Packaging structure and manufacturing method thereof
By using an insulating film with a resin-rich region and a filler-rich region in the semiconductor packaging structure, the problem of insufficient adhesion strength between the insulating film and the rewiring layer in the existing technology is solved, and the stability and resistance in high-temperature cycle tests are achieved. Increase in bending stress.
Patent Information
- Application Number
- CN201910923175.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-09-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-06-26
AI Technical Summary
Existing semiconductor packaging structures are prone to delamination problems between the insulating film and the rewiring layer during high-temperature cycle tests, resulting in insufficient adhesion strength and inability to effectively withstand bending stress.
An insulating film with a resin-rich area and a filler-rich area is used. The insulating film is formed by adjusting the viscosity of the resin material to ensure its adhesion strength to the rewiring layer, and multiple antenna elements are set up in the structure to improve the stability of the overall package. .
It improves the adhesion strength between the insulating film and the rewiring layer, avoids delamination problems caused by thermal expansion coefficient mismatch, and enhances the stability and bending stress resistance of the package structure in thermal cycle tests.
Smart Images

Figure CN111223830B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a packaging structure, and more particularly to a packaging structure and a manufacturing method thereof. Background Art
[0002] Semiconductor devices and integrated circuits used in various electronic applications (e.g., cell phones and other mobile electronic equipment) are typically manufactured on a single semiconductor wafer. The die of the wafer can be processed at the wafer level and packaged with other semiconductor devices (e.g., antennas) or dies, and various technologies have been developed for wafer-level packaging. Summary of the invention
[0003] A packaging structure of an embodiment of the present disclosure includes at least one semiconductor die, an insulating package, a first redistribution layer, a second redistribution layer, a plurality of antenna elements, and a first insulating film. The insulating package encapsulates the at least one semiconductor die, and the insulating package has a first surface and a second surface opposite to the first surface. The first redistribution layer is arranged on the first surface of the insulating package. The second redistribution layer is arranged on the second surface of the insulating package. A plurality of antenna elements are located on the second redistribution layer. The first insulating film is arranged between the second redistribution layer and the plurality of antenna elements, wherein the first insulating film includes a resin-rich region and a filler-rich region, the resin-rich region is located between the filler-rich region and the second redistribution layer and separates the filler-rich region from the second redistribution layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0004] The various aspects of the present disclosure will be best understood by reading the following detailed description in conjunction with the accompanying drawings. It should be noted that, in accordance with standard practice in the industry, the various features are not drawn to scale. In fact, the size of the various features may be arbitrarily increased or reduced for clarity of discussion.
[0005] Figure 1A to Figure 1B are schematic cross-sectional views of various stages in a method of manufacturing an insulating film according to some exemplary embodiments of the present disclosure.
[0006] Figure 1C is an enlarged view of an insulating film stacked on a dielectric layer according to some exemplary embodiments of the present disclosure.
[0007] Figures 2A to 2H are schematic cross-sectional views of various stages in a method of manufacturing a package structure according to some exemplary embodiments of the present disclosure.
[0008] Figures 3A to 3G are schematic cross-sectional views of various stages in a method of manufacturing a package structure according to some exemplary embodiments of the present disclosure.
[0009] Figure 4This is a packaging structure according to some embodiments of the present disclosure.
[0010] Figure 5 Detailed description of the invention The invention relates to a packaging structure according to some other embodiments of the present invention.
[0011] [Explanation of Symbols]
[0012] 102: Support
[0013] 104: Insulation film
[0014] 104A: First insulating film
[0015] 104B: Second insulating film
[0016] 104-Fi: Filler-rich area
[0017] 104-Re: Resin-rich area
[0018] 105S: Bottom surface
[0019] 202, 212: Rewiring layer
[0020] 202A, 212A: Dielectric layer
[0021] 202B, 212B: Conductive layer
[0022] 202-BS, BS: rear surface
[0023] 204: Hole through insulation layer
[0024] 204-Ts, 206-Ts, 208-Ts, 210-Ts: Top surface
[0025] 206: Semiconductor die
[0026] 206a-1: Semiconductor substrate
[0027] 206a-2, 212C: Conductive pad
[0028] 206a-3: Passivation layer
[0029] 206a-4: Conductive column
[0030] 206a-5: Protective layer / polished protective layer
[0031] 207: Die bonding film
[0032] 208: Dipole Antenna
[0033] 210: Insulation material
[0034] 210-S1: First Surface
[0035] 210-S2: Second surface
[0036] 210': Insulation package
[0037] 214: Conductive ball
[0038] 301: Tape
[0039] 302: Framework
[0040] AL: Adhesive layer
[0041] AL1: First adhesive layer
[0042] AL2: Second adhesive layer
[0043] AP: Antenna Pattern
[0044] AS: effective surface
[0045] CR: Carrier
[0046] DB: Debonding layer
[0047] DI: Dielectric layer
[0048] DL: Cutting Line
[0049] IF, IF1, IF2: Interface
[0050] Fx: Filler
[0051] PK1, PK2, PK3: Package structure
[0052] RL: Resin layer
[0053] RL1: First resin layer
[0054] RL2: Second resin layer
[0055] Rx: Resin material / Adhesive resin material
[0056] T1, T2: thickness DETAILED DESCRIPTION
[0057] The following disclosure provides many different embodiments or examples for implementing the different features of the provided subject matter. Specific examples of components, values, operations, materials, arrangements, etc. are described below to simplify the present disclosure. Of course, these are only examples and are not intended to be limiting. It is expected that there are other components, values, operations, materials, arrangements, etc. For example, the following description in which the first feature is formed "on" or "on" the second feature may include an embodiment in which the first feature and the second feature are formed to be in direct contact, and may also include an embodiment in which additional features may be formed between the first feature and the second feature so that the first feature and the second feature may not be in direct contact. In addition, the present disclosure may reuse reference numbers and / or letters in various examples. This repetition is for the purpose of brevity and clarity, rather than indicating the relationship between the various embodiments and / or configurations discussed by itself.
[0058] Additionally, for ease of description, spatially relative terms such as "beneath," "below," "lower," "above," "upper," etc. may be used herein to describe the relationship of one element or feature illustrated in a figure to another (other) element or feature. The spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations), and the spatially relative descriptors used herein may be interpreted accordingly.
[0059] Other features and processes may also be included. For example, a test structure may be included to help perform verification testing on a three-dimensional (3D) package or a three-dimensional integrated circuit (3DIC) device. The test structure may include, for example, a test pad formed in a redistribution layer or on a substrate so that the 3D package or 3DIC can be tested, probes and / or probe cards can be used, etc. Verification testing can be performed on intermediate structures as well as final structures. In addition, the structures and methods disclosed herein can be used in conjunction with a test method that includes intermediate verification of a known good die to improve yield and reduce costs.
[0060] Figure 1A to Figure 1B Schematic cross-sectional views of various stages in a method for manufacturing an insulating film according to some exemplary embodiments of the present disclosure. Figure 1A, a carrier or support 102 is provided. The carrier or support 102 may be any type of carrier or support suitable for forming an insulating film on the carrier or support 102. In one embodiment, the support 102 includes a mold for accommodating and shaping. In some embodiments, a resin material Rx is provided on the support 102. The resin material Rx may include a base material that can harden when heated or cured. For example, the base material of the resin material Rx may be an epoxy resin-based adhesive material, an acrylic resin-based adhesive material, an amino resin-based adhesive material, or a silicone resin-based material, but the present disclosure is not limited thereto. In some embodiments, other types of adhesive materials may be appropriately used as the resin material Rx. As Figure 1A As shown in , the resin material Rx includes a plurality of fillers Fx dispersed in a matrix material of the resin material Rx. The plurality of fillers Fx may be, for example, inorganic particles (e.g., silica particles), metal oxide particles (e.g., Al2O3 particles), etc., but the present disclosure is not limited thereto. The material and / or size of the filler Fx may be selected according to the mechanical properties or electrical properties required by the product. In some embodiments, the filler Fx may be spherical particles and may have various sizes.
