Porous silicon-containing composite, method for preparing the same, carbon composite, electrochemically active material composite, electrode, lithium battery and device
By adopting a combination of porous silicon-containing composite and carbonaceous material, the problems of volume expansion and electrode disintegration of silicon material in lithium-ion batteries are solved, and the capacity retention rate and efficiency of lithium batteries are improved and life extension are extended.
Patent Information
- Application Number
- CN201910961964.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-10-25
- Filing Date
- 2019-10-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2039-10-11
AI Technical Summary
The volume expansion of the existing lithium-ion battery negative electrode active material, silicon material, during charging, leads to an increase in the specific surface area of the electrical isolation and the active material, thereby accelerating the electrolyte decomposition reaction, resulting in poor battery performance.
Using porous silicon-containing composites, the improved silicon-containing composites are prepared by combining silicon particles with different shapes and oxidation degrees with graphene to form a porous silicon-containing composite with a double core/shell structure, and a carbonaceous coating layer is formed on its surface. Electrode material.
It effectively suppresses the volume expansion of silicon and the collapse of electrodes, improves the capacity retention rate and initial efficiency of lithium batteries, and extends the battery life.
Smart Images

Figure CN111106329B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to and the benefits of Korean Patent Application No. 10-2018-0128321 filed in the Korean Intellectual Property Office on October 25, 2018, and all rights arising therefrom, the contents of which are incorporated herein by reference in their entirety. Technical Field
[0003] The present disclosure relates to a porous silicon-containing composite, a carbon composite using the porous silicon-containing composite, and an electrode, a lithium battery, and an electronic device each including the porous silicon-containing composite. Background Art
[0004] Among negative electrode active materials for lithium-ion batteries, silicon has a high theoretical capacity of 4,200 mAh / g and low cost, and thus has been actively studied for use as a negative electrode material. However, during charging of the battery, as Li 4.4 Si alloys, silicon can undergo a large volume expansion, and thus an electrically isolated (insulated) active material can be produced in the electrode. In addition, the increase in the specific surface area of the active material can accelerate the electrolyte decomposition reaction. In order to address these shortcomings, it has been proposed to develop a structure for suppressing the volume expansion of silicon and the crushing that occurs during the volume expansion of silicon, and to form a coating layer such as carbon on the surface of silicon.
[0005] However, currently available silicon materials are still unsatisfactory in terms of their effects on the reduction of volume expansion and the charging and discharging efficiency of batteries.Therefore, there is still a need for improved negative electrode active materials. Summary of the invention
[0006] A porous silicon-containing composite is provided.
[0007] A carbon composite including the porous silicon-containing composite and a carbonaceous material is provided.
[0008] Provided is a lithium battery having improved lifespan, capacity, and efficiency by using an electrode including the porous silicon-containing composite or a carbon composite including the porous silicon-containing composite and a carbonaceous material.
[0009] A device (apparatus) including the porous silicon-containing composite or a carbon composite including the porous silicon-containing composite and a carbonaceous material is provided.
[0010] Additional aspects will be set forth in part in the description which follows and, in part, will be apparent from the description, or may be learned by practice of the presented embodiments.
[0011] According to one aspect of the embodiment, a porous silicon-containing composite includes: a porous core including porous silicon composite secondary particles; and a shell on at least one surface of the porous core, the shell including a first graphene, wherein the porous silicon composite secondary particles include an aggregate of: a first primary particle including silicon, a second primary particle including a structure, and a second graphene on at least one surface of the first primary particle and the second primary particle, and wherein at least one of the shape and degree of oxidation of the first primary particle and the second primary particle is different.
[0012] In an embodiment, the structure may include silicon, germanium (Ge), tin (Sn), aluminum (Al), zinc (Zn), antimony (Sb), alloys thereof, or combinations thereof.
[0013] The structure may be silicon.
[0014] According to one aspect, a method for preparing a porous silicon-containing composite includes: contacting a first primary particle having a first shape and a first degree of oxidation and a second primary particle having a second shape and a second degree of oxidation to form porous silicon secondary particles, wherein at least one of the first and second shapes or the first and second degrees of oxidation are different; and heat treating the porous silicon secondary particles and a carbon source gas to prepare the porous silicon-containing composite.
[0015] According to one aspect, an electrochemically active material composite includes: an electrochemically active material; and the porous silicon-containing composite, wherein the porous silicon-containing composite is on a surface of the electrochemically active material.
[0016] An electrode includes the porous silicon-containing composite.
[0017] According to one aspect, a carbon composite includes the porous silicon-containing composite and a carbonaceous material.
[0018] According to one aspect, a lithium battery includes the electrode.
[0019] According to one aspect, a device comprises: the porous silicon-containing composite.
[0020] In embodiments, the device may be a field emission device, a biosensor, a semiconductor device, or a thermoelectric device. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] These and / or other aspects will become apparent and more readily appreciated from the following description of the embodiments considered in conjunction with the accompanying drawings, in which:
[0022] Figure 1 A schematic diagram illustrating an embodiment of the structure of a porous silicon-containing composite;
[0023] Figure 2For illustration Figure 1 A schematic diagram of an embodiment of the structure of a silicon composite primary particle of a porous silicon-containing composite;
[0024] Figures 3A-3C An image showing the results of transmission electron microscopy (TEM) analysis of the porous silicon-containing composite according to Preparation Comparative Example 1;
[0025] Figures 4A-4D is an image showing the results of transmission electron microscopy (TEM) analysis of the surface of the porous silicon-containing composite according to Preparation Example 1;
[0026] Figure 5 is a graph of capacity retention (percent, %) versus cycle number, which shows the high rate characteristics of the coin half-unit cells of Example 5 and Comparative Examples 4 and 5;
[0027] Figures 6A-6C are the results of scanning electron microscopy (SEM) analysis of the coin full-cell battery of Example 1, which respectively show the surface state of the negative electrode at the initial stage and after the 1st and 20th charge-discharge cycles;
[0028] Fig. 7A is the differential capacity (dQ / dV, mAh / gV) versus voltage (V, relative to Li / Li + ) which illustrates the evaluation results of the differential charge and discharge characteristics (dQ / dV) of the coin half-cell batteries of Example 5 and Comparative Example 4 at the first cycle;
[0029] Figure 7B is the differential capacity (dQ / dV, mAh / gV) versus voltage (V, relative to Li / Li + ) which illustrates the evaluation results of the differential charge and discharge characteristics (dQ / dV) of the coin half-cell batteries of Example 5 and Comparative Example 5 at the first cycle;
[0030] Figure 8 is a schematic diagram of an implementation of a lithium battery;
[0031] Fig. 9 is a schematic diagram of an embodiment of a thermoelectric module;
[0032] Fig.10 A schematic diagram illustrating an embodiment of a thermoelectric cooler utilizing the Peltier effect;
[0033] Fig.11 A schematic diagram for illustrating an embodiment of a thermoelectric generator utilizing the Seebeck effect; and
[0034] Fig.12 A cross-sectional view illustrating the structure of an embodiment of an electrode of a biosensor. DETAILED DESCRIPTION
[0035] Embodiments will now be described in detail, examples of which are shown in the accompanying drawings, wherein the same reference numerals refer to the same elements throughout. In this regard, the disclosed embodiments may have different forms and should not be construed as being limited to the descriptions set forth herein. Therefore, the following merely describes the embodiments to illustrate aspects by reference to the accompanying drawings. As used herein, the term "and / or" includes any and all combinations of one or more of the related enumerated items. Expressions such as "at least one (kind) of..." modify the entire list of elements when before or after a list of elements without modifying the individual elements of the list.
[0036] It will be understood that when an element is referred to as being “on” another element, it can be directly on the other element or intervening elements may be present therebetween. In contrast, when an element is referred to as being “directly on” another element, there are no intervening elements present.
[0037] It will be understood that although the terms "first", "second", "third", etc. may be used herein to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings herein, the "first element", "component", "region", "layer" or "part" discussed below may be referred to as a second element, component, region, layer or part.
[0038] The terms used herein are only for the purpose of describing specific embodiments and are not intended to be restrictive. As used herein, the singular forms "one (kind) (indefinite article, a, an)" and "said (the)" are intended to include plural forms, including "at least one (kind)", unless the content clearly indicates otherwise. "At least one (kind)" should not be interpreted as limiting "one (kind)". "Or" means "and / or". It will be further understood that the term "comprising" or "including" when used in this specification indicates the presence of stated features, regions, wholes, steps, operations, elements, and / or components, but does not exclude the presence or addition of one or more other features, regions, wholes, steps, operations, elements, components, and / or their collections.
[0039] In addition, relative terms such as "lower" or "bottom" and "upper" or "top" may be used herein to describe the relationship of one element to another element as shown in the figure. It will be understood that in addition to the orientation depicted in the figure, the relative terms are also intended to cover different orientations of the device. For example, if the device in one of the figures is turned over, the element described as being on the "lower" side of the other element will be oriented on the "upper" side of the other element. Therefore, depending on the specific orientation of the figure, the exemplary term "lower" can cover both "lower" and "upper" orientations. Similarly, if the device in one of the figures is turned over, the element described as "below" or "below" the other element will be oriented "above" the other element. Therefore, the exemplary terms "below..." or "below..." can cover both "above..." and "below..." orientations.
[0040] As used herein, "about" or "approximately" includes the stated value and means within an acceptable range of deviation for the particular value as determined by one of ordinary skill in the art taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" can mean that the deviation from the stated value is within one or more standard deviations, or within a range of ±30%, 20%, 10%, or 5%.
[0041] Unless otherwise defined, all terms (including technical and scientific terms) used in this article have the same meaning as commonly understood by ordinary technicians in the field to which the present disclosure belongs. It will be further understood that terms, such as those defined in commonly used dictionaries, should be interpreted as their meanings consistent with their meanings in the context of the present disclosure and the relevant art, and will not be interpreted in an idealized or overly formal sense unless clearly defined in this article.
[0042] Exemplary embodiments are described herein with reference to cross-sectional views as schematic diagrams of idealized embodiments. Thus, deviations from the shapes of the figures as a result of, for example, manufacturing techniques and / or tolerances are expected. Thus, the embodiments described herein should not be construed as being limited to the specific shapes of the regions as shown herein, but rather include deviations in shape resulting from, for example, manufacturing. For example, a region illustrated or described as flat may typically have rough and / or nonlinear features. In addition, the illustrated sharp corners may be rounded. Thus, the regions shown in the figures are schematic in nature, and their shapes are not intended to illustrate the precise shapes of the regions, and are not intended to limit the scope of the claims.
[0043] The term "graphene" as used in this specification means a polycyclic aromatic molecule formed by a plurality of carbon atoms covalently bonded to each other. The covalently bonded carbon atoms may form a six-membered ring as a repeating unit, and may further include at least one of a five-membered ring and a seven-membered ring. Therefore, graphene comprises a monolayer of covalently bonded carbon atoms with sp2 hybridization. Multiple graphene layers are often referred to as graphite in the art. However, for convenience, "graphene" as used in this article may be a monolayer, or may also include a plurality of carbon layers such as 1-100 carbon layers or 1-30 carbon layers. Therefore, graphene as used in this article may have a multi-layered structure formed by stacking a monolayer of graphene.
[0044] Hereinafter, embodiments of a porous silicon-containing composite, an electrode including an electrode active material including the porous silicon-containing composite, a lithium battery including the electrode, and a device using the porous silicon-containing composite will be described in more detail.
[0045] According to one aspect, a porous silicon-containing composite includes: a porous core including porous silicon composite secondary particles; and a shell on at least one surface of the porous core, the shell including a first graphene, wherein the porous silicon composite secondary particles include an aggregate of: a first primary particle including silicon, a second primary particle including a structure, and a second graphene on at least one surface of the first primary particle and the second primary particle, and wherein at least one of the shape and oxidation degree of the first primary particle and the second primary particle is different.
[0046] The porous core may include at least one porous silicon composite secondary particle.
[0047] The structure may include silicon (Si), germanium (Ge), tin (Sn), aluminum (Al), zinc (Zn), antimony (Sb), alloys thereof, or combinations thereof. The structure is silicon (Si).
[0048] For example, the second primary particles may be different from the first primary particles in shape and degree of oxidation.
[0049] The first primary particle may have an oxygen content of about 3 atomic percent (atomic %)-about 15 atomic %, about 4 atomic %-about 13 atomic %, or about 5 atomic %-about 10 atomic % based on the total content of the first primary particle, and a relatively high degree of oxidation. The second primary particle may have an oxygen content of about 0.01 atomic % or greater to less than 3 atomic % and a lower degree of oxidation than the first primary particle. For example, the first primary particle may have an oxygen content of about 4 atomic %-about 8 atomic % or about 3 atomic %-about 5 atomic % based on the total content of the first primary particle. For example, the second primary particle may have an oxygen content of about 0.1 atomic %-about 2 atomic %, for example, about 1 atomic %-about 1.5 atomic % based on the total content of the second primary particle.
[0050] The oxidation degrees of the first primary particles and the second primary particles may be inversely proportional to the sizes of the first primary particles and the second primary particles, respectively.
[0051] The shapes of the first primary particles and the second primary particles may not be particularly limited.
[0052] The first primary particle may have a plate shape, a needle shape, a cubic shape, or a rod shape, or a combination thereof. The second primary particle may have, for example, a spherical form or a nanowire form.
[0053] When the second primary particle may have a spherical form or a nanowire form, the first primary particle may have a plate shape, a needle shape, or a combination thereof. The second primary particle may have a spherical shape. The preparation method of the first primary particle and the second primary particle is not particularly limited. For example, the first primary particle can be prepared by crushing or grinding. For example, the second primary particle can be prepared by a gas phase synthesis method.
[0054] The first primary particle and the second primary particle may have shapes different from each other. The porous silicon-containing composite may further include: a third primary particle including silicon, the third primary particle having a nanotube shape, a nanorod shape, a wafer shape, a nanobelt shape, or a combination thereof. The second primary particle can form a network by connecting to the first primary particle.
[0055] The first primary particles may have a plate shape, a needle shape, or a combination thereof, and the second primary particles may have a spherical shape. The first primary particles, which are silicon obtained by crushing a silicon source, may have a high degree of oxidation due to contact with heat and air during crushing of the silicon source.
