Semi-flexible pavement pressure grouting device and pavement construction method
By using pressure grouting equipment and screed vibration technology in semi-flexible pavement construction, the problem of cement-based mortar being unable to exclude air from large-pore asphalt mixtures has been solved, achieving denser and more uniform pavement structure and extending the life of the pavement. service life.
Patent Information
- Application Number
- CN201911356463.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-12-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2039-12-25
AI Technical Summary
In the existing semi-flexible pavement construction, the cement-based mortar cannot effectively eliminate the air in the large-pore asphalt mixture, resulting in an uneven pavement structure and affecting its service life.
A semi-flexible pavement pressure grouting device is used to inject cement-based mortar into the large-pore asphalt mixture through pressure grouting, and use the vibration of the leveler to expel residual air bubbles to form a dense and uniform pavement structure.
Effectively remove air from the pavement, ensure the complete combination of cement-based mortar and asphalt mixture, and improve the structural quality and service life of the pavement.
Smart Images

Figure CN110939046B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to road construction equipment and method, and in particular to a semi-flexible pavement pressure grouting device and a pavement construction method. Background Art
[0002] At present, semi-flexible pavement is mostly based on large-pore asphalt mixture as the matrix, and cement-based mortar materials are penetrated to form a dense structure with good road performance. While ensuring the integrity of the pavement structure and preventing the occurrence of pavement cracks, it can improve the high-temperature stability of the overall pavement structure and prevent the occurrence of pavement rutting diseases. It is an excellent new type of pavement structure material, especially for typical road areas prone to pavement rutting diseases such as heavy-loaded pavements, intersections, bus stations, and toll stations. The key difficulty of semi-flexible pavement construction lies in how to completely expel the air in the asphalt mixture matrix so that the cement-based mortar is completely filled to form a dense large-pore mixture-cement-based slurry structure.
[0003] During the construction of the semi-flexible pavement of the prior art, the fluidity of the cement-based mortar itself is used to automatically penetrate into the large pores of the asphalt mixture. Due to the effect of air resistance in the large pores of the asphalt mixture, the automatically penetrated cement-based mortar cannot effectively remove the air in the large pores. After the construction is completed, a large number of closed gaps still exist inside the semi-flexible pavement, which seriously affects the structural quality and service life of the pavement. Summary of the invention
[0004] The purpose of the present invention is to provide a semi-flexible pavement pressure grouting device and a pavement construction method, which uses pressure grouting to expel the air in the pores inside the large-pore asphalt pavement, so that the cement-based mortar and the large-pore asphalt mixture matrix are completely combined, and cooperates with a leveling machine for vibration leveling to form a dense and uniform pavement structure to ensure the quality of the pavement.
[0005] The present invention is achieved in that:
[0006] A semi-flexible pavement pressure grouting device comprises an agitator, a grouting pump, a conduit, a branch pipe and a nozzle. A cement-based mortar tank is installed in the agitator. The discharge port of the agitator is connected to the feed port of the grouting pump, and the discharge port of the grouting pump is connected to the feed port of the conduit. The conduit is placed parallel to the top of a macroporous asphalt mixture matrix. A plurality of discharge holes are arranged at the bottom of the conduit, and a plurality of branch pipes are respectively arranged on the discharge holes of the conduit. A plurality of injection holes are arranged at intervals at the bottom of each branch pipe, and a plurality of nozzles are correspondingly installed on the injection holes of the branch pipes, and a nozzle matrix is formed above the macroporous asphalt mixture matrix, and the injection direction of each nozzle is perpendicular to the macroporous asphalt mixture matrix.
[0007] The pressure grouting device is installed on a locomotive, which moves along the paving direction of the road surface and drives the nozzle matrix to move synchronously above the macroporous asphalt mixture matrix.
[0008] The conduit and the branch pipe are arranged vertically, and a plurality of branch pipes are arranged at equal intervals.
[0009] The length of the conduit is equivalent to the width of the macroporous asphalt mixture matrix, so that the nozzle matrix can evenly cover the entire macroporous asphalt mixture matrix.
