Scintillating crystal and well logging equipment and medical imaging equipment including the same

By doping elements such as Sr and Ca, the energy resolution and pulse decay time of the NaX:Tl scintillation crystal are optimized, which solves the shortcomings of the NaI:Tl scintillation crystal in terms of energy resolution and pulse decay time, and improves the performance of radiation detection equipment. .

CN111443374BActive Publication Date: 2024-10-11LUXIUM SOLUTIONS LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010392322.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2015-02-16
Filing Date
2016-02-15
Publication Date
2024-10-11
Estimated Expiration
2036-02-15

AI Technical Summary

Technical Problem

Existing NaI:Tl scintillation crystals have deficiencies in energy resolution and pulse decay time, making it difficult to meet the needs of certain radiation detection applications.

Method used

By doping different elements, such as Sr and Ca, a NaX:Tl,Sr or NaX:Tl,Ca scintillation crystal is formed to optimize its energy resolution and pulse decay time, and improve light output and quantum efficiency.

Benefits of technology

It achieves energy resolution of less than 6.4% and shorter pulse decay time at 662keV, improving the performance and accuracy of radiation detection equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111443374B_ABST
    Figure CN111443374B_ABST
Patent Text Reader

Abstract

The present application relates to scintillation crystals and well logging equipment and medical imaging equipment including the same. A scintillation crystal may include a sodium halide co-doped with thallium and another element. In an embodiment, the scintillation crystal may include NaX:Tl,Me, where X represents a halogen and Me represents a Group 1 element, a Group 2 element, a rare earth element, or any combination thereof. In a specific embodiment, the scintillation crystal has properties including: an emission maximum at a wavelength of no more than 430 nm for radiation in the range of 300 nm to 700 nm; or an energy resolution of less than 6.4% when measured at 662 keV, 22° C., and 1 microsecond integration time. In another embodiment, the co-dopant may be Sr or Ca. Compared to sodium halide doped only with thallium, the scintillation crystal may have lower energy resolution, better ratio, shorter pulse decay time, or any combination thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an invention patent application with an application date of February 15, 2016, application number 201680010159.9, and invention name "Scintillator crystals including co-doped sodium halide and radiation detection equipment including the scintillator crystals". Technical Field

[0002] The present disclosure relates to scintillation crystals comprising rare earth halides and radiation detection devices comprising such scintillation crystals. Background Art

[0003] NaI:Tl is a very common and well known scintillation crystal. Further improvements to NaI:Tl scintillation crystals are desired. Summary of the invention

[0004] The present application provides a scintillation crystal comprising NaX:Tl,Me, wherein:

[0005] X represents a halogen;

[0006] Me represents a Group 1 element, a Group 2 element, a rare earth element or any combination thereof;

[0007] Each of Tl and Me has at least 1×10 -5 mol% dopant concentration; and

[0008] The scintillation crystal has the following properties:

[0009] An energy resolution of less than 6.4% when measured at 662 keV, 22°C and 1 microsecond integration time; or

[0010] Less than the pulse decay time of another scintillation crystal with a NaX:Tl composition.

[0011] The present application provides a scintillation crystal, which comprises NaX:Tl,Sr, wherein:

[0012] X represents a halogen; and

[0013] Each of Tl and Sr has at least 1×10 -5 mol% concentration.

[0014] The present application provides a scintillation crystal comprising NaX:Tl,Ca, wherein:

[0015] X represents a halogen;

[0016] Each of Tl and Ca has at least 1×10 -5 mol% concentration; and

[0017] When the scintillation crystal and the NaI:Tl crystal are measured at 22°C, the scintillation crystal has a shorter pulse decay time or both compared to the NaI:Tl crystal.

[0018] The present application provides a scintillation crystal comprising NaX:Tl,Me, wherein:

[0019] X represents a halogen;

[0020] Me represents a Group 1 element and has a -5 Concentrations ranging from mol% to 9mol%.

[0021] The present application provides a method comprising:

[0022] Providing a scintillation crystal according to any one of the preceding claims;

[0023] capturing radiation within said scintillation crystal;

[0024] determining a pulse decay time and actual light output of said captured radiation;

[0025] determining an estimated light output corresponding to the pulse decay time; and

[0026] An adjusted light output is calculated, the adjusted light output being the product of the actual light output multiplied by the light output of NaX:Tl divided by the estimated light output. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The embodiments are illustrated by way of example and not limitation in the drawings.

[0028] Figure 1 Included is an illustration of a radiation detection device according to an embodiment that may be used for medical imaging.

[0029] Figure 2 and Figure 3 Included are illustrations of radiation detection devices according to embodiments that may be used for drilling or logging.

[0030] Figure 4 Included are those obtained for Sr co-doped and standard samples exposed to 662 keV gamma radiation at room temperature and 1 microsecond pulse integration.

[0031] Figure 5 Included are those obtained for La co-doped and standard samples exposed to gamma radiation with an energy of 662 keV at room temperature and 1 microsecond pulse integration.

[0032] Figure 6 Included are plots of relative light output as a function of energy for Sr co-doped, Ca co-doped, and standard samples.

[0033] Figure 7 Included are plots of scintillation light output versus pulse decay time for NaI:Tl crystals co-doped with different concentrations of Ca.

[0034] Skilled technicians should understand that the elements in the figures are shown for simplicity and clarity only and are not necessarily drawn to scale. For example, the size of some elements in the figures may be exaggerated relative to other elements to help improve understanding of embodiments of the present invention. DETAILED DESCRIPTION

[0035] The following description is provided in conjunction with the accompanying drawings to help understand the teachings disclosed herein. The following discussion will focus on specific implementations and examples of the teachings. This focus is provided to help describe the teachings and should not be interpreted as a limitation on the scope or applicability of the teachings.

[0036] The group numbers corresponding to the columns in the Periodic Table of the Elements use the "new notation" convention as found in the CRC Handbook of Chemistry and Physics, 81st Edition (2000-2001).

[0037] The terms "rare earth" or "rare earth elements" are intended to refer to Y, Sc, and the lanthanides (La through Lu) of the periodic table.

[0038] As used herein, the terms "comprises / comprising", "includes / including", "has / having" or any other variations thereof are intended to cover a non-exclusive inclusion. For example, a process, method, article, or apparatus that comprises a list of features is not necessarily limited to only those features, but may include other features not expressly listed or inherent to such process, method, article, or apparatus. In addition, unless expressly stated to the contrary, "or" refers to an inclusive or and not an exclusive or. For example, condition A or B is satisfied by any of the following: A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), and both A and B are true (or exist).

[0039] The use of "a" or "an" is used to describe elements and components described herein. This is done only for convenience and to give a general sense of the scope of the invention. Unless it is obvious that it is intended otherwise, this description should be understood to include one or at least one and the singular also includes the plural, or vice versa.

[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. The materials, methods, and examples are illustrative only and are not intended to be limiting. To the extent not described herein, many details regarding specific materials and processing actions are conventional and can be found in textbooks and other sources in the field of scintillation and radiation detection.

[0041] The scintillation crystal may include a sodium halide co-doped with thallium and another element. Co-doping may improve energy resolution, ratio, light output, decay time, another suitable scintillation parameter, or any combination thereof. In an embodiment, the scintillation crystal may include NaX:Tl,Me, where X represents a halogen, and Me represents a Group 1 element, a Group 2 element, a rare earth element, or any combination thereof. The selection of a specific co-dopant may depend on the specific scintillation parameter to be improved. As used in this specification, a co-doping may include two or more different elements (Tl and one or more other elements), and a co-dopant refers to one or more dopants other than Tl.

