged on two sides of the substrate (1); the first hard reinforcing layer (3-1) is arranged on the surface of the first photochromic gradient layer (2-1); and the second hard reinforcing layer (3-2) is arranged on the surface of the second photochromic gradient layer (2-2).

[0077] The preparation method is as follows:

[0078] (1) a substrate (refractive index 1.74) was subjected to ultrasonic treatment at 55° C. for 12 min in a 12% NaOH aqueous solution, washed with pure water, dried, cooled to room temperature, placed in a photochromic coating liquid, dipped at 12° C. for 5 s, and then pulled out at a constant speed of 0.8 mm / s, dried at 80° C. for 15 min, and then cured at 110° C. for 60 min, and cooled to room temperature to obtain a photochromic layer substrate I;

[0079] (2) placing the photochromic layer substrate I obtained in step (1) in a 12% NaOH aqueous solution, ultrasonically treating at 55° C. for 12 min, washing with pure water, drying, and cooling to room temperature to obtain a photochromic layer substrate II;

[0080] (3) placing the photochromic layer substrate II obtained in step (2) in a fading solution (propylene glycol methyl ether, cyclohexanone, tetrahydrofuran and methyl pyrrolidone in a volume ratio of 1:3:4:2), dipping at 12° C. for 5 seconds, pulling out at a uniform speed of 0.2 mm / s, drying at 80° C. for 15 minutes, and cooling to room temperature to obtain a photochromic gradient layer substrate;

[0081] (4) placing the photochromic gradient layer substrate obtained in step (3) in a hard strengthening coating liquid, dipping it at 12° C. for 5 seconds, pulling it out at a uniform speed of 0.8 mm / s, drying it at 80° C. for 15 minutes, curing it at 110° C. for 60 minutes, and cooling it to room temperature to obtain the photochromic lens.

[0082] Example 2

[0083] The present embodiment provides a photochromic lens, which comprises a substrate (1), a first photochromic gradient layer (2-1), a second photochromic gradient layer (2-2), a first hard reinforcing layer (3-1) and a second hard reinforcing layer (3-2); the first photochromic gradient layer (2-1) and the second photochromic gradient layer (2-2) are respectively arranged on two sides of the substrate (1); the first hard reinforcing layer (3-1) is arranged on the surface of the first photochromic gradient layer (2-1); and the second hard reinforcing layer (3-2) is arranged on the surface of the second photochromic gradient layer (2-2).

[0084] The preparation method is as follows:

[0085] (1) a substrate (refractive index 1.67) was subjected to ultrasonic treatment at 60° C. for 18 min in an 18% KOH aqueous solution, washed with pure water, dried, cooled to room temperature, placed in a photochromic coating liquid, dipped at 18° C. for 15 s, and then pulled out at a constant speed of 1.2 mm / s, dried at 90° C. for 20 min, and then cured at 120° C. for 120 min, and cooled to room temperature to obtain a photochromic layer substrate I;

[0086] (2) placing the photochromic layer substrate I obtained in step (1) in an 18% KOH aqueous solution, ultrasonically treating it at 60° C. for 18 min, washing it with pure water, drying it, and cooling it to room temperature to obtain a photochromic layer substrate II;

[0087] (3) placing the photochromic layer substrate II obtained in step (2) in a fading solution (methanol, ethanol and isopropanol in a volume ratio of 8:1:1), dipping at 18° C. for 15 seconds, pulling out at an initial speed of 5.0 mm / s and decreasing the speed by 0.2 mm / s every 3 mm, drying at 90° C. for 20 minutes, and cooling to room temperature to obtain a photochromic gradient layer substrate;

[0088] (4) placing the photochromic gradient layer substrate obtained in step (3) in a hard strengthening coating liquid, dipping it at 18° C. for 15 seconds, then pulling it out at a uniform speed of 1.2 mm / s, drying it at 90° C. for 20 minutes, curing it at 120° C. for 120 minutes, and cooling it to room temperature to obtain the photochromic lens.