[0010] The spacing between the plurality of branch pipes is 10-30 cm.
[0011] The plurality of nozzles on each branch pipe are arranged at equal intervals, and each branch pipe is provided with 2-5 nozzles.
[0012] The spraying pressure of the nozzle is 5-20MPa.
[0013] A construction method for a semi-flexible pavement, after the middle surface layer of the asphalt pavement is paved, the semi-flexible upper surface layer is paved;
[0014] The construction method comprises the following steps:
[0015] Step 1: Isolate the grouting construction area from the curbstone and asphalt pavement;
[0016] Step 2: Open-graded macroporous asphalt mixture is paved on the surface of the middle surface layer to form a macroporous asphalt mixture matrix, and then rolled by a roller;
[0017] Step 3: After the temperature of the macroporous asphalt mixture matrix is cooled, cement-based mortar is injected into the macropores through a pressure grouting device to form a semi-flexible upper layer;
[0018] Step 4: Use a leveling machine to vibrate and level the semi-flexible upper layer. The leveling machine can expel the bubbles remaining in the macroporous asphalt mixture matrix through vibration.
[0019] Step 5: Cure the semi-flexible top layer.
[0020] In the step 2, the roller does not start the vibration mode when rolling the macroporous asphalt mixture matrix, so that the porosity of the macroporous asphalt mixture matrix after rolling is 20%-30%.
[0021] In the semi-flexible top layer, the weight percentage of the open-graded macroporous asphalt mixture is 70%-80%, and the weight percentage of the cement-based mortar is 20%-30%; the porosity in the macroporous asphalt mixture matrix is 20%-30%, and the cement-based mortar is filled in the macropores of the macroporous asphalt mixture matrix through pressure grouting.
[0022] The present invention uses pressure grouting to expel the air in the pores inside the large-pore asphalt pavement, so that the cement-based mortar and the large-pore asphalt mixture matrix are completely combined, and cooperates with a leveling machine for vibration leveling to form a dense and uniform pavement structure, ensure the quality of the pavement, and facilitate the promotion and application of semi-flexible pavement technology. It has good application prospects and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a construction schematic diagram of the semi-flexible pavement pressure grouting device of the present invention;
[0024] Figure 2 is a construction cross-sectional view of the semi-flexible pavement of the present invention;
[0025] Figure 3 It is a cross-sectional view of the isolation structure of the grouting construction area in the semi-flexible pavement of the present invention.
[0026] In the figure, 1 is agitator, 2 is grouting pump, 3 is conduit, 4 is branch pipe, 5 is nozzle, 6 is large-pore asphalt mixture matrix, 10 isolating grouting construction area, 20 is curbstone, 30 is asphalt pavement, 301 is semi-flexible upper layer, 302 is middle layer, 303 is lower layer, 304 is base layer, 305 is roadbed improvement layer, 306 is roadbed. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0028] Please see attached Figure 1 A semi-flexible pavement pressure grouting device comprises a stirrer 1, a grouting pump 2, a conduit 3, a branch pipe 4 and a nozzle 5. The cement-based mortar tank is installed in the stirrer 1. The discharge port of the stirrer 1 is connected to the feed port of the grouting pump 2, and the discharge port of the grouting pump 2 is connected to the feed port of the conduit 3. The conduit 3 is placed parallel to the top of a macroporous asphalt mixture matrix 6. The bottom of the conduit 3 is provided with a plurality of discharge holes (not shown in the figure), and a plurality of branch pipes 4 are respectively arranged on the discharge holes of the conduit 3. The bottom of each branch pipe 4 is provided with a plurality of injection holes (not shown in the figure) at intervals, and a plurality of nozzles 5 are correspondingly installed on the injection holes of the branch pipe 4, and a nozzle matrix is formed above the macroporous asphalt mixture matrix 6. The injection direction of each nozzle 5 is perpendicular to the macroporous asphalt mixture matrix 6.
