Method for manufacturing solid electrolyte, solid electrolyte manufactured using the method, and all-solid-state battery containing the solid electrolyte

The solution method is used to make solid electrolytes, which solves the limitations of the use of expensive compounds and grinding process in traditional methods, and achieves high yield and low cost crystalline solid electrolyte production, improves lithium ion conductivity and discharge capacity, and enhances battery safety and energy density.

CN111063936BActive Publication Date: 2024-11-01HYUNDAI MOTOR CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910307539.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-10-16
Filing Date
2019-04-16
Publication Date
2024-11-01
Estimated Expiration
2039-04-16

AI Technical Summary

Technical Problem

The use of expensive compounds and grinding processes in traditional methods for manufacturing solid electrolytes limits mass production and particle size control, resulting in low stability and energy density of lithium secondary batteries and a safety risk of explosion or fire.

Method used

Solid electrolytes are manufactured by solution method. By mixing the solid electrolyte precursor with a solvent, drying and heat treatment, a crystalline solid electrolyte is formed, which avoids the grinding process, improves the yield and reduces the manufacturing cost.

Benefits of technology

It has achieved high yield and low cost crystalline solid electrolyte production, improved lithium ion conductivity and discharge capacity, enhanced battery safety and energy density, and reduced accident risk.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111063936B_ABST
    Figure CN111063936B_ABST
Patent Text Reader

Abstract

The present application discloses a method for manufacturing a solid electrolyte, a solid electrolyte manufactured using the method, and an all-solid battery comprising the solid electrolyte. The method comprises preparing an electrolyte mixture comprising a solid electrolyte precursor and a solvent; drying the electrolyte mixture and removing the solvent from the electrolyte mixture to form a dried electrolyte mixture; and heat treating the dried electrolyte mixture to form a crystalline solid electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a solid electrolyte, a solid electrolyte manufactured using the method, and an all-solid battery comprising the solid electrolyte. Specifically, the method can produce a crystalline solid electrolyte with a significantly improved yield without performing a milling process, thereby achieving energy saving. Background Art

[0002] In recent years, secondary batteries have been widely used as high-performance energy sources for small portable electronic devices such as mobile phones, cameras and laptop computers, as well as large-capacity storage batteries for vehicles and power storage systems. With the increase in the application fields of secondary batteries, research has been conducted to reduce the weight of components constituting portable electronic devices and the power consumption of portable electronic devices, so as to reduce the size of portable electronic devices and enable the continuous use of portable electronic devices for a long time. Therefore, there is a need for secondary batteries with smaller size and larger capacity.

[0003] Especially lithium secondary batteries, a type of secondary battery, have the advantages of higher energy density, larger capacity per unit area, lower self-discharge rate and longer life compared with nickel-manganese batteries or nickel-cadmium batteries. In addition, since lithium secondary batteries do not have a memory effect, lithium secondary batteries are easy to use and show a longer life. However, as the next generation of batteries for electric vehicles, lithium secondary batteries have low stability, low energy density and low output. In particular, lithium secondary batteries use flammable organic solvents as electrolyte solvents. Therefore, when a lithium secondary battery is short-circuited due to physical damage, the lithium secondary battery may easily explode or catch fire. Lithium secondary batteries have in fact caused a large number of accidents.

[0004] Therefore, in recent years, all-solid batteries that use solid electrolytes instead of liquid electrolytes as electrolytes to improve their safety have attracted considerable attention. Since all-solid batteries use non-flammable or flame-retardant solid electrolytes instead of flammable liquid electrolytes, problems related to fires caused by liquid electrolytes are solved. In addition, the bipolar structure is controllable, whereby the energy density of all-solid batteries can be increased to five times that of conventional all-solid batteries. The solid electrolyte, which is the core element of the all-solid battery, may include oxide-based materials and sulfur-based materials as main components.

[0005] Meanwhile, traditionally, the use of Li 2 S and P 2 S 5However, in this conventional method of manufacturing a solid electrolyte, very expensive compounds (e.g., about 500 million won / kg worth) such as Li 2 S as a starting material, large-scale production is limited, and the control of particle size is also limited. These problems are the biggest obstacles to the commercialization of batteries based on large-scale energy storage technology. Therefore, a new solid electrolyte synthesis method that can solve the above problems is needed.