[0061] In one embodiment, the viscosity of the resin material Rx is adjusted or reduced by adding one or more solvents. By adding an appropriate amount of solvent or diluent, the viscosity of the resin material Rx becomes lower, so that the dispersed filler Fx can settle and gather in one area or one side of the resin material Rx to define a filler-rich area 104-Fi. For example, when the viscosity becomes lower, the filler Fx settles at the lower side and gathers in the filler-rich area 104-Fi by the action of the gravity, while the upper side with a small amount of filler or no filler becomes a resin-rich area 104-Re. In some embodiments, the viscosity of the resin material Rx is in the range of 1 cP to 40000 cP. In some embodiments, the viscosity of the resin material Rx is adjusted or reduced to 3000 cP or less than 3000 cP. In some embodiments, the viscosity of the resin material Rx is adjusted or reduced to a range of 10 cP to 1500 cP. In some embodiments, the viscosity of the resin material Rx is adjusted or reduced to a range of 10 cP to 500 cP. In one embodiment, the viscosity of the resin material Rx is adjusted with the aid of a solvent. In some embodiments, the viscosity of the resin material Rx is adjusted with the aid of a solvent, and baking is also performed to help the filler Fx precipitate. In another embodiment, the viscosity of the resin material Rx is adjusted using a reactive diluent. In some other embodiments, in addition to adding more diluent, more filler Fx may also be added. However, the present disclosure is not limited thereto, and other suitable methods may be applied to adjust the viscosity or form a resin-rich zone.
[0062] Reference Figure 1B , after adjusting the viscosity and forming a resin-rich region and a filler-rich region in the resin material Rx, a curing process is performed to solidify or harden the resin material Rx, thereby forming an insulating film 104. In an exemplary embodiment, the insulating film 104 contains a resin-rich region 104-Re and a filler-rich region 104-Fi, and the interface IF is located between the resin-rich region 104-Re and the filler-rich region 104-Fi. In some embodiments, the filler-rich region 104-Fi may constitute a resin layer RL, wherein the resin layer RL includes a plurality of fillers Fx. In certain embodiments, the resin-rich region 104-Re may constitute an adhesive layer AL, wherein the adhesive layer AL substantially has no filler or contains very little filler. For example, in one embodiment, the content of the filler Fx in the resin layer RL (filler-rich region 104-Fi) is greater than 80% by weight based on the total weight of the insulating film 104. In certain embodiments, the content of the filler Fx in the adhesive layer AL (resin-rich region 104-Re) is less than 10% by weight based on the total weight of the insulating film 104. In some embodiments, the content of the filler Fx in the adhesive layer AL (resin-rich region 104-Re) is less than 5 wt % based on the total weight of the insulating film 104. In some other embodiments, the content of the filler Fx in the adhesive layer AL (resin-rich region 104-Re) is less than 1 wt % based on the total weight of the insulating film 104.
[0063] In an exemplary embodiment, the resin layer RL (filler-rich area 104-Fi) and the adhesive layer AL (resin-rich area 104-Re) are made of the same resin material Rx. In addition, in some embodiments, the ratio of the thickness T1 of the adhesive layer AL to the thickness T2 of the resin layer RL is in the range of 1:75 to 1:360. For example, in one embodiment, the thickness T1 of the adhesive layer AL (resin-rich area 104-Re) is in the range of 0.5 μm to 2 μm. In some embodiments, the thickness T2 of the resin layer RL (filler-rich area 104-Fi) is in the range of 150 μm to 180 μm. By controlling the ratio (T1 / T2) of the thickness of the resin layer RL (filler-rich area 104-Fi) to the thickness of the adhesive layer AL (resin-rich area 104-Re) within this range, the adhesion strength of the insulating film 104 can be ensured. The insulating film 104 shown in this article can also be peeled off or peeled off from the support 102 as required and the insulating film 104 can be stacked on other structures. At this point, the preparation of the insulating film 104 according to some exemplary embodiments of the present disclosure is completed.
[0064] Figure 1C FIG. 1 is an enlarged view of an insulating film 104 stacked on a dielectric layer DI according to some exemplary embodiments of the present disclosure. Figure 1C As shown in , for example, Figure 1BThe insulating film 104 obtained in the above step is laminated or attached to the dielectric layer DI (or any other type of adherent). Figure 1C In the enlarged view shown in, in some embodiments, the interface IF between the resin-rich region 104-Re (adhesion layer AL) and the filler-rich region 104-Fi (resin layer RL) is an unsmooth interface. For example, the profile of the interface IF between the resin-rich region 104-Re and the filler-rich region 104-Fi may be granular and contain gravel. In certain embodiments, the interface IF has a wavy profile (unsmooth profile). In some embodiments, since the interface IF is defined along the surface of the stacked filler Fx, the profile of the interface IF between the resin-rich region 104-Re and the filler-rich region 104-Fi is basically defined by the arrangement and configuration of the filler Fx in the filler-rich region 104-Fi (resin layer RL), and is uneven and unsmooth. In some embodiments, when compared with the interface IF, the bottom surface 105S of the insulating film 104 is a relatively smooth surface. That is, the bottom surface 105S of the insulating film 104 (or the interface between the insulating film 104 and the dielectric layer DI) has a roughness less than the roughness of the interface IF. In some embodiments, the bottom surface 105S of the insulating film 104 has a surface roughness of about 0.1 μm to 1 μm. In addition, in some embodiments, the bottom surface 105S of the insulating film 104 (or the interface between the insulating film 104 and the dielectric layer DI) has a substantially linear profile.
[0065] Figures 2A to 2H Schematic cross-sectional views of various stages in a method for manufacturing a package structure according to some exemplary embodiments of the present disclosure. Figure 2A In some embodiments, a carrier CR is provided. In some embodiments, the carrier CR may be a glass carrier or any carrier suitable for carrying a semiconductor wafer or a reconstituted wafer for a method of manufacturing a package structure. In some embodiments, the carrier CR is coated with a peeling layer DB. The material of the peeling layer DB may be any material suitable for bonding and peeling the carrier CR relative to an upper layer or any wafer disposed on the carrier CR.
[0066] In some embodiments, the peeling layer DB may include a dielectric material layer made of a dielectric material (including any suitable polymer-based dielectric material, such as benzocyclobutene (BCB), polybenzoxazole (PBO)). In an alternative embodiment, the peeling layer DB may include a dielectric material layer made of an epoxy-based thermal release material (e.g., a light-to-heat-conversion (LTHC) release coating film) that loses its adhesive properties when heated. In another alternative embodiment, the peeling layer DB may include a dielectric material layer made of an ultraviolet (UV) glue that loses its adhesive properties when exposed to ultraviolet (UV) light. In certain embodiments, the peeling layer DB may be dispensed in liquid form and cured, or may be a laminated film laminated to the carrier CR, or may be a similar material. The top surface of the peeling layer DB opposite to the bottom surface contacting the carrier CR may be flattened and may have a high degree of coplanarity. In certain embodiments, the release layer DB is, for example, a LTHC layer having good chemical resistance, and such a layer can be released from the carrier CR at room temperature by applying laser irradiation, but the present disclosure is not limited thereto.