[0029] The pressure grouting device is installed on a locomotive, and the locomotive is driven along the paving direction of the road surface (i.e. Figure 1 The nozzle matrix moves in the direction of the middle arrow) and drives the nozzle matrix to move synchronously above the macroporous asphalt mixture matrix 6 for grouting operations.
[0030] The conduit 3 and the branch pipe 4 are arranged vertically, and a plurality of branch pipes 4 are arranged at equal intervals to ensure that the nozzles 5 in the nozzle matrix are evenly distributed.
[0031] The length of the conduit 3 is equivalent to the width of the macroporous asphalt mixture matrix 6, so that the nozzle matrix can evenly cover the entire macroporous asphalt mixture matrix 6, ensuring the uniformity of grouting. The grouting operation is completed in one time, improving the construction efficiency and quality.
[0032] The spacing between the plurality of branch pipes 4 is 10-30 cm. The branch pipes 4 can be arranged at a suitable spacing according to the grouting requirements, so as to facilitate the arrangement of the nozzles 5 .
[0033] The plurality of nozzles 5 on each branch pipe 4 are arranged at equal intervals, further ensuring that the nozzles 5 in the nozzle matrix are evenly distributed.
[0034] Each branch pipe 4 is provided with 2-5 nozzles 5, and a suitable number of nozzles 5 can be provided according to the grouting requirements to achieve the best exhaust grouting process effect.
[0035] The injection pressure of the nozzle 5 is 5-20 MPa, which ensures that the air in the macropores of the open-grade macropore asphalt mixture can be completely removed during grouting and the cement-based mortar can be completely injected.
[0036] Preferably, the agitator 1 can adopt the cement mixing equipment of the prior art, so that the materials can be evenly mixed in the mixing container through the stirring rod driven by the motor, and the grouting pump 2 can adopt the slurry delivery pump used in the construction industry, which can output the cement-based mortar in the agitator 1 into the conduit 3 and pressurize it while outputting, ensuring that the cement-based mortar reaches the designed injection pressure when it is sprayed out through the nozzle 5 for grouting.
[0037] When paving the semi-flexible pavement, the moving speed of the locomotive is determined according to the spreading speed of the nozzle 5. The cement-based slurry is evenly stirred by the stirrer 1 and then transported to the conduit 3 and the branch pipe 4 through the grouting pump 2. After being sprayed by the nozzle 5, uniform grouting is achieved in the large pores of the open-graded large-pore asphalt mixture.
[0038] Please see attached Figure 2 and attached Figure 3A construction method of a semi-flexible pavement, after the middle surface layer 302 of the asphalt pavement 30 is paved, the paving construction of the semi-flexible upper layer 301 is carried out. The asphalt pavement 30 includes a roadbed improvement layer 305, a base layer 304, a lower layer 303, a middle surface layer 302 and a semi-flexible upper layer 301 paved on the roadbed 306 from bottom to top. The roadbed 306, the roadbed improvement layer 305, the base layer 304, the lower layer 303 and the middle surface layer 302 can adopt the asphalt pavement paving method of the existing technology, which will not be repeated in the present invention. Among them, the middle surface layer 302 is preferably an SMA-16 mixture, using SBS modified asphalt; the lower layer 303 is preferably an AC-20 mixture, using 70# base petroleum asphalt; the total thickness of the asphalt pavement 30 is 16-18cm. The base layer 304 is preferably made of water-stable crushed stone with a thickness of not less than 40 cm, and uses 42.5 cement with a dosage of 4%; the roadbed improvement layer 305 can be made of gravel material with good permeability and a thickness of not less than 15 cm.
[0039] The construction method comprises the following steps:
[0040] Step 1: Isolate the grouting construction area 10 from the curbstone 20 and the asphalt pavement 30. The grouting construction area 10 is sealed around to prevent the cement-based mortar from being left out during grouting.
[0041] Step 1.1: Use a blowing and drying device or manually clean the surroundings of the asphalt pavement 30 adjacent to the grouting construction area 10.