[0006] The above information disclosed in this Background section is only for enhancement of understanding of the background of the invention and therefore it may contain information that does not form the prior art that is already known in this country to one of ordinary skill in the art. Summary of the invention

[0007] In a preferred aspect, a method for manufacturing a solid electrolyte using a solution method without a grinding process, a method for manufacturing a solid electrolyte capable of producing a crystalline solid electrolyte with a significantly improved yield, a solid electrolyte having lithium ion conductivity suitable for a secondary battery, and an all-solid-state battery having a discharge capacity suitable for a secondary battery are provided.

[0008] The term "all-solid cell" or "all-solid battery" as used herein refers to a battery that includes only solid or substantially solid components, such as solid electrodes (e.g., anodes and cathodes) and solid electrolytes. Therefore, in preferred aspects, the all-solid battery does not include fluid and / or flowable electrolyte components as materials or components.

[0009] Aspects of the present invention are not limited to those described above. Aspects of the present invention can be clearly understood from the following description and can be achieved by the means defined in the claims and their combinations.

[0010] In one aspect, a method for manufacturing a solid electrolyte for an all-solid battery is provided. The method may include preparing an electrolyte mixture comprising a solid electrolyte precursor and a solvent; drying the electrolyte mixture and removing the solvent to form a dried electrolyte mixture; and heat treating the dried electrolyte mixture to form a crystalline solid electrolyte. Preferably, the solid electrolyte precursor may be dissolved in the solvent.

[0011] Preferably, no grinding process may be performed.

[0012] The solid electrolyte precursor may appropriately include an element selected from the group consisting of lithium (Li), sulfur (S), phosphorus (P), bromine (Br), iodine (I), lithium sulfide (Li 2 S), phosphorus pentasulfide (P 2S 5 ), one or more of the group consisting of lithium bromide (LiBr), lithium chloride (LiCl) and lithium iodide (LiI).

[0013] The solvent may suitably include one or more selected from the group consisting of ethanol, propanol, butanol, dimethyl carbonate, ethyl acetate, tetrahydrofuran, 1,2-dimethoxyethane, propylene glycol dimethyl ether, and acetonitrile.

[0014] Preferably, the electrolyte mixture may include lithium (Li), phosphorus (P), sulfur (S), and chlorine (Cl) in a molar ratio of about 6:1:5:1.

[0015] Preferably, the drying may be performed at a temperature of about 25° C. to 200° C. for about 1 to 3 hours.

[0016] Preferably, the heat treatment may be performed at a temperature of about 400°C to 600°C.

[0017] The crystalline solid electrolyte may have an argyrodite-type crystal structure.

[0018] As used herein, the term "argyrodite" or "argyrodite-type crystal structure" refers to a crystalline structure similar to naturally occurring Ag. 8 G JZ 6 For example, the argyrodite crystal may have a Pna2 1 space group, and has a = 15.149, b = 7.476, An orthorhombic crystal with a unit cell of Z=4.

[0019] The crystalline solid electrolyte may have a 4 3- The argyrodite-type crystal structure.

[0020] In another aspect, a solid electrolyte manufactured using the method described herein and an all-solid-state battery comprising the solid electrolyte are provided.

[0021] The all-solid battery may include a solid electrolyte layer including a solid electrolyte; a positive electrode disposed on a first surface of the solid electrolyte layer, the positive electrode including a solid electrolyte; and a negative electrode disposed on a second surface of the solid electrolyte layer. The first surface and the second surface of the solid electrolyte layer are opposite surfaces.

[0022] The positive electrode may further include an active material and a conductive agent, and the negative electrode may include a lithium (Li) element.

[0023] Also provided is a vehicle comprising the all-solid-state battery described herein.