[0056] In order to provide improved active material properties including improved capacity and improved life characteristics, in a porous silicon-containing composite including silicon composite primary particles comprising the first primary particles, the size of the first primary particles is preferably reduced to about 80 nanometers (nm) or less. However, due to the limitations of the crushing process, this can increase the time and energy required to reduce the particle size of the first primary particles to 100nm or less, thereby resulting in significantly increased preparation costs and time. Therefore, it is not practical or easy to reduce the particle size to a suitable size. In addition, due to the increase in the degree of oxidation of the first primary particles that occurs during the crushing process, the capacity and initial efficiency characteristics of the battery may be limited.
[0057] Furthermore, due to the large specific surface area of the first primary particles, it is preferable to suppress a side reaction of the porous silicon-containing composite including the first primary particles with an electrolyte.
[0058] In order to solve these problems of using silicon composite primary particles including the first primary particles to manufacture lithium batteries with improved specific capacity and initial efficiency without reduced life, the inventors use the second primary particles together with the first primary particles, and the second primary particles have different oxidation degrees and / or different shapes from those of the first primary particles. The second primary particles can be prepared by a vapor deposition method. Silicon with a size of tens of nanometers can be obtained by using the second primary particles, and the second primary particles can have a lower oxidation degree than the first primary particles because no oxidation occurs during the preparation of the second primary particles. The second primary particles may have a low oxidation degree as described above, but have a large specific surface area. The second primary particles have limitations in commercialization due to high manufacturing costs. The porous silicon-containing composite obtained using such a second primary particle may have a lower oxidation degree than the porous silicon-containing composite prepared using the first primary particles, and has a high specific capacity, but a large specific surface area and a low initial efficiency. Therefore, during repeated charging and discharging, the porous silicon-containing composite using the second primary particles may deteriorate, so that the initial efficiency and life characteristics of the battery may be unsatisfactory.
[0059] Therefore, the first primary particles and the second primary particles described above may be used together to prepare a porous silicon-containing composite according to one or more embodiments to provide a desired smaller size, excellent specific surface area, and improved specific capacity, initial efficiency, and capacity characteristics.
[0060] The mixing weight ratio of the first primary particles to the second primary particles may be about 1:99 to about 99:1, for example, about 10:90 to about 90:10, and for example, about 90:10 to about 50:50.
[0061] The porous silicon-containing composite can use two types of primary particles containing silicon as described above together, or can use three or more types of primary particles containing silicon. For example, multiple types of silicon can differ in the degree of oxidation and / or shape.
[0062] The porous silicon-containing composite can further include, for example, third primary particles in the form of nanotubes, nanorods, nanobelts, or a combination thereof.
[0063] The porous silicon-containing composite can further include a silicon suboxide of the formula SiO x (where 0 < x < 2) between the silicon and the second graphene. The silicon suboxide can be in the form of a film or a matrix.
[0064] The first graphene and the second graphene can be in the form of a film, particles, a matrix, or a combination thereof. The first graphene and the second graphene can be the same.
[0065] As used herein, the term "silicon suboxide" can be a single composition represented by SiO x (where 0 < x < 2), or can be a composition including, for example, Si and SiO 2 to have an average composition represented by SiO x (where 0 < x < 2). For example, the silicon suboxide can include SiO 2 .
[0066] In the porous silicon-containing composite according to one or more embodiments, the total amount of silicon, i.e., the total amount of the first primary particles and the second primary particles, can be about 0.01 parts by weight - about 99 parts by weight, for example about 0.01 parts by weight - about 40 parts by weight, each relative to the total weight of 100 parts by weight of the porous silicon-containing composite. When the total amount of silicon is within these ranges, a lithium battery including the porous silicon-containing composite can have improved specific capacity, initial efficiency, and life characteristics.
[0067] The porous silicon-containing composite can further include a carbonaceous coating layer on at least one of its surfaces. The density of the porous silicon-containing composite and the carbonaceous coating layer can be evaluated by measuring the porosity of, for example, the porous silicon-containing composite and the carbonaceous coating layer respectively. For example, the density of the porous silicon-containing composite can be the same as or less than the density of the carbonaceous coating layer.
[0068] The porous silicon-containing composite may have a reduced porosity and an increased density compared to a porous silicon-containing composite including only the first primary particles. The porous silicon-containing composite according to one or more embodiments may have a porosity of about 60% or less, such as about 30% to about 60%. As used herein, a non-porous structure may refer to a structure having a porosity of about 10% or less, such as about 5% or less, such as about 0.01% to about 5% or less, or such as 0%. Porosity can be measured by mercury intrusion.
[0069] The second primary particle may have a size that is the same as the size of the first primary particle or a size that is smaller than the size of the first primary particle. The sizes of the first primary particle and the second primary particle may each independently have an average particle size of about 10nm-about 30 microns (μm). The size of the first primary particle may be, for example, about 20nm-about 180nm, for example, about 60nm-about 150nm. The size of the second primary particle may be about 100nm or less, for example, about 30nm-about 100nm.
[0070] The first primary particles may be in the form of needle-shaped particles. For example, the needle-shaped silicon particles may have a length of about 100 nm to about 160 nm, and in some embodiments, about 108 nm to about 125 nm; and may have a thickness of about 10 nm to about 100 nm, and in some embodiments, about 20 nm to about 50 nm, and in some other embodiments, about 40 nm.
[0071] The size of the first primary particle and the second primary particle may refer to the average particle size of the first primary particle and the second primary particle when the first primary particle and the second primary particle are spherical particles, and may refer to the major axis length, length, or thickness of the first primary particle and the second primary particle when the first primary particle and the second primary particle are non-spherical particles such as plate-shaped particles or needle-shaped particles. The second graphene (second graphene A) in the form of about 1 to about 30 layers is located on the first primary particle, and the second graphene (second graphene B) in the form of about 1 to about 5 layers is located on the second primary particle. The second graphene in the form of flakes (flakes) is located on the second graphene A and the second graphene B. Since the first primary particle and the second primary particle have different shapes and / or different degrees of oxidation, the second graphene on the first primary particle and the second graphene on the second primary particle may be of different types.
[0072] As used herein, "average particle size" refers to the particle size corresponding to 50% of the particles in a distribution curve in which the particles are accumulated in order of particle size from the smallest particle to the largest particle and the total number of accumulated particles is 100%. The average particle size can be measured by methods known to those skilled in the art. For example, the average particle size can be measured with a particle size analyzer or can be measured by using a transmission electron microscope (TEM) or a scanning electron microscope (SEM) image. As an example of other measurement methods, the average particle size can be measured using a measurement device using dynamic light scattering, the number of particles within a predetermined size range can be counted, and the average particle size can be calculated therefrom.
[0073] For example, the first graphene and the second graphene may each be a polycyclic aromatic molecule including a plurality of carbon atoms covalently bonded to each other, and the covalently bonded carbon atoms may form a 6-membered ring as a basic repeating unit, but a 5-membered ring and / or a 7-membered ring may be included in the first or second graphene. 2 The first and second graphenes may include a single layer or a plurality of carbon layers stacked one on top of another, such as 1 layer to about 100 layers, about 2 layers to about 100 layers, or about 3 layers to about 50 layers.
[0074] The first graphene and the second graphene may each have a structure of a nanosheet, a layer (or film), a nanographene nanosheet, or a scale. As used herein, the term "nanosheet" may refer to a structure of irregularly formed graphene on the silicon suboxide. The term "layer (or film)" may refer to a continuous, uniform layered structure of graphene on the silicon suboxide.
[0075] Figure 1 Schematic diagram for explaining the structure of a porous silicon-containing composite 10 according to an embodiment. The porous silicon-containing composite may be in the form of a cluster, for example. As used herein, the term "cluster" may refer to an aggregate of two or more primary particles, and may be interpreted as having substantially the same meaning as "secondary particle".
[0076] Reference Figure 1 The porous silicon-containing composite 10 may include a core 1 and a shell 2 on the core 1 , the core 1 including a porous silicon composite secondary particle, and the shell 2 including a first graphene 10 a .
[0077] The porous silicon composite secondary particle may include an aggregate of at least two silicon composite primary particles. The silicon composite primary particle may include a first primary particle 11, a second primary particle 12, and a second graphene 10b on the first primary particle 11 and the second primary particle 12. The first primary particle 11 is, for example, a first silicon, and the second primary particle 12 is, for example, a second silicon.
[0078] The second graphene 10b of the silicon composite primary particles can form a shell on the surface of the silicon suboxide, and the first graphene 10a of the silicon composite secondary particles can form a shell 2 on the core 1. Thus, the porous silicon-containing composite 10 can have a double core / shell structure. When the porous silicon-containing composite 10 has such a double core / shell structure, volume expansion can be suppressed and side reactions with the electrolyte are reduced.
[0079] The first primary particles 11 and the second primary particles 12 can form a network. The second primary particles 12 as described above can be embedded between the first primary particles. Due to this structure, the porous silicon-containing composite 10 can have improved physical properties and increased density due to reduced voids.
[0080] Silicon suboxide (SiO x )(where 0 < x < 2) can further be on the first primary particles 11 and the second primary particles 12. The second graphene 10b can be on the silicon suboxide (SiO x )(where 0 < x < 2).
[0081] Figure 2 To illustrate the local structure of the silicon composite primary particles constituting Figure 1 the porous silicon-containing composite shown in.
[0082] The first primary particles 21 have a flake and needle shape and have the second graphene 20b thereon. As Figure 2 shown in, the second graphene 20b can be disposed on the first primary particles 21. The second graphene in layer form can be disposed on the second primary particles 22, and the second graphene in flake form can be disposed on the second graphene in layer form. Thus, the second graphene 20b includes the second graphene in layer form disposed on the second primary particles 22 and the second graphene in flake form disposed on the second graphene in layer form.
[0083] Silicon suboxide can further be on the first primary particles 21 and the second primary particles 22.
[0084] The porous silicon-containing composite according to one or more embodiments can include both the first primary particles 21 and the second primary particles 22, as Figure 2As shown in , and having a structure in which the second primary particle 22 is between the first primary particles 21, and therefore may have a reduced specific surface area compared to a porous silicon-containing composite including only the first primary particles, and has a reduced area of side reactions with the liquid electrolyte, resulting in improved particle bonding strength. As a result, a lithium battery including a porous silicon-containing composite according to one or more embodiments may have improved initial efficiency and durability to charge and discharge. A porous silicon-containing composite including both the first primary particle 21 and the second primary particle 22 may have an improved density of silicon particles and an improved slip network, and result in reduced volume expansion. The first primary particle 21 may be connected to the surface of the second primary particle 22 via a second graphene 20b present on the surface of the second primary particle 22 in the form of flakes, thereby enhancing the conductive network. As a result, a lithium battery with improved rate characteristics can be manufactured using a porous silicon-containing composite according to any embodiment.
[0085] The number of layers of the second graphene 10 b of the core 1 may be the same as or different from the number of layers of the first graphene 10 a of the shell 2 .
[0086] The first graphene 10a of the shell 2 may have a higher density than the second graphene 10b of the core 1. In one or more embodiments, the number of layers of the second graphene 10b in the core 1 may be in the range of 1 layer to about 30 layers, for example, about 5 layers to about 15 layers, and for example, about 10 layers. The number of layers of the first graphene 10a in the shell 2 may be in the range of 1 layer to about 50 layers, for example, about 20 layers to about 30 layers.
[0087] The porous silicon-containing composite according to an embodiment may further include an outermost layer having a higher density than the core 1. Although the thickness of the outermost layer is not particularly limited, the outermost layer may have a thickness of about 20 nm to about 60 nm.
[0088] The core 1 and the shell 2 may further include graphite.
[0089] The diameter ratio of the porous silicon composite secondary particle to the porous silicon-containing composite may be about 1:1 to about 1:30, such as about 1:2 to about 1:30, and such as about 1:1 to about 1:25, and such as about 1:21. The diameter ratio of the porous silicon composite secondary particle to the porous silicon-containing composite may refer to a diameter ratio when both the porous silicon composite secondary particle and the porous silicon-containing composite are spherical, and may refer to a ratio of the lengths of the major axes when both the porous silicon composite secondary particle and the porous silicon-containing composite are non-spherical.
[0090] In the porous silicon-containing composite according to an embodiment, the core may have a diameter of about 3 μm to about 10 μm, and the shell may have a thickness of about 10 nm to about 5,000 nm (about 0.01 μm to about 5 μm), such as about 10 nm to about 1,000 nm. The ratio of the diameter of the core including the porous silicon composite secondary particles to the thickness of the shell may be about 1:0.001 to about 1:1.67, such as about 1:001, about 1:1.67, about 1:0.0033, or about 1:0.5.
[0091] In the porous silicon-containing composite according to one or more embodiments, the total content of the first graphene and the second graphene may be about 0.1 part by weight to about 2,000 parts by weight, and in some embodiments about 0.1 part by weight to about 300 parts by weight, and in some embodiments about 0.1 part by weight to about 90 parts by weight, and in an embodiment about 5 parts by weight to about 30 parts by weight, each relative to 100 parts by weight of the silicon. When the total content of the first graphene and the second graphene is within these ranges, the volume expansion of the silicon can be effectively suppressed and improved electrical conductivity characteristics can be obtained.
[0092] The second graphene in the silicon composite primary particles may be at a distance of about 10 nm or less from the surface of the silicon suboxide (SiO x )(where 0 < x < 2), and may include at least one graphene layer, such as about 1 to 30 graphene layers. The total thickness of the second graphene may be about 0.3 nm to about 50 nm, such as about 0.6 nm to about 50 nm, and such as about 1 nm to about 30 nm. The second graphene may be oriented at an angle of about 0° to about 90° with respect to the main axis of the silicon.
[0093] In the porous silicon-containing composite according to an embodiment, the first graphene may be at a distance of about 1,000 nm or less, and in some embodiments about 500 nm or less, and in some embodiments about 10 nm or less, and in an embodiment about 1 nm or less, and in some other embodiments about 0.00001 nm to about 1 nm from the surface of the silicon suboxide (SiO x )(where 0 < x < 2) of the porous silicon composite secondary particles. The first graphene may include at least one graphene layer, such as about 1 to 30 graphene layers, and the total thickness of the first graphene may be about 0.6 nm to about 50 nm, such as about 1 nm to about 50 nm. The first graphene may be oriented at an angle of about 0° to about 90° with respect to the main axis of the silicon.
[0094] The silicon suboxide (SiO x)(where 0 < x < 2) may have a thickness of about 30 μm or less, such as about 1 μm or less, such as about 0.1 nm - about 10 nm.