[0042] Regarding the composition of the sodium halide, X may be I, or a combination of I and Br. When X is a combination of I and Br, X may include at least 50 mol%, at least 70 mol%, or at least 91 mol% of I. In an embodiment, Tl may have at least 1×10 -4 mol%, at least 1×10 -3 mol% or at least 0.01mol%, and in another embodiment, Tl has a concentration of no more than 5mol%, no more than 0.2mol%, or no more than 0.15mol%. In a specific embodiment, Tl has a concentration of 1×10 -4 mol% to 5mol%, 1×10 -3 In a more specific embodiment, Tl has a concentration in the range of 0.03 mol % to 0.15 mol %, exhibiting good performance, such as high light output and good energy resolution.

[0043] In an embodiment, when the co-dopant is a Group 1 element or a Group 2 element, the dopant concentration of the Group 1 element or the Group 2 element is at least 1×10 -4 mol%, at least 1×10 -3 mol% or at least 0.01 mol%, and in another embodiment, the concentration is no greater than 5 mol%, no greater than 0.9 mol%, or no greater than 0.2 mol%. In a specific embodiment, the concentration of the Group 1 element or the Group 2 element is 1×10 -4 mol% to 5mol%, 1×10 -3mol% to 0.9mol% or 0.01mol% to 0.2mol%. In an embodiment, when the co-dopant is a rare earth element, the dopant concentration of the rare earth element is at least 5×10 -4 mol% or at least 8×10 -4 mol%, and in another embodiment, the dopant concentration is no greater than 0.5 mol%, 0.05 mol%, or 5×10 -3 mol%. All the aforementioned dopant concentrations are for dopant concentrations in the crystal.

[0044] In a specific embodiment, the scintillator crystal is a single crystal. The dopant concentration in the crystal may be different from or the same as the dopant concentration in the melt from which the scintillator crystal is formed. The concentrations of Tl and Group 1 and Group 2 co-dopants in the melt from which the crystal is formed may include any of the values ​​previously described. Rare earth elements, and especially La and heavy elements, are relatively large compared to Na atoms, and therefore, significantly lower concentrations of rare earth elements may be produced. Therefore, in one embodiment, the dopant concentration in the melt may be higher for rare earth elements, such as at least 1×10 -3 mol%, at least 5×10 -3 mol % or at least 0.01 mol %. After reading this specification in its entirety, a skilled artisan will be able to determine the amount of dopant to be in the melt to achieve a desired dopant concentration in the scintillation crystal after taking into account the segregation coefficient of such dopants.

[0045] In selecting a co-dopant, different considerations may determine which specific elements are better suited to improving a particular scintillation parameter than other elements.The following description is intended as a general guide and is not to be construed as limiting a particular scintillation parameter to a particular co-dopant.

[0046] In an embodiment, the wavelength of the emission maximum of the NaX:Tl,Me scintillation crystal may be relatively maintained the same as NaX:Tl, so that the quantum efficiency of a photosensor coupled or to be coupled to the scintillation crystal is not significantly altered. For radiation in the range of 300 nm to 700 nm, NaI:Tl has an emission maximum between 415 nm and 420 nm when the scintillation crystal is exposed to gamma radiation with an energy of 60 keV. In an embodiment, for radiation in the range of 300 nm to 700 nm, the co-doped scintillation crystal has an emission maximum at a wavelength of at least 400 nm, at least 405 nm, or at least 410 nm when the scintillation crystal is exposed to gamma radiation with an energy of 60 keV, and in another embodiment, the co-doped scintillation crystal has an emission maximum at a wavelength of no greater than 430 nm, no greater than 425 nm, or no greater than 420 nm when the scintillation crystal is exposed to gamma radiation with an energy of 60 keV. In specific embodiments, the co-doped scintillator crystal has an emission maximum at a wavelength in the range of 400 nm to 430 nm, 405 nm to 425 nm, or 410 nm to 420 nm when the scintillator crystal is exposed to gamma radiation having an energy of 60 keV.

[0047] Many Group 1, Group 2, and rare earth elements can be co-dopants in NaX:Tl,Me without significantly affecting the wavelength of the emission maximum compared to NaX:Tl. Co-doping with rare earth elements can increase light output. Some rare earth elements may be better suited for use without affecting the emission maximum. For example, co-doping with Sc, Y, La, LU, and Yb is less likely to significantly affect the wavelength of the emission maximum. Eu can shift the emission maximum to about 440nm, and such a shift can result in reduced quantum efficiency or the selection of a different photosensor with higher quantum efficiency at 440nm. Other rare earth elements that are co-doped with are more likely to cause a considerable shift in the wavelength of the emission maximum may include Sm, Pr, Nd, and Tb.

[0048] Scintillating crystals including co-doping with both a divalent metal element (e.g., a Group 2 element) and a rare earth element (other than Tl) can provide improved performance. The combination of a divalent metal element and a rare earth element as a co-dopant in a scintillating crystal can have improved (lower) energy resolution, improved (faster) pulse decay time, and suppression of defect color centers. Specific embodiments include NaX:Tl co-doped with Sr and Y or co-doped with Ca and Y.

[0049] Energy resolution (also called pulse height resolution or PHR) is improved because it can be smaller for co-doped scintillator crystals. Unless otherwise specified, the industry standard for determining energy resolution is to expose the scintillator crystal to 137Cs, which emits gamma radiation at 662keV energy. In a specific test method, the test is performed at room temperature (such as 20°C to 25°C and 22°C). The energy resolution is the full width at half the maximum value of the 662keV peak divided by the peak height. The energy resolution is usually expressed as a percentage. The energy resolution can be determined by the integration time (also called the shaping time). Good energy resolution at a relatively short integration time corresponds to a shorter time to correctly identify the radiation source.

[0050] In an embodiment, the scintillation crystal has an energy resolution of less than 6.4%, less than 6.2%, or less than 6.0% when measured at 662 keV, 22°C, and an integration time of 1 microsecond. In another embodiment, the scintillation crystal has an energy resolution of less than 6.1%, less than 6.0%, or less than 5.9% when measured at 662 keV, 22°C, and any integration time in the range of 1 microsecond to 4 microseconds. Although the lower limit of the energy resolution is not known at this time, the scintillation crystal may have an energy resolution of at least 0.1% at any integration time in the range of 1 microsecond to 4 microseconds. As a basis for comparison, NaI:Tl has an energy resolution of greater than 6.2% at integration times of 1, 2, and 4 microseconds.

[0051] Group 2 elements are particularly well suited to achieve good energy resolution. Ca and Sr are particularly well suited to achieve low energy resolution. NaI:Tl,Sr can achieve an energy resolution of 5.3% at 1 microsecond integration time, and NaI:Tl,Ca can achieve an energy resolution of 5.4% at 1 microsecond integration time. With further optimization, even lower energy resolutions can be achieved. Such energy resolutions are compared to NaI:Tl,Eu, which is reported to have an energy resolution of greater than 6.4% at 1 microsecond integration time and greater than 6.2% at 4 microsecond integration time. In a specific embodiment, the energy resolution is at least 0.1% at an integration time of 1 microsecond.