[0024] Other aspects of the invention are discussed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The above and other features of the present invention will now be described in detail with reference to certain exemplary embodiments shown in the accompanying drawings, which are given hereinafter by way of illustration only and therefore do not constitute a limitation of the present invention. In which:

[0026] Figure 1 An exemplary method of manufacturing an exemplary solid electrolyte for an exemplary all-solid battery according to an exemplary embodiment of the present invention is shown;

[0027] Figure 2 is a flow chart schematically illustrating an exemplary method of manufacturing an exemplary solid electrolyte for an exemplary all-solid battery according to an exemplary embodiment of the present invention;

[0028] Figure 3 An exemplary apparatus for manufacturing an exemplary solid electrolyte for an exemplary all-solid battery according to an exemplary embodiment of the present invention is shown;

[0029] Figure 4 is a Raman graph of a solid electrolyte for an exemplary all-solid battery according to an exemplary embodiment of the present invention;

[0030] Figure 5 shows the results of X-ray diffraction analysis based on X-ray diffraction spectroscopy (XRD) of an exemplary solid electrolyte for an exemplary all-solid battery according to an exemplary embodiment of the present invention;

[0031] Figure 6 Shown are measurement results of a discharge capacity of an exemplary all-solid battery to which an exemplary solid electrolyte for an exemplary all-solid battery according to an exemplary embodiment of the present invention is applied after charging and discharging the all-solid battery. DETAILED DESCRIPTION

[0032] Hereinafter, reference will be made in detail to various embodiments of the present invention, examples of which are shown in the accompanying drawings and described below. However, the present invention may be embodied in many different forms and should not be construed as limited to the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention thorough and complete and to fully convey the scope of the present invention to those skilled in the art. The present invention is limited only by the categories of the claims. Whenever possible, the same reference numerals will be used throughout the drawings to represent the same or similar parts.

[0033] Unless otherwise defined, all terms (including technical and scientific terms) used in this specification have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. It should also be understood that those terms as defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant field and the present invention, and will not be interpreted in an idealized or overly formal manner unless explicitly defined in this article.

[0034] In addition, the terms used in this specification are only for explaining specific embodiments, not for limiting the present invention. Singular forms may include plural forms, unless it can be seen from the context that it indicates a different meaning. It should also be understood that when used in this specification, the terms "including", "having" and the like indicate the presence of the elements, features, quantities, steps and / or operations described, but do not exclude the presence or addition of one or more other elements, features, numbers, steps and / or operations. It should be understood that the term "and / or" refers to one or more possible combinations of specific related items, and includes such combinations.

[0035] In addition, it should be understood that when an element such as a layer, film, region or substrate is referred to as being "on" another element, it can be directly on the other element or intervening elements may be present therebetween. It should also be understood that when an element such as a layer, film, region or substrate is referred to as being "under" another element, it can be directly under the other element or intervening elements may be present therebetween.

[0036] Unless otherwise clearly stated in the context, all numerical values, numbers and / or expressions used in this specification that represent the amount of ingredients, reaction conditions, polymer compositions and mixtures are approximate values, which reflect the various uncertainties in the measurements that inevitably occur when obtaining these numbers. Therefore, it should be understood that in all cases, the term "about" should be understood to modify all numerical values, numbers and / or expressions. Unless otherwise specified or obvious from the context, the term "about" used herein should be understood to be within the normal allowable range of this field, such as within 2 standard deviations of the mean value. "About" can be understood to be within 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, 0.1%, 0.05% or 0.01% of the numerical value.

[0037] In addition, when numerical ranges are disclosed in the specification, these ranges are continuous and include all numerical values ​​(including the maximum value) from the minimum value to the maximum value within the range, unless otherwise defined. In addition, when a range refers to an integer, it includes all integers (including the maximum value) from the minimum value to the maximum value within the range, unless otherwise defined.

[0038] It should be understood that in the specification, when a range refers to a parameter, the parameter includes all numbers within the range (including the disclosed endpoints). For example, the range "5 to 10" includes the numbers 5, 6, 7, 8, 9, 10, and any sub-ranges such as the ranges 6 to 10, 7 to 10, 6 to 9, and any numbers between appropriate integers falling within the range, such as 5.5, 6.5, 7.5, 5.5 to 8.5, 6.5 to 9. In addition, for example, the range "10% to 30%" includes all integers, including the numbers 10%, 11%, 12%, 13% and 30%, and any sub-ranges 10% to 15%, 12% to 18% or 20% to 30%, and any numbers between appropriate integers falling within the range, such as 10.5%, 15.5%, 25.5%.