[0067] In an alternative embodiment, a buffer layer (not shown) may be coated on the peeling layer DB, wherein the peeling layer DB is sandwiched between the buffer layer and the carrier CR, and the top surface of the buffer layer may also provide a high degree of coplanarity. In some embodiments, the buffer layer may be a dielectric material layer. In some embodiments, the buffer layer may be a polymer layer made of polyimide, PBO, BCB, or any other suitable polymer-based dielectric material. In some embodiments, the buffer layer may be an Ajinomoto Buildup Film (ABF), a Solder Resist (SR) film, or a similar film. In other words, the buffer layer is optional and may be omitted as needed, so the present disclosure is not limited thereto.
[0068] In addition, if Figure 2A As shown in FIG. 1 , a redistribution layer 202 is formed on the carrier CR. For example, Figure 2A In some embodiments, the redistribution layer 202 is formed on the stripping layer DB, and the formation of the redistribution layer 202 includes sequentially forming one or more dielectric layers 202A and one or more conductive layers 202B alternately. In some embodiments, the redistribution layer 202 includes two dielectric layers 202A and one conductive layer 202B. Figure 2A, where the conductive layer 202B is sandwiched between the dielectric layers 202A. However, the present disclosure is not limited thereto. The number of dielectric layers 202A and conductive layers 202B included in the redistribution layer 202 is not limited thereto, and can be specified and selected as needed. For example, the number of dielectric layers 202A and conductive layers 202B can be one or more than one.
[0069] In some embodiments, the material of the dielectric layer 202A may be polyimide, polybenzoxazole (PBO), benzocyclobutene (BCB), nitride (e.g., silicon nitride), oxide (e.g., silicon oxide), phosphosilicate glass (PSG), borosilicate glass (BSG), boron-doped phosphosilicate glass (BPSG), or a combination thereof, which can be patterned by photolithography and / or etching processes. In some embodiments, the material of the dielectric layer 202A may be formed by a suitable fabrication technique, such as spin-on coating, chemical vapor deposition (CVD), or plasma-enhanced chemical vapor deposition (PECVD). The present disclosure is not limited thereto.
[0070] In some embodiments, the material of the conductive layer 202B may be made of a conductive material (e.g., aluminum, titanium, copper, nickel, tungsten, and / or alloys thereof) formed by electroplating or deposition and may be patterned using photolithography and etching processes. In some embodiments, the conductive layer 202B may be a patterned copper layer or other suitable patterned metal layer. Throughout this specification, the term "copper" is intended to include substantially pure elemental copper, copper containing unavoidable impurities, and copper alloys containing small amounts of elements such as tantalum, indium, tin, zinc, manganese, chromium, titanium, germanium, strontium, platinum, magnesium, aluminum, or zirconium.
[0071] Reference Figure 2B, after forming the redistribution layer 202, at least one semiconductor die 206 and a plurality of through-insulation layer holes 204 are provided on the redistribution layer 202 on the carrier CR. In some embodiments, the through-insulation layer holes 204 are integrated fan-out ("InFO") through-holes. In one embodiment, forming the through-insulation layer holes 204 includes: forming a mask pattern (not shown) having an opening; then forming a metal material (not shown) filling the opening by electroplating or deposition; and removing the mask pattern to form the through-insulation layer holes 204 on the redistribution layer 202. In some embodiments, the through-insulation layer holes 204 are filled into the through-hole openings that expose the conductive layer 202B of the redistribution layer 202, so that the through-insulation layer holes 204 can be electrically connected to the redistribution layer 202. In some embodiments, the material of the mask pattern may include positive photoresist or negative photoresist. In one embodiment, the material of the through-insulation layer holes 204 may include a metal material, such as copper or a copper alloy. However, the present disclosure is not limited thereto.
[0072] In an alternative embodiment, the through-insulation layer hole 204 may be formed by: forming a seed layer (not shown) on the redistribution layer 202; forming a mask pattern having an opening that exposes a portion of the seed layer; forming a metal material on the exposed portion of the seed layer by plating to form the through-insulation layer hole 204; removing the mask pattern; and then removing the portion of the seed layer exposed by the through-insulation layer hole 204. For example, the seed layer may be a titanium / copper composite layer. For simplicity, in Figure 2B Only two through-insulation layer holes 204 are shown. However, it should be noted that the number of through-insulation layer holes 204 is not limited thereto and can be selected according to requirements.
[0073] In addition, in some embodiments, during the formation of the through-insulation layer hole 204, at least one dipole antenna 208 may be formed. In some embodiments, the size (e.g., width) of the dipole antenna 208 is larger than the size (e.g., width) of the through-insulation layer hole 204. However, the present disclosure is not limited thereto. In alternative embodiments, the size (e.g., width) of the dipole antenna 208 is substantially equal to or smaller than the size (e.g., width) of the through-insulation layer hole 204. For example, the dipole antenna 208 may be disposed on the redistribution layer 202 and may be adjacent to the through-insulation layer hole 204.
[0074] like Figure 2BAs shown in , at least one semiconductor die 206 is picked up and placed on the redistribution layer 202. In some embodiments, the semiconductor die 206 has an active surface AS and a backside surface BS opposite to the active surface AS. For example, the backside surface BS of the semiconductor die 206 can be attached to the redistribution layer 202 by a die attach film 207. The use of the die attach film 207 ensures better adhesion between the semiconductor die 206 and the redistribution layer 202. In the exemplary embodiment, only one semiconductor die 206 is shown. However, it should be noted that the number of semiconductor dies placed on the redistribution layer 202 is not limited thereto, and this can be adjusted according to design requirements.
[0075] In an exemplary embodiment, the semiconductor die 206 includes a semiconductor substrate 206a-1, a plurality of conductive pads 206a-2, a passivation layer 206a-3, a plurality of conductive pillars 206a-4, and a protective layer 206a-5. Figure 2B As shown in , the plurality of conductive pads 206a-2 are disposed on a semiconductor substrate 206a-1. A passivation layer 206a-3 is formed on the semiconductor substrate 206a-1 and has an opening, wherein the opening partially exposes the conductive pads 206a-2 on the semiconductor substrate 206a-1. The semiconductor substrate 206a-1 may be a bulk silicon substrate or a silicon-on-insulator (SOI) substrate, and further includes active components (e.g., transistors, etc.) formed in the semiconductor substrate 206a-1 and passive components (e.g., resistors, capacitors, inductors, etc.) as required. The conductive pad 206a-2 may be an aluminum pad, a copper pad, or other suitable metal pad. The passivation layer 206a-3 may be a silicon oxide layer, a silicon nitride layer, a silicon oxynitride layer, or a dielectric layer formed of any suitable dielectric material. In addition, in some embodiments, a post-passivation layer (not shown) is formed on the passivation layer 206a-3 as required. The back passivation layer covers the passivation layer 206a-3 and has a plurality of contact openings. The conductive pad 206a-2 is partially exposed by the contact openings of the back passivation layer. The back passivation layer may be a benzocyclobutene (BCB) layer, a polyimide layer, a polybenzoxazole (PBO) layer, or a dielectric layer formed by other suitable polymers. In some embodiments, the conductive column 206a-4 is formed on the conductive pad 206a-2 by plating. In some embodiments, the protective layer 206a-5 is formed on the passivation layer 206a-3 or on the back passivation layer, and covers the conductive column 206a-4 to protect the conductive column 206a-4.