[0089] Example 3

[0090] The present embodiment provides a photochromic lens, wherein the photochromic lens comprises a substrate (1), a first photochromic gradient layer (2-1), a second photochromic gradient layer (2-2), a first hard reinforcing layer (3-1) and a second hard reinforcing layer (3-2); the first photochromic gradient layer (2-1) and the second photochromic gradient layer (2-2) are respectively arranged on two sides of the substrate (1); the first hard reinforcing layer (3-1) is arranged on the surface of the first photochromic gradient layer (2-1); and the second hard reinforcing layer (3-2) is arranged on the surface of the second photochromic gradient layer (2-2).

[0091] The preparation method is as follows:

[0092] (1) a substrate (refractive index 1.60) was subjected to ultrasonic treatment at 57° C. for 15 min in a 15% NaOH aqueous solution, washed with pure water, dried, cooled to room temperature, placed in a photochromic coating liquid, dipped at 15° C. for 10 s, and then pulled out at a constant speed of 1.0 mm / s, dried at 85° C. for 18 min, and then cured at 115° C. for 90 min, and cooled to room temperature to obtain a photochromic layer substrate I;

[0093] (2) placing the photochromic layer substrate I obtained in step (1) in a 15% NaOH aqueous solution, ultrasonically treating it at 58° C. for 15 min, washing it with pure water, drying it, and cooling it to room temperature to obtain a photochromic layer substrate II;

[0094] (3) placing the photochromic layer substrate II obtained in step (2) in a decolorizing solution (methyl pyrrolidone), dipping at 15° C. for 10 seconds, pulling it out at a uniform speed of 0.5 mm / s, drying at 85° C. for 18 minutes, and cooling to room temperature to obtain a photochromic gradient layer substrate;

[0095] (4) placing the photochromic gradient layer substrate obtained in step (3) in a hard strengthening coating liquid, dipping it at 15° C. for 10 seconds, then pulling it out at a uniform speed of 1.0 mm / s, drying it at 85° C. for 17 minutes, curing it at 115° C. for 90 minutes, and cooling it to room temperature to obtain the photochromic lens.

[0096] Example 4

[0097] The present embodiment provides a photochromic lens, which comprises a substrate (1), a first photochromic gradient layer (2-1), a second photochromic gradient layer (2-2), a first hard reinforcing layer (3-1) and a second hard reinforcing layer (3-2); the first photochromic gradient layer (2-1) and the second photochromic gradient layer (2-2) are respectively arranged on two sides of the substrate (1); the first hard reinforcing layer (3-1) is arranged on the surface of the first photochromic gradient layer (2-1); and the second hard reinforcing layer (3-2) is arranged on the surface of the second photochromic gradient layer (2-2).

[0098] The preparation method is as follows:

[0099] (1) a substrate (refractive index 1.50) was subjected to ultrasonic treatment at 58° C. for 14 min in a 15% KOH aqueous solution, washed with pure water, dried, cooled to room temperature, placed in a photochromic coating liquid, dipped at 15° C. for 12 s, and then pulled out at a constant speed of 1.1 mm / s, dried at 87° C. for 15 min, and then cured at 118° C. for 100 min, and cooled to room temperature to obtain a photochromic layer substrate I;

[0100] (2) placing the photochromic layer substrate I obtained in step (1) in a 15% KOH aqueous solution, ultrasonically treating it at 57° C. for 16 min, washing it with pure water, drying it, and cooling it to room temperature to obtain a photochromic layer substrate II;

[0101] (3) placing the photochromic layer substrate II obtained in step (2) in a fading solution (methanol, ethanol and tetrahydrofuran in a volume ratio of 1:1:2), dipping at 14° C. for 13 seconds, pulling out at a uniform speed of 1.0 mm / s, drying at 88° C. for 16 minutes, and cooling to room temperature to obtain a photochromic gradient layer substrate;

[0102] (4) placing the photochromic gradient layer substrate obtained in step (3) in a hard strengthening coating liquid, dipping it at 16° C. for 8 seconds, then pulling it out at a uniform speed of 0.9 mm / s, drying it at 85° C. for 15 minutes, curing it at 115° C. for 80 minutes, and cooling it to room temperature to obtain the photochromic lens.

[0103] Example 5

[0104] The present embodiment provides a photochromic lens, which comprises a substrate (1), a first photochromic gradient layer (2-1), a second photochromic gradient layer (2-2), a first hard reinforcing layer (3-1) and a second hard reinforcing layer (3-2); the first photochromic gradient layer (2-1) and the second photochromic gradient layer (2-2) are respectively arranged on two sides of the substrate (1); the first hard reinforcing layer (3-1) is arranged on the surface of the first photochromic gradient layer (2-1); and the second hard reinforcing layer (3-2) is arranged on the surface of the second photochromic gradient layer (2-2).