[0052] Group 1 elements may also improve energy resolution. While not being bound by theory, the use of relatively large Group 1 elements replacing Na atoms may stretch the lattice and improve hole mobility. Thus, K, Rb, and Cs may be used. K has a relatively high radioisotope concentration, so Rb and Cs may be better candidates for co-dopants.

[0053] There has been much recent interest in the ratio of scintillation crystals. Ideally, light output is a perfectly linear function of energy. Thus, at any energy for a particular scintillation crystal composition, identification of the radiation source can be performed more easily and with greater confidence because the curve of light output versus energy is an ideally straight line. In practice, light output can deviate from perfect linearity, and such deviations are generally greater at lower energies. One method of determining the ratio of scintillation crystals is to measure the light output at high energies, such as 2615 keV. In the curve of light output versus energy, the straight line goes from a point (0,0) corresponding to zero light output, zero energy to another point (LY 0,0) corresponding to light output at 2615 keV, 2615 keV. 2615 , 2615).

[0054] According to the equation, the relative light output at a specific energy (in keV) (normalized to the light output at 2615 keV) is:

[0055]

[0056] where the actual light output is at a specific energy and the predicted light output is:

[0057]

[0058] Among them, LY 2615 is the actual light output at 2615 keV.

[0059] The average relative light output may be obtained by integrating the relative light output over a specific energy range to obtain an integrated value, and dividing the integrated value by the specific energy range.

[0060] A relative light output of 1.00 corresponds to a perfect ratio. As the deviation increases (either above 1.00 or below 1.00), the ratio becomes worse. For example, a relative light output of 0.98 is better than 1.05 because 1.00 is closer to 0.98 than 1.05.

[0061] In an embodiment, at an energy in the range of 32 keV to 81 keV, the scintillation crystal has an average relative light output as normalized to the light output at 2615 keV of at least 1.01, at least 1.04, or at least 1.07. In another embodiment, at an energy in the range of 32 keV to 81 keV, the scintillation crystal has an average relative light output as normalized to the light output at 2615 keV of no greater than 1.15, no greater than 1.13, or no greater than 1.11. In a specific embodiment, at an energy in the range of 32 keV to 81 keV, the scintillation crystal has an average relative light output as normalized to the light output at 2615 keV in the range of 1.01 to 1.15, 1.04 to 1.13, or 1.07 to 1.11. As a basis for comparison, at an energy in the range of 32 keV to 81 keV, NaI:Tl has an average relative light output as normalized to the light output at 2615 keV of more than 1.15.

[0062] Although not significant, improvements are visible at moderate energies. In an embodiment, at energies in the range of 122 keV to 511 keV, the scintillation crystal has an average relative light output as normalized to the light output at 2615 keV of at least 1.01, at least 1.02, or at least 1.03. In another embodiment, at energies in the range of 122 keV to 511 keV, the scintillation crystal has an average relative light output as normalized to the light output at 2615 keV of no greater than 1.07, no greater than 1.06, or no greater than 1.05. In a specific embodiment, at energies in the range of 122 keV to 511 keV, the scintillation crystal has an average relative light output as normalized to the light output at 2615 keV in the range of 1.01 to 1.07, 1.02 to 1.06, or 1.03 to 1.05. As a basis of comparison, at energies ranging from 122 keV to 511 keV, NaI:Tl has an average relative light output of about 1.08 as normalized to the light output at 2615 keV.

[0063] In terms of achieving ratios, Group 2 elements are good. For relatively low and medium energy ranges, Ca and Sr are particularly suitable for achieving a ratio closer to 1.00. For energies in the range of 32keV to 81keV, NaI:Tl,Sr can achieve an average relative light output of 1.09 as normalized to the light output at 2615keV, and NaI:Tl,Ca can achieve an average relative light output of 1.15 as normalized to the light output at 2615keV. For energies in the range of 122keV to 511keV, NaI:Tl,Sr can achieve an average relative light output of 1.04 as normalized to the light output at 2615keV, and NaI:Tl,Ca can achieve an average relative light output of 1.06 as normalized to the light output at 2615keV.

[0064] The scintillation pulse decay time may be reduced with the co-dopant compared to a composition without the co-dopant. In an embodiment, the scintillation crystal with the co-dopant has a pulse decay time that is at least 5%, at least 11%, or at least 20% less than the pulse decay time of the NaI:Tl crystal when the scintillation crystal and the NaI:Tl crystal are measured at 22°C and exposed to gamma radiation with an energy of 662keV. In another embodiment, the scintillation crystal with the co-dopant has a pulse decay time that is no more than 80%, no more than 65%, or no more than 50% less than the pulse decay time of the NaI:Tl crystal when the scintillation crystal and the NaI:Tl crystal are measured at 22°C and exposed to gamma radiation with an energy of 662keV. In specific embodiments, the scintillation crystal with the co-dopant has a pulse decay time that is 5% to 80%, 11% to 65%, or 20% to 50% less than the pulse decay of the NaI:Tl crystal when the scintillation crystal and the NaI:Tl crystal are measured at 22°C and exposed to gamma radiation with an energy of 662keV. In terms of actual times, the NaI:Tl crystal may have a pulse decay time of about 230ns, and the NaI:Tl,Sr crystal may have a pulse decay time as low as 160ns. Similar improvements may occur with the NaI:Tl,Ca case.

[0065] The scintillating crystals may be formed using any of a variety of crystal growth techniques including Bridgman, Czochralski, Kyropoulos, Edge-defined Film-fed Growth (EFG), Stepanov, etc. The starting materials include sodium halide and a halide of a dopant. In an embodiment, the starting materials may include NaI and TlI, and depending on the co-dopant, the starting materials may include CaI 2 , SrI 2 ,LaI 3 , YI3 ScI 3 , LuI 3 , RbI, CsI, etc. If a relatively small amount of bromine is to be added, then any one of the dopants (either Tl or co-dopants) can be the corresponding bromide. If more bromine is needed, then NaBr can replace some of the NaI. After determining the desired composition of the scintillation crystal, a skilled artisan will be able to use the segregation coefficient of the dopant relative to the base material (e.g., NaI) to determine the amount of starting material to use in the melt. The crystal growth conditions can be the same as those used to form NaI:Tl or can have relatively few changes to optimize the crystal formation process.

[0066] Any of the scintillation crystals as previously described can be used in a variety of applications. Exemplary applications include gamma ray spectroscopy, isotope identification, single positron emission computed tomography (SPECT) or positron emission tomography (PET) analysis, x-ray imaging, oil well logging detectors, and detecting the presence of radioactivity. Scintillator crystals can be used in other applications, and therefore, the enumeration is merely exemplary and non-limiting. Several specific applications are described below.

[0067] Figure 1 An embodiment of a radiation detection device 100 is shown, which can be used for gamma ray analysis, such as single positron emission computed tomography (SPECT) or positron emission tomography (PET) analysis. In the illustrated embodiment, the radiation detection device 100 includes a light sensor 101, an optical interface 103, and a scintillation device 105. Although the light sensor 101, the optical interface 103, and the scintillation device 105 are shown separated from each other, a skilled person will understand that the light sensor 101 and the scintillation device 105 can be coupled to the optical interface 103, wherein the optical interface 103 is disposed between the light sensor 101 and the scintillation device 105. The scintillation device 105 and the light sensor 101 can be optically coupled to the optical interface 103 using other known coupling methods, such as using an optical gel or adhesive or directly through the molecular binding force of the optical coupling element.