[0042] Step 1.2: Attach one surface of the double-sided tape 40 to the curbstones 20 and the asphalt pavement 30 adjacent to the edges of the grouting construction area 10 .
[0043] Step 1.3: Press and adhere the lightweight foam strip 50 to the middle of the other side of the double-sided adhesive tape 40 along the length direction of the double-sided adhesive tape 40 .
[0044] Step 1.4: Cover the light foam strip 50 with a film 60 , and the two side edges of the film 60 are attached to the other side of the double-sided tape 40 , so that the light foam strip 50 is wrapped between the film 60 and the double-sided tape 40 .
[0045] Step 2: Open-graded large-pore asphalt mixture is paved on the surface of the middle surface layer 302 to form a large-pore asphalt mixture matrix 6, and then rolled by a common roller.
[0046] When rolling the macroporous asphalt mixture matrix 6, the vibration mode is not turned on, so that the porosity of the macroporous asphalt mixture matrix 6 after rolling is 20%-30%, which is used for cement-based mortar to be poured into the macropores of the macroporous asphalt mixture matrix 6 at a certain pressure.
[0047] Step 3: After the temperature of the macroporous asphalt mixture matrix 6 is cooled, cement-based mortar is injected into the macropores through a pressure grouting device to form a semi-flexible upper layer 301.
[0048] Step 4: The semi-flexible upper layer 301 is vibrated and leveled by a leveling machine. The leveling machine uses vibration energy to discharge the bubbles remaining in the macroporous asphalt mixture matrix 6, making the road surface dense and uniform.
[0049] Step 5: Maintain the semi-flexible upper layer 301. The maintenance can be carried out in the same way as the concrete pavement maintenance: after the cement-based mortar is initially set, the floating slurry on the surface of the asphalt pavement 30 is cleaned with a water gun to expose the road surface aggregate and ensure the pavement structure depth to ensure the anti-skid performance of the asphalt pavement 30.
[0050] The weight percentage of the open-graded macroporous asphalt mixture in the semi-flexible upper layer 301 is 70%-80%, and the weight percentage of the cement-based mortar is 20%-30%; the porosity in the macroporous asphalt mixture matrix 6 is 20%-30%, and the cement-based mortar is filled in the macropores of the macroporous asphalt mixture matrix 6 by pressure grouting.
[0051] Preferably, the open-graded macroporous asphalt mixture comprises coarse aggregate, fine aggregate, filler and asphalt, wherein the coarse aggregate comprises first coarse aggregate and second coarse aggregate; the ratio of the first coarse aggregate, the second coarse aggregate and the fine aggregate is 45-50:40-45:5-15 by weight. The filler is 1.0-2.0% of the aggregate, and the asphalt is 2%-4%.
[0052] The coarse aggregate can be basalt or diabase.
[0053] The particle size of the first coarse aggregate of the coarse aggregate is [10mm, 15mm].
[0054] The particle size of the second coarse aggregate of the coarse aggregate is [5mm, 15mm].
[0055] The fine aggregate may be limestone.
[0056] The particle size of the fine aggregate is (0mm, 5mm].
[0057] The filler is mineral powder, preferably limestone mineral powder.
[0058] The asphalt can be 70# base petroleum asphalt, and the dosage is 2%-4%. The dosage refers to the weight percentage of asphalt in the open-graded macroporous asphalt mixture.
[0059] The main parameters of the open-graded macroporous asphalt mixture made according to the above ingredients and their proportions are shown in Table 1:
[0060] Table 1: Performance parameters of open-graded macroporous asphalt mixture
[0061] project <![CDATA[Density (g / cm 3 )]]> Marshall stability (kN) Flow value (0.1mm) Porosity (%) Index requirements ≥1.95 ≥2.8 25~45 20~30
[0062] The cement-based mortar comprises, by mass, 1-2 parts of cement, 0.15-0.3 parts of fly ash, 0.2-0.4 parts of slag powder, 0.1-0.2 parts of water reducing agent, 0.3-0.6 parts of water and 0.6-1.2 parts of polymer emulsion.