[0105] The preparation method is as follows:

[0106] (1) a substrate (refractive index 1.60) was subjected to ultrasonic treatment at 57° C. for 16 min in a 16% KOH aqueous solution, washed with pure water, dried, cooled to room temperature, placed in a photochromic coating liquid, dipped at 17° C. for 8 s, and then pulled out at a constant speed of 0.9 mm / s, dried at 83° C. for 18 min, and then cured at 114° C. for 120 min, and cooled to room temperature to obtain a photochromic layer substrate I;

[0107] (2) placing the photochromic layer substrate I obtained in step (1) in a 16% KOH aqueous solution, ultrasonically treating it at 55° C. for 15 min, washing it with pure water, drying it, and cooling it to room temperature to obtain a photochromic layer substrate II;

[0108] (3) placing the photochromic layer substrate II obtained in step (2) in a fading solution (the volume ratio of tetrahydrofuran and cyclohexanone is 1:1), dipping at 16° C. for 7 seconds, pulling out at an initial speed of 4.0 mm / s and decreasing the speed by 0.2 mm / s every 5 mm, drying at 85° C. for 18 minutes, and cooling to room temperature to obtain a photochromic gradient layer substrate;

[0109] (4) placing the photochromic gradient layer substrate obtained in step (3) in a hard strengthening coating liquid, dipping it at 14° C. for 12 seconds, then pulling it out at a uniform speed of 1.1 mm / s, drying it at 88° C. for 15 minutes, curing it at 115° C. for 70 minutes, and cooling it to room temperature to obtain the photochromic lens.

[0110] Example 6

[0111] The difference between this embodiment and embodiment 1 is that the dipping time in step (3) is 10 s, and the pulling is a uniform pulling speed of 0.6 mm / s.

[0112] Example 7

[0113] The difference between this embodiment and embodiment 1 is that the dipping time in step (3) is 10 s, and the pulling is a fixed-interval variable speed pulling with an initial speed of 3.3 mm / s and a speed reduction of 0.2 mm / s every 5 mm of pulling.

[0114] Comparative Example 1

[0115] The difference between this comparative example and Example 1 is that step (3) is not performed, that is, the substrate is not dipped in the fading liquid.

[0116] Comparative Example 2

[0117] The difference between this comparative example and Example 1 is that the dipping time in step (3) is 3 s, and the pulling is a uniform pulling speed of 6.0 mm / s.

[0118] Comparative Example 3

[0119] The difference between this comparative example and Example 1 is that the dipping time in step (3) is 20 s, and the pulling is a uniform pulling speed of 0.18 mm / s.

[0120] Performance Testing:

[0121] Light transmittance test: At room temperature, place the test piece under ultraviolet light for 2 minutes, then take it out and put it into a haze meter (BYK-Gardner haze-gurd plus haze meter) to measure the light transmittance value. For specific test methods, refer to the instrument manual.

[0122] The light transmittance of the photochromic lenses provided in Examples 1 to 7 and Comparative Examples 1 to 3 was tested according to the above method. The specific test data are shown in Table 1:

[0123] Table 1

[0124]

[0125]

[0126] In Table 1, the “average thickness of the photochromic gradient layer” is the average thickness of the first photochromic gradient layer and the second photochromic gradient layer of the photochromic lens.

[0127] From the data in Table 1, it can be seen that the photochromic lenses provided in Examples 1 to 7 of the present invention are specially designed with a photochromic gradient layer. During the preparation process, the photochromic lenses obtained are treated with the decolorizing liquid in step (3), so that the photochromic lenses exhibit different light transmittances under light activation. The light transmittance of a photochromic lens under light activation can be gradually increased from 10 to 26% to 21 to 65%, and the difference between the maximum light transmittance and the minimum light transmittance is 3 to 40%. The photochromic lenses provided in Examples 1 to 7 of the present invention can protect the eyes from strong light damage, and at the same time can meet the needs of users for different color change depths when looking at near and far outdoors, and avoid the discomfort caused by sudden changes in color depth to users, such as dizziness or instantaneous inability to see objects.