[0068] The light sensor 101 may be a photomultiplier tube (PMT), a semiconductor-type photomultiplier tube, or a hybrid light sensor. The light sensor 101 may receive photons emitted by the scintillation device 105 via the input window 116, and generate electrical pulses based on the number of photons received by it. The light sensor 101 is electrically coupled to the electronic module 130. The electrical pulses may be shaped, digitized, analyzed, or any combination thereof by the electronic module 130 to provide a count or other information of the photons received at the light sensor 101. The electronic module 130 may include an amplifier, a pre-amplifier, a discriminator, an analog / digital signal converter, a photon counter, a pulse shape analyzer or discriminator, another electronic component, or any combination thereof. The light sensor 101 may be housed in a tube or housing made of a material (such as a metal, a metal alloy, other materials, or any combination thereof) capable of protecting the light sensor 101, the electronic module 130, or a combination thereof.

[0069] The scintillation device 105 includes a scintillation crystal 107, which may be any of the previously described scintillation crystals represented by the general formula NaX:Tl,Me, where X represents a halogen and Me represents a Group 1 element, a Group 2 element, a rare earth element, or any combination thereof. The scintillation crystal 107 is substantially surrounded by a reflector 109. In one embodiment, the reflector 109 may include polytetrafluoroethylene (PTFE), another material suitable for reflecting light emitted by the scintillation crystal 107, or a combination thereof. In an illustrative embodiment, the reflector 109 may be substantially surrounded by a shock absorbing member 111. The scintillation crystal 107, the reflector 109, and the shock absorbing member 111 may be housed within a housing 113.

[0070] The scintillation device 105 includes at least one stabilization mechanism adapted to reduce relative movement between the scintillation crystal 107 and other elements of the radiation detection device 100 (e.g., the optical interface 103, the housing 113, the shock absorbing member 111, the reflector 109, or any combination thereof). The stabilization mechanism may include a spring 119, an elastomer, another suitable stabilization mechanism, or a combination thereof. The stabilization mechanism may be adapted to apply a lateral force, a horizontal force, or a combination thereof to the scintillation crystal 107 to stabilize its position relative to one or more other elements of the radiation detection device 100.

[0071] As shown, the optical interface 103 is adapted to couple between the light sensor 101 and the scintillation device 105. The optical interface 103 is also adapted to facilitate optical coupling between the light sensor 101 and the scintillation device 105. The optical interface 103 may include a polymer such as silicone rubber, which is polarized to adjust the reflective index of the scintillation crystal 107 and the input window 116. In other embodiments, the optical interface 103 may include a gel or colloid including a polymer and additional elements.

[0072] Scintillator crystals are used in well logging applications. Figure 2A drawing of a drilling apparatus 10 is included, including an upper drive 12 connected to the upper end of a drill string 14, which is suspended in a wellbore 16 by a pulling workpiece 17. A rotary table 18 including a pipe sleeve can be used in connection with the upper drive 12 or in place of the upper drive 12 to maintain a proper drill string orientation. A downhole telemetry measurement and transmission device 20 (commonly referred to as a measurement while drilling (MWD) device) is part of a downhole tool connected to the lower end of the drill string 14. The MWD device transmits drilling-related parameters to the surface through mud pulses or electromagnetic transmissions. These signals are received at the surface by a data receiving device 22. The downhole tool includes a curved section 23, a downhole motor 24, and a drill bit 26. The curved section 23 is adjacent to the MWD device and is used to assist in drilling an inclined wellbore. The downhole motor 24, such as a positive displacement motor (PDM) or a downhole turbine, drives the drill bit 26 and is at the distal end of the downhole tool.

[0073] The downhole signal received by the data receiving device 22 is provided to a computer 28, an output device 30, or both. The computer 28 may be located at the well site or remotely linked to the well site. The analyzer device may be part of the computer 28 or may be located in a downhole tool close to the MWD device 20. The computer 28 and the analyzer device may include a processor that can receive input from a user. The signal is also sent to the output device 30, which may be a display device, a hard copy log printing device, a meter, an audiovisual alarm, or any combination thereof. The computer 28 is operatively connected to the control member of the pulling workpiece 17 and to the control electronic component 32 associated with the upper drive device 12 and the rotary table 18 to control the rotation of the drill string and the drill bit. The computer 28 may also be coupled to a control mechanism associated with the mud pump of the drilling equipment to control the rotation of the drill bit. The control electronic component 32 may also receive manual input, such as a drilling rig operator.

[0074] Figure 3 A drawing showing a portion of a MWD device 20 within a downhole tool 16 is shown. The MWD device 20 includes a housing 202, a temperature sensor 204, a scintillation crystal 222, an optical interface 232, a light sensor 242, and an analyzer device 262. The housing 202 may include a material capable of protecting the scintillation crystal 222, the light sensor 242, the analyzer device 262, or a combination thereof, such as a metal, a metal alloy, other materials, or any combination thereof. The temperature sensor 204 is positioned adjacent to the scintillation crystal 222, the light sensor 242, or both. The temperature sensor 204 may include a thermocouple, a thermistor, or another suitable device capable of determining that the temperature within the housing exceeds the normal operating temperature of the MWD device 20. The radiation detection device includes a scintillation crystal 222 optically coupled to the light sensor 242, which is coupled to the analyzer device 262.

[0075] The scintillation crystal 222 has a composition more suitable for high temperature applications, such as greater than 120° C., at least 130° C., at least 140° C., at least 150° C., and higher. In an embodiment, the scintillation crystal 222 may be any of the previously described scintillation crystals represented by the general formula NaX:Tl,Me, where X represents a halogen and Me represents a Group 1 element, a Group 2 element, a rare earth element, or any combination thereof.

[0076] In another embodiment, a radiation detection device having a scintillation crystal as described herein may be configured for another application. In a specific embodiment, the radiation detection device may be configured for use in prompt gamma neutron activation analysis. The reduced pulse decay time may allow for a simpler design of the radiation detection device. Specifically, a scintillator crystal without a co-dopant may need to be heated (above room temperature) to achieve the desired pulse decay time. The heater may complicate the design of the radiation detection device and may cause undesirable noise. With co-doping, the pulse decay time may be fast enough at room temperature (e.g., 22° C.), thus avoiding the need for a heater and simplifying the design.

[0077] In another embodiment, the actual light output from the scintillation event can be adjusted to improve energy resolution. The concentration of the dopant within the scintillation crystal can vary throughout the crystal, and the concentration of the dopant can affect the decay time and light output of the scintillation crystal. Therefore, the decay time and light output can depend on the location where the gamma ray energy is captured within the scintillation crystal. Because the light output is used to determine the energy of the interacting gamma rays, there can be variations in the energy measurement. In other words, the energy resolution will be poor. In another embodiment, the actual light output can be adjusted for variations in the light output based on the pulse decay time. The method described below is particularly suitable for co-dopants such as Ca, Sr, Ba, La, or any other co-dopants whose decay time depends on the concentration of the co-dopant.

[0078] Before adjustment, an equation is generated that relates the pulse decay time to the light output. When detecting a specific gamma ray source emitting gamma rays at an energy of 662 keV, such as 137 Cs, data can be collected for different dopant concentrations of the co-dopant in the scintillation crystal. A curve of decay time versus light output provides a linear relationship between the scintillation light output and decay time. The pulse decay time is the time interval between the moment of peak photon flux in each pulse and the moment when the photon flux drops to a factor of 1 / e (36.8%) of the peak photon flux. Therefore, a least squares fit of the data corresponding to the curve can produce the following equation 1.