[0039] It should be understood that the term "vehicle" or "vehicle-like" or other similar terms used herein include a broad range of motor vehicles, such as passenger motor vehicles, including sports utility vehicles (SUVs), buses, trucks, various commercial vehicles, water vehicles including various ships, vessels, aircraft, etc.; and also include hybrid vehicles, electric vehicles, plug-in hybrid electric vehicles, hydrogen-powered vehicles and other alternative fuel vehicles (e.g., fuels derived from resources other than petroleum). As mentioned herein, a hybrid vehicle is a vehicle having two or more power sources, such as a vehicle including gasoline power and electric power.

[0040] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings.

[0041] Figure 1 and Figure 2 is an exemplary process and flow chart schematically illustrating an exemplary method of manufacturing an exemplary solid electrolyte for an exemplary all-solid battery according to an exemplary embodiment of the present invention.

[0042] like Figure 1 As shown, the method for manufacturing a solid electrolyte for an all-solid battery can be significantly different from the conventional manufacturing method in that the solid electrolyte is manufactured using a solution method without the need for a grinding process. For example, the method for manufacturing a solid electrolyte can produce a crystalline solid electrolyte with a high yield without the need for a grinding process, thereby achieving energy saving. In addition, the formation of impurities due to contamination of the balls used in the grinding process can be prevented to the greatest extent. In addition, the method for manufacturing a solid electrolyte according to the present invention has the economic effect of reducing manufacturing costs, because most of the starting materials used in conventional grinding processes are expensive. At the same time, in the present invention, the solution method may include the following processes. For example, the method for manufacturing a solid electrolyte may include a process of mixing a solid electrolyte precursor and a solvent, a dissolution and / or reaction process, and a heat treatment process, but does not include a grinding process.

[0043] like Figure 2 As shown, the method for manufacturing a solid electrolyte for an all-solid-state battery according to an exemplary embodiment of the present invention may include the steps of forming an electrolyte mixture by, for example, adding a solid electrolyte precursor to a solvent (S100) and dissolving the solid electrolyte precursor in the solvent (S200); a step of drying the electrolyte mixture and removing the solvent to form a dried electrolyte mixture (S300); and a step of heat-treating the dried electrolyte mixture to form a crystalline solid electrolyte (S400).

[0044] Specifically, in the method for manufacturing a solid electrolyte according to the present invention, the solid electrolyte precursor may appropriately include an element selected from lithium (Li), sulfur (S), phosphorus (P), bromine (Br), iodine (I), lithium sulfide (Li 2 S), phosphorus pentasulfide (P 2 S 5 ), lithium bromide (LiBr), lithium chloride (LiCl) and lithium iodide (LiI) The solid electrolyte precursor may include one or more of the following: lithium (Li), sulfur (S), lithium sulfide (Li 2 S) and phosphorus pentasulfide (P 2 S 5 ). However, the present invention is not limited thereto.

[0045] The solvent may suitably include one or more selected from the group consisting of ethanol, propanol, butanol, dimethyl carbonate, ethyl acetate, tetrahydrofuran, 1,2-dimethoxyethane, propylene glycol dimethyl ether and acetonitrile. In particular, acetonitrile may suitably be included in the solvent of the present invention. However, the present invention is not limited thereto.

[0046] In the step of dissolving the solid electrolyte precursor in a solvent to form a mixed electrolyte (S200), the composition ratio (molar ratio) of lithium (Li): phosphorus (P): sulfur (S): chlorine (Cl) in the mixed electrolyte may be about 6:1:5:1. However, the present invention is not limited thereto.

[0047] After the step (S200) of dissolving the solid electrolyte precursor in the solvent to form a mixed electrolyte, a step (S300) of drying the mixed electrolyte to remove the solvent to form a dried electrolyte mixture is performed, in which the mixed electrolyte can be dried at a temperature of about 25°C to 200°C. When the mixed electrolyte is dried at a temperature below about 25°C, the mixed electrolyte may not be fully dried. When the mixed electrolyte is dried at a temperature above about 200°C, the composition of the solid electrolyte finally manufactured may vary due to uneven evaporation of the mixed electrolyte. As a result, a solid electrolyte having an ionic conductivity or a discharge capacity lower than expected and a battery containing such a solid electrolyte may be manufactured. For these reasons, the process of drying the mixed electrolyte can be carried out at a temperature of, for example, about 25°C, 50°C, 100°C, 150°C, or 200°C. However, the present invention is not limited thereto.