[0076] In some embodiments, when more than one semiconductor die 206 is placed on the redistribution layer 202, the semiconductor die 206 may be arranged in an array, and when the semiconductor die 206 is arranged in an array, the through-insulation layer holes 204 may be classified into groups. The number of semiconductor dies 206 may correspond to the number of groups of through-insulation layer holes 204. In an exemplary embodiment, after the through-insulation layer holes 204 are formed, the semiconductor die 206 may be picked up and placed on the redistribution layer 202. However, the present disclosure is not limited thereto. In some alternative embodiments, the semiconductor die 206 may be picked up and placed on the redistribution layer 202 before the through-insulation layer holes 204 are formed.
[0077] In some embodiments, the semiconductor die 206 may be selected from the following chips: an application-specific integrated circuit (ASIC) chip, an analog chip (e.g., a wireless and radio frequency chip), a digital chip (e.g., a baseband chip), an integrated passive device (IPD), a voltage regulator chip, a sensor chip, a memory chip, etc. The present disclosure is not limited thereto.
[0078] Reference Figure 2C , an insulating material 210 is formed on the redistribution layer 202 and above the semiconductor die 206. In some embodiments, the insulating material 210 is formed by, for example, a compression molding process and fills the gap between the semiconductor die 206 and the through-insulation layer hole 204 to encapsulate the semiconductor die 206. The insulating material 210 also fills the gap between the adjacent through-insulation layer hole 204 and the dipole antenna 208 to encapsulate the through-insulation layer hole 204 and the dipole antenna 208. The conductive pillars 206a-4 and the protective layer 206a-5 of the semiconductor die 206 are encapsulated and fully protected by the insulating material 210. In other words, the conductive pillars 206a-4 and the protective layer 206a-5 of the semiconductor die 206 are not exposed but are fully protected by the insulating material 210.
[0079] In some embodiments, the insulating material 210 includes a polymer (e.g., epoxy resin, phenolic resin, silicone resin, or other suitable resin), a dielectric material with low permittivity (Dk) and low loss tangent (Df) properties, or other suitable materials. In alternative embodiments, the insulating material 210 may include an acceptable insulating package material. In some embodiments, the insulating material 210 may also include an inorganic filler or inorganic compound (e.g., silica, clay, etc.) that can be added to the insulating material 210 to optimize the coefficient of thermal expansion (CTE) of the insulating material 210. The present disclosure is not limited thereto.
[0080] Reference Figure 2D In some embodiments, the insulating material 210 is partially removed to expose the conductive pillar 206a-4, the through-insulating layer hole 204, and the dipole antenna 208. In some embodiments, the insulating material 210 and the protective layer 206a-5 are ground or polished by a planarization step. For example, the planarization step is performed by a mechanical grinding process and / or a chemical mechanical polishing (CMP) process until the top surface 206-Ts of the conductive pillar 206a-4 is exposed. In some embodiments, the through-insulating layer hole 204 can be partially polished so that the top surface 204-Ts of the through-insulating layer hole 204 is flush with the top surface 206-Ts of the conductive pillar 206a-4, or flush with the active surface AS of the semiconductor die 206. Similarly, the dipole antenna 208 may be partially polished so that the top surface 208-Ts of the dipole antenna 208 is flush with the top surface 206-Ts of the conductive pillar 206a-4, or flush with the active surface AS of the semiconductor die 206. In other words, the conductive pillar 206a-4, the through-insulation layer via 204, and the dipole antenna 208 may also be lightly ground / polished.
[0081] In the illustrated embodiment, the insulating material 210 is polished to form an insulating package body 210'. In some embodiments, the top surface 210-Ts of the insulating package body 210', the top surface 204-Ts of the through-insulating layer hole 204, the top surface 206-Ts of the conductive pillar 206a-4, the top surface of the polished protective layer 206a-5, and the top surface 208-Ts of the dipole antenna 208 are coplanar and flush with each other. In some embodiments, after the mechanical grinding or chemical mechanical polishing (CMP) step is performed, a cleaning step may be performed as needed. For example, a cleaning step is performed to clean and remove residues generated from the planarization step. However, the present disclosure is not limited thereto, and the planarization step may be performed by any other suitable method.
[0082] Reference Figure 2E After the planarization step, a redistribution layer 212 is formed on the insulating package 210', the through-insulating layer hole 204, the dipole antenna 208, and the semiconductor die 206. For example, the redistribution layer 212 is formed on the top surface 204-Ts of the through-insulating layer hole 204, the top surface 206-Ts of the conductive pillar 206a-4, and the top surface 210-Ts of the insulating package 210'. In some embodiments, the redistribution layer 212 is electrically connected to the through-insulating layer hole 204, and is electrically connected to the semiconductor die 206 through the conductive pillar 206a-4. In some embodiments, the semiconductor die 206 is electrically connected to the through-insulating layer hole 204 through the redistribution layer 212. In certain embodiments, the redistribution layer 212 is electrically connected to the dipole antenna 208. In the illustrated embodiment, the insulating package 210' has a first surface 210-S1 and a second surface 210-S2, wherein the second surface 210-S2 is opposite to the first surface 210-S1. The redistribution layer 202 is located on the second surface 210 - S2 of the insulating package body 210 ′, and the redistribution layer 212 is located on the first surface 210 - S1 of the insulating package body 210 ′.
[0083] In some embodiments, forming the redistribution layer 212 includes sequentially forming one or more dielectric layers 212A and one or more conductive layers 212B that alternate with each other. In some embodiments, the conductive layer 212B is sandwiched between the dielectric layers 212A. Although only two conductive layers 212B and three dielectric layers 212A are shown herein, the scope of the present disclosure is not limited by the embodiments of the present disclosure. In other embodiments, the number of conductive layers 212B and dielectric layers 212A can be adjusted according to product requirements. In some embodiments, the conductive layer 212B is electrically connected to the conductive pillars 206a-4 of the semiconductor die 206. In addition, the conductive layer 212B is electrically connected to the through-insulation layer hole 204 and the dipole antenna 208. In some embodiments, the materials of the dielectric layer 212A and the conductive layer 212B of the redistribution layer 212 are similar to the materials of the dielectric layer 202A and the conductive layer 202B described for the redistribution layer 202. Therefore, the dielectric layer 212A and the conductive layer 212B will not be described in detail herein.
[0084] After forming the redistribution layer 212, a plurality of conductive pads 212C may be disposed on the exposed top surface of the topmost layer of the conductive layer 212B to electrically connect to the conductive balls. In some embodiments, the conductive pads 212C are, for example, under-ball metallurgy (UBM) patterns for ball mounting. Figure 2E As shown in , the conductive pad 212C is formed on the redistribution layer 212 and is electrically connected to the redistribution layer 212. In some embodiments, for example, the material of the conductive pad 212C may include copper, nickel, titanium, tungsten or an alloy thereof, and may be formed by an electroplating process. The number of the conductive pads 212C is not limited in the present disclosure and may be selected according to the design layout. In some alternative embodiments, the conductive pad 212C may be omitted. In other words, the conductive ball 214 formed in a subsequent step may be directly disposed on the redistribution layer 212.