[0063] The main parameters of the cement-based mortar made according to the above ingredients and their proportions are: 60min fluidity is not more than 15s (flow cone method), 7d flexural strength is not less than 3MPa, 28d flexural strength is not less than 4.5Mpa, and 60-day shrinkage rate is -0.4 to 0.4.
[0064] The above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A semi-flexible pavement pressure grouting device, characterized by: It comprises a stirrer (1), a grouting pump (2), a conduit (3), a branch pipe (4) and a nozzle (5); a cement-based mortar tank is installed in the stirrer (1); the discharge port of the stirrer (1) is connected to the feed port of the grouting pump (2); the discharge port of the grouting pump (2) is connected to the feed port of the conduit (3); the conduit (3) is placed parallel to the top of a macroporous asphalt mixture matrix (6); a plurality of discharge holes are arranged at the bottom of the conduit (3); a plurality of branch pipes (4) are arranged correspondingly on the discharge holes of the conduit (3); a plurality of injection holes are arranged at intervals at the bottom of each branch pipe (4); a plurality of nozzles (5) are installed correspondingly on the injection holes of the branch pipe (4), and a nozzle matrix is formed above the macroporous asphalt mixture matrix (6); the injection direction of each nozzle (5) is perpendicular to the macroporous asphalt mixture matrix (6); The conduit (3) and the branch pipe (4) are arranged vertically, and a plurality of branch pipes (4) are arranged at equal intervals; The length of the conduit (3) is equivalent to the width of the macroporous asphalt mixture matrix (6), so that the nozzle matrix can evenly cover the entire macroporous asphalt mixture matrix (6); The plurality of branch pipes (4) are arranged at a spacing of 10-30 cm; The spraying pressure of the nozzle (5) is 5-20 MPa.
2. The semi-flexible pavement pressure grouting device according to claim 1 is characterized in that: The pressure grouting device is installed on a locomotive, and the locomotive moves along the paving direction of the road surface and drives the nozzle matrix to move synchronously above the macroporous asphalt mixture matrix (6).
3. The semi-flexible pavement pressure grouting device according to claim 1 is characterized in that: The plurality of nozzles (5) on each branch pipe (4) are arranged at equal intervals, and each branch pipe (4) is provided with 2-5 nozzles (5).
4. A construction method for paving a semi-flexible pavement using the semi-flexible pavement pressure grouting device according to claim 1, wherein after the middle surface layer (302) of the asphalt pavement (30) is paved, the semi-flexible upper surface layer (301) is paved; Its characteristics are: The construction method comprises the following steps: Step 1: Isolating the grouting construction area (10) from the curbstone (20) and the asphalt pavement (30); Step 2: paving the surface of the middle surface layer (302) with an open-graded macroporous asphalt mixture to form a macroporous asphalt mixture matrix (6), and rolling it with a roller; Step 3: After the temperature of the macroporous asphalt mixture matrix (6) is cooled, cement-based mortar is injected into the macropores through a pressure grouting device to form a semi-flexible upper layer (301); Step 4: The semi-flexible upper layer (301) is vibrated and leveled by a leveler, and the leveler discharges the bubbles remaining in the macroporous asphalt mixture matrix (6) through vibration energy; Step 5: curing the semi-flexible upper layer (301); In the step 2, the roller does not start the vibration mode when rolling the macroporous asphalt mixture matrix (6), so that the porosity of the macroporous asphalt mixture matrix (6) after rolling is 20%-30%.
5. The construction method for semi-flexible pavement paving according to claim 4 is characterized in that: In the semi-flexible top layer (301), the weight percentage of the open-graded macroporous asphalt mixture is 70%-80%, and the weight percentage of the cement-based mortar is 20%-30%; the porosity in the macroporous asphalt mixture matrix (6) is 20%-30%, and the cement-based mortar is filled into the macropores of the macroporous asphalt mixture matrix (6) by pressure grouting.
Citation Information
Cited By
Cold mixing semi-flexible pavement construction method
CN119266059A