[0095] The porous silicon composite secondary particles may have an average particle size (D50) of about 200 nm - about 50 μm, and in some embodiments about 1 μm - about 30 μm, and in some embodiments about 2 μm - about 25 μm, and in some embodiments about 3 μm - about 20 μm, and in some other embodiments about 1 μm - about 15 μm, and in still other embodiments about 7 μm - about 11 μm. For example, the porous silicon composite secondary particles may have a D10 of about 0.001 μm - about 10 μm, and in some embodiments about 0.005 μm - about 5 μm, and in some other embodiments about 0.01 μm - about 1 μm. For example, the porous silicon composite secondary particles may have a D90 of about 10 μm - about 60 μm, and in some embodiments about 12 μm - about 28 μm, and in some other embodiments about 14 μm - about 26 μm.
[0096] The porous silicon composite secondary particles may have a specific surface area of about 0.1 square meters per gram (m 2 / g) - about 100 m 2 / g, and in some embodiments 1 m 2 / g - about 30 m 2 / g, and in some embodiments about 1 m 2 / g - about 10 m 2 / g, and in some other embodiments about 1 m 2 / g - about 5 m 2 / g. The porous silicon composite secondary particles may have a density of about 0.1 grams per cubic centimeter (g / cc) - about 2.8 g / cc, and in some embodiments about 0.1 g / cc - about 2.57 g / cc, and in some other embodiments about 0.5 g / cc - about 2 g / cc, and in some other embodiments about 1.1 g / cc - about 1.2 g / cc, and in some other embodiments about 1.18 g / cc.
[0097] The porous silicon-containing composite may further include a carbonaceous coating on at least one surface thereof. When the carbonaceous coating is further included, the porous silicon-containing composite can be used to manufacture a lithium battery with improved life characteristics, although it may have a reduced initial efficiency. The carbonaceous coating may include amorphous carbon, which may promote the migration of lithium during charging and discharging. The carbonaceous coating may completely or partially cover the surface of the porous silicon-containing composite. For example, the coverage of the carbonaceous coating relative to the total surface area of the porous silicon-containing composite may be about 10%-about 99%, and in some embodiments about 20%-about 95%, and in some other embodiments about 40%-about 90%.
[0098] The ratio of the diameter of the porous silicon-containing composite to the thickness of the carbonaceous coating layer may be about 1:0.0001 to about 1:50, and in some embodiments about 1:1 to about 1:40, and in some other embodiments about 1:0.0001 to about 1:1. The carbonaceous coating layer may have a thickness of about 1 nm to about 5,000 nm, for example about 10 nm to about 2,000 nm.
[0099] The carbonaceous coating layer may include a carbonaceous material. For example, the carbonaceous material may be graphene, amorphous carbon, carbon nanotubes, pitch carbon, fullerene, carbon fiber, or a combination thereof.
[0100] The carbonaceous coating layer may have a single layer structure including amorphous carbon and crystalline carbon. The carbonaceous coating layer may have a double layer structure having first and second carbonaceous coating layers including amorphous carbon and crystalline carbon, respectively.
[0101] For example, the carbonaceous coating layer may have a structure in which a first carbonaceous coating layer including amorphous carbon and a second carbonaceous coating layer including crystalline carbon are sequentially stacked in the order described on the porous silicon-containing composite, or a structure in which a second carbonaceous coating layer including crystalline carbon and a first carbonaceous coating layer including amorphous carbon are sequentially stacked in the order described on the porous silicon-containing composite.
[0102] The porous silicon-containing composite according to the embodiment may have a narrow particle size distribution. For example, the porous silicon-containing composite may have a D50 of about 1 μm to about 30 μm, a D10 of about 0.001 μm to about 10 μm, and a D90 of about 10 μm to about 60 μm. The porous silicon-containing composite may be formed into secondary particles.
[0103] The porous silicon-containing composite according to the embodiment may have a narrow particle size distribution within the above range. Unlike the porous silicon-containing composite according to the embodiment, the conventional silicon composite secondary particles obtained from the silicon composite primary particles may have an irregular secondary particle size distribution, and thus it may be difficult to control the particle size of the negative electrode active material to improve the unit cell performance.
[0104] In the porous silicon-containing composite according to one or more embodiments, the oxygen content may be about 0.01 atomic % to about 15 atomic %, and in some embodiments about 3.5 atomic % to about 5 atomic %, and in some other embodiments about 3.5 atomic % to about 3.8 atomic %, each based on the total content of oxygen, carbon, and silicon atoms in the porous silicon-containing composite. The oxygen content of the porous silicon-containing composite according to the embodiment is less than that of a conventional silicon-based material due to the oxidation of silicon that is suppressed by using a dispersant such as stearic acid when preparing the porous silicon-containing composite. This reduced oxygen content can lead to increased silicon capacity and improved initial efficiency.
[0105] The porous silicon-containing composite having a dual core / shell structure can form a uniform charge and discharge network, thereby preventing cracking due to volume expansion and contraction of silicon and causing a stable solid electrolyte interface (SEI) layer to be formed on its surface during charge and discharge. Therefore, a negative electrode having improved durability to charge and discharge can be manufactured using the porous silicon-containing composite according to the embodiment.
[0106] The operating principle of a negative electrode using the porous silicon-containing composite according to any one of the embodiments as a negative electrode active material will now be described.
[0107] The negative electrode active material layer including the porous silicon-containing composite may be on a copper current collector for the negative electrode. The porous silicon-containing composite may have a small Brunauer-Emmett-Teller (BET) specific surface area, and thus inhibit the penetration of the electrolyte and have a reduced area for side reactions with the electrolyte to effectively inhibit side reactions with the electrolyte and inhibit the delithiation of the active material and the expansion of the electrode. As a result, a lithium battery using a negative electrode including a porous silicon-containing composite according to any embodiment may have improved initial efficiency and durability during charging and discharging. In the porous silicon-containing composite according to an embodiment, the first primary particles and the second primary particles may be connected to each other by graphene, and a slip network may be well formed, resulting in an improved volume expansion inhibition effect.
[0108] Graphene can inhibit particle crushing or pulverization that occurs with conventional silicon particles. The graphene slip layer can function as a clamping layer to prevent the collapse of silicon particles, and can also allow alloying reactions of lithium ions with silicon (Si) to provide significant specific capacity and continuous conduction channels between particles.
[0109] The graphene layers can slide over each other as the silicon particles expand, and then slide back to their relaxed positions during delithiation. This movement occurs because the van der Waals forces are greater than the friction between the layers.
[0110] The clamping effect of the graphene layer can be verified from the fact that after repeated lithiation / delithiation cycles, the graphene layer remains intact and still functions as a clamping layer to prevent disintegration of the silicon particles.
[0111] The porous silicon-containing composite according to an embodiment may have excellent capacity characteristics of about 600 milliampere hours / cubic centimeter (mAh / cc) to about 2,000 mAh / cc.
[0112] In the porous silicon-containing composite according to an embodiment, the second graphene may completely or partially cover the surface of the first primary particle or the second primary particle. When the silicon suboxide is on the first primary particle and the second primary particle, the second graphene may completely or partially cover the surface of the silicon suboxide. For example, the coverage of the second graphene relative to the surface area of the first primary particle, the second primary particle, or the silicon suboxide may be about 10% to about 99%, and in some embodiments about 20% to about 95%, and in some other embodiments about 40% to about 90%.
[0113] In the porous silicon-containing composite according to the embodiment, the first graphene may completely or partially cover the surface of the porous silicon composite secondary particle. For example, the coverage of the first graphene relative to the surface area of the porous silicon composite secondary particle may be about 10% to about 99%, and in some embodiments, about 20% to about 95%, and in some embodiments, about 40% to about 90%.
[0114] The porous silicon-containing composite may have a non-spherical shape. For example, the porous silicon-containing composite may have a roundness of about 0.9 or less, and in some embodiments, about 0.7 to about 0.9, and in some other embodiments, about 0.85 to about 0.9.
[0115] Circularity can be determined according to Equation 1, where A is the area and P is the perimeter.
[0116] Equation 1
[0117]
[0118] The first graphene and the second graphene may be any carbonaceous material having a scale shape. Examples of the carbonaceous material may be graphene, graphite, carbon fiber, graphite carbon, or graphene oxide.
[0119] The first graphene and the second graphene may have structures such as nanosheets, layers (or films), graphene nanosheets, flakes, etc. As used herein, the term "nanosheet" may refer to an irregularly formed structure on the first primary particle, the second primary particle, or the silicon suboxide, and the term "layer" may refer to a continuous, uniform film formed on the first primary particle, the second primary particle, or the silicon suboxide.
[0120] The amorphous carbon of the carbonaceous coating layer may include pitch carbon, soft carbon, hard carbon, mesophase pitch carbonization product, sintered coke, carbon fiber, or a combination thereof. The carbonaceous coating layer may be a non-porous, continuous coating layer. For example, the carbonaceous coating layer may have a thickness of about 1 nm to about 5000 nm.
[0121] The carbonaceous coating layer may further include crystalline carbon. When the carbonaceous coating layer further includes crystalline carbon, the carbonaceous coating layer may exhibit promoted buffering of volume expansion of the porous silicon-containing composite.
[0122] The crystalline carbon may be natural graphite, artificial graphite, graphene, fullerene, carbon nanotube, or a combination thereof.
[0123] In the porous silicon-containing composite according to the embodiment, the mixing ratio of the total carbon (first carbon) of the first graphene and the second graphene to the carbon (second carbon) of the carbonaceous coating layer may be about 30: 1 to about 1: 3 by weight, for example, about 20: 1 to about 1: 1 by weight, and for example, about 10: 1 to about 1: 0.9 by weight. The term "first carbon" may refer to the sum of the carbon of the first graphene and the second graphene. When the mixing ratio of the first carbon to the second carbon is within these ranges, a lithium battery with improved discharge capacity and improved capacity retention can be manufactured using the porous silicon-containing composite.
[0124] The mixing ratio of the first carbon to the second carbon can be confirmed by thermogravimetric analysis (TGA). The first carbon is associated with a peak appearing at about 700°C-750°C, and the second carbon is associated with a peak appearing at about 600°C-650°C.
[0125] TGA can be performed, for example, at a temperature of 25° C. to about 1,000° C. under atmospheric conditions at a heating rate of about 10° C. / min.
[0126] The first carbon may be crystalline carbon, and the second carbon may be amorphous carbon.
[0127] A mixing ratio of the total weight of the first graphene and the second graphene to the total weight of the first carbon and the second carbon may be about 1:1.03 to about 1:10, for example, about 1:1.03 to about 1:4.
[0128] In the porous silicon-containing composite according to the embodiment, the porous silicon composite secondary particles may have a size of about 3 μm to about 10 μm, and the first graphene and the second graphene may have a size of about 10 nm to about 100 nm, respectively. As used herein, the term "size" may refer to a diameter or a length of a major axis. When the first graphene and the second graphene have a spherical shape, the term "size" means a diameter. In the case where the first graphene and the second graphene have a non-spherical shape, the term "size" means a major axis length.
[0129] In the porous silicon-containing composite according to the embodiment, the porous silicon composite secondary particle may have a diameter of about 3 μm to about 10 μm, and the shell may have a thickness of about 10 nm to about 5,000 nm (about 0.01 μm to about 5 μm), for example, about 10 nm to about 1,000 nm. The ratio of the diameter of the core including the porous silicon composite secondary particle to the thickness of the carbonaceous coating layer may be about 1:0.001 to about 1:1.67, and in some embodiments about 1:001, about 1:1.67, about 1:0.0033, or about 1:0.5.
[0130] In the porous silicon-containing composite according to an embodiment, the total amount of the first graphene and the second graphene may be about 0.1 parts by weight to about 2,000 parts by weight, for example, about 0.1 parts by weight to about 1,000 parts by weight, for example, about 0.1 parts by weight to about 500 parts by weight, for example, about 0.1 parts by weight to about 300 parts by weight, for example, about 0.1 parts by weight to about 90 parts by weight, and for example, about 5 parts by weight to about 30 parts by weight, relative to 100 parts by weight of the silicon. Herein, the term "silicon" includes both the first primary particles and the second primary particles. When the amount of the first and second graphenes is within these ranges, the first primary particles and the second primary particles may have an improved volume expansion suppression effect and improved conductivity characteristics.
[0131] The first graphene and the second graphene may be, for example, graphene flakes (sheets).
[0132] In the porous silicon-containing composite, the first graphene may be a graphene flake, and the first graphene may be at a distance from the silicon suboxide (SiO x)(where 0 < x < 2) at a distance of about 1,000 nm or less, such as about 500 nm or less, such as about 100 nm or less, such as about 50 nm or less, such as about 10 nm or less, such as about 1 nm or less, and such as about 0.00001 nm - about 1 nm. The first graphene may include at least one graphene layer, such as about 1 - 30 graphene layers. The total thickness of the first graphene may be about 0.6 nm - about 50 nm, such as about 1 nm - about 50 nm. The first graphene may be oriented at an angle of about 0° - about 90°, such as about 10° - about 80°, and such as about 20° - about 70°, each relative to the main axis of the silicon (e.g., the Y-axis).
[0133] The second graphene of the silicon composite primary particles may be graphene flakes, and the graphene flakes may be at a distance of about 10 nm or less, such as about 5 nm or less, such as about 3 nm or less, and such as about 1 nm or less from the silicon suboxide (SiO x )(where 0 < x < 2). The second graphene may include graphene layers. For example, the total thickness of the second graphene may be about 1,000 nm or less, such as about 0.3 nm - about 1,000 nm, such as about 0.3 nm - about 50 nm, such as about 0.6 nm - about 50 nm, and such as about 1 nm - about 30 nm. In the porous silicon-containing composite according to an embodiment, the second graphene may be oriented at an angle of about 0° - about 90°, such as about 10° - about 80°, and such as about 20° - about 70°, each relative to the main axis of the silicon (e.g., the Y-axis). As used herein, the term "main axis" may refer to the Y-axis.
[0134] For example, the silicon suboxide (SiO x )(where 0 < x < 2) may have a thickness of about 30 μm or less, such as about 10 μm or less, such as about 1 nm - about 100 nm, such as about 1 nm - about 50 nm, and such as about 10 nm. The silicon suboxide may completely or partially cover the surface of the silicon. For example, the coverage rate of the silicon suboxide may be about 10% - about 99%, such as about 20% - about 95%, such as about 30% - about 93%, and such as about 40% - about 90%, each based on the surface area of the silicon.