[0085] After forming the conductive pad 212C, a plurality of conductive balls 214 are disposed on the conductive pad 212C and on the redistribution layer 212. In some embodiments, the conductive balls 214 may be disposed on the conductive pad 212C by a ball placement process or a reflow process. In some embodiments, the conductive balls 214 are, for example, solder balls or ball grid array (BGA) balls. In some embodiments, the conductive balls 214 are connected to the redistribution layer 212 through the conductive pad 212C. In certain embodiments, some of the conductive balls 214 may be electrically connected to the semiconductor die 206 through the redistribution layer 212. In addition, some of the conductive balls 214 may be electrically connected to the through-insulation layer via 204 through the redistribution layer 212. The number of the conductive balls 214 is not limited to the present disclosure and may be specified and selected according to the number of the conductive pads 212C. In some alternative embodiments, an integrated passive device (IPD) (not shown) may be disposed on the redistribution layer 212 and electrically connected to the redistribution layer 212 as desired.
[0086] Reference Figure 2F In some embodiments, after forming the redistribution layer 212 and the conductive balls 214, Figure 2E The structure shown in FIG. 3 is turned upside down and attached to a tape 301 (eg, dicing tape) supported by a frame 302. Figure 2F As shown in , the carrier CR is peeled off and separated from the redistribution layer 202. In some embodiments, the peeling process includes projecting light (e.g., laser light or UV light) on the peeling layer DB (e.g., LTHC release layer) so that the carrier CR can be easily removed together with the peeling layer DB. During the peeling step, before peeling the carrier CR and the peeling layer DB, a tape 301 is used to fix the package structure. After the peeling process, the back side surface 202-BS of the redistribution layer 202 is revealed or exposed. In some embodiments, the dielectric layer 202A of the redistribution layer 202 is revealed or exposed.
[0087] Reference Figure 2G In the next step, the first insulating film 104A is laminated on the redistribution layer 202 to cover the exposed backside surface 202-BS of the redistribution layer 202. In some embodiments, the first insulating film 104A is laminated on the redistribution layer 202 by a vacuum laminator. In addition, in some embodiments, after lamination, the first insulating film 104A is cured at a temperature range of 150° C. to 180° C. so that the first insulating film 104A can be properly adhered to the redistribution layer 202. In an exemplary embodiment, a first insulating film 104A is laminated on the redistribution layer 202 to cover the exposed backside surface 202-BS of the redistribution layer 202. In some embodiments, the first insulating film 104A is laminated on the redistribution layer 202 by a vacuum laminator. In some embodiments, the first insulating film 104A is cured at a temperature range of 150° C. to 180° C. so that the first insulating film 104A can be properly adhered to the redistribution layer 202. Figure 1A , Figure 1BThe first insulating film 104A is prepared by the same method as described for the insulating film 104 in the above, and the first insulating film 104A has Figure 1C Similar arrangement. In other words, the first insulating film 104A contains a resin-rich area 104-Re and a filler-rich area 104-Fi. In some embodiments, the filler-rich area 104-Fi may constitute a first resin layer RL1, wherein the first resin layer RL1 includes a plurality of fillers Fx. In certain embodiments, the resin-rich area 104-Re may constitute a first adhesive layer AL1, wherein the first adhesive layer AL1 substantially has no filler. In addition, the interface IF1 is located between the resin-rich area 104-Re and the filler-rich area 104-Fi. The thickness ratio of the first adhesive layer AL1 to the first resin layer RL1 is the same as the thickness ratio described for the adhesive layer AL and the resin layer RL. In addition, the details of the resin material Rx and the filler Fx used in the first insulating film 104A are the same as the details of the resin material Rx and the filler Fx used in the insulating film 104, and will not be repeated herein.
[0088] like Figure 2G As shown in , the resin-rich region 104-Re (first adhesive layer AL1) is sandwiched between the filler-rich region 104-Fi (first resin layer RL1) and the redistribution layer 202. In some embodiments, the resin-rich region 104-Re (first adhesive layer AL1) separates the filler-rich region 104-Fi (first resin layer RL1) from the redistribution layer 202. In addition, the resin-rich region 104-Re (first adhesive layer AL1) physically contacts the dielectric layer 202A of the redistribution layer 202. In some embodiments, the contact surface between the resin-rich region 104-Re (first adhesive layer AL1) and the dielectric layer 202A does not have the filler Fx. In other words, the contact surface between the resin-rich region 104-Re (first adhesive layer AL1) and the dielectric layer 202A is substantially planar.
[0089] After the first insulating film 104A is stacked on the redistribution layer 202, a plurality of antenna patterns AP are formed on the first insulating film 104A. The first insulating film 104A is located, for example, between the antenna pattern AP and the redistribution layer 202. Figure 2GAs shown in , the antenna pattern AP is formed on the surface of the first insulating film 104A opposite to the side where the redistribution layer 202 is located. In some embodiments, the antenna pattern AP is electrically coupled to some of the conductive layers 202B of the redistribution layer 202, wherein the conductive layers 202B can be used as ground planes. In certain embodiments, the antenna pattern AP can be electrically connected to some of the conductive layers 202B of the redistribution layer 202 through a feed line (not shown), but the present disclosure is not limited thereto. In some embodiments, the antenna pattern AP is formed by forming a metallization layer (not shown) by electroplating or deposition on the first insulating film 104A and then patterning the metallization layer by photolithography and etching processes. In an alternative embodiment, the antenna pattern AP is formed by forming a metallization layer (not shown) using a plating process. In some embodiments, the antenna pattern AP may include a patch antenna.
[0090] Reference Figure 2H After forming the antenna pattern AP, along the cutting line DL (at Figure 2G The wafer structure PK1 is cut into a plurality of package structures PK1 by performing a cutting process (shown in FIG. 1 ) to cut the entire wafer structure (cut through the first insulating film 104A, the insulating package body 210', and the redistribution layers 202 and 212). In an exemplary embodiment, the cutting process is a wafer dicing process including mechanical blade sawing or laser cutting. In subsequent processes, the separated package structures PK1 can be set on a circuit substrate or on other components as required.
[0091] Figures 3A to 3G Schematic cross-sectional views of various stages in a method for manufacturing a package structure according to some exemplary embodiments of the present disclosure. Figures 3A to 3G The method of making the package structure shown in Figures 2A to 2H Therefore, the same reference numerals will be used to refer to the same or similar components, and they will not be described in detail herein. The difference between the embodiments lies in the order of the manufacturing process.
[0092] Reference Figure 3A , a resin material Rx is provided on a peeling layer DB on a carrier CR, and a plurality of fillers Fx are dispersed in the resin material Rx. Figure 3B, adjust or reduce the viscosity of the resin material Rx to form the first insulating film 104A. For example, the viscosity of the resin material Rx is adjusted or reduced so that the dispersed fillers Fx can be gathered on one side of the resin material Rx to define the filler-rich area 104-Fi (first resin layer RL1) and the resin-rich area 104-Re (first adhesive layer AL1). The filler-rich area 104-Fi (first resin layer RL1) is, for example, located between the resin-rich area 104-Re (first adhesive layer AL1) and the peeling layer DB, and an interface IF1 exists between the filler-rich area 104-Fi (first resin layer RL1) and the resin-rich area 104-Re (first adhesive layer AL1).
[0093] Reference Figure 3C , a redistribution layer 202 is formed on the first insulating film 104A. For example, the dielectric layer 202A of the redistribution layer 202 is adhered to the resin-rich region 104-Re (first adhesive layer AL1) of the first insulating film 104A. Figure 3D After forming the redistribution layer 202, the same processing steps may be performed to dispose a semiconductor die 206 on the redistribution layer 202, and to form a through-insulation layer hole 204 and a dipole antenna 208 on the redistribution layer 202. Thereafter, an insulating material 210 is formed on the redistribution layer 202 to cover the semiconductor die 206, the through-insulation layer hole 204, and the dipole antenna 208.