[0128] If the photochromic lens is not subjected to the fading liquid treatment process described in step (3) during the preparation process (Comparative Example 1), the transmittance of the obtained photochromic lens at all locations under light activation is the same, that is, the lens does not have a gradient color effect; if the dipping time in the fading liquid treatment process described in step (3) during the preparation process of the photochromic lens is too short and the speed is too fast (Comparative Example 2), the transmittance of the photochromic lens at all locations under light activation is basically the same, and the lens does not have a gradient transmittance effect; if the dipping time in the fading liquid treatment process described in step (3) during the preparation process of the photochromic lens is too long and the speed is too slow (Comparative Example 3), the photochromic coating in the photochromic lens will fade excessively, the color depth of the photochromic lens under strong light is low, and the function of blocking strong light and ultraviolet rays cannot be effectively exerted.

[0129] The applicant declares that the present invention uses the above embodiments to illustrate the photochromic lens and its preparation method and application, but the present invention is not limited to the above process steps, that is, it does not mean that the present invention must rely on the above process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A photochromic lens, characterized in that: The photochromic lens comprises a substrate (1), a first photochromic gradient layer (2-1), a second photochromic gradient layer (2-2), a first hard reinforcing layer (3-1) and a second hard reinforcing layer (3-2); The first photochromic gradient layer (2-1) and the second photochromic gradient layer (2-2) are respectively arranged on two surfaces of the substrate (1); The first hard reinforcing layer (3-1) is disposed on the surface of the first photochromic gradient layer (2-1); and the second hard reinforcing layer (3-2) is disposed on the surface of the second photochromic gradient layer (2-2); The first photochromic gradient layer (2-1) and the second photochromic gradient layer (2-2) are coatings formed by soaking a photochromic coating in a fading liquid and drying the coating; The decolorizing liquid is an organic solvent, and the organic solvent is selected from any one or a combination of at least two of methanol, ethanol, isopropanol, propylene glycol methyl ether, cyclohexanone, tetrahydrofuran or methyl pyrrolidone; The soaking time is 5 to 15 seconds; The photochromic coating is soaked in a fading liquid and then pulled out, and the pulling speed is 0.2-5.0 mm / s.

2. The photochromic lens according to claim 1, characterized in that: The thickness of the first photochromic gradient layer (2-1) and the second photochromic gradient layer (2-2) are independently 5 to 15 μm.

3. The photochromic lens according to claim 1, characterized in that: The photochromic coating is a mixed coating of polymer and color-changing powder; The polymer is polyurethane and / or polyacrylate; The color-changing powder is selected from any one of spiropyran compounds, diarylethene compounds or spirophenylamine compounds, or a combination of at least two thereof.

4. The photochromic lens according to claim 1, characterized in that: The first hard strengthening layer (3-1) and the second hard strengthening layer (3-2) are organic silicon compound coatings; The thickness of the first hard strengthening layer (3-1) and the second hard strengthening layer (3-2) are independently 1 to 5 μm; The material of the substrate (1) is an optically transparent polymer material; The refractive index of the optical transparent polymer material is 1.50 to 1.74; The difference between the maximum light transmittance and the minimum light transmittance of the photochromic lens under sunlight activation is 1 to 50%.

5. The photochromic lens according to claim 4, characterized in that: The difference between the maximum light transmittance and the minimum light transmittance of the photochromic lens under sunlight activation is 3-40%.

6. A method for preparing a photochromic lens according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: (1) placing a substrate in a photochromic coating liquid, dipping, pulling out, drying, and curing to obtain a photochromic layer substrate I; (2) treating and washing the photochromic layer substrate I obtained in step (1) in an alkali solution to obtain a photochromic layer substrate II; (3) soaking the photochromic layer substrate II obtained in step (2) in a fading liquid, pulling it out, and drying it to obtain a photochromic gradient layer substrate; (4) placing the photochromic gradient layer substrate obtained in step (3) in a hard strengthening coating liquid for dipping, pulling out, drying, and curing to obtain the photochromic lens.