[0135] Hereinafter, a method for preparing a porous silicon-containing composite according to an embodiment will be described. First, a composition including silicon and a silicon suboxide (SiO on the silicon may be x, the structural body pulverization (where 0 < x < 2) is performed to obtain first primary particles which are the pulverized primary particles. The pulverized first primary particles can be mixed with second primary particles, a dispersant, and a solvent to obtain a composition. Then, porous silicon composite secondary particles can be obtained from the composition. The porous silicon composite secondary particles can have a porosity of, for example, about 0.1% - about 50%, such as about 1% - about 40%, and for example about 5% - about 30%, and can have a pore size of about 10 nm - about 500 nm, such as about 20 nm - about 200 nm, and for example about 30 nm - about 300 nm.
[0136] Preparing the porous silicon composite secondary particles from the composition can be carried out using any of a variety of methods such as co - precipitation, spray drying, or solid - phase methods. For example, the porous silicon composite secondary particles can be prepared by using spray drying. When the porous silicon composite secondary particles are prepared by spray drying, their particle size can be controlled by appropriately selecting the spray type, the pressurized gas supply rate, the composition supply rate, the drying temperature, etc.
[0137] The spray drying can be carried out at an atmosphere temperature of about room temperature (25 °C) - about 500 °C, such as about 50 °C - about 300 °C, and in some embodiments about 50 °C - about 250 °C, and in some other embodiments about 70 °C - about 200 °C. When the spray drying is carried out within these temperature ranges, particle agglomeration caused by moisture condensation near the particle discharge outlet and blockage of the particle discharge outlet can be prevented, and the porous silicon composite secondary particles can have a suitable porosity.
[0138] In the spray drying, the spray pressure can be about 1 bar - about 5 bar.
[0139] Before the spray drying, the surface area of the starting material can be increased as much as possible, for example, by pulverization. For this purpose, pulverized silicon primary particles can be used as the starting material.
[0140] For example, when the porous silicon composite secondary particles are formed by spray drying, the obtained porous silicon composite secondary particles can be spherical. The dispersant, such as stearic acid, can partially remain (be retained) on the surface of the porous silicon composite secondary particles.
[0141] Next, when a carbon source gas is supplied, the porous silicon composite secondary particles can be heat - treated so that graphene can be distributed on the porous silicon composite secondary particles, thereby preparing a porous silicon - containing composite.
[0142] Then a carbonaceous coating layer can be formed on the porous silicon - containing composite, thereby obtaining a porous silicon - containing composite including the carbonaceous coating layer.
[0143] After the pores in the porous silicon composite secondary particles are filled with the carbon source gas, graphene may grow on the outer surfaces of the porous silicon composite secondary particles.
[0144] The solvent may be an alcohol solvent. The alcohol solvent may be, for example, ethanol, methanol, or isopropanol. When these alcohol solvents are used and heat treatment is performed, the dispersant may be used together with the solvent so that the amount of the dispersant remaining in the porous silicon-containing composite may be reduced. As a result, a porous silicon-containing composite having a reduced amount of oxygen may be obtained.
[0145] The dispersant can evenly disperse silicon primary particles. Non-limiting examples of the dispersant can be stearic acid, resorcinol, polyvinyl alcohol, carbon pitch, or a combination thereof. Based on 100 parts of the total weight of the composition, the amount of the dispersant can be about 1 part by weight to about 15 parts by weight, such as about 5 parts by weight to about 10 parts by weight. When the amount of the dispersant is within these ranges, silicon and graphene can be evenly dispersed without agglomeration.
[0146] The carbon source gas may be a compound represented by Formula 1, a compound represented by Formula 2, and a first oxygen-containing compound represented by Formula 3.
[0147] Formula 1
[0148] C n H (2n+2-a) [OH] a
[0149] In Formula 1, n may be an integer of 1-20, for example, an integer of 2-18, or an integer of 4-16, and a may be 0 or 1.
[0150] Formula 2
[0151] C n H (2n)
[0152] In Formula 2, n may be an integer of 2-6.
[0153] Formula 3
[0154] C x H y O z
[0155] In Formula 3, x may be an integer of 1-20, for example, an integer of 2-18, or an integer of 4-16; y may be 0 or an integer of 1-20, or an integer of 2-18; and z may be 1 or 2.
[0156] The carbon source gas may be, for example, methane, ethylene, propylene, methanol, ethanol, propanol, acetylene, or a combination thereof.
[0157] The heat treatment can be carried out at a temperature of about 750 °C to about 1,100 °C and, for example, at a temperature of about 700 °C to about 1,000 °C. When the heat treatment is carried out within these temperature ranges, graphene can be produced at a high density in both the core and / or the shell.
[0158] When the graphene is carbon nanotube flakes, carbon fiber flakes, graphite carbon flakes, or graphene oxide flakes, the graphene can be prepared using conventional methods known in the art.
[0159] The method may further include dry-mixing a composition comprising the prepared porous silicon-containing composite according to an embodiment, a carbonaceous material, and a solvent to obtain a porous silicon-containing composite comprising a carbonaceous coating layer. For example, the amount of the carbonaceous material may be about 0.001 parts by weight to about 99 parts by weight, relative to the total weight of 100 parts by weight of the porous silicon-containing composite and the carbonaceous material.
[0160] When the silicon composite primary particles comprise a low-valence silicon oxide (SiO x )(where 0 < x < 2) on the first primary particle and the second primary particle, the low-valence silicon oxide, as an oxygen-deficient material unstable compared to silicon oxide (SiO 2 ), may tend to form a stable material by reacting with another reactive material such as a carbon source gas. Based on this tendency, the low-valence silicon oxide (SiO x )(where 0 < x < 2) can be used as a seed layer for forming graphene.
[0161] The thickness of the low-valence silicon oxide (SiO x )(where 0 < x < 2) on the silicon can significantly affect the shape and / or structure of the graphene.
[0162] The thickness of the low-valence silicon oxide (SiO x )(where 0 < x < 2) can be changed by controlling the processes involved in graphene formation, for example, by controlling the composition of the carbon source gas used for forming graphene. The low-valence silicon oxide (SiO x )(where 0 < x < 2) can have a thickness of about 300 μm or less.
[0163] The low-valence silicon oxide (SiO x , where 0 < x < 2) can have a thickness of about 10 nm or less, and in some embodiments about 0.1 nm to about 10 nm, and in some other embodiments about 0.1 nm to about 5 nm. When the thickness of the low-valence silicon oxide is within these ranges, a method including the low-valence silicon oxide (SiO xmanufacturing a lithium battery having improved capacity characteristics with the porous silicon-containing composite of the silicon composite primary particles (where 0 < x < 2).
[0164] In an embodiment, by using non-catalytic chemical vapor deposition, graphene can be formed on the sub-valent silicon oxide (SiO x where 0 < x < 2) on the silicon.
[0165] According to chemical vapor deposition, graphene can be directly grown on silicon covered with sub-valent silicon oxide (SiO x ), and thus the silicon and the graphene can have strong adhesion to each other.
[0166] In some embodiments, even when there is no sub-valent silicon oxide (SiO x ) on the silicon, through the reaction process of a carbon-containing mixed gas and an oxygen-containing mixed gas, a sub-valent silicon oxide (SiO x ) layer can be first formed on the silicon due to the reaction of the oxygen-containing mixed gas, and then graphene can be formed thereon due to the reaction of the carbon-containing mixed gas.
[0167] The degree of adhesion between the first primary particle or the second primary particle and the second graphene can be evaluated by measuring the distance between the sub-valent silicon oxide (SiO x ) and the second graphene via scanning electron microscopy (SEM). The second graphene can be at a distance of about 10 nm or less from the sub-valent silicon oxide. In some embodiments, the second graphene can be spaced apart from the sub-valent silicon oxide by a distance of about 1 nm or less, such as about 0.005 nm - about 1 nm. The second graphene can be oriented at an angle of about 0° - about 90° with respect to the main axis of the silicon, and in some embodiments about 10° - about 80°, and in some other embodiments about 20° - about 70°. The second graphene can include at least 1 - 30 graphene layers, and in some embodiments about 2 - 25 graphene layers, and in some other embodiments about 4 - 20 graphene layers, and can have a total thickness of about 0.6 nm - about 12 nm, and in some embodiments about 1 nm - about 10 nm, and in some other embodiments about 2 nm - about 8 nm. The second graphene can be oriented at an angle of 0° - about 90° with respect to the main axis of the silicon. As used herein, the main axis can refer to the Y-axis.
[0168] The porous silicon-containing composite can further include a metal oxide or a metal fluoride. When the porous silicon-containing composite according to any embodiment further includes a metal oxide, the formation of a solid electrolyte interface (SEI) layer can be prevented due to the suppression of side reactions.
[0169] The metal oxide may include magnesium oxide, manganese oxide, aluminum oxide, titanium oxide, zirconium oxide, tantalum oxide, tin oxide, hafnium oxide, or a combination thereof. The metal fluoride may include aluminum fluoride (AlF 3 ).
[0170] According to another aspect, a carbon composite comprises the porous silicon-containing composite according to any of the above embodiments, and a carbonaceous material.
[0171] The amount of the porous silicon-containing composite in the carbon composite may be about 0.001 parts by weight to about 99.999 parts by weight, for example, about 1 parts by weight to about 95 parts by weight, for example, about 3 parts by weight to about 85 parts by weight, for example, about 5 parts by weight to about 70 parts by weight, and for example, about 5 parts by weight to about 50 parts by weight, each relative to 100 parts by weight of the total weight of the carbon composite.
[0172] The carbon composite may have further improved initial efficiency, specific capacity characteristics, rate performance, and durability compared to those of the porous silicon-containing composite.
[0173] The carbonaceous material may be, for example, graphene, graphite, fullerene, carbon fiber, carbon nanotube, or a combination thereof. For example, relative to 100 parts by weight of the carbon composite, the amount of the carbonaceous material may be about 0.001 parts by weight to about 99.999 parts by weight. For example, the amount of the carbonaceous material may be about 10 parts by weight to about 97 parts by weight, such as about 50 parts by weight to about 97 parts by weight, each relative to 100 parts by weight of the carbon composite. When the amount of the carbonaceous material in the carbon composite is within these ranges, the carbon composite may have improved capacity and conductivity.
[0174] The carbon composite may include, for example, graphite and the porous silicon-containing composite on the graphite.
[0175] The graphite may be, for example, SFG6 graphite, and may have an average particle size of about 6 μm. When the carbon composite is used to form an electrode, the amount of the carbon composite in the electrode may be, for example, about 0.001 parts by weight to about 99.999 parts by weight, for example, about 1 part by weight to about 95 parts by weight, for example, about 50 parts by weight to about 90 parts by weight, and for example, about 68 parts by weight to about 87 parts by weight, each relative to 100 parts by weight of the total weight of the electrode, and the amount of the binder may be, for example, about 13 parts by weight to about 32 parts by weight. For example, relative to 100 parts by weight of the total weight of the carbon composite, the amount of graphite in the carbon composite may be, for example, 1 part by weight to about 99 parts by weight.
[0176] The binder may be, for example, a lithium-substituted polyacrylate.
[0177] The compound represented by Formula 1 and the compound represented by Formula 2 may each independently be methane, ethylene, propylene, methanol, ethanol, propanol, or a combination thereof.
[0178] The first oxygen-containing compound represented by Formula 3 may include, for example, carbon dioxide (CO 2 ), carbon monoxide (CO), or a mixture thereof.
[0179] In addition to the carbon source gas, an inert gas such as nitrogen, helium, argon, or a combination thereof may be further used.
[0180] The first oxygen-containing compound may be carbon monoxide, carbon dioxide, water vapor, or a combination thereof.
[0181] When the first oxygen-containing compound is used as the carbon source gas, the silicon suboxide may be formed to have a thickness greater than that of a native silicon oxide layer. For example, the thickness of the silicon suboxide may be controlled to be about 10 nm or less, such as about 0.5 nm to about 5 nm. By using the silicon suboxide having a thickness within these ranges, the shape and thickness of the graphene may be controlled. In particular, when the silicon suboxide is formed to have a thickness greater than that of a native oxide layer, the graphene thereon may have a denser structure than a graphene nanosheet. The graphene may have a structure including, for example, about 5-10 layers.
[0182] When the carbon source gas includes water vapor, the porous silicon-containing composite obtained therefrom may have further improved electrical conductivity. Although not limited to this theory, it is understood that since carbon with high crystallinity can be deposited on the silicon coated with the silicon suboxide by reaction with the carbon source gas in the presence of water vapor, the porous silicon-containing composite may have high electrical conductivity even when coated with a small amount of carbon. Although not particularly limited, the amount of water vapor in the carbon source gas may be, for example, in the range of about 0.01 volume % to about 10 volume %, based on 100% of the volume of the carbon source gas.
[0183] The carbon source gas may be, for example, methane; a mixture of methane and an inert gas; an oxygen-containing compound; or a mixture of methane and an oxygen-containing compound. In some embodiments, the carbon source gas may be CH 4 and CO 2 A mixture of gases, or CH 4 , CO 2 , and H 2 O mixed gas.
[0184] CH 4 and CO 2The mixed gas may be supplied at a molar ratio of about 1:0.20 to about 1:0.50, and in some embodiments at a molar ratio of about 1:0.25 to about 1:0.45, and in some other embodiments at a molar ratio of about 1:0.30 to about 1:0.40.
[0185] CH 4 , CO 2 and H 2 The mixed gas of O may be supplied at a molar ratio of about 1:0.20-0.50:0.01-1.45, and in some embodiments at a molar ratio of about 1:0.25-0.45:0.10-1.35, and in some other embodiments at a molar ratio of about 1:0.30-0.40:0.50-1.0.
[0186] The carbon source gas may be carbon monoxide (CO) or carbon dioxide (CO 2 In some other embodiments, the carbon source gas may be CH 4 and N 2 of mixed gases.
[0187] CH 4 and N 2 The mixed gas may be supplied at a molar ratio of about 1:0.20 to about 1:0.50, and in some embodiments at a molar ratio of about 1:0.25 to 1:0.45, and in some other embodiments at a molar ratio of about 1:0.30 to about 1:0.40. In some embodiments, the carbon source gas may not include an inert gas such as nitrogen.
[0188] The heat treatment may be performed at a temperature of about 750°C to about 1100°C, and in some embodiments, about 800°C to about 1000°C.
[0189] The heat treatment can be carried out without restriction at any pressure level. The pressure level for the heat treatment can be appropriately selected considering the target amount of heat treatment temperature, the composition of the gas mixture and the coated carbon. The pressure level for the heat treatment can be controlled by changing the amount of the inflow and outflow of the gas mixture. For example, the pressure for the heat treatment can be about 1 atmosphere (atm) or more and about 2atm or more, about 3atm or more, about 4atm or more, or about 5atm or more in some embodiments. However, embodiments are not limited thereto.