[0094] Reference Figure 3E In a subsequent step, the insulating material 210 is planarized to form an insulating package 210'. Afterwards, a redistribution layer 212 is formed on the insulating package 210', the through-insulating layer hole 204, the dipole antenna 208, and the semiconductor die 206. For example, the redistribution layer 212 is electrically connected to the through-insulating layer hole 204, the semiconductor die 206, and the dipole antenna 208. Subsequently, a plurality of conductive pads 212C may be disposed on the redistribution layer 212 and the plurality of conductive pads 212C may be electrically connected to the conductive layer 212B. Then, a conductive ball 214 may be disposed on the conductive pad 212C by a ball implantation process or a reflow process.
[0095] Reference Figure 3F After forming the redistribution layer 212 and the conductive balls 214, Figure 3E The structure shown in FIG is turned upside down and attached to a tape supported by a frame (not shown). Subsequently, the carrier CR is peeled off and separated from the first insulating film 104A to reveal the back side of the first insulating film 104A. For example, the peeling process includes projecting light (such as laser or UV light) on the peeling layer DB (for example, LTHC release layer) so that the carrier CR can be easily removed together with the peeling layer DB. After the peeling process, a plurality of antenna patterns AP are then formed on the first insulating film 104A.
[0096] Reference Figure 3G After forming the antenna pattern AP, along the cutting line DL (at Figure 3F The wafer structure PK1 is cut into a plurality of package structures PK1 by performing a cutting process (shown in FIG. 1 ) to cut the entire wafer structure (cut through the first insulating film 104A, the insulating package body 210', and the redistribution layers 202 and 212). In an exemplary embodiment, the cutting process is a wafer cutting process including mechanical blade sawing or laser cutting. In subsequent processes, the separated package structures PK1 can be set on a circuit substrate or on other components as required.
[0097] Figure 4 This is a packaging structure according to some embodiments of the present disclosure. Figure 4 The package structure PK2 shown in FIG. is similar to Figure 2H and Figure 3G Therefore, the same reference numerals will be used to refer to the same or similar components, and they will not be described in detail herein. The difference between the embodiments is that a second insulating film 104B is further provided.
[0098] like Figure 4 As shown in FIG. 1 , after laminating the first insulating film 104A on the redistribution layer 202, the second insulating film 104B is laminated on the first insulating film 104A. In some embodiments, the second insulating film 104B is laminated on the first insulating film 104A by a vacuum laminator. In addition, in some embodiments, after lamination, the second insulating film 104B is cured at a temperature range of 150° C. to 180° C. so that the second insulating film 104B can be properly adhered to the first insulating film 104A. In an exemplary embodiment, a method for Figure 1A , Figure 1B The second insulating film 104B is prepared by the same method as described for the insulating film 104 in the above, and the second insulating film 104B has Figure 1CSimilar arrangement. In other words, the second insulating film 104B contains a resin-rich area 104-Re and a filler-rich area 104-Fi. In some embodiments, the filler-rich area 104-Fi may constitute a second resin layer RL2, wherein the second resin layer RL2 includes a plurality of fillers Fx. In certain embodiments, the resin-rich area 104-Re may constitute a second adhesive layer AL2, wherein the second adhesive layer AL2 does not substantially have a filler. In addition, the interface IF2 is located between the resin-rich area 104-Re (the second adhesive layer AL2) and the filler-rich area 104-Fi (the second resin layer RL2). The thickness ratio of the second adhesive layer AL2 to the second resin layer RL2 is the same as the thickness ratio described for the adhesive layer AL and the resin layer RL. In addition, the details of the resin material Rx and the filler Fx used in the second insulating film 104B are the same as the details of the resin material Rx and the filler Fx used in the insulating film 104, and will not be repeated herein.
[0099] In addition, if Figure 4 As shown in , the resin-rich region 104-Re (second adhesive layer AL2) is sandwiched between the filler-rich region 104-Fi (second resin layer RL2) of the second insulating film 104B and the filler-rich region 104-Fi (first resin layer RL1) of the first insulating film 104A. In addition, the resin-rich region 104-Re (second adhesive layer AL2) of the second insulating film 104B physically contacts the filler-rich region 104-Fi (first resin layer RL1) of the first insulating film 104A. Although only two insulating films (104A / 104B) are shown herein, the present disclosure is not limited to this. In some other embodiments, more than two insulating films may be provided on the redistribution layer 202, wherein the insulating films are adhered to each other through the resin-rich region (adhesive layer). In some embodiments, the plurality of antenna patterns AP are provided on the second insulating film 104B. In some embodiments, the second insulating film 104B is sandwiched between the antenna pattern AP and the first insulating film 104A.
[0100] Figure 5 Detailed description of the invention The invention relates to a packaging structure according to some other embodiments of the present invention. Figure 5 The package structure PK3 shown in Figure 4 Therefore, the same reference numerals will be used to refer to the same or similar components, and they will not be described in detail herein. Figure 5 The resin rich region 104-Re (second adhesive layer AL2) of the second insulating film 104B is omitted.
[0101] like Figure 5As shown in , after stacking the first insulating film 104A on the redistribution layer 202, the second insulating film 104B is stacked on the first insulating film 104A. In an exemplary embodiment, the second insulating film 104B contains a filler-rich region 104-Fi (second resin layer RL2), and the resin-rich region is omitted. For example, the filler-rich region 104-Fi (second resin layer RL2) of the second insulating film 104B physically contacts the filler-rich region 104-Fi (first resin layer RL1) of the first insulating film 104A. Since both the filler-rich region 104-Fi of the first insulating film 104A and the filler-rich region 104-Fi of the second insulating film 104B contain an adhesive resin material Rx, the first insulating film 104A and the second insulating film 104B can still be fully adhered to each other. However, there is a resin-rich region 104-Re (first adhesive layer AL1) in the first insulating film 104A to prevent delamination between the redistribution layer 202 and the first insulating film 104A.
[0102] According to the above embodiments, since the package structure includes an insulating film having a filler-rich area (resin layer having a filler) and a resin-rich area (adhesive layer), the insulating film can have a higher adhesion strength to the redistribution layer. In addition, it is not necessary to further modify the material or surface treat the redistribution layer to improve the adhesion strength. Therefore, by using an insulating film with such a design, the delamination problem between the insulating film and the redistribution layer caused by the stress caused by the CTE (thermal expansion coefficient) mismatch of various materials can be solved. In addition, due to the improved adhesion strength, the package structure can withstand bending stress during thermal cycle testing without delamination.
[0103] In some embodiments of the present disclosure, a packaging structure is provided, the packaging structure comprising at least one semiconductor die, an insulating package, a first redistribution layer, a second redistribution layer, a plurality of antenna elements and a first insulating film. The insulating package encapsulates the at least one semiconductor die, and the insulating package has a first surface and a second surface opposite to the first surface. The first redistribution layer is disposed on the first surface of the insulating package. The second redistribution layer is disposed on the second surface of the insulating package. The plurality of antenna elements are located on the second redistribution layer. The first insulating film is disposed between the second redistribution layer and the plurality of antenna elements, wherein the first insulating film comprises a resin-rich region and a filler-rich region, the resin-rich region is located between the filler-rich region and the second redistribution layer and separates the filler-rich region from the second redistribution layer.