[0048] In addition, the drying process may be performed for about 1 to 3 hours. For example, the process of drying the mixed electrolyte may be performed using a vacuum drying device at a temperature of about 25° C. for about 1 to 3 hours, at a temperature of about 50° C. for about 1 to 3 hours, at a temperature of about 100° C. for about 1 to 3 hours, at a temperature of about 150° C. for about 1 to 3 hours, or at a temperature of about 200° C. for about 1 to 3 hours. However, the present invention is not limited thereto.

[0049] When the time for drying the mixed electrolyte is less than about 1 hour, the mixed electrolyte may not be completely dried. When the time for drying the mixed electrolyte exceeds about 3 hours, the composition of the finally manufactured solid electrolyte may vary due to uneven evaporation of the mixed electrolyte.

[0050] In addition, after the step (S300) of drying the mixed electrolyte to remove the solvent to form a dried electrolyte mixture, a step (S400) of heat-treating the dried electrolyte mixture to form a crystalline solid electrolyte is performed, and the heat treatment process may be performed at a temperature of about 400° C. to 600° C. The crystals of the solid electrolyte may be grown by the process of heat-treating the dried electrolyte mixture.

[0051] When the dried electrolyte mixture is heat-treated at a temperature below about 400° C., the solid electrolyte may be non-uniformly crystallized, and thus the finally manufactured solid electrolyte may have a non-uniform crystal structure. When the dried electrolyte mixture is heat-treated at a temperature above about 600° C., an unexpected crystalline phase may appear in the finally manufactured solid electrolyte.

[0052] The process of heat-treating the dried electrolyte mixture may be performed at, for example, 400° C., 450° C., 500° C., 550° C., or 600° C. However, the present invention is not limited thereto.

[0053] In addition, the solid electrolyte manufactured using the manufacturing method (S100 to S400) according to the present invention may include a crystalline solid electrolyte, and in particular may have a argyrodite-type crystal structure. Here, the term "argyrodite" may refer to a crystalline phase. In particular, the crystalline solid electrolyte manufactured using the manufacturing method (S100 to S400) according to the present invention may have a PS 4 3- However, the present invention is not limited thereto. For example, the crystalline solid electrolyte manufactured using the manufacturing method (S100 to S400) according to the present invention may have a crystalline solid electrolyte containing another compound (e.g., Li 6 PS 5 Cl) of the argyrodite-type crystal structure.

[0054] Meanwhile, when the dried electrolyte mixture is heat-treated at a temperature lower than about 400° C., as described above, the solid electrolyte may be non-uniformly crystallized, whereby the amount of argyrodite-type crystals of the solid electrolyte may be reduced, and the solid electrolyte may have a non-uniform crystal structure. On the other hand, when the dried electrolyte mixture is heat-treated at a temperature higher than about 600° C., an undesirable crystal structure other than the argyrodite-type crystal structure may be formed in the finally manufactured solid electrolyte. As a result, the ionic conductivity or discharge capacity of the solid electrolyte may be reduced.

[0055] Figure 3 An exemplary apparatus for manufacturing a solid electrolyte for an exemplary all-solid battery according to an exemplary embodiment of the present invention is shown. Figure 1 and Figure 2 The content described is different from the part.

[0056] like Figure 3 As shown, the manufacturing method according to the present invention described above (see Figure 2 Some or all of the steps S100 to S400 of the present invention may be performed by a manufacturing device. The manufacturing device may include a reactor, an inlet formed above the reactor, a stirrer for stirring the material in the reactor, a thermostat formed on the outer surface of the reactor, and a pressure reducer connected to the inside of the reactor. For example, a solid electrolyte precursor and a solvent may be supplied to the reactor through the inlet. In the reactor, the solid electrolyte precursor and the solvent may be stirred at a predetermined speed by the stirrer to mix and dissolve them (see Figure 2 In addition, the mixing and dissolving may be performed at a predetermined temperature and / or a predetermined pressure by a thermostat and / or a pressure reducer.