[0190] The heat treatment time may not be particularly limited, and may be appropriately controlled depending on the target amount of heat treatment temperature, heat treatment pressure, gas mixture and coated carbon. For example, the heat treatment time may be in the range of about 10 minutes to about 100 hours and in the range of about 30 minutes to about 90 hours in some embodiments and in the range of about 50 minutes to about 40 hours in some other embodiments. However, embodiments are not limited thereto. Although not limited to this theory, it is understood that the longer the heat treatment time, the larger the amount of graphene (carbon) that can be deposited, and the better the electrical properties of the composite. However, these effects may not be directly proportional to the heat treatment time. For example, after a predetermined duration, the deposition of graphene may stop or its deposition rate may become low.
[0191] The method for preparing the porous silicon-containing composite by the gas phase reaction of the carbon source gas as described above can also be performed on the surface of the porous silicon-containing composite covered with the silicon suboxide (SiO x ) provides a uniform coating layer on the graphene on silicon. The graphene and the silicon suboxide (SiO x ) may not substantially occur. When the thickness of the silicon suboxide is appropriately controlled, the separation of the graphene may be even further suppressed. In this regard, the thickness of the silicon suboxide that may effectively suppress the separation of the graphene may be about 10 nm or less, such as about 0.1 nm to about 10 nm, such as about 0.1 nm to about 5 nm.
[0192] Due to the coating of the graphene on the silicon by the gas phase reaction, a coating layer having high crystallinity may be formed. When the porous silicon-containing composite is used as a negative electrode active material, the negative electrode active material may have improved conductivity without structural changes.
[0193] The process of preparing the carbon composite using the porous silicon-containing composite may be as follows.
[0194] The porous silicon-containing composite and the carbonaceous material according to any embodiment may be mixed together and then heat-treated. The heat treatment may be performed at a temperature of about 750° C. to about 1100° C., for example, about 700° C. to about 1,000° C. When the heat treatment temperature is within these ranges, a carbon composite having improved capacity characteristics may be obtained.
[0195] According to another aspect, an electrochemically active material composite includes: an electrochemically active material; and a porous silicon-containing composite according to any of the above embodiments, a carbon composite including the porous silicon-containing composite and a carbonaceous material, or a combination thereof, wherein the porous silicon-containing composite, the carbon composite, or a combination thereof is coated on the surface of the electrochemically active material.
[0196] The electrochemically active material may be any positive electrode active material or negative electrode active material that can be generally used in batteries.
[0197] The porous silicon-containing composite or carbon composite according to any embodiment may be used, for example, in a battery, a field emission material for a display, a thermoelectric device, or a biosensor.
[0198] According to another aspect, an electrode comprises the porous silicon-containing composite or carbon composite according to any of the above embodiments. The electrode may be an electrode for a lithium battery.
[0199] The electrode may be, for example, a cathode.
[0200] The porous silicon-containing composite or carbon composite according to any embodiment can be used as an electrode active material such as a negative electrode active material. When the porous silicon-containing composite or the carbon composite is used as a negative electrode active material, the volume expansion and collapse of silicon can be reduced or prevented. The negative electrode active material can have improved conductivity and can improve the high rate characteristics of the battery. Moreover, since a small amount of graphene can be coated on the silicon covered with the silicon suboxide, the negative electrode active material can have an improved energy density per volume.
[0201] According to another aspect, a lithium battery includes an electrode including the porous silicon-containing composite according to any embodiment, or a carbon composite including the porous silicon-containing composite according to any embodiment and a carbonaceous material.
[0202] The negative electrode can be manufactured as follows.
[0203] The negative electrode may be formed by molding a negative electrode active material composition including, for example, a porous silicon-containing composite or a carbon composite according to any embodiment as a negative electrode active material, a conductive agent, and a binder into a predetermined shape, or coating the negative electrode active material composition on a current collector such as a copper (Cu) foil. The negative electrode active material composition may not include a conductive agent.
[0204] In some embodiments, the negative active material composition may be formed as a film on a separator without using a current collector.
[0205] For example, the negative electrode active material composition can be prepared by mixing the negative electrode active material, a conductive agent, a binder, and a solvent. The negative electrode active material composition can be directly coated on a metal current collector to form a negative electrode plate. In some other embodiments, the negative electrode active material composition can be cast on a separate carrier to form a negative electrode active material film. The negative electrode active material film can be separated from the carrier and then laminated on a metal current collector to form a negative electrode plate. The negative electrode can have any of various forms, not limited to the forms listed above.
[0206] In addition to the above-mentioned negative electrode active materials, the negative electrode active material composition may further include a carbonaceous negative electrode active material. For example, the carbonaceous negative electrode active material may be natural graphite, artificial graphite, expanded graphite, graphene, carbon black, fullerene soot, carbon nanotubes, graphite carbon, carbon fiber, or a combination. However, embodiments are not limited thereto. Any suitable carbonaceous negative electrode active material available in the art may be used.
[0207] The conductive agent may be acetylene black, ketjen black, natural graphite, artificial graphite, carbon black, carbon fiber, or metal powder or metal fiber of copper, nickel, aluminum or silver. The conductive agent may include one or more conductive materials such as polyphenylene derivatives in combination. However, the embodiment is not limited thereto. Any suitable conductive agent available in the art may be used.
[0208] The binder may be a vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene, or a mixture thereof, a styrene-butadiene rubber-based polymer, polyacrylic acid, polyamide-imide, or polyimide. However, the embodiment is not limited thereto. Any suitable binder available in the art may be used.
[0209] The solvent may be N-methylpyrrolidone, acetone, or water. However, the embodiment is not limited thereto. Any suitable solvent available in the art may be used.
[0210] The amount of the negative electrode active material, the conductive agent, the binder, and the solvent may be the same level as that commonly used in lithium batteries. Depending on the use and structure of the lithium battery, at least one of the conductive agent, the binder, and the solvent may be omitted.
[0211] The lithium battery may include the negative electrode. The lithium battery may be manufactured in the following manner.
[0212] First, the negative electrode may be manufactured according to the above method.
[0213] Next, a positive active material composition may be prepared by mixing a positive active material, a conductive agent, a binder, and a solvent. The positive active material composition may be directly coated on a metal current collector and dried to manufacture a positive plate. In some other embodiments, the positive active material composition may be cast on a separate carrier to form a positive active material film. The positive active material film may then be separated from the carrier and then laminated on a metal current collector to manufacture a positive plate.
[0214] The positive electrode active material may include lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium manganese oxide, or a combination thereof. However, the embodiment is not limited thereto. Any positive electrode active material available in the art may be used.
[0215] For example, the positive electrode active material may be a metal oxide containing lithium. Any suitable positive electrode active material commonly used in the art may be used. For example, the positive electrode active material may be a composite lithium oxide having at least one of the following: cobalt (Co), manganese (Mn), and nickel (Ni), or a combination thereof. For example, the positive electrode active material may be a compound represented by one of the following formulas: Li a A 1-b B' b D 2 (where 0.90≤a≤1, and 0≤b≤0.5); Li a E 1-b B' b O 2-c D c (where 0.90≤a≤1, 0≤b≤0.5, and 0≤c≤0.05); LiE 2-b B' b O 4-c D c (where 0≤b≤0.5 and 0≤c≤0.05); Li a Ni 1-b-c Co b B' c D α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α≤2); Li a Ni 1-b-c Co b B' c O 2-α F' α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Co b B' c O 2-α F' 2 (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Mn b B' c D α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α≤); Li a Ni 1-b-c Mn b B' c O 2-α F' α(where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b- c Mn b B' c O 2-α F' 2 (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni b E c G d O 2 (where 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5, and 0.001≤d≤0.1); Li a Ni b Co c Mn d G e O 2 (where 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, and 0.001≤e≤0.1); Li a NeG b O 2 (where 0.90≤a≤1, and 0.001≤b≤0.1); Li a CoG b O 2 (where 0.90≤a≤1, and 0.001≤b≤0.1); Li a MnG b O 2 (where 0.90≤a≤1, and 0.001≤b≤0.1); Li a Mn 2 G b O 4 (where 0.90≤a≤1, and 0.001≤b≤0.1); QO 2 ;QS 2 ;LiQS 2 ; V 2 O 5 ;LiV 2 O 5 ;LiI'O 2 ;LiNiVO 4 ;Li (3-f) J 2 (PO 4 ) 3 (where 0≤f≤2); Li (3-f) Fe 2 (PO 4 ) 3(where 0≤f≤2); and LiFePO 4 .
[0216] In the above formula, A can be nickel (Ni), cobalt (Co), manganese (Mn), or a combination thereof; B' can be aluminum (Al), nickel (Ni), cobalt (Co), manganese (Mn), chromium (Cr), iron (Fe), magnesium (Mg), strontium (Sr), vanadium (V), rare earth elements, or a combination thereof; D can be oxygen (O), fluorine (F), sulfur (S), phosphorus (P), or a combination thereof; E can be cobalt (Co), manganese (Mn), or a combination thereof; F' can be fluorine (F), sulfur (S), phosphorus (P), or a combination thereof ; G may be aluminum (Al), chromium (Cr), manganese (Mn), iron (Fe), magnesium (Mg), lanthanum (La), cerium (Ce), strontium (Sr), vanadium (V), or a combination thereof; Q may be titanium (Ti), molybdenum (Mo), manganese (Mn), or a combination thereof; I' may be chromium (Cr), vanadium (V), iron (Fe), scandium (Sc), yttrium (Y), or a combination thereof; and J may be vanadium (V), chromium (Cr), manganese (Mn), cobalt (Co), nickel (Ni), copper (Cu), or a combination thereof.
[0217] The compounds listed above as positive electrode active materials may have a surface coating layer (hereinafter, "coating layer"). Alternatively, a mixture of a compound without a coating layer and a compound with a coating layer may be used, the compound being selected from the compounds listed above. The coating layer may include at least one compound of a coating element such as an oxide, a hydroxide, an oxyhydroxide, an oxycarbonate, a hydroxycarbonate, or a combination thereof. The compound used for the coating layer may be amorphous or crystalline. The coating element used for the coating layer may be magnesium (Mg), aluminum (Al), cobalt (Co), potassium (K), sodium (Na), calcium (Ca), silicon (Si), titanium (Ti), vanadium (V), tin (Sn), germanium (Ge), gallium (Ga), boron (B), arsenic (As), zirconium (Zr), or a mixture thereof. The coating layer may be formed by any method that does not adversely affect the physical properties of the positive electrode active material when a compound is used as the coating element, such as by a spraying method, an impregnation method, etc. This will be understood by those skilled in the art, and therefore a detailed description thereof will be omitted.
[0218] For example, the positive electrode active material may be LiNiO 2 、LiCoO 2 、LiMn x O 2x (where x = 1 or 2), LiNi 1- x Mn x O 2 (where 0 <x<1)、LiNi 1-x-y Co x Mny O 2 (where 0≤x≤0.5 and 0≤y≤0.5), LiFeO 2 、V 2 O 5 , TiS, or MoS.
[0219] The conductive agent, binder and solvent used in the positive active material composition may be the same as those used in the above-mentioned negative active material composition. In some embodiments, a plasticizer may be further added to the positive active material composition and / or the negative active material composition to obtain an electrode including pores.
[0220] The amount of the positive electrode active material, the conductive agent, the binder, and the solvent may be the same level as that commonly used in lithium batteries. Depending on the use and structure of the lithium battery, at least one of the conductive agent, the binder, and the solvent may be omitted.
[0221] Next, a separator to be disposed between the positive electrode and the negative electrode can be prepared. The separator can be any separator commonly used in lithium batteries. In some embodiments, the separator can have a low resistance to ion migration in the electrolyte and have good electrolyte retention. For example, the separator can be glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or a combination thereof, each of which can be a nonwoven or a textile. For example, a windable separator including polyethylene or polypropylene can be used in a lithium ion battery. A separator with good organic electrolyte solution retention can be used in a lithium ion polymer battery. For example, the separator can be manufactured in the following manner.
[0222] In some embodiments, a polymer resin, a filler, and a solvent may be mixed together to prepare a separator composition. The separator composition may then be directly coated on a support and then dried to form the separator. In some other embodiments, the separator composition may be cast on a support and dried to form a separator film. The separator film may be separated from the support and laminated on an electrode to form the separator.
[0223] The polymer resin used to manufacture the separator may be any material generally used as a binder for electrode plates. For example, the polymer resin may be vinylidene fluoride / hexafluoropropylene copolymer, PVDF, polyacrylonitrile, polymethyl methacrylate, or a mixture thereof.
[0224] The separator may include a ceramic component to improve its performance as a membrane. For example, the separator may be coated with an oxide or may be formed to include ceramic particles.
[0225] Next, the electrolyte may be prepared.
[0226] For example, the electrolyte may be an organic electrolyte solution. The electrolyte may be solid. For example, the electrolyte may be boron oxide or lithium oxynitride. However, the embodiment is not limited thereto. Any suitable solid electrolyte available in the art may be used. The solid electrolyte may be formed on the negative electrode by a method such as sputtering.
[0227] For example, an organic electrolyte solution may be prepared by dissolving a lithium salt in an organic solvent.
[0228] The organic solvent may be any organic solvent available in the art. For example, the organic solvent may be propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, chloroethylene carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, cyclopentane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or a mixture thereof.
[0229] The lithium salt may be any lithium salt available in the art. For example, the lithium salt may be LiPF 6 , LiBF 4 、LiSbF 6 、LiAsF 6 、LiClO 4 、LiCF 3 SO 3 、Li(CF 3 SO 2 ) 2 N、Li(FSO 2 ) 2 N、LiC 4 F 9 SO 3 、LiAlO 2 、LiAlCl 4 、LiN(C x F 2x+1 SO 2 )(C y F 2y+1 SO 2 )(wherein x and y may be natural numbers), LiCl, LiI, or a mixture thereof.
[0230] Reference Figure 8, the lithium battery 121 according to the embodiment may include a positive electrode 123, a negative electrode 122, and a separator 124. The positive electrode 123, the negative electrode 122, and the separator 124 may be wound or folded and then contained in a battery case 125. Then, the battery case 125 may be filled with an organic liquid electrolyte and sealed with a cap assembly 126, thereby completing the manufacture of the lithium battery 121. The battery case 125 may be cylindrical, rectangular, or thin-film. For example, the lithium battery 121 may be a thin-film battery. For example, the lithium battery 121 may be a lithium-ion battery.