[0104] In some embodiments, the resin-rich region physically contacts the dielectric layer of the second redistribution layer. In some embodiments, the content of filler in the resin-rich region is less than 5 weight percent based on the total weight of the first insulating film. In some embodiments, the content of filler in the filler-rich region is greater than 80 weight percent based on the total weight of the first insulating film. In some embodiments, the ratio of the thickness of the resin-rich region to the thickness of the filler-rich region is in the range of 1:75 to 1:360. In some embodiments, the packaging structure further includes a second insulating film disposed between the first insulating film and the plurality of antenna elements. In some embodiments, the second insulating film includes a resin-rich region and a filler-rich region, and the resin-rich region of the second insulating film is located between the filler-rich region of the second insulating film and the first insulating film.
[0105] In some other embodiments of the present disclosure, a packaging structure is provided, the packaging structure comprising an insulating package body, at least one semiconductor die, a first redistribution layer, a second redistribution layer, a plurality of antenna elements, a first resin layer and a first adhesive layer. The insulating package body has a first surface and a second surface opposite to the first surface. The at least one semiconductor die is embedded in the insulating package body. The first redistribution layer is arranged on the first surface of the insulating package body. The second redistribution layer is arranged on the second surface of the insulating package body. The plurality of antenna elements are located above the second redistribution layer. The first resin layer is arranged between the second redistribution layer and the plurality of antenna elements, wherein the first resin layer contains filler. The first adhesive layer is arranged between the first resin layer and the second redistribution layer, wherein the first adhesive layer and the first resin layer are made of the same resin material.
[0106] In some embodiments, the first adhesive layer physically contacts the dielectric layer of the second redistribution layer, and the interface between the dielectric layer and the first adhesive layer has a substantially linear profile, and the interface between the first adhesive layer and the first resin layer has an uneven profile. In some embodiments, the content of the filler in the first resin layer is greater than 80% by weight based on the total weight of the first resin layer and the first adhesive layer. In some embodiments, the ratio of the thickness of the first adhesive layer to the thickness of the first resin layer is in the range of 1:75 to 1:360. In some embodiments, a second resin layer is further included between the first resin layer and the plurality of antenna elements, wherein the second resin layer contains filler. In some embodiments, a second adhesive layer is further included between the first resin layer and the second resin layer, wherein the second adhesive layer and the second resin layer are made of the same resin material. In some embodiments, the package structure further includes at least one dipole antenna embedded in the insulating package body.
[0107] In another embodiment of the present disclosure, a method for making a packaging structure is described. The method includes the following steps. A bottom redistribution layer is formed on a carrier. At least one semiconductor die is placed on the bottom redistribution layer. An insulating package is formed to encapsulate the at least one semiconductor die. A top redistribution layer is formed on the insulating package. The carrier is peeled off to reveal the rear surface of the bottom redistribution layer. A first insulating film is stacked on the rear surface of the bottom redistribution layer, wherein the first insulating film includes a resin-rich region and a filler-rich region, the resin-rich region is located between the filler-rich region and the bottom redistribution layer and separates the filler-rich region from the second redistribution layer. A plurality of antenna elements are provided on the first insulating film.
[0108] In some embodiments, the first insulating film having the filler-rich region and the resin-rich region is preformed by reducing the viscosity of the resin material to a range of 10 cP to 500 cP to form the first insulating film, so that the filler gathers on one side of the resin material to define the filler-rich region and the resin-rich region. In some embodiments, the first insulating film is laminated on the bottom redistribution layer by a vacuum laminator. In some embodiments, the method for making a packaging structure further includes: curing the first insulating film at a temperature range of 150° C. to 180° C. after lamination. In some embodiments, the method for making a packaging structure further includes: laminating a second insulating film on the first insulating film before providing the plurality of antenna elements; and providing the plurality of antenna elements on the second insulating film. In some embodiments, the second insulating film includes a filler-rich region and a resin-rich region, and the second insulating film is preformed by reducing the viscosity of the resin material to a range of 10 cP to 500 cP to form the second insulating film, so that the filler gathers on one side of the resin material to define the filler-rich region and the resin-rich region in the second insulating film.
[0109] The features of several embodiments are summarized above so that those skilled in the art can better understand the various aspects of the present disclosure. Those skilled in the art will understand that they can easily use the present disclosure as a basis for designing or modifying other processes and structures to implement the same purposes and / or achieve the same advantages as the embodiments described herein. Those skilled in the art will also recognize that these equivalent constructions do not depart from the spirit and scope of the present disclosure, and that they can make various changes, substitutions and modifications to them without departing from the spirit and scope of the present disclosure.
Claims
1. A packaging structure, comprising: at least one semiconductor die; an insulating package encapsulating the at least one semiconductor die, the insulating package having a first surface and a second surface opposite to the first surface; A first redistribution layer is disposed on the first surface of the insulating package; A second redistribution layer is disposed on the second surface of the insulating package; A plurality of antenna elements are located on the second redistribution layer; as well as A first insulating film is arranged between the second redistribution layer and the multiple antenna elements, wherein the first insulating film includes a resin-rich area and a filler-rich area, the resin-rich area is located between the filler-rich area and the second redistribution layer and separates the filler-rich area from the second redistribution layer, wherein the ratio of the thickness of the resin-rich area to the thickness of the filler-rich area is in the range of 1:75 to 1:
360. 2 . The package structure according to claim 1 , wherein the resin-rich region physically contacts the dielectric layer of the second redistribution layer. 3 . The package structure according to claim 1 , wherein a content of the filler in the resin-rich region is less than 5 wt % based on a total weight of the first insulating film. 4 . The package structure according to claim 1 , wherein the content of the filler in the filler-rich region is greater than 80 wt % based on the total weight of the first insulating film. 5 . The package structure according to claim 1 , further comprising a second insulating film provided between the first insulating film and the plurality of antenna elements. 6 . The package structure according to claim 5 , wherein the second insulating film comprises a resin-rich region and a filler-rich region, and the resin-rich region of the second insulating film is located between the filler-rich region of the second insulating film and the first insulating film. 7 . The package structure according to claim 1 , further comprising a plurality of through-insulation-layer holes embedded in the insulating package body and surrounding the at least one semiconductor die.
8. A packaging structure, comprising: An insulating package body having a first surface and a second surface opposite to the first surface; at least one semiconductor die embedded in the insulating package; A first redistribution layer is disposed on the first surface of the insulating package; A second redistribution layer is disposed on the second surface of the insulating package; A plurality of antenna elements are located on the second redistribution layer; a first resin layer disposed between the second redistribution layer and the plurality of antenna elements, wherein the first resin layer contains a filler; a first adhesive layer disposed between the first resin layer and the second redistribution layer, wherein the first adhesive layer and the first resin layer comprise the same resin material; as well as The second resin layer is provided between the first resin layer and the plurality of antenna elements, wherein the second resin layer contains a filler.
9. The packaging structure according to claim 8, wherein the first adhesive layer physically contacts the dielectric layer of the second redistribution layer, and the interface between the dielectric layer and the first adhesive layer has a straight line profile, and the interface between the first adhesive layer and the first resin layer has a non-smooth profile. 10 . The packaging structure according to claim 8 , wherein the content of the filler in the first resin layer is greater than 80 weight % based on the total weight of the first resin layer and the first adhesive layer. 11 . The package structure according to claim 8 , wherein a ratio of a thickness of the first adhesive layer to a thickness of the first resin layer is in a range of 1:75 to 1:
360. 12 . The package structure according to claim 8 , further comprising a second adhesive layer disposed between the first resin layer and the second resin layer, wherein the second adhesive layer and the second resin layer are made of the same resin material.