[0057] In one aspect, the all-solid battery may include a positive electrode, a negative electrode, and a solid electrolyte layer, the solid electrolyte layer comprising Figure 2 The all-solid-state battery according to an exemplary embodiment of the present invention may include a solid electrolyte manufactured using the above-mentioned manufacturing method (see S100 to S400). Figure 2 A solid electrolyte layer of a solid electrolyte manufactured by S100 to S400 of the present invention; a positive electrode disposed on a first surface of the solid electrolyte layer, the positive electrode comprising the solid electrolyte; and a negative electrode disposed on a second surface of the solid electrolyte layer. The first surface and the second surface are opposite surfaces, so the negative electrode can be disposed on the opposite surface of the positive electrode.

[0058] Specifically, in an exemplary all-solid battery according to the present invention, in addition to using the above-mentioned manufacturing method (see Figure 2 In addition to the solid electrolyte manufactured by S100 to S400 of the present invention, the positive electrode may also include an active material (e.g., a positive electrode active material including niobium (Nb)) and a conductive agent (e.g., a conductive agent containing carbon (C)). Moreover, in an exemplary all-solid battery according to the present invention, the negative electrode may include a lithium (Li) element.

[0059] Example

[0060] Hereinafter, the present invention will be described in more detail with reference to Examples and Evaluation Examples. However, the following Examples are only for illustration to help understand the present invention, and the present invention is not limited to the following Examples.

[0061] Example 1: Preparation of solid electrolyte for all-solid-state battery

[0062] The following steps were performed to fabricate a solid electrolyte using a solution process.

[0063] Li powder (Sigma Aldrich Company), S powder (Sigma Aldrich Company), P 2 S 5 Powder (Sigma Aldrich Company) and LiCl powder (Sigma Aldrich Company) were used as starting materials. 1.29 g of Li powder, 2.98 g of S powder, 4.14 g of P 2 S 5 powder and 1.57 g of LiCl powder to have a 6 PS 5 Cl with the same composition ratio (molar ratio), and mixed to prepare a powder mixture. The powder mixture and 100 g of acetonitrile solvent were added to a 100 ml reactor (see Figure 3The mixed solution was vacuum dried at a temperature of about 200° C. for 2 hours to remove residual acetonitrile. Subsequently, the dried powder mixture was heat-treated at a temperature of 550° C. for 5 hours to crystallize the dried powder mixture, thereby obtaining a solid electrolyte.

[0064] Example 2: Fabrication of an all-solid-state battery comprising a solid electrolyte

[0065] The solid electrolyte manufactured as described above was compressed to form a solid electrolyte layer with a thickness of 500 μm. A powder containing an active material (NCM622 coated with niobium (Nb)), a solid electrolyte having the same composition as that of the solid electrolyte for the solid electrolyte layer, and a conductive agent (Super C) were used as a positive electrode. A positive electrode was formed on one surface of the solid electrolyte layer to have a conductivity of 5.8 mg / cm 2 The active material loading amount and thickness of 30 μm. A lithium foil with a thickness of 100 μm was used as the negative electrode. The negative electrode was formed on the other surface of the solid electrolyte layer to be opposite to the positive electrode.

[0066] Evaluation Example 1: Analysis of Solid Electrolyte Using Raman Spectroscopy

[0067] exist Figure 4 In the mixture of the solid electrolyte prepared according to Example 1, PS 4 3- This means that when a solid electrolyte is produced using the solution method according to the present invention, a crystalline phase framework of the solid electrolyte precursor is formed.

[0068] Evaluation Example 2: Measurement of Lithium Ion Conductivity of Solid Electrolyte

[0069] The solid electrolyte prepared according to Example 1 was compressed to form a sample for measurement (13 mm in diameter and 0.6 mm in thickness). An alternating potential of 10 mV was applied to the sample, and then 1×10 6 The frequency was scanned from 100 Hz to 100 Hz to measure the impedance value, thereby determining the lithium ion conductivity. The lithium ion conductivity of the sample containing the solid electrolyte manufactured according to Example 1 was measured to be 1.0×10 -3 S / cm. This means that the solid electrolyte according to the present invention exhibits higher ion conductivity.