[0231] A separator 124 may be inserted between the positive electrode 123 and the negative electrode 122 to form a battery assembly. A plurality of such battery assemblies may be stacked in a bi-cell structure and impregnated with an organic electrolyte solution. The resulting battery assembly may then be placed in a bag and hermetically sealed, thereby completing the manufacture of a lithium-ion battery.
[0232] In some embodiments, multiple battery assemblies may be stacked on top of each other to form a battery pack, which may be used in any device requiring high capacity and high output, such as laptop computers, smartphones, electric vehicles, and the like.
[0233] When the number of charge-discharge cycles of the lithium battery is 100 times or less, the porous silicon-containing composite according to any embodiment may include first primary particles and second primary particles, wherein graphene flakes may be grown on the second primary particles.
[0234] A lithium battery including such a battery pack may have improved high-rate characteristics and lifespan characteristics, and thus may be suitably used in electric vehicles (EVs), for example, hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs).
[0235] According to another aspect, a device comprises the porous silicon-containing composite according to any embodiment or a carbon composite comprising the porous silicon-containing composite according to any embodiment and a carbonaceous material.
[0236] The device may be, for example, a field emission device, a biosensor, a semiconductor device, or a thermoelectric device.
[0237] Field emission devices are devices that utilize the migration of electrons. Typically, a field emission device may include at least a reduction electrode, an emitter (emitter) tip, and an oxidation electrode spaced apart from the reduction electrode (see US 7,009,331; US 6,976,897; US 6,911,767; and US 2006 / 0066217, the contents of which are incorporated by reference in their entirety). When a voltage is applied between the reduction electrode and the oxidation electrode, the emitter tip may emit electrons. The electrons may migrate from the reduction electrode toward the oxidation electrode. Field emission devices according to embodiments of the present disclosure may be used for a variety of purposes, such as in, for example, ultrasonic vacuum tubes (e.g., X-ray tubes), power amplifiers, ion guns, high-energy accelerators, free electron lasers, and electron microscopes, and in particular in flat panel display devices. Flat panel display devices may be used as a substitute for conventional cathode tubes, and may also be used in TVs or computer monitors.
[0238] The porous silicon-containing composite according to any embodiment or the carbon composite including the same may be used as the emitter tip.
[0239] Conventional emitter tips can be made using metals such as molybdenum (Mo) or semiconductors such as silicon. One of the concerns with using metal emitters is the relatively high control voltage of about 100V required for emission. In addition, due to the non-uniformity of such conventional emitter tips, the current density of individual pixels of a field emission device using conventional emitter tips can be non-uniform.
[0240] When the porous silicon-containing composite or the carbon composite according to any of the embodiments is used as the emitter tip, improved field emission characteristics may be obtained.
[0241] The porous silicon-containing composite or carbon composite according to any embodiment may be used to manufacture an electroluminescent device.
[0242] According to another aspect, a thermoelectric material and a thermoelectric device including the same are provided, wherein the thermoelectric material includes: the porous silicon-containing composite according to any embodiment or a carbon composite including the porous silicon-containing composite according to any embodiment and a carbonaceous material.
[0243] The thermoelectric material may have good electrical properties and thus improved thermoelectric performance. The thermoelectric material may be used in a thermoelectric device, a thermoelectric module () assembly, or a thermoelectric system.
[0244] The porous silicon-containing composite or carbon composite according to any embodiment may include graphene, and thus when used in a thermoelectric material, provides the thermoelectric material with high electrical conductivity and low thermal conductivity according to the characteristics of graphene. Therefore, the thermoelectric material may have improved performance.
[0245] In the porous silicon-containing composite or carbon composite according to any of the above embodiments, the crystalline properties and electronic structure at the interface between the metallic graphene and the semiconducting silicon can be changed to improve its Seebeck coefficient and accelerate the transport of charged particles, which can thus lead to an increase in conductivity and charge mobility. In addition, phonon scattering at the interface between the graphene and the silicon can be promoted, and it becomes possible to control the thermal conductivity of the thermoelectric material.
[0246] As described above, the porous silicon-containing composite or carbon composite according to any of the above embodiments can be effectively used as a thermoelectric material. The thermoelectric device can be manufactured by processing the thermoelectric material into a shape, such as by cutting. The thermoelectric device can be a p-type thermoelectric device. The thermoelectric device can be a structure formed by molding the thermoelectric material into a predetermined shape, such as a rectangular parallelepiped shape.
[0247] The thermoelectric device may have a cooling effect when it is combined with an electrode and a current is applied thereto, and may be an element having a power generation effect based on a temperature difference.
[0248] Fig. 9 FIG. 2 is a diagram of a thermoelectric module 200 including a thermoelectric device according to an embodiment. Fig. 9 , an upper electrode (first electrode) 212 and a lower electrode (second electrode) 222 are patterned on an upper insulating substrate 211 and a lower insulating substrate 221, respectively. The upper electrode 212 and the lower electrode 222 may contact the p-type thermoelectric component 215 and the n-type thermoelectric component 216. The upper electrode 212 and the lower electrode 222 may be connected to the outside of the thermoelectric device through a lead electrode 224. The p-type thermoelectric component 215 may be a thermoelectric device according to any of the above-described embodiments. The n-type thermoelectric component 216 may not be particularly limited and may be any material known in the art.
[0249] The upper and lower insulating substrates 211 and 221 may include gallium arsenide (GaAs), sapphire, silicon, Pyrex, or quartz. The upper and lower electrodes 212 and 222 may include, for example, copper, aluminum, nickel, gold, or titanium, and may have a variety of sizes. The upper and lower electrodes 212 and 222 may be formed using any common patterning method such as a lift-off semiconductor process, a deposition method, or a photolithography technique.
[0250] One of the first and second electrodes 212 and 222 in the thermoelectric module may be exposed to a heat source, such as Fig.10 and 11In some embodiments, one of the first and second electrodes 212 and 222 in the thermoelectric device module may be electrically connected to a power source, or to the outside of the thermoelectric module, for example, to an electrical device (eg, a battery) that consumes or stores electrical energy.
[0251] One of the first and second electrodes 212 and 222 in the thermoelectric module may be electrically connected to a power source.
[0252] Also disclosed is a biosensor comprising: the porous silicon-containing composite, or a carbon composite comprising the porous silicon-containing composite and a carbonaceous material.
[0253] The porous silicon-containing composite or carbon composite according to any embodiment may be used to manufacture an electrode of the biosensor.
[0254] Fig.12 2 is a cross-sectional view illustrating the structure of an electrode 300 of a biosensor according to an embodiment.
[0255] Reference Fig.12 The electrode 300 of the biosensor according to the embodiment may include: a substrate 310; a first layer 320 on the substrate 310, the first layer 320 including a porous silicon-containing composite or a carbon composite according to any embodiment; and a second layer 330 on the first layer 320. The biomaterial 340 may be supported by the second layer 330 or fixed in the second layer 330 in various ways.
[0256] The substrate 310 may be any plate on which graphene can be deposited or formed, and may be, for example, glass, plastic, metal, ceramic, silicon, or a combination thereof. The type of the substrate 310 is not particularly limited as long as graphene can be deposited or formed thereon.
[0257] The biological material 340 can be an enzyme, an aptamer, a protein, a nucleic acid, a microorganism, a cell, a lipid, a hormone, DNA, PNA, RNA, or a combination thereof. Any suitable biological material not described herein can also be used.
[0258] Reference Fig.12 In the electrode 300 of the biosensor, the biomaterial 340 may be an enzyme, and the second layer 330 may be a layer capable of supporting the enzyme or immobilizing the enzyme therein. Fig.12 In the embodiment, the enzyme as the biomaterial 340 is shown to be carried by the second layer 330 or fixed in the second layer 330, but the position of the enzyme is not limited thereto, and the enzyme may partially or completely protrude through the surface of the second layer 330 and be exposed. When the biosensor has this structure including an enzyme having substrate specificity to selectively respond to a target molecule in a mixture, the biosensor can selectively sense an analyte (e.g., blood sugar) to which the enzyme responds.
[0259] According to another aspect of the inventive concept, a semiconductor device includes: a porous silicon-containing composite according to any embodiment or a carbon composite including the porous silicon-containing composite and a carbonaceous material.
[0260] The porous silicon-containing composite or the carbon composite according to any embodiment can be used to fabricate an electrode of the semiconductor device.
[0261] A thermoelectric material and a thermoelectric device including the thermoelectric material are also disclosed, wherein the thermoelectric material includes: a porous silicon-containing composite according to any embodiment or a carbon composite including the porous silicon-containing composite and a carbonaceous material.
[0262] The performance of the thermoelectric material is evaluated using a dimensionless figure of merit (ZT) defined by Equation 2.
[0263] Equation 2
[0264] ZT = (S 2 σT) / k
[0265] In Equation 2, ZT is the figure of merit, S is the Seebeck coefficient, σ is the electrical conductivity, T is the absolute temperature, and k is the thermal conductivity.
[0266] As shown in Equation 2, a higher ZT value of the thermoelectric material can be obtained by: increasing the Seebeck coefficient (S) and the electrical conductivity (σ) of the thermoelectric material, i.e., the power factor (S 2 σ), and decreasing the thermal conductivity of the thermoelectric material.
[0267] Embodiments will now be described in further detail with reference to the following examples. However, these examples are for illustrative purposes only and are not intended to limit the scope of one or more embodiments of the present disclosure.
[0268] Examples
[0269] Preparation Example 1 for Preparation: Preparation of First Primary Particles
[0270] Needle-shaped silicon is pulverized using a wet bead mill to obtain plates and needle-shaped silicon (first primary particles) having a layer of silicon suboxide (SiO x )(where 0 < x < 2) on its surface (having a thickness of about 0.1 nm - about 10 nm), having a length (D90) of about 150 nm and a thickness of about 40 nm. The rotation speed is 1 - 20 m / s, for example, about 10 m / s, and the rotation time is 1 hour - 72 hours, for example, about 10 hours.
[0271] Preparation Example 1
[0272] Mix 25 parts by weight of silicon, which is a 9:1 mixture (by weight) of first primary particles obtained according to Preparation Example 1 and spherical silicon (second primary particles, available from NanoAmor) having an average diameter of about 50 nm obtained by vapor phase synthesis, with 10 parts by weight of stearic acid and 65 parts by weight of isopropyl alcohol to obtain a composition. Spray dry the composition, and then further dry it to obtain porous silicon secondary particles having an average particle size of about 4.5 μm. A silicon suboxide (SiO x )(where 0 < x < 2) layer (having a thickness of about 0.1 nm - about 10 nm) is on the surface of the second primary particles.
[0273] Use a spray dryer (MMSD Micro Mist Spray Dryers, Fujisaki Electric) to perform spray drying by controlling the nozzle size, the pressure in the N 2 atmosphere, and the powder spray atmosphere temperature (about 200 °C) to remove isopropyl alcohol and thereby prepare porous silicon secondary particles. The nozzle size is controlled to be about 150 μm, and the nozzle pressure is about 0.6 MPa.
[0274] Load the porous silicon secondary particles into a reactor. After purging the reactor with nitrogen, methane (CH 4 ) as a reaction gas is introduced into the reactor to create an atmosphere of the reaction gas. The pressure level inside the reactor achieved by the inflow of the gas is about 1 atm. Heat-treat the reactor by raising the internal temperature (at a rate of about 23 °C / minute) to about 1000 °C under the atmosphere of the gas, and while maintaining this temperature for about 1 hour and continuously flowing the gas into the reactor. Let the resulting product stand for about 3 hours. Then, stop the supply of the gas, cool the reactor to room temperature (25 °C), and then purge it with nitrogen to obtain a porous silicon-containing composite.
[0275] Relative to the total weight of 100 parts by weight of the porous silicon-containing composite, the total amount of first graphene and second graphene in the porous silicon-containing composite is about 25 parts by weight.
[0276] Preparation Example 2
[0277] Prepare a porous silicon-containing composite in the same manner as in Preparation Example 1, except that: the mixing weight ratio of the first primary particles to the second primary particles is about 8:2.
[0278] Preparation Examples 3 - 4
[0279] A porous silicon-containing composite was prepared in the same manner as in Preparation Example 1, except that: first primary particles and second primary particles having the sizes shown in Table 1 were used.
[0280] Table 1
[0281]
[0282] In Table 1, the size of the first primary particles represents the average length of the first primary particles, and the size of the second primary particles represents the average diameter of the second primary particles.
[0283] Preparation of Comparative Example 1
[0284] A porous silicon-containing composite was obtained in the same manner as in Preparation Example 1, except that: only the first primary particles were used.
[0285] Preparation of Comparative Example 2
[0286] A porous silicon-containing composite mixture was obtained by mixing the porous silicon-containing composite of Comparative Example 1 and the porous silicon-containing composite of Comparative Example 3 at a weight ratio of about 80:20.
[0287] Preparation of Comparative Example 3
[0288] 25 parts by weight of spherical silicon (second primary particles) having an average diameter of about 50 nm obtained by vapor phase synthesis (available from NanoAmor), 10 parts by weight of stearic acid, and 65 parts by weight of isopropyl alcohol were mixed to prepare a composition. The composition was spray-dried and then further dried to obtain porous silicon secondary particles having an average particle size of about 4.5 μm. A silicon suboxide (SiO x )(where 0 < x < 2) layer (having a thickness of about 0.1 nm) was on the surface of the spherical silicon.
[0289] Spray drying was carried out using a spray dryer (MMSD Micro Mist Spray Dryers, Fujisaki Electric) by controlling the nozzle size, the pressure in the N 2 atmosphere, and the powder spray atmosphere temperature (about 200 °C) to remove isopropyl alcohol and thereby prepare porous silicon secondary particles.
[0290] The porous silicon secondary particles were loaded into a reactor. After purging the reactor with nitrogen, methane (CH 4) flows into the reactor to produce an atmosphere of the reaction gas. The pressure level inside the reactor reached by the inflow of the gas is about 1 atm. The internal temperature of the reactor is raised to about 1000° C. (at a rate of about 23° C. / minute) under the atmosphere of the gas, and heat treatment is performed while maintaining the temperature for about 1 hour and continuously flowing the gas into the reactor. The resulting product is allowed to stand for about 3 hours. Then, the supply of the gas is stopped, and the reactor is cooled to room temperature (25° C.), and then purged with nitrogen, thereby obtaining a porous silicon-containing composite.