13. The package structure according to claim 8, further comprising at least one dipole antenna embedded in the insulating package body. 14 . The package structure according to claim 8 , further comprising a plurality of through-insulation-layer holes embedded in the insulating package body and electrically connecting the first redistribution layer to the second redistribution layer.
15. A method for manufacturing a packaging structure, comprising: forming a bottom redistribution layer on the carrier; placing at least one semiconductor die on the bottom redistribution layer; forming an insulating package encapsulating the at least one semiconductor die; forming a top redistribution layer on the insulating package; peeling off the carrier to expose the rear surface of the bottom redistribution layer; stacking a first insulating film on the rear side surface of the bottom redistribution layer, wherein the first insulating film includes a resin-rich region and a filler-rich region, the resin-rich region being located between the filler-rich region and the bottom redistribution layer and separating the filler-rich region from a second redistribution layer; and A plurality of antenna elements are provided over the first insulating film.
16. The method for manufacturing a packaging structure according to claim 15, wherein the first insulating film having the filler-rich area and the resin-rich area is pre-formed in the following manner: the viscosity of the resin material is reduced to a range of 10 cP to 500 cP to form the first insulating film, so that the filler is gathered on one side of the resin material to define the filler-rich area and the resin-rich area. 17 . The method for manufacturing a package structure according to claim 15 , wherein the first insulating film is laminated on the bottom redistribution layer by a vacuum laminator.
18. The method for manufacturing a packaging structure according to claim 15, further comprising: After lamination, the first insulating film is cured at a temperature ranging from 150°C to 180°C.
19. The method for manufacturing a packaging structure according to claim 15, further comprising: before providing the plurality of antenna elements, laminating a second insulating film on the first insulating film; as well as The plurality of antenna elements are provided over the second insulating film.
20. The method for manufacturing a packaging structure according to claim 19, wherein the second insulating film includes a filler-rich area and a resin-rich area, and the second insulating film is pre-formed in the following manner: the viscosity of the resin material is reduced to a range of 10 cP to 500 cP to form the second insulating film, so that the filler is gathered on one side of the resin material to define the filler-rich area and the resin-rich area in the second insulating film.
21. A packaging structure, comprising: a first insulating film including a resin-rich region and a filler-rich region, wherein a ratio of a thickness of the resin-rich region to a thickness of the filler-rich region is in a range of 1:75 to 1:360; a plurality of antenna patterns disposed on the surface of the filler-rich region; a dielectric layer connected to the surface of the resin-rich region; a semiconductor die disposed on the dielectric layer; as well as A redistribution layer is disposed on the semiconductor die and is electrically connected to the semiconductor die. 22 . The package structure of claim 21 , further comprising a conductive layer disposed between the semiconductor die and the dielectric layer, wherein the conductive layer is electrically connected to the redistribution layer.
23. The package structure according to claim 22, wherein: The conductive layer is electrically connected to the redistribution layer through a plurality of through-insulation-layer vias surrounding the semiconductor die.
24. The packaging structure according to claim 21, wherein the content of the filler located in the resin-rich area is less than 5 weight % based on the total weight of the first insulating film, and the content of the filler located in the filler-rich area is greater than 80 weight % based on the total weight of the first insulating film. 25 . The package structure according to claim 21 , further comprising an insulating package body disposed between the redistribution layer and the dielectric layer and encapsulating the semiconductor die. 26 . The package structure according to claim 21 , further comprising a second insulating film disposed between the first insulating film and the plurality of antenna patterns. 27 . The package structure according to claim 26 , wherein the second insulating film comprises a resin-rich region and a filler-rich region, and the resin-rich region of the second insulating film is located between the filler-rich region of the second insulating film and the filler-rich region of the first insulating film.
28. A packaging structure, comprising: Backside redistribution layer; A semiconductor die is disposed on the backside redistribution layer; a top redistribution layer disposed on the semiconductor die and electrically connected to the semiconductor die and the back redistribution layer; a resin material layer disposed on the back redistribution layer, wherein the resin material layer includes a first surface and a second surface opposite to the first surface, the first surface is connected to the back redistribution layer, and the second surface faces away from the back redistribution layer, and the amount of filler located in the resin material layer increases from the first surface to the second surface; a second resin material layer disposed on a second surface of the resin material layer, wherein the second resin material layer includes a filler; and The antenna pattern is arranged on the second resin material layer.
29. The packaging structure of claim 28, wherein the second resin material layer includes a third surface and a fourth surface opposite to the third surface, the third surface is connected to the second surface of the resin material layer, and the antenna pattern is connected to the fourth surface of the second resin material layer, and the amount of filler located in the second resin material layer increases from the third surface to the fourth surface.
30. The packaging structure according to claim 28, wherein the resin material layer comprises a resin-rich area having the first surface and a filler-rich area having the second surface, and the content of the filler located in the resin-rich area is less than 5 weight % based on the total weight of the resin material layer, and the content of the filler located in the filler-rich area is greater than 80 weight % based on the total weight of the resin material layer. 31 . The package structure according to claim 30 , wherein the first surface has a straight line profile, and an interface between the resin-rich region and the filler-rich region has a non-smooth profile.
32. The package structure of claim 30, wherein a ratio of a thickness of the resin-rich region to a thickness of the filler-rich region is in a range of 1:75 to 1:
360.
33. The package structure according to claim 28, further comprising: an insulating package body disposed between the top redistribution layer and the backside redistribution layer, wherein the insulating package body encapsulates the semiconductor die; as well as A plurality of through-insulation layer holes are embedded in the insulating package and electrically connect the top redistribution layer to the back redistribution layer.
34. The package structure of claim 33, further comprising at least one dipole antenna embedded in the insulating package body.
35. A method for manufacturing a packaging structure, comprising: Providing a resin material on a carrier, and dispersing a plurality of fillers in the resin material; adjusting the viscosity of the resin material so that the plurality of fillers gather on one side of the resin material to form a first insulating film having a resin-rich region and a filler-rich region; forming a redistribution layer on the first insulating film, wherein the redistribution layer adheres to the resin rich region of the first insulating film; placing a semiconductor die on the redistribution layer; forming a second redistribution layer on the semiconductor die, wherein the second redistribution layer is electrically connected to the semiconductor die and the redistribution layer; peeling off the carrier to reveal the filler-rich region of the first insulating film; as well as A plurality of antenna patterns are formed on the first insulating film. 36 . The method for manufacturing a package structure according to claim 35 , wherein the viscosity of the resin material is reduced to a range of 10 cP to 500 cP so that the plurality of fillers are gathered on one side of the resin material.
37. The method for manufacturing a package structure according to claim 35, wherein adjusting the viscosity of the resin material comprises: The viscosity of the resin material is reduced by adding a solvent or a diluent.
38. The method for manufacturing a package structure according to claim 37, further comprising baking the resin material after adding the solvent.
39. The method for manufacturing a packaging structure according to claim 35, further comprising before forming the plurality of antenna patterns, stacking a second insulating film on the first insulating film; and The plurality of antenna patterns are formed on the second insulating film.
40. A method for manufacturing a packaging structure according to claim 39, wherein the second insulating film includes a filler-rich area and a resin-rich area, and the second insulating film is formed in advance by reducing the viscosity of the resin material to a range of 10 cP to 500 cP, thereby causing the filler to gather on one side of the resin material to form the filler-rich area and the resin-rich area in the second insulating film.
Citation Information
Patent Citations
Semiconductor package
CN107644850A
Integrated circuit package
CN108735683A