[0070] Evaluation Example 3: X-ray Diffraction Analysis Based on X-ray Diffraction Spectroscopy (XRD) of Solid Electrolyte

[0071] exist Figure 5 In the XRD pattern of the solid electrolyte prepared according to Example 1, there is a peak of the argyrodite crystalline phase. The argyrodite crystalline phase can be formed in the solid electrolyte using the solution method according to the present invention.

[0072] Evaluation Example 4: Measurement of Discharge Capacity of All-Solid State Battery

[0073] The measured discharge capacity of the all-solid-state battery manufactured according to Example 2 is shown in Figure 6 The all-solid-state battery was charged and discharged at a charge rate (Crate) of 0.02C, a voltage of 2.0V to 3.58V, and a constant current (CC) to measure its discharge capacity. Figure 6 In the embodiment 2, the all-solid battery manufactured according to the embodiment 2 has a discharge capacity of about 160 mAh / g. This means that the solid electrolyte and the all-solid battery manufactured according to the manufacturing method of the present invention show very excellent performance.

[0074] As is apparent from the foregoing, the method of manufacturing a solid electrolyte according to an exemplary embodiment of the present invention can manufacture a crystalline solid electrolyte with significantly improved yield.

[0075] In addition, the crystalline solid electrolyte can be produced without performing a grinding process, thereby achieving energy saving in the manufacturing process of the solid electrolyte.

[0076] Additionally, the crystalline solid electrolyte can be produced without using expensive starting materials used in conventional milling processes, thereby reducing manufacturing costs.

[0077] The effects of the present invention are not limited to those described above. It should be understood that the effects of the present invention include all effects that can be inferred from the foregoing description of the present invention.

[0078] Although specific embodiments of the present invention have been described and illustrated, it will be understood by those skilled in the art that the present invention is not limited to the described embodiments and that various modifications may be made without departing from the main concept of the present invention as defined in the claims. Therefore, it should be noted that these modifications cannot be understood separately from the technical concepts or aspects of the present invention, and it should be understood that these modifications should all fall within the scope of the claims of the present invention.

Claims

1. A method for manufacturing a solid electrolyte for an all-solid-state battery, include: preparing an electrolyte mixture comprising a solid electrolyte precursor and a solvent; drying the electrolyte mixture and removing the solvent to form a dried electrolyte mixture; and thermally treating the dried electrolyte mixture to form a crystalline solid electrolyte; The solid electrolyte precursor includes one selected from the group consisting of lithium, sulfur, phosphorus, bromine, iodine, phosphorus pentasulfide, lithium bromide, lithium chloride, lithium iodide and combinations thereof, and the solid electrolyte precursor does not include lithium sulfide. wherein no grinding process is performed, and Wherein, the solvent includes acetonitrile.

2. The method according to claim 1, in, The solid electrolyte precursor is dissolved in the solvent.

3. The method according to claim 1, in, The electrolyte mixture includes lithium, phosphorus, sulfur, and chlorine in a molar ratio of 6:1:5:

1.

4. The method according to claim 1, in, The drying is performed at a temperature of 25° C. to 200° C. for 1 to 3 hours.

5. The method according to claim 1, in, The heat treatment is performed at a temperature of 400°C to 600°C.

6. The method according to claim 1, in, The crystalline solid electrolyte has an argyrodite-type crystal structure.

7. The method according to claim 6, in, The crystalline solid electrolyte comprises PS 4 3- The argyrodite-type crystal structure.

8. A solid electrolyte manufactured using the method according to claim 1.

9. An all-solid-state battery, include: A solid electrolyte layer comprising the solid electrolyte according to claim 8; a positive electrode disposed on a first surface of the solid electrolyte layer, the positive electrode comprising the solid electrolyte; and a negative electrode disposed on a second surface of the solid electrolyte layer, The first surface and the second surface of the solid electrolyte layer are opposing surfaces.

10. The all-solid battery according to claim 9, wherein The positive electrode further comprises an active material and a conductive agent; and The negative electrode contains lithium.

11. A vehicle comprising the all-solid-state battery according to claim 9.