[0291] Example 1: Fabrication of negative electrode and full cell
[0292] The porous silicon-containing composite prepared in Preparation Example 1, graphite, lithium polyacrylate (Li-PAA), and deionized (DI) water as a solvent were mixed to prepare a slurry. The ratio of the mixture of the porous silicon-containing composite and graphite of Preparation Example 1 to lithium polyacrylate was about 95:5 by weight on a solid basis. The ratio of the porous silicon-containing composite of Preparation Example 1 to graphite in the mixture was about 15:85 by weight.
[0293] After the slurry was applied to a copper (Cu) foil using a doctor blade to form a film having a thickness of about 40 μm, the film was vacuum dried at about 120° C. for about 2 hours and roll-pressed, thereby manufacturing a negative electrode.
[0294] Use LiNi 0.6 Co 0.2 Mn 0.2 O 2 、LiNi 0.6 Co 0.2 Al 0.2 O 2 The positive electrode is made of a slurry obtained by mixing a superconducting acetylene black (Denka Black), polyvinylidene fluoride (PVdF) as a binder, and N-methylpyrrolidone (NMP) as a solvent. The LiNi in the slurry 0.6 Co 0.2 Mn 0.2 O 2 、LiNi 0.6 Co 0.2 Al 0.2 O 2 The mixing ratio of , superconductive acetylene black, and PVdF as a binder is about 75:9:3:3 by weight. The slurry is applied to an aluminum (Al) foil using a doctor blade to form a film having a thickness of about 40 μm. The film is vacuum dried at about 120° C. for about 2 hours and rolled to manufacture a positive electrode.
[0295] A coin full-cell battery was fabricated using the negative electrode and the positive electrode. A polypropylene film (CELLGARD 3510) was used as a separator. The electrolyte used was 1.3 M LiPF in a mixed solvent of ethylene carbonate (EC), diethyl carbonate (DEC), and fluoroethylene carbonate (FEC) in a volume ratio of about 50:25:25. 6 of solution.
[0296] Example 2-4: Fabrication of negative electrode and full cell
[0297] A negative electrode and a full-cell were manufactured in the same manner as in Example 1, except that the porous silicon-containing composites of Preparation Examples 2 to 4 were used instead of the porous silicon-containing composite of Preparation Example 1, respectively.
[0298] Example 5: Fabrication of negative electrode and coin half cell
[0299] The porous silicon-containing composite prepared in Preparation Example 1, graphite, lithium polyacrylate (Li-PAA), and deionized (DI) water as a solvent were mixed to prepare a slurry. The ratio of the mixture of the porous silicon-containing composite and graphite of Preparation Example 1 to lithium polyacrylate was about 95:5 by weight on a solid basis. The ratio of the porous silicon-containing composite of Preparation Example 1 to graphite in the mixture was about 15:85 by weight.
[0300] After the slurry was applied to a copper (Cu) foil using a doctor blade to form a film having a thickness of about 40 μm, the film was vacuum dried at about 120° C. for about 2 hours and roll-pressed, thereby manufacturing a negative electrode.
[0301] A coin half-cell was fabricated using the negative electrode and lithium metal as a counter electrode. A polypropylene film (CELLGARD 3510) was used as a separator. The electrolyte used was 1.3 M LiPF in a mixed solvent of ethylene carbonate (EC), diethyl carbonate (DEC), and fluoroethylene carbonate (FEC) in a volume ratio of about 2:6:2. 6 of solution.
[0302] Examples 6-8: Fabrication of negative electrodes and coin half-cell batteries
[0303] A negative electrode and a coin half-cell were manufactured in the same manner as in Example 5, except that the porous silicon-containing composites of Preparation Examples 2 to 4 were used instead of the porous silicon-containing composite of Preparation Example 1, respectively.
[0304] Comparative Example 1: Fabrication of negative electrode and full cell
[0305] A negative electrode and a full-cell were manufactured in the same manner as in Example 1, except that the porous silicon-containing composite of Comparative Preparation Example 1 was used instead of the porous silicon-containing composite of Preparation Example 1.
[0306] Comparative Example 2-3: Fabrication of negative electrode and full cell
[0307] A negative electrode and a full-cell battery were manufactured in the same manner as in Example 1, except that the materials prepared in Comparative Preparation Examples 2 and 3 were used instead of the porous silicon-containing composite of Preparation Example 1, respectively.
[0308] Comparative Examples 4-6: Fabrication of Negative Electrode and Coin Half Cell
[0309] A negative electrode and a coin half-cell were manufactured in the same manner as in Example 5, except that the materials prepared in Comparative Preparation Examples 1 to 3 were used instead of the porous silicon-containing composite of Preparation Example 1, respectively.
[0310] Evaluation Example 1: Oxygen Content
[0311] The porous silicon-containing composites prepared in Preparation Examples 1 and 2, and the porous silicon-containing composites prepared in Preparation Comparative Example 1 and the porous silicon-containing composites prepared in Preparation Comparative Example 3 were analyzed by X-ray photoelectron spectroscopy (XPS) to analyze oxygen and carbon contents. The analysis results are shown in Table 2.
[0312] XPS analysis was performed using Quantum 2000 (available from Physical Electronics Inc.) (accelerating voltage: 0.5 to 15 kV, 300 W, energy resolution: about 1.0 eV, and sputtering rate: 0.1 nm / min).
[0313] Table 2
[0314] Example Oxygen (atomic %) Preparation Example 1 5.8 Preparation Example 2 5.2 Preparation Comparative Example 1 6.9 Preparation Comparative Example 3 1.0
[0315] In Table 2, the oxygen content is defined as the oxygen content corresponding to the O1s peak.
[0316] Referring to Table 2, the porous silicon-containing composites of Preparation Examples 1 and 2 had reduced oxidation degrees compared to that of Preparation Comparative Example 1. It was found that the porous silicon-containing composite of Preparation Comparative Example 3 prepared using spherical silicon obtained by vapor phase synthesis had a small oxygen content and the lowest oxidation degree.
[0317] Evaluation Example 2: Specific surface area and density
[0318] The specific surface area and density of the porous silicon-containing composites obtained in Preparation Examples 1 and 2 and Comparative Preparation Examples 1 and 3 were measured. The results are shown in Table 3. The specific surface area was measured using the BET method, and the density was measured by using an envelope pycnometer before pressing each sample.
[0319] Table 3
[0320] Example <![CDATA[Specific surface area (m 2 / g)]]> Density(g / cc) Preparation Example 1 6.9 1.18 Preparation Example 2 41.6 1.11 Preparation Comparative Example 1 5.9 1.09 Preparation Comparative Example 3 128.3 0.95
[0321] Referring to Table 3, it was found that the porous silicon-containing composite of Comparative Preparation Example 3 prepared using silicon obtained by vapor phase synthesis had a very large specific surface area.
[0322] Compared with the porous silicon-containing composite of Preparation Comparative Example 3, the porous silicon-containing composites of Preparation Examples 1 and 2 have significantly smaller specific surface areas, which can suppress side reactions with the electrolyte.
[0323] The porous silicon-containing composites of Preparation Examples 1 and 2 were found to have higher density than the porous silicon-containing composite of Preparation Comparative Example 1, and the improved particle strength of the porous silicon-containing composites of Preparation Examples 1 and 2 was expected.
[0324] Evaluation Example 3: Transmission Electron Microscopy (TEM) Analysis
[0325] The porous silicon-containing composites obtained in Preparation Example 1 and Preparation Comparative Example 1 were analyzed using transmission electron microscopy (TEM) using Titan cubed G2 60-300 (FEI).
[0326] The TEM analysis results of the surface of the porous silicon-containing composite prepared in Comparative Example 1 are shown in Figures 3A-3C The TEM analysis results of the porous silicon-containing composite of Preparation Example 1 are shown in Figures 4A-4D middle.
[0327] Reference Figure 4A and 4B It was found that the porous silicon-containing composite of Preparation Example 1 included spherical second primary particles and needle- and plate-shaped first primary particles, and thus had a reduced porosity compared to the porous silicon-containing composite of Preparation Comparative Example 1, thereby providing improved electron conductivity.
[0328] The first primary particles and the second primary particles may form a network through the second graphene, such as Figure 4D As shown in , and a structure in which the second primary particles are embedded between the first primary particles can be formed. In the porous silicon-containing composite prepared in Comparative Example 1, a disconnected electron channel region was observed, such as Figure 3B and only one type of silicon with plate-like and needle-like forms was observed, as Figure 3C as shown in .
[0329] like Figure 4C As shown in , the second graphene and the silicon suboxide are very close to each other with adhesion of about 1 nm or less, and the second graphene on the first primary particle has a layered shape, and the second graphene on the second primary particle has a single layer shape with scales grown thereon.
[0330] Evaluation Example 4: Raman Analysis
[0331] By using Raman 2010 Spectra (NT-MDT Development Co.) (laser system: 473nm, 633nm, 785nm, minimum Raman shift: ~50cm -1 , spatial resolution: about 500 nm) Raman analysis was performed on the porous silicon-containing composites of Preparation Example 1 and Preparation Comparative Examples 1 and 3.
[0332] The intensity ratio of the D peak to the G peak (D / G) was calculated based on the Raman analysis results.
[0333] In the Raman spectrum of graphene, at 1350 cm -1 、1580cm -1 and 2700cm -1 A peak appears at 1580 cm-1, which gives information about the thickness, crystallinity and charge doping state of graphene. -1 The peak at 2700 cm (also called the G-mode peak) is due to the oscillation mode corresponding to the stretching of the C-C bond, and the energy of the G-mode is determined by the density of excess charges doped on graphene. -1 The peak at 1350 cm (also called 2D-mode peak) is useful in evaluating the thickness of graphene. -1 The peak at SP 2 It occurs when the crystal structure has defects. The D / G intensity ratio gives information about the degree of disorder in the crystal of graphene.
[0334] Table 4
[0335] Example D / G intensity ratio Preparation Example 1 1.19 Preparation Comparative Example 1 1.09 Preparation Comparative Example 3 1.72
[0336] Evaluation Example 5: Charging and Discharging Characteristics of Coin Full-Cell Battery
[0337] The charge and discharge characteristics of the coin full-cell batteries of Example 1, Example 2, and Comparative Examples 1-3 were evaluated in the following manner. The charge and discharge cycle was repeated 100 times under the following charge and discharge conditions: (charge: 1.0C / cutoff: 4.2V-0.01C, discharge: 1.0C / cutoff: 2.5V).
[0338] The coin full-cell battery is charged at about 25°C with a constant current at a rate of 0.1C until a voltage of 4.2V (relative to Li) is reached, and then charged with a constant current of 4.2V (constant voltage mode) until a cutoff current of 0.01C rate is reached, and then discharged with a constant current at a rate of 0.1C until a voltage of 2.5V (relative to Li) is reached (1st cycle, formation cycle).
[0339] After the first cycle, the coin full-cell battery was charged at about 25°C with a constant current at a rate of 0.2C until a voltage of 4.2V (relative to Li) was reached, and then charged with a constant voltage of 4.2V (constant voltage mode) until a cutoff current of 0.01C rate was reached, and then discharged with a constant current at a rate of 0.2C until a voltage of 2.5V (relative to Li) was reached (second cycle, formation cycle).
[0340] After the 2nd cycle, the coin full-cell battery was charged at about 25° C. with a constant current of 1.0 C rate until a voltage of 4.2 V (relative to Li) was reached, and then charged with a constant voltage of 4.2 V (constant voltage mode) until a cut-off current of 0.01 C rate was reached, and then discharged with a constant current of 1.0 C rate until a voltage of 2.5 V (relative to Li) was reached (3rd cycle). This cycle was repeated 100 times to the 103rd cycle under the same conditions. Throughout the charging and discharging cycles, a rest time of about 10 minutes was allowed after each charging and discharging cycle.
[0341] Some of the charge and discharge test results are shown in Table 5. In Table 5, the charge and discharge efficiency is for the 0.1C condition of the first cycle of the coin full cell, and the specific capacity is about 0.2C discharge capacity after 0.1C charge / discharge of the coin full cell.
[0342] The discharge capacity retention rate at the 103rd cycle is defined using Equation 3.
[0343] Equation 3
[0344] Capacity retention rate [%] = [discharge capacity at the 103rd cycle / discharge capacity at the 3rd cycle] × 100%
[0345] Table 5
[0346] Example Specific capacity (mAh / g) Initial efficiency (%) Charging and discharging efficiency (%) life(%) Example 1 1700 89.4 85.8 93.3 Example 2 1800 86.8 85.0 84.6 Comparative Example 1 1560 86.6 84.8 92.1 Comparative Example 2 1710 85.5 84.5 83.3 Comparative Example 3 2300 82.2 84.1 65.6
[0347] Referring to Table 5, it was found that the coin full-cell batteries of Examples 1 and 2 had comparable or improved life characteristics, and improved initial efficiency compared to the coin full-cell batteries of Comparative Examples 1 to 3. It was found that the coin full-cell battery of Example 2 had poor life characteristics compared to the coin full-cell battery of Comparative Example 1, but had improved initial efficiency and charge and discharge efficiency, which is more advantageous for practical applications.
[0348] Evaluation Example 6: Charging and Discharging Characteristics of Coin Half Cells
[0349] The charge and discharge characteristics of the coin half-cell batteries of Example 5 and Comparative Examples 4 and 5 were evaluated in the following manner.
[0350] The coin half-cell battery was charged at about 25°C with a constant current at a rate of 0.1C until a voltage of 0.01V (relative to Li) was reached, then charged with a constant voltage of 0.01V (constant voltage mode) until a cutoff current of 0.01C rate was reached, and then discharged with a constant current at a rate of 0.1C until a voltage of 1.5V (relative to Li) was reached (formation cycle).
[0351] After the formation cycle, the coin half-cell was charged at about 25°C with a constant current at a rate of 0.1C until a voltage of 0.01V (relative to Li) was reached, and then charged with a constant voltage of 0.01V (constant voltage mode) until a cutoff current of 0.01C rate was reached, and then discharged with a constant current at a rate of 0.1C until a voltage of 1.5V (relative to Li) was reached (1st cycle).
[0352] After the 1st cycle, the coin half cell was charged at about 25°C with a constant current of 0.2C rate until a voltage of 0.01V (relative to Li) was reached, and then discharged with a constant current of 0.2C rate until a voltage of 1.5V (relative to Li) was reached (2nd cycle).
[0353] After the 2nd cycle, the coin half cell was charged at about 25°C with a constant current of 0.5C rate until a voltage of 0.01V (relative to Li) was reached, and then discharged with a constant current of 0.5C rate until a voltage of 1.5V (relative to Li) was reached (3rd cycle).
[0354] After the 3rd cycle, the coin half cell was charged at about 25°C with a constant current at a rate of 1C until a voltage of 0.01 V (relative to Li) was reached, and then discharged with a constant current at a rate of 1C until a voltage of 1.5 V (relative to Li) was reached (4th cycle).
[0355] Throughout the charge and discharge cycles, a rest time of approximately 10 minutes was allowed after each charge and discharge cycle.
[0356] The high rate characteristics are defined using Equation 4.
[0357] Equation 4
[0358] High rate characteristics [%] = [discharge capacity at the 4th cycle (1C rate) / discharge capacity at the 1st cycle (0.1C rate)] × 100%
[0359] Some of the charge and discharge evaluation results are shown in Tables 6 and Figure 5 middle. Figure 5 Graphs showing high rate characteristics of coin half-cell batteries of Example 5 and Comparative Examples 4 and 5.
[0360] Table 6
[0361]
[0362] Referring to Table 6, it was found that the coin half-cell battery of Example 5 had improved high-rate characteristics compared with the coin half-cell batteries of Comparative Examples 4 and 5.
[0363] Evaluation Example 7: Scanning Electron Microscopy (SEM) Analysis after Charge and Discharge Cycles
[0364] Evaluation of the coin full cell of Example 1 was performed by scanning electron microscopy (SEM) of the surface and cross section of the negative electrode active material in the negative electrode before charging and discharging, after the 1st cycle, and after repeated charging and discharging to the 20th cycle in the same manner as in Evaluation Example 5. The evaluation results are shown in Figures 6A-6C middle. Fig. 6A is a SEM image of the negative electrode active material in the initial state before charging and discharging, Figure 6B is the SEM image of the negative electrode active material after the first cycle, and Figure 6C is a SEM image of the negative electrode active material after 20 charge-discharge cycles.
[0365] Reference Figures 6A-6C , it was found that when the number of charge-discharge cycles was less than 100, the secondary particles maintained a silicon-containing structure including plate- and sheet-shaped first primary particles and spherical second primary particles. When such a negative electrode active material having a stable structure after charge and discharge is used, a battery with low expansion and excellent durability can be manufactured.
[0366] Evaluation Example 8: Charging and Discharging Test
[0367] The charge and discharge characteristics of the coin half cells of Example 5 and Comparative Examples 4 and 5 were evaluated under the following charge and discharge conditions in the following manner: (charge: 1.0 C / cutoff: 0.01 V-0.01 C, discharge: 1.0 C / cutoff: 1.5 V).
[0368] The differential charge and discharge characteristics (dQ / dV) of each coin half cell at the first cycle, which shows the difference in lithium-silicon reaction potential, were evaluated. The results are shown in Fig. 7A and 7B middle. Fig. 7A The evaluation results of the differential charge and discharge characteristics (dQ / dV) of the coin half-cell batteries of Example 5 and Comparative Example 4 at the first cycle are described. Figure 7B The evaluation results of the differential charge and discharge characteristics (dQ / dV) of the coin half-cell batteries of Example 5 and Comparative Example 5 at the first cycle are described.
[0369] Reference Fig. 7A and 7B It was found that the coin half-cells of Comparative Examples 4 and 5 had discharge peaks shifted relative to the discharge peak of the coin half-cell of Example 5, indicating structural changes occurring in the coin half-cells of Comparative Examples 4 and 5.
[0370] In the dQ / dV curve of the coin half cell of Example 5 at the 1st cycle, a smooth oxidation-reduction peak was observed in the voltage range of about 0.2V to about 0.8V.
[0371] As described above, by using an electrode including the porous silicon-containing composite according to any embodiment, a lithium battery having improved capacity, initial efficiency, lifespan characteristics, and high rate characteristics may be manufactured.
[0372] It should be understood that the embodiments described herein should be considered in a descriptive sense only and not for purposes of limitation. Descriptions of features or aspects within each embodiment should typically be considered as available for other similar features or aspects in other embodiments.
[0373] Although embodiments have been described with reference to the accompanying drawings, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the spirit and scope as defined by the following claims.
Claims
1. A porous silicon-containing composite, include: a porous core comprising a porous silicon composite secondary particle; and a shell on at least one surface of the porous core, the shell comprising a first graphene, The porous silicon composite secondary particles include the following aggregates: A first primary particle comprising silicon, A second primary particle comprising the structure, and a second graphene on at least one surface of the first primary particle and the second primary particle, and wherein at least one of the shape and the degree of oxidation of the first primary particle and the second primary particle is different, The first primary particles have a plate shape, a needle shape, a cube shape, a rod shape, or a combination thereof, and the second primary particles have a spherical form, a nanowire form, or a combination thereof.
2. The porous silicon-containing composite of claim 1, wherein the structure comprises silicon, germanium, tin, aluminum, zinc, antimony, alloys thereof, or combinations thereof. The porous silicon-containing composite of claim 1 , wherein the structure is silicon.
4. The porous silicon-containing composite according to claim 1, wherein the first primary particles have an oxygen content of 3 atomic % to 15 atomic % based on the total content of the first primary particles, and The second primary particles have an oxygen content of 0.01 atomic % to 3 atomic % based on the total content of the second primary particles.
5. The porous silicon-containing composite according to claim 1, further comprising a silicon-containing matrix having a formula of SiO between the first primary particle and the second primary particle and the second graphene. x Silicon suboxide, of which 0 <x<2。 6. The porous silicon-containing composite according to claim 1, wherein the first primary particles and the second primary particles have shapes different from each other, and The porous silicon-containing composite further comprises third primary particles, the third primary particles comprise silicon, and the third primary particles have a nanotube shape, a nanorod shape, a nanobelt shape, or a combination thereof.
7. The porous silicon-containing composite of claim 1, wherein the first primary particles have a plate shape, a needle shape, or a combination thereof, and The second primary particles have a spherical shape. 8 . The porous silicon-containing composite according to claim 1 , wherein the first primary particles and the second primary particles form a network, or the second primary particles are embedded between the first primary particles.
9. The porous silicon-containing composite of claim 1, wherein the size of the second primary particle is the same as or smaller than the size of the first primary particle, wherein "size" refers to the diameter or the length of the major axis.
10. The porous silicon-containing composite of claim 1, wherein the first primary particles and the second primary particles each independently have a size of 10 nm-30 μm, the first primary particles have a size of 20 nm-180 nm, and the second primary particles have a size of 100 nm or less, wherein "size" refers to a diameter or a length of a major axis. 11 . The porous silicon-containing composite according to claim 1 , wherein a mixing weight ratio of the first primary particles to the second primary particles is 1:99-99:
1.
12. The porous silicon-containing composite according to claim 1, wherein the second graphene in the form of 1 to 30 layers is located on the first primary particle, and The second graphene in the form of 1 to 5 layers is located on the second primary particle, and the second graphene in the form of flakes is located on the second graphene in the form of 1 to 5 layers.
13. The porous silicon-containing composite according to claim 1, wherein the porous silicon-containing composite has a specific surface area of 0.1 m2 / g to 100 m2 / g and a density of 0.1 g / cm3 to 2.8 g / cm3.
14. The porous silicon-containing composite of claim 1, wherein the second graphene is directly disposed on a surface of a silicon suboxide, and the first graphene is directly disposed on a surface of the porous silicon composite secondary particle. 15 . The porous silicon-containing composite according to claim 1 , wherein the amount of silicon is 0.1 parts by weight to 99 parts by weight relative to 100 parts by weight of the total weight of the porous silicon-containing composite.
16. The porous silicon-containing composite as claimed in claim 1, wherein the porous silicon-containing composite has a dual core / shell structure. 17 . The porous silicon-containing composite according to claim 1 , wherein a total amount of the first graphene and the second graphene is 0.1 parts by weight to 2,000 parts by weight relative to 100 parts by weight of silicon.
18. The porous silicon-containing composite according to claim 5, wherein the first primary particles, the second primary particles, and the second graphene on at least one surface of the first primary particles and the second primary particles are included in the silicon composite primary particles, and the second graphene is disposed at a distance of 10 nanometers or less from the surface of the silicon suboxide of the formula SiO x where 0 < x < 2 in the silicon composite primary particles. The second graphene includes 1 to 30 graphene layers and has a total thickness of 0.3 nanometers to 1,000 nanometers, and x is formed by chemical vapor deposition or physical vapor deposition, and the second graphene is doped with boron, nitrogen, phosphorus, sulfur, or a combination thereof, and the doping concentration of the dopant is 0.01 atomic% to 10 atomic%. The second graphene is oriented at an angle of 0°-90° relative to a major axis of the silicon.
19. The porous silicon-containing composite according to claim 1, wherein the first graphene is disposed at a distance of 1000 nanometers or less from the surface of the silicon suboxide of the formula SiO x where 0 < x < 2 in the porous silicon composite secondary particles, the first graphene comprises 1 to 30 graphene layers, and has a total thickness of 0.6 nanometers to 50 nanometers, and x wherein the first graphene is disposed at a distance of 1000 nanometers or less from the surface of the silicon suboxide of the formula SiO x where 0 < x < 2 in the porous silicon composite secondary particles, the first graphene comprises 1 to 30 graphene layers, and has a total thickness of 0.6 nanometers to 50 nanometers, and The first graphene is oriented at an angle of 0°-90° relative to a major axis of the silicon.
20. The porous silicon-containing composite of claim 5, wherein the silicon suboxide has a thickness of 30 microns or less.
21. The porous silicon-containing composite of claim 1, wherein the porous silicon composite secondary particles have an average particle size of 1 μm to 30 μm, a specific surface area of 0.1 m2 / g to 100 m2 / g, and a density of 0.1 g / cm3 to 2.57 g / cm3.
22. The porous silicon-containing composite according to claim 1, wherein the oxygen content of the porous silicon-containing composite is 0.1 atomic % to 15 atomic % relative to the total content of oxygen, carbon and silicon atoms.
23. The porous silicon-containing composite of claim 1, wherein the porous silicon-containing composite further comprises a carbonaceous coating layer comprising amorphous carbon on at least one surface of the porous silicon-containing composite.
24. The porous silicon-containing composite of claim 23, wherein the carbonaceous coating further comprises crystalline carbon.
25. The porous silicon-containing composite according to claim 24, wherein the crystalline carbon is fullerene, natural graphite, artificial graphite, graphene, carbon nanotube, or a combination thereof, and The amorphous carbon is pitch carbon, soft carbon, hard carbon, sintered coke, carbon fiber, or a combination thereof.
26. The porous silicon-containing composite of claim 25, wherein the pitch carbon is a mesophase pitch carbonization product.
27. The porous silicon-containing composite of claim 24, wherein the carbonaceous coating layer is a non-porous continuous coating layer and has a thickness of 1 nm to 5000 nm.
28. A method for preparing a porous silicon-containing composite according to any one of claims 1 to 27, wherein the method include: contacting first primary particles having a first shape and a first degree of oxidation and second primary particles having a second shape and a second degree of oxidation to form porous silicon secondary particles, wherein at least one of the first and second shapes or the first and second degrees of oxidation are different; and The porous silicon secondary particles and the carbon source gas are heat-treated to prepare the porous silicon-containing composite.
29. The method of claim 28, wherein the porous silicon secondary particles are formed from a composition comprising the first primary particles, the second primary particles, a dispersant, and a solvent.
30. The method of claim 29, wherein the solvent is an alcohol, and forming the porous silicon secondary particles from the composition comprises spray drying the composition.
31. The method of claim 29, wherein the dispersant is stearic acid, resorcinol, polyvinyl alcohol, carbon pitch, or a combination thereof.
32. The method of claim 28, wherein the carbon source gas comprises a compound represented by Formula 1, a compound represented by Formula 2, an oxygen-containing gas represented by Formula 3, or a combination thereof: Formula 1 C n H (2n+2-a) [OH] a Wherein in Formula 1, n is an integer of 1-20, and a is 0 or 1, Formula 2 C n H (2n) Wherein in Formula 2, n is an integer of 2-6, Formula 3 C x H y O z Wherein in Formula 3, x is an integer of 1-20, y is 0 or an integer of 1-20, and z is 1 or 2, and in, In Formulas 1 and 2, n is independently selected.
33. The method of claim 28, wherein the carbon source gas further comprises a second oxygen-containing compound represented by Formula 3a, the second oxygen-containing compound being different from the oxygen-containing gas represented by Formula 3: Formula 3a C x H y O z in, In Formula 3a, x is 0 or an integer of 1-20, y is 0 or an integer of 1-20, and z is 1 or 2.
34. The method of claim 28, wherein the carbon source gas comprises methane, ethylene, propylene, acetylene, methanol, ethanol, propanol, or a combination thereof.
35. The method of claim 28, wherein the heat treatment is performed at 750°C to 1100°C.
36. The method of claim 28, further comprising mixing a composition comprising the porous silicon-containing composite, a carbonaceous material, and a solvent to obtain a porous silicon-containing composite comprising a carbonaceous coating.
37. A carbon composite comprising the porous silicon-containing composite according to any one of claims 1 to 27 and a carbonaceous material.
38. The carbon composite of claim 37, wherein an amount of the carbonaceous material is 0.001 parts by weight to 99.999 parts by weight relative to 100 parts by weight of the carbon composite.
39. The carbon composite of claim 37, wherein the carbonaceous material is graphene, graphite, fullerene, carbon fiber, carbon nanotube, or a combination thereof.
40. The carbon composite of claim 37, wherein an amount of the porous silicon-containing composite is 0.001 parts by weight to 99.999 parts by weight relative to 100 parts by weight of the carbon composite.
41. An electrochemically active material composite, include: Electrochemically active materials; and The porous silicon-containing composite according to any one of claims 1 to 27, or the carbon composite according to any one of claims 37 to 40, wherein the porous silicon-containing composite is on the surface of the electrochemically active material.
42. Electrode, which include: The porous silicon-containing composite according to any one of claims 1 to 27; or A carbon composite as claimed in any one of claims 37 to 40.
43. A lithium battery comprising the electrode as claimed in claim 42.
44. The lithium battery of claim 43, wherein the porous silicon-containing composite comprises the first primary particles and the second primary particles after 100 or fewer charge and discharge cycles of the lithium battery, wherein graphene flakes are grown on the second primary particles.
45. Device, which include: A porous silicon-containing composite as claimed in any one of claims 1 to 27, or a carbon composite as claimed in any one of claims 37 to 40.
46. The device of claim 45, wherein the device is a field emission device, a biosensor, a semiconductor device, or a thermoelectric device.