[0079] LY est =m*DT+b, (Equation 1)

[0080] Among them: LY estTo estimate the light output,

[0081] DT is the pulse decay time,

[0082] m is the slope of the line, and

[0083] b is the y-intercept of the line.

[0084] As a non-limiting example, Figure 7 The scintillation light output and pulse decay time curve of NaI:Tl crystal co-doped with Ca (triangle mark). Figure 7 The data in are generated from samples where the concentration of Ca in the NaI:Tl crystals was different in each sample. The ordinate of the curve is the scintillation light output in photon / gamma ray energy MeV. The abscissa is the scintillation pulse decay time in nanoseconds. Reference Figure 7 , the straight line is a least squares fit to the data, and the equation for this line is

[0085] LY est =206.28*DT-8360.3, (Equation 2)

[0086] Among them: LY est is the estimated light output in photons / MeV, and

[0087] DT is the pulse decay time in nanoseconds.

[0088] If needed or desired, different equations may be generated for different co-dopants, different radiation sources, or both. The equation has the same format as Equation 1 and may have different values ​​for m and b for different co-dopants, radiation sources, or both.

[0089] After the values ​​of m and b for Equation 1 have been generated, the pulse decay time and actual measurement of light output for a subsequent scintillation event can be determined. The pulse decay time can be used to determine the estimated light output according to Equation 1.

[0090] The actual measured light output can be adjusted using the following equation 3 by the ratio of the light output for the scintillator of the same composition without co-dopant (which is NaX:Tl).

[0091] LY adj =LY act *LY std / LY est , (Equation 3)

[0092] in:

[0093] LY adj To adjust the light output,

[0094] LYact is the light output as measured,

[0095] LY std is the light output of a scintillation crystal without a co-dopant (e.g. NaI:Tl), and

[0096] LY est is the estimated light output calculated based on the measured pulse decay time.

[0097] LY std LY may have a previously known value or may be calculated using the pulse decay time for a scintillator crystal without a co-dopant. For NaI:Tl, the pulse decay time may be 230 ns, and Equation 2 may be used to determine LY std .

[0098] Conditioning allows the light output of each individual pulse to be scaled by a compensation factor to reduce the variation in the measured light output within the same crystal or between different crystals with different co-dopant contents. This process can improve the energy resolution of the crystal. Thus, the radiation source can be identified more quickly and accurately than using actual measurements without conditioning.

[0099] Many different aspects and embodiments are possible. Some of those aspects and embodiments are described herein. After reading this specification, the skilled person will understand that those aspects and embodiments are merely illustrative and do not limit the scope of the invention. Embodiments may be according to any one or more of the embodiments listed below.

[0100] Embodiment 1. A scintillation crystal comprising NaX:Tl,Me, wherein:

[0101] X represents a halogen;

[0102] Me represents a Group 1 element, a Group 2 element, a rare earth element or any combination thereof;

[0103] Each of Tl and Me has at least 1×10 -5 mol% dopant concentration; and

[0104] The scintillation crystal has the following properties:

[0105] For radiation in the range of 300 nm to 700 nm, the emission maximum is at a wavelength not greater than 430 nm;

[0106] An energy resolution of less than 6.4% when measured at 662 keV, 22°C and 1 microsecond integration time; or

[0107] Less than the pulse decay time of another scintillation crystal with a NaX:Tl composition.

[0108] Embodiment 2. The scintillation crystal according to embodiment 1, wherein Me is a rare earth element.

[0109] Embodiment 3. The scintillation crystal according to embodiment 2, wherein Me is La, Sc, Y, Lu, Yb or any combination thereof.

[0110] Embodiment 4. The scintillation crystal according to embodiment 2 or embodiment 3, wherein Me has at least 5×10 -4 mol% or at least 8×10 -4 mol% dopant concentration.

[0111] Embodiment 5. The scintillation crystal according to any one of embodiments 2 to 4, wherein Me has an amount not greater than 0.9 mol%, 0.05 mol%, or 5×10 -3 mol% dopant concentration.

[0112] Embodiment 6. The scintillation crystal according to embodiment 1, wherein Me is a Group 1 element.

[0113] Embodiment 7. The scintillator crystal according to embodiment 1, wherein Me is a Group 2 dopant.

[0114] Embodiment 8. The scintillation crystal according to embodiment 7, wherein Me is Ca, Sr or any combination thereof.

[0115] Embodiment 9. A scintillation crystal comprising NaX:Tl,Sr, wherein:

[0116] X represents a halogen; and

[0117] Each of Tl and Sr has at least 1×10 -5 mol% concentration.

[0118] Embodiment 10. The scintillation crystal of embodiment 9, wherein the scintillation crystal has a greater light output than the NaI:Tl crystal when the scintillation crystal and the NaI:Tl crystal are measured at 22°C.

[0119] Embodiment 11. A scintillation crystal comprising NaX:Tl,Ca, wherein:

[0120] X represents a halogen;

[0121] Each of Tl and Ca has at least 1×10 -5 mol% concentration; and

[0122] When the scintillation crystal and the NaI:Tl crystal are measured at 22° C., the scintillation crystal has a greater light output, a shorter pulse decay time, or both, compared to the NaI:Tl crystal.

[0123] Example 12. A scintillation crystal comprising NaX:Tl,Me 2+ and RE, where:

[0124] X represents a halogen;

[0125] Me 2+ It represents a divalent metal element;

[0126] RE represents a rare earth element; and

[0127] Each of Tl and Sr has at least 1×10 -5 mol% concentration.

[0128] Embodiment 13. The scintillation crystal according to embodiment 12, wherein Me 2+ is Ca, Sr or any combination thereof; and RE is La, Sc, Y, L, Yb or any combination thereof.

[0129] Embodiment 14. A scintillation crystal comprising NaX:Tl,Me, wherein:

[0130] X represents a halogen;

[0131] Me represents a Group 1 element and has a -5 Concentrations ranging from mol% to 9mol%.

[0132] Embodiment 15. The scintillation crystal according to embodiment 6 or embodiment 14, wherein Me is Rb, Cs or any combination thereof.

[0133] Embodiment 16. The scintillation crystal according to any one of embodiments 6 to 15, wherein the Group 1 element, the Group 2 element, Sr, Ca, Me 2+ or RE has at least 1×10 -4 mol%, at least 1×10 -3 mol% or a concentration of at least 0.01 mol%.

[0134] Embodiment 17. The scintillation crystal according to any one of embodiments 6 to 16, wherein the Group 1 element, the Group 2 element, Sr, Ca, Me 2+ Or RE has a concentration of not more than 5 mol%, not more than 0.9 mol%, or not more than 0.2 mol%.

[0135] Embodiment 18. The scintillation crystal according to any one of embodiments 6 to 17, wherein the Group 1 element, the Group 2 element, Sr, Ca, Me 2+ or RE has a value in 1×10 -4mol% to 5mol%, 1×10 -3 mol% to 0.9mol% or 0.01mol% to 0.2mol%.

[0136] Embodiment 19. The scintillation crystal according to any one of the preceding embodiments, wherein Tl has at least 1×10 - 4 mol%, at least 1×10 -3 mol% or a concentration of at least 0.01 mol%.

[0137] Embodiment 20. The scintillation crystal of any preceding embodiment, wherein Tl has a concentration of no greater than 5 mol %, no greater than 0.9 mol %, or no greater than 0.2 mol %.

[0138] Embodiment 21. The scintillation crystal according to any one of the preceding embodiments, wherein Tl has a -4 mol% to 5mol%, 1×10 -3 mol% to 0.9mol% or 0.01mol% to 0.2mol%.

[0139] Embodiment 22. The scintillation crystal according to any one of the preceding embodiments, wherein X is I.

[0140] Embodiment 23. The scintillation crystal of any one of embodiments 1 to 21, wherein X is a combination of I and Br.

[0141] Embodiment 24. The scintillation crystal of embodiment 23, wherein X comprises at least 50 mol %, at least 70 mol %, or at least 91 mol % I.

[0142] Embodiment 25. A scintillation crystal according to any of the preceding embodiments, wherein when the scintillation crystal is exposed to gamma radiation having an energy of 60 keV, the scintillation crystal has an emission maximum at a wavelength of at least 400 nm, at least 405 nm or at least 410 nm for radiation in the range of 300 nm to 700 nm.

[0143] Embodiment 26. A scintillation crystal according to any of the preceding embodiments, wherein when the scintillation crystal is exposed to gamma radiation having an energy of 60 keV, the scintillation crystal has an emission maximum at a wavelength of no greater than 430 nm, no greater than 425 nm or no greater than 420 nm for radiation in the range of 300 nm to 700 nm.

[0144] Embodiment 27. A scintillation crystal according to any of the preceding embodiments, wherein when the scintillation crystal is exposed to gamma radiation having an energy of 60 keV, for radiation in the range of 300 nm to 700 nm, the scintillation crystal has an emission maximum at a wavelength in the range of 400 nm to 430 nm, 405 nm to 425 nm or 410 nm to 420 nm.

[0145] Embodiment 28. The scintillation crystal of any preceding embodiment, wherein the scintillation crystal has an energy resolution of less than 6.4%, less than 6.2%, less than 6.0%, or less than 5.5% when measured at 662 keV, 22° C., and 1 microsecond integration time.

[0146] Embodiment 29. A scintillation crystal according to any of the preceding embodiments, wherein the scintillation crystal has an energy resolution of less than 6.1%, less than 6.0% or less than 5.9% when measured at 662 keV, 22° C. and any integration time in the range of 1 μsec to 4 μsec.

[0147] Embodiment 30. The scintillation crystal of any preceding embodiment, wherein at energies in the range of 32 keV to 81 keV, the scintillation crystal has an average relative light output of at least 1.01, at least 1.04, or at least 1.07 as normalized to the light output at 2615 keV.

[0148] Embodiment 31. A scintillation crystal according to any of the preceding embodiments, wherein at energies in the range of 32 keV to 81 keV, the scintillation crystal has an average relative light output of no greater than 1.15, no greater than 1.13, or no greater than 1.11 as normalized to the light output at 2615 keV.

[0149] Embodiment 32. A scintillation crystal according to any of the preceding embodiments, wherein at energies in the range of 32 keV to 81 keV, the scintillation crystal has an average relative light output in the range of 1.01 to 1.15, 1.04 to 1.13, or 1.07 to 1.11 as normalized to the light output at 2615 keV.

[0150] Embodiment 33. A scintillation crystal according to any of the preceding embodiments, wherein at energies in the range of 122 keV to 511 keV, the scintillation crystal has an average relative light output of at least 1.01, at least 1.02, or at least 1.03 as normalized to the light output at 2615 keV.

[0151] Embodiment 34. A scintillation crystal according to any of the preceding embodiments, wherein at energies in the range of 122 keV to 511 keV, the scintillation crystal has an average relative light output of no greater than 1.07, no greater than 1.06, or no greater than 1.05 as normalized to the light output at 2615 keV.

[0152] Embodiment 35. A scintillation crystal according to any of the preceding embodiments, wherein at energies in the range of 122 keV to 511 keV, the scintillation crystal has an average relative light output in the range of 1.01 to 1.07, 1.02 to 1.06, or 1.03 to 1.05 as normalized to the light output at 2615 keV.

[0153] Embodiment 36. The scintillation crystal of any one of embodiments 30 to 35, wherein the relative light output at a specific energy (in keV) as normalized to the light output at 2615 keV is:

[0154]

[0155] wherein the actual light output is at the specific energy and the predicted light output is:

[0156]

[0157] Among them, LY 2615 is the actual light output at 2615 keV.

[0158] Embodiment 37. The scintillation crystal of any one of embodiments 30 to 36, wherein the average relative light output is an integral of the relative light output over a specific energy range divided by the specific energy range.

[0159] Embodiment 38. A scintillation crystal according to any of the preceding embodiments, wherein when the scintillation crystal and the NaI:Tl crystal are measured at 22° C. and exposed to gamma radiation with an energy of 662 keV, the scintillation crystal has a pulse decay time that is at least 5%, at least 11% or at least 20% less than the pulse decay time of the NaI:Tl crystal.

[0160] Embodiment 39. A scintillation crystal according to any of the preceding embodiments, wherein when the scintillation crystal and the NaI:Tl crystal are measured at 22° C. and exposed to gamma radiation having an energy of 662 keV, the scintillation crystal has a pulse decay time that is no more than 80%, no more than 65% or no more than 50% less than the pulse decay time of the NaI:Tl crystal.

[0161] Embodiment 40. A scintillation crystal according to any of the preceding embodiments, wherein when the scintillation crystal and the NaI:Tl crystal are measured at 22° C. and exposed to gamma radiation with an energy of 662 keV, the scintillation crystal has a pulse decay time that is less than the pulse decay of the NaI:Tl crystal in the range of 5% to 80%, 11% to 65% or 20% to 50%.

[0162] Embodiment 41. The scintillation crystal according to any one of the preceding embodiments, wherein the scintillation crystal is a single crystal.

[0163] Embodiment 42. A radiation detection device comprising:

[0164] The scintillation crystal according to any one of the preceding embodiments; and

[0165] A light sensor is optically coupled to the scintillation crystal.

[0166] Embodiment 43. The radiation detection apparatus according to Embodiment 42, further comprising a window disposed between the scintillation crystal and the light sensor.

[0167] Embodiment 44 The radiation detecting apparatus of Embodiment 42 or Embodiment 43, further comprising a transparent adhesive attached to a surface of the scintillator crystal closest to the light sensor.

[0168] Embodiment 45. The radiation detection device according to any one of Embodiments 42 to 44, wherein the radiation detection device is configured to perform prompt gamma neutron activation analysis.

[0169] Embodiment 46. A method comprising:

[0170] Providing a scintillation crystal according to any one of the preceding embodiments;

[0171] capturing radiation within said scintillation crystal;

[0172] determining a pulse decay time and actual light output of said captured radiation;

[0173] determining an estimated light output corresponding to the pulse decay time; and

[0174] An adjusted light output is calculated, the adjusted light output being the product of the actual light output multiplied by the light output of NaX:Tl divided by the estimated light output.

[0175] Examples

[0176] The concepts described herein will be further described in the examples, which do not limit the scope of the invention described in the claims. The examples demonstrate the performance of scintillation crystals of different compositions. For convenience, the values ​​disclosed in this example section may be averaged, approximated, or rounded from multiple readings. The samples were formed using the vertical Bridgman crystal growth technique.

[0177] Scintillator crystals were formed to compare the light output (PH) and energy resolution (PHR) of the co-doped samples with NaI:Tl standards. The composition of the scintillator crystals is listed in Table 1. The scintillator crystals were heated at room temperature (about 22°C) by exposing them to 137 Cs and the test was performed using a photomultiplier tube and a multichannel analyzer to obtain the spectrum.

[0178] Table 1 - Standards, Sr and La compositions

[0179] sample TlI (mol%) <![CDATA[SrI 2 (mol%)]]> <![CDATA[LaI 3 (mol%)]]> NaI:Tl(standard) 0.1000 - - NaI:Tl,Sr 0.05 0.11 - NaI:Tl,La 0.0880 - <![CDATA[8.6×10 -5 ]]>

[0180] Figure 4 and Figure 5 Included are spectra comparing a NaI:Tl standard with a Sr co-doped sample and a La co-doped sample. Energy resolution was performed using a 1 microsecond integration time. Figure 4 As can be seen in the Figure 1, the Sr co-doped sample has a significantly better energy resolution of about 5.3% compared to the NaI:Tl standard (which is about 6.5%). The La co-doped sample has a light output of about 109% of the light output of the NaI:Tl standard (i.e., 9% more light output).

[0181] The Ca co-doped samples were also compared to the NaI:Tl standard. Table 2 includes the crystal compositions. The Ca#1 sample, Ca#2 sample, and Ca#3 sample correspond to locations near the top, middle, and bottom of the Ca co-doped crystal, respectively. The scintillation crystals were exposed to 137 Cs and the test was performed using a photomultiplier tube and a multichannel analyzer to obtain the spectrum.

[0182] Table 2 - Standards and Ca Composition

[0183] sample TlI (mol%) <![CDATA[CaI 2 (mol%)]]> NaI:Tl(standard) 0.100 - NaI:Tl,Ca#1 0.06 0.09 NaI:Tl,Ca#2 0.03 0.21 NaI:Tl,Ca#3 0.07 0.47

[0184] Table 3 includes the light output (PH) and energy resolution (PHR) of the samples when using integration times of 1 μs, 2 μs, and 4 μs. For PH, the light output of the Ca co-doped samples was compared to that of the NaI:Tl standard.

[0185] Table 3 - pH and PHR of Ca co-doped samples

[0186]

[0187]

[0188] The best pulse height resolution was 5.4% in the case of the Ca co-doped sample. Further work may be performed to determine whether the Ca concentration, the relative concentration of Ca to Tl, or both have a significant effect on the energy resolution. For example, a Ca concentration at 0.09 mol% to 0.47 mol% or a Ca:Tl ratio of 1.5 to 7.0 may provide better energy resolution for the Ca co-doped sample, as compared to another Ca co-doped sample outside of either or both of the ranges. Further studies may help provide a better understanding of the effect of concentration on energy resolution.

[0189] The ratio was tested by comparing the Sr co-doped samples and the Ca co-doped samples with the NaI:Tl standard. Table 4 includes the crystal composition. The Sr#1 sample, the Sr#2 sample, and the Sr#3 sample correspond to locations near the top, middle, and bottom of the Sr co-doped crystal, respectively.

[0190] Table 4 - Standards, Sr and Ca compositions

[0191] sample TlI (mol%) <![CDATA[SrI 2 (mol%)]]> <![CDATA[CaI 2 (mol%)]]> NaI:Tl(standard) 0.100 - - NaI:Tl,Sr#1 0.05 0.11 - NaI:Tl.Sr#2 0.029 0.135 - NaI:Tl,Sr#3 0.030 0.137 - NaI:Tl,Ca 0.053 - 0.020

[0192] For each of the samples, light output data was collected at a variety of different energies by exposing the sample to a radiation source emitting different energies. Each sample was normalized to the light output at 2615 keV for the same sample. The relative light output (normalized to the light output at 2615 keV) at a specific energy (in keV) is:

[0193]

[0194] where the actual light output is at a specific energy and the predicted light output is:

[0195]

[0196] Among them, LY 2615 is the actual light output at 2615 keV. Ideally, the curve should have all points under 1.00. The average relative light output is obtained by integrating the relative light output over a specific energy range to obtain an integrated value, and dividing the integrated value by the specific energy range.

[0197] Figure 6 Includes a plot of relative light output as a function of energy for a sample. Figure 6As can be seen in the graph, as the energy decreases, the ratio becomes worse. Compared to the Ca co-doped and standard samples, the Sr co-doped sample has the best ratio. At low energies, the improvement is extremely obvious. At energies in the range of 32keV to 81keV, the average light output of the Sr co-doped sample is about 1.09. For the same energy range, the Ca-doped sample (about 1.15) shows an improvement over the standard sample (about 1.16). Improvements are still visible at medium energies. For energies in the range of 122keV to 511keV, the Sr co-doped sample has a relative light output of about 1.04, the Ca co-doped sample has a relative light output of about 1.06, and the standard sample has a relative light output of about 1.07.

[0198] Single crystals were obtained from melts containing NaI,Tl at 0.1 atomic % relative to NaI, with or without co-doping. 2+ 0.1 atomic %, 0.3 atomic % and 0.6 atomic % are present, and Sr 2+ Present at 0.05 atomic %, 0.1 atomic %, 0.2 atomic % and 0.4 atomic %. Crystals formed from the melt had the compositions listed in Table 5 below.

[0199] Table 5 - Crystal Composition

[0200] <![CDATA[Codoping a > <![CDATA[[Tl + ] b ]]> <![CDATA[[Sr 2+ ] b or [Ca 2+ ] b ]]> <![CDATA[Only Tl + > 0.08±0.03% 0 <![CDATA[0.05%Sr 2+ ]]> 0.08±0.05% 0.05±0.02% <![CDATA[0.1%Sr 2+ ]]> 0.05±0.02% 0.11±0.01% <![CDATA[0.2%Sr 2+ ]]> 0.06±0.04% 0.18±0.01% <![CDATA[0.4%Sr 2+ ]]> 0.09±0.06% 0.52±0.08% <![CDATA[0.1%Ca 2+ ]]> 0.06±0.03% 0.09±0.03% <![CDATA[0.3%Ca 2+ ]]> 0.03±0.01% 0.21±0.03% <![CDATA[0.6%Ca 2+ ]]> 0.07±0.02% 0.47±0.02%

[0201] a Relative to Na + Atomic % in the melt.

[0202] b Measured in grown crystals using Inductively Coupled Plasma - Optical Emission Spectroscopy (ICP-OES); in atomic %.

[0203] The decay time of the test crystals was determined by fitting the average trace corresponding to the 662keV photopeak with an exponential decay function. Thirty traces were averaged for each measurement. The scintillation pulses were fitted with a double exponential decay function. A summary of the fast and slow decay times is listed in Table 6.

[0204] Table 6 - Crystal attenuation components

[0205] Co-doping <![CDATA[τ 初级 (ns)]]> <![CDATA[τ 次级 (ns)]]> <![CDATA[Only Tl + > <![CDATA[220±10 a (96%) b ]]> 1500±200(4%) <![CDATA[0.05%Sr 2+ ]]> 201±21(94%) 860±240(6%) <![CDATA[0.1%Sr 2+ ]]> 172±10(92%) 860±160(8%) <![CDATA[0.2%Sr 2+ ]]> 195±16(96%) 690±90(4%) <![CDATA[0.4%Sr 2+ ]]> 195±7(96%) 1000±300(4%) <![CDATA[0.1%Ca 2+ ]]> 199±10(95%) 1030±150(5%) <![CDATA[0.3%Ca 2+ ]]> 173±12(94%) 830±230(6%) <![CDATA[0.6%Ca 2+ ]]> 186±11(94%) 870±110(6%)

[0206] a The uncertainty is the standard deviation of sample measurements from the same crystal ingot.

[0207] b The values ​​in parentheses are the percentage of the total scintillation light that is in that particular decay component. The uncertainty is 1% to 2%.

[0208] On average, with 0.1% Sr 2+ and 0.3% Ca 2+ The co-doped crystals of 1:1 and 1:2 show the shortest decay among their counterparts. Both show an exceptionally fast primary decay time of about 170 ns, which is much faster than the standard NaI:Tl. + The primary decay time is 20% faster. The fastest decay recorded is from 0.3% Ca 2+ Sample of co-doped crystal. The sample shows a decay time of 155ns (92%) + 530ns (8%).

[0209] It should be noted that not all activities described in the general description or examples above are required, a portion of a specific activity may not be required, and one or more other activities in addition to the activities described may be performed. Further, the order in which the activities are listed is not necessarily the order in which they are performed.

[0210] For the sake of clarity, certain features described herein in the context of separate embodiments may also be provided in combination in a single embodiment. Conversely, for the sake of brevity, various features described in the context of a single embodiment may also be provided individually or in any sub-combination. In addition, reference to values ​​stated in ranges includes every value within the range.

[0211] Benefits, other advantages, and solutions to problems are described above with respect to specific embodiments. However, these benefits, advantages, solutions to problems, and any feature(s) that may make any benefit, advantage, or solution occur or become more significant should not be construed as important, necessary, or essential features of any or all claims.

[0212] The description and illustration of the embodiments described herein are intended to provide a general understanding of the structures of different embodiments. The description and illustration are not intended to serve as a detailed and comprehensive description of all elements and features of the equipment and systems using the structures or methods described herein. In a single embodiment, a separate embodiment can also be provided in combination, and conversely, for the sake of brevity, the various features described in the case of a single embodiment can also be provided individually or in any sub-combination. In addition, the values ​​stated in the range are mentioned to include each value in the range. Only after reading this specification, a skilled person can understand many other embodiments. Other embodiments can be used and the embodiments can be derived from the present disclosure, so that without departing from the scope of the present invention, structural substitution, logical substitution or another change can be performed. Therefore, the present disclosure should be regarded as illustrative and not restrictive.

Claims

1. A scintillation crystal comprising NaX:Tl,ME, wherein: X represents a halogen; ME is Sc, Y, Lu, Yb or any combination thereof; Tl has 1×10 -5 mol% to 0.2mol% dopant concentration; and ME has 1×10 -5 mol% to 0.5mol% dopant concentration; and The scintillation crystal has the following properties: For radiation in the range of 300 nm to 700 nm, the emission maximum is at a wavelength no greater than 430 nm upon exposure to gamma radiation having an energy of 60 keV.

2. The scintillation crystal according to claim 1, wherein RE has at least 1×10 -4 mol% dopant concentration. The scintillation crystal of claim 1 , wherein X is a combination of I and Br. The scintillation crystal of claim 1 , wherein X is I.

5. A method comprising: Providing a scintillation crystal according to claim 1; capturing radiation within said scintillation crystal; determining a pulse decay time and actual light output of said captured radiation; determining an estimated light output corresponding to said pulse decay time; and An adjusted light output is calculated, the adjusted light output being the product of the actual light output multiplied by the light output of NaX:Tl divided by the estimated light output.

6. A scintillation crystal comprising NaX:Tl,Me 2+ and RE, where: X represents a halogen; Me 2+ It represents a divalent metal element; RE stands for rare earth element; Tl has 1×10 -5 dopant concentrations ranging from mol% to 0.2mol%; Me 2+ having a dopant concentration in the range of 0.9 mol % to 5 mol %; and Wherein the scintillation crystal has a pulse decay time that is at least 5% less than a pulse decay time of the NaI:Tl crystal when the scintillation crystal and the NaI:Tl crystal are measured at 22° C. and exposed to gamma radiation having an energy of 662 keV.

7. The scintillation crystal of claim 6, wherein Me 2+ It is Sr, and has a concentration of not more than 0.9 mol%.

8. The scintillation crystal of claim 6, having an energy resolution of less than 6.4% when measured at 662 keV, 22°C, and 1 microsecond integration time.

9. A scintillation crystal comprising NaX:Tl,Me 2+ and RE, where: X represents a halogen; Me 2+ It represents a divalent metal element; RE stands for rare earth element; Tl has 1×10 -5 mol% to 0.2mol% dopant concentration; and Wherein the scintillation crystal has a pulse decay time that is at least 5% less than a pulse decay time of the NaI:Tl crystal when the scintillation crystal and the NaI:Tl crystal are measured at 22° C. and exposed to gamma radiation having an energy of 662 keV.

10. The scintillation crystal of claim 9, wherein Me 2+ Having a concentration of not more than 5 mol%.

11. The scintillation crystal of claim 9, wherein the scintillation crystal has an energy resolution of less than 6.4% when the scintillation crystal and the NaI:Tl crystal are measured at 662 keV, 22°C, and 1 microsecond integration time.

12. The scintillation crystal of claim 9, wherein at energies in the range of 32 keV to 81 keV, the scintillation crystal has an average relative light output as normalized to the light output at 2615 keV of no greater than 1.

15.

13. The scintillation crystal of claim 9, wherein at energies in the range of 122 keV to 511 keV, the scintillation crystal has an average relative light output as normalized to the light output at 2615 keV of no greater than 1.

07.

14. A scintillating crystal comprising NaX:Tl,Me, wherein: X represents a halogen; Me represents a Group 1 element, a Group 2 element or any combination thereof; Tl has 1×10 -5 dopant concentrations ranging from mol% to 0.2mol%; Me has a dopant concentration in the range of 0.9 mol % to 5 mol %; and The scintillation crystal has the following properties: An energy resolution of less than 6.4% when measured at 662 keV, 22°C and 1 microsecond integration time; or The pulse decay time is lower than that of another scintillation crystal having a NaX:Tl composition.

15. The scintillation crystal according to claim 14, wherein Me represents a Group 1 element and has a -5 Concentrations ranging from mol% to 9mol%. The scintillation crystal according to claim 15 , wherein Me is Rb, Cs or any combination thereof.

17. A well logging device comprising: A scintillation crystal in the well logging device, wherein the scintillation crystal comprises the scintillation crystal of claim 6.

18. A medical imaging device comprising: A scintillation crystal in the medical imaging device, the scintillation crystal comprising NaX:Tl,Me 2+ and R.E. in: X represents a halogen; Me 2+ It represents a divalent metal element; RE represents a rare earth element; and Tl has 1×10 -5 dopant concentrations ranging from mol% to 0.2mol%; The scintillation crystal has the following properties: For radiation in the range of 300 nm to 700 nm, the emission maximum is at a wavelength no greater than 430 nm upon exposure to gamma radiation having an energy of 60 keV.

19. A medical imaging device comprising: A scintillation crystal in the medical imaging device, the scintillation crystal comprising the scintillation crystal according to claim 14.

20. The medical imaging device of claim 19, wherein the scintillator crystal has an energy resolution of less than 6.4% when measured at 662 keV, 22°C, and 1 microsecond integration time.