7. The preparation method according to claim 6, characterized in that: The substrate in step (1) is a pre-treated substrate; The pretreatment method is: placing the substrate in an alkali solution for ultrasonic treatment, cleaning, and drying; The treatment time is 12 to 18 minutes; The treatment temperature is 55-60°C; The mass percentage of the solute in the alkali solution is 12-18%; The photochromic coating liquid in step (1) is a mixed solution of polyurethane and spiropyran type color-changing powder; The mass percentage of polyurethane in the photochromic coating liquid of step (1) is 40-60%; The polyurethane is hexamethylene diisocyanate; The mass percentage of the spiropyran color-changing powder in the photochromic coating liquid in step (1) is 5-15%.

8. The preparation method according to claim 7, characterized in that: The mass percentage of the spiropyran color-changing powder in the photochromic coating liquid in step (1) is 8-12%.

9. The preparation method according to claim 6, characterized in that: The hard strengthening coating liquid in step (4) is a glycidoxytrimethoxysilane solution; The mass percentage of glycidoxytrimethoxysilane in the hard strengthening coating liquid in step (4) is 20-50%.

10. The preparation method according to claim 9, characterized in that: The mass percentage of glycidoxytrimethoxysilane in the hard strengthening coating liquid in step (4) is 30-40%.

11. The preparation method according to claim 6, characterized in that: The dipping time in step (1) and step (4) is independently 5 to 15 seconds; The dipping temperatures in step (1), step (3) and step (4) are each independently 12 to 18° C.; The pulling speeds in step (1) and step (4) are independently 0.8 to 1.2 mm / s; The drying temperatures in step (1), step (3) and step (4) are each independently 80 to 90° C.; The drying time in step (1), step (3) and step (4) is independently 15 to 20 minutes; The curing temperatures in step (1) and step (4) are independently 110 to 120° C. The curing time in step (1) and step (4) is independently 60 to 120 minutes.

12. The preparation method according to claim 6, characterized in that: The treatment method in step (2) is ultrasonic treatment; The treatment time in step (2) is 12 to 18 minutes; The treatment temperature in step (2) is 55-60° C. The alkali solution in step (2) is a sodium hydroxide aqueous solution and / or a potassium hydroxide aqueous solution; The mass percentage of the solute in the alkali solution of step (2) is 12-18%; The cleaning in step (2) is performed with pure water.

13. The preparation method according to claim 6, characterized in that: The pulling in step (3) is uniform speed pulling or variable speed pulling; The speed change interval of the speed change pull is fixed or not fixed.

14. The preparation method according to claim 6, characterized in that: The preparation method comprises the following specific steps: (1) placing a substrate that has been ultrasonically treated with 12-18% alkali solution at 55-60° C. for 12-18 min, washed with pure water, dried, and cooled to room temperature in a photochromic coating liquid, dipping for 5-15 s at 12-18° C., pulling out at a speed of 0.8-1.2 mm / s, drying at 80-90° C. for 15-20 min, curing at 110-120° C. for 60-120 min, and cooling to room temperature to obtain a photochromic layer substrate I; (2) placing the photochromic layer substrate I obtained in step (1) in a 12-18% alkali solution, ultrasonically treating it at 55-60° C. for 12-18 min, washing it with pure water, drying it, and cooling it to room temperature to obtain a photochromic layer substrate II; (3) placing the photochromic layer substrate II obtained in step (2) in a fading solution, soaking it at 12-18° C. for 5-15 seconds, pulling it out at a constant speed or variable speed of 0.2-5.0 mm / s, drying it at 80-90° C. for 15-20 minutes, and cooling it to room temperature to obtain a photochromic gradient layer substrate; (4) placing the photochromic gradient layer substrate obtained in step (3) in a hard strengthening coating liquid, dipping it at 12-18° C. for 5-15 s, pulling it out at a speed of 0.8-1.2 mm / s, drying it at 80-90° C. for 15-20 min, curing it at 110-120° C. for 60-120 min, and cooling it to room temperature to obtain the photochromic lens.

15. A color-changing glasses, characterized in that: The photochromic glasses include the photochromic lenses according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Color changing process for resin lens

    CN105892093A

  • Preparation method of photochromic lens and photochromic lens prepared by method

    CN107099230A

  • Photochromic eye lens and preparation method thereof

    CN109752866A

  • Abrasion-resistant organosiloxane / metal oxide coating