A medical fabric with high dimensional stability and preparation method thereof

By using a multi-layered interwoven structure and conductive yarn design, the problems of poor elasticity, poor breathability, and easy wrinkling of medical fabrics are solved, achieving high dimensional stability and multiple durability functions, and improving the comfort and protective performance of medical clothing.

CN111575896BActive Publication Date: 2024-11-29ZHEJIANG ADIENT WANFANG TEXTILE TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202010332589.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-04-24
Publication Date
2024-11-29
Estimated Expiration
2040-04-24

AI Technical Summary

Technical Problem

Existing medical fabrics have poor elasticity, poor breathability, poor dimensional stability, and are prone to wrinkling. They also have limited functionality, which affects the comfort and professional dignity of medical staff.

Method used

The fabric employs a multi-layer structure design, including a first polyester filament layer, a second polyester filament layer, a first extension layer, a matrix layer, and a second extension layer. These layers are interwoven in a fully threaded manner to form a medical fabric with high dimensional stability. The matrix layer is formed by combining conductive yarn with cotton yarn, and titanium dioxide and conductive filaments are added to enhance wrinkle resistance and conductivity.

Benefits of technology

It achieves high elasticity, breathability, and wrinkle resistance, while also possessing multiple durable functions such as antibacterial, antistatic, moisture-wicking and quick-drying, and easy stain removal, thus improving the overall protective performance and wearing comfort of medical protective clothing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111575896B_ABST
    Figure CN111575896B_ABST
Patent Text Reader

Abstract

The invention discloses a medical fabric with high dimensional stability, comprising: a first polyester layer, which is formed by polyester yarns being strung and looped in sequence in a full-threading manner; a second polyester layer, which is formed by polyester yarns being strung and looped in sequence in a full-threading manner; a first extension layer, which is formed by polyester yarns being strung and looped in sequence in a full-threading manner, and is continuous with the second polyester layer; a base layer, which is formed by first cotton yarn and conductive yarn being strung and looped in sequence in a full-threading manner, and the conductive yarn is formed by conductive yarn and second cotton yarn being paralleled; and a second extension layer, which is formed by polyester yarns being strung and looped in sequence in a full-threading manner, and is continuous with the first polyester layer. The invention not only has relatively excellent elasticity and dimensional stability, but also has good air permeability and wrinkle resistance, and at the same time has a variety of durable composite functions such as antibacterial, antistatic, moisture absorption and quick drying, easy decontamination, etc., which meets the use of medical staff in a variety of occasions, protects the privacy of medical staff, and maintains the professional dignity of medical staff.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textile fabrics, and in particular relates to a medical fabric with high dimensional stability and a preparation method thereof. Background Art

[0002] The development of medicine has provided better protection for human health, but the working environment of medical staff is still very easy to be exposed to toxic and harmful gases or aerosols, harmful blood or body fluids, and harmful infectious viruses. Therefore, medical staff need to wear professional medical clothing to isolate germs, viruses, and harmful ultrafine dust, etc., to keep the environment healthy and clean. Medical professional clothing is a professional uniform for medical staff and an identity label. While ensuring that medical staff can cope with a variety of work occasions, it also reflects the professional dignity of medical staff.

[0003] The characteristics of medical fabrics determine the characteristics of their final products. Currently, most medical fabrics are woven fabrics, which have disadvantages such as poor elasticity, poor air permeability, poor dimensional stability, and easy wrinkling after washing. At the same time, the functionality is relatively single and will be significantly weakened with the increase in the number of washings, which seriously affects the wearing comfort of medical staff and reduces the professional dignity that medical staff should have. Therefore, it is urgent to innovate medical fabrics to address the above problems and develop new medical fabrics with stable dimensions and multiple durable functions. Summary of the invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the shortcomings of the prior art medical fabrics such as poor elasticity, poor air permeability, poor dimensional stability and easy wrinkling after washing, while giving the product a variety of durable functions.

[0005] To this end, the technical solution adopted is that a medical fabric with high dimensional stability of the present invention comprises:

[0006] Including the following settings:

[0007] The first polyester yarn layer is formed by stringing polyester yarns in sequence into loops in a full-threading manner;

[0008] The second polyester yarn layer is formed by stringing polyester yarns in sequence into loops in a full-threading manner;

[0009] The first stretching layer is formed by full-threading polyester yarns in sequence and is continuous with the second polyester yarn layer;

[0010] The base layer is formed by full-threading of the first cotton yarn and the conductive yarn, wherein the conductive yarn is formed by paralleling the conductive silk and the second cotton yarn, and the distance between any two conductive yarns is 1.5 cm to 2.1 cm;

[0011] The second stretching layer is formed by polyester yarns being threaded back and forth in sequence in a full-threading manner and is continuous with the first polyester yarn layer.

[0012] Preferably, the conductive thread is made by blending or composite spinning conductive microparticles and high molecular polymers, and the specification of the conductive thread is 20-30D.

[0013] Preferably, the first polyester filament layer includes a plurality of first yarns, and each of the first yarns completes a reciprocating lateral movement in front of two adjacent knitting needles to form a first coil;

[0014] The second polyester filament layer includes a plurality of second yarns, each of which moves back and forth in front of two knitting needles to form a second coil;

[0015] The first extension layer includes a plurality of third yarns, the third yarns are continuous with the second yarns, and each of the third yarns completes a reciprocating transverse movement on the back of two knitting needles to form an inner layer extension line;

[0016] The second extension layer includes a plurality of fourth yarns, which are continuous with the first yarns. Each of the fourth yarns completes a reciprocating lateral movement on the backs of two adjacent knitting needles to form an outer extension line.

[0017] Preferably, in the base layer, the twist of the conductive yarn is 250 to 350 twists / m, and the ratio of the conductive yarn to the first cotton yarn is 1:20 to 1:35.

[0018] Preferably, the cotton yarn is a single-ply combed pure cotton yarn of 28 to 60 counts or a double-ply combed pure cotton yarn of 56 to 120 counts, and the usage ratio is 10 to 20%.

[0019] Preferably, the polyester yarn is full-dull yarn, and the content of titanium dioxide in the polyester yarn is greater than or equal to 2.5%.

[0020] Preferably, the first cotton yarn and the second cotton yarn are replaced by a first polyester yarn and a second polyester yarn, respectively.

[0021] The present invention also provides a method for preparing the medical fabric with high dimensional stability as described above, characterized in that it comprises the following steps:

[0022] The following steps are involved:

[0023] Prepare conductive yarn for standby use, parallel the conductive yarn and the second cotton yarn / polyester yarn to form conductive yarn, and control the distance between any two conductive yarns after paralleling to be 1.5 cm to 2.1 cm;

[0024] Warping, on a warping machine, respectively warping the first cotton yarn, the conductor yarn and the polyester yarn;

[0025] Warp weaving, weaving the warped conductive yarn and the first cotton yarn in the form of weft insertion to form a base layer, weaving the polyester yarn and the base layer at the same time to form a first polyester yarn layer and a second extension layer, a second polyester yarn layer and a first extension layer respectively inserted on both sides of the base layer, and obtaining the grey cloth of the fabric after weaving, and storing it;

[0026] The grey cloth is scourged and bleached in a high temperature and high pressure liquid flow dyeing machine at a temperature of 90-110°C, a bleaching time of 30-60 minutes, and a bath ratio of 1:8-1:15;

[0027] For the first shaping, positive overfeeding process is adopted, the cloth feeding speed is greater than the speed of the stenter or shaping machine, the temperature is 180-220℃, and the cloth feeding speed is 15-30m / min;

[0028] Dyeing, adding dyes, moisture absorbing quick-drying aids and antibacterial agents for dyeing, and after dyeing, using a soaping-hot washing-neutralization process for post-treatment;

[0029] The second shaping process uses a positive overfeeding process to obtain medical fabrics after shaping.

[0030] Preferably, in the warping step, the warping speed of the polyester yarn is 300 to 700 m / min, and the warping tension is 0.15 to 0.25 cn / dtex;

[0031] For the warping of cotton yarn, the warping speed is 200-600 m / min and the warping tension is 0.15-0.20 cn / dtex.

[0032] Preferably, the first polyester filament layer includes a plurality of first yarns, and each of the first yarns completes a reciprocating lateral movement in front of two adjacent knitting needles to form a first coil;

[0033] The second polyester filament layer includes a plurality of second yarns, each of which moves back and forth in front of two knitting needles to form a second coil;

[0034] The first extension layer includes a plurality of third yarns, the third yarns are continuous with the second yarns, and each of the third yarns completes a reciprocating transverse movement on the back of two knitting needles to form an inner layer extension line;

[0035] The second extension layer includes a plurality of fourth yarns, which are continuous with the first yarns. Each of the fourth yarns completes a reciprocating lateral movement on the backs of two adjacent knitting needles to form an outer extension line.

[0036] Preferably, in the step of scouring and bleaching the grey cloth, 3 to 5 g / L of hydrogen peroxide and 3 to 5 g / L of sodium hydroxide are added as bleaching aids.

[0037] Preferably, in the first shaping step, the temperature is selected to be 180-220° C. and the speed is selected to be 15-30 m / min.

[0038] Preferably, in the dyeing step, the dyeing temperature is 125-135° C., the dyeing time is 30-60 min, and the bath ratio is 1:8-1:15.

[0039] Preferably, in the second shaping step, the temperature is selected to be 180-200° C., the speed is 15-30 m / min, and a resin finishing agent is added.

[0040] The technical solution of the present invention has the following advantages: the present invention not only has relatively excellent elasticity and dimensional stability, but also has good air permeability and wrinkle resistance, and at the same time has multiple durable composite functions such as antibacterial, antistatic, moisture absorption and quick drying, easy decontamination, etc. The medical professional clothing made of it is more comfortable due to its good elasticity, durable and shrink-proof due to its good dimensional stability, not stuffy due to its good air permeability, and wrinkle-free after washing due to its good wrinkle resistance. It meets the use of medical staff in various occasions such as instrument rooms, wards and offices. While effectively improving the comprehensive protection performance, it also protects the privacy of medical staff and maintains the professional dignity of medical staff.

[0041] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures particularly pointed out in the written description, claims, and drawings.

[0042] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0044] Figure 1 is a side view of the present invention;

[0045] Figure 2 A top view of the present invention;

[0046] Figure 3 It is a schematic diagram of the structure of the second polyester filament layer and the first extension layer in the present invention;

[0047] Figure 4 It is a schematic diagram of the structure of the substrate layer in the present invention;

[0048] Figure 5A schematic diagram of the structure of the first polyester yarn layer and the second stretching layer in the present invention.

[0049] The markings in the attached drawings are as follows: 1-first polyester filament layer; 2-second polyester filament layer; 3-first extension layer, 4-base layer; 5-second extension layer. DETAILED DESCRIPTION

[0050] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0051] In the description of the present application, it should be understood that the orientation or positional relationship indicated by the terms "middle", "top", "bottom", "inside", "outside", etc. is based on the orientation or positional relationship shown in the accompanying drawings, and is only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. The terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0052] In addition, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0053] In the present application, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0054] See also Figure 1-Figure 5 As shown, the present invention provides a medical fabric with high dimensional stability, comprising:

[0055] The first polyester yarn layer 1 is formed by sequentially stringing polyester yarns into loops in a full-threading manner;

[0056] The second polyester yarn layer 2 is formed by sequentially stringing polyester yarns into loops in a full-threading manner;

[0057] The first stretching layer 3 is formed by full-threading polyester yarns in sequence and is continuous with the second polyester yarn layer;

[0058] The base layer 4 is formed by the first cotton yarn and the conductive yarn being fully threaded back and forth, the conductive yarn is formed by the conductive filament and the second cotton yarn being paralleled, and the twist of the conductive yarn is 250-350 twists / m;

[0059] The second stretching layer 5 is formed by polyester yarns being threaded back and forth in sequence in a full-thread manner, and is continuous with the first polyester yarn layer.

[0060] Among them, the first polyester silk layer 1 includes a plurality of first yarns, each of which completes a reciprocating lateral movement in front of the needles of two adjacent knitting needles to form a first coil. The second polyester silk layer 2 includes a plurality of second yarns, each of which completes a reciprocating lateral movement in front of the needles of two knitting needles (the first and the third) to form a second coil. The first extension layer 3 includes a plurality of third yarns, the third yarn is continuous with the second yarn, and actually belongs to the same continuous yarn, and each third yarn completes a reciprocating lateral movement on the back of the needles of two knitting needles (the first and the third) to form an inner extension line. The second extension layer 5 includes a plurality of fourth yarns, the fourth yarn is continuous with the first yarn, and actually belongs to the same continuous yarn, and each fourth yarn completes a reciprocating lateral movement on the back of the needles of two adjacent knitting needles to form an outer extension line.

[0061] In this structure, the first polyester filament layer 1, the second polyester filament layer 2, the first extension layer 3, the second extension layer 5 and the base layer 4 all adopt a "full-through" yarn threading method. The base layer 4 has no connection with the other layers and is wrapped in the middle. This structure can greatly improve the air permeability and moisture absorption and quick-drying properties of the fabric, ensuring that it is not stuffy when worn, and has better elasticity to ensure comfortable wearing. In addition, the multi-layer structure can greatly improve the stability of the fabric.

[0062] In order to achieve low reflection and low light transmittance of the product, the content of titanium dioxide in the polyester yarn is not less than 2.5%, which is a fully matte yarn. Titanium dioxide, commonly known as titanium dioxide, is a white opaque powder. As an additive, it can reduce the transparency of polyester yarn. As its addition amount increases, the reflection and light transmittance on the polyester yarn decrease. According to its addition amount, from high to low, they are respectively high gloss yarn (0%), glossy yarn (0.1%), semi-matte yarn (0.3% to 0.5%) and fully matte yarn (2.5% and above). The number of pores increases the number of reflections and refractions of light on the polyester yarn, further reducing the reflection and light transmittance of the product. At the same time, for yarns of the same thickness, due to the increase in the number of pores, the single fiber diameter is less than 1.1dtex (fine denier fiber), giving the fabric a more delicate surface style and comfortable feel. The special-shaped cross-section increases the specific surface area of ​​the fiber and improves the moisture absorption and quick-drying performance.

[0063] Preferably, the present invention uses full-dull fine-denier polyester yarn with a specification of 45 to 90 deniers, the number of holes is selected to be 24 to 144 holes, the fiber cross-section is round or shaped, etc., and it is woven in the form of warp plain or warp satin organization.

[0064] The fully matte sliced ​​polyester yarn not only reduces the reflection and glittering of the fiber, but also makes the subsequent fiber have the advantages of soft luster, good deep dyeing, high fabric drape, strong shielding performance, etc., which can meet the needs of making advanced medical clothing.

[0065] Regarding the base layer 4, the conductive yarn is formed by paralleling the conductive yarn with the second cotton yarn. The conductive yarn after paralleling improves the overall strength, facilitates the knitting operation, and will not break. Then, the conductive yarn after paralleling is interwoven with the first cotton yarn in a full-threading manner. The distance between any two conductive yarns is 1.5cm to 2.1cm, and the ratio of the conductive yarn to the first cotton yarn is 1:20 to 1:35. The base layer formed by this structure improves the strength and stability of the medical fabric with high dimensional stability after weaving.

[0066] Furthermore, the conductive yarn can adopt a hollow structure of three concentric circles, or a solid structure, and the conductive component is sandwiched in the middle layer to form a composite fiber. This sandwich structure allows the conductive component to be close to the surface and wrapped in the middle, so the whiteness is increased and it is resistant to washing and friction, and the conductive effect is good and durable. The non-conductive component and the conductive component in the conductive yarn are in a ratio of 80:20 to 60:40. Since the higher the proportion of the conductive component, the better the antistatic performance, but the flexibility decreases, the conductive yarn using this ratio of the present invention has better conductive performance, and the flexibility also meets the requirements.

[0067] After the conductive carbon powder is fully mixed with the molten polyamide, it is compounded with the matrix polyamide through the spinneret hole to form a two-component conductive yarn, the outer layer of which is an ultra-thin skin-like conductive polymer with high conductivity, and the inner part is completely nylon 6 polymer. This conductive yarn has a larger conduction area and more stable and durable antistatic performance.

[0068] Cotton yarn has good hygroscopicity and capillary effect, which can significantly improve the air permeability and skin touch of fabrics. However, due to its strength, hairiness, yarn knots and yarn dryness and other technical factors, it is difficult to produce on a warp knitting machine. In order to overcome this problem, in the present invention, all the first cotton yarns used are single-strand combed pure cotton yarns of 28 to 60 or double-strand combed pure cotton yarns of 56 to 120, and the use ratio is 10 to 20%. It is woven in the form of weft insertion. Combed cotton refers to the process of adding a delicate combing procedure during the spinning process. The method is to comb out the shorter fibers and remove impurities in the cotton to produce smooth yarn, making the cotton more resilient and not easy to pilling, and the quality of the cotton is more stable. This first cotton yarn has greater strength and toughness, and more perfect performance. In the present invention, the first cotton yarn and the second cotton yarn can be selected as cotton yarns with the same specifications and performance.

[0069] In the present invention, the first cotton yarn and the second cotton yarn can also be replaced by the first polyester yarn and the second polyester yarn, or the first nylon and the second nylon, etc. That is, when the conductive yarn is formed by the conductive yarn and the second cotton yarn in parallel, the base layer 1 is formed by the conductive yarn after the paralleling and the first cotton yarn interwoven. When the conductive yarn is formed by the conductive yarn and the second polyester yarn in parallel, the base layer 1 is formed by the conductive yarn after the paralleling and the first polyester yarn interwoven. The first polyester yarn and the second polyester yarn can also be selected as polyester yarns with the same specifications and performance. However, it is usually not the customized full matte yarn described above, but usually polyester yarns of other thicknesses, whose thickness is close to the thickness of the first cotton yarn and the second cotton yarn, so as to facilitate the combination with the conductive yarn or conductive yarn.

[0070] The conductive yarn is made of conductive microparticles and high molecular polymers blended or composite spinning. The corona discharge effect can avoid high voltage static electricity accumulation. Since its conductive performance is mainly based on the movement of free electrons and does not rely on moisture absorption and ion transfer, it still has excellent conductive and antistatic properties under relatively low humidity.

[0071] Preferably, the specification of the conductive yarn is 20-30D, and the proportion of the conductive yarn is controlled to be not less than 0.1%. After being paralleled with the second cotton yarn / the second polyester yarn, the conductive yarn is woven into the yarn in the form of weft insertion.

[0072] The present invention also provides a method for preparing the medical fabric with high dimensional stability as described above, comprising the following steps:

[0073] Prepare conductive yarn for standby use, and perform parallel processing on the conductive yarn and the second cotton yarn / polyester yarn to form conductive yarn, and control the twist of the conductive yarn after paralleling to be 250-350 twists / meter. The specific paralleling method and parameter ratio are as described above and will not be repeated here;

[0074] Warping, on a warping machine, respectively warping the first cotton yarn, the conductor yarn and the polyester yarn;

[0075] Warp knitting, the warped conductive yarn and the first cotton yarn are knitted in the form of weft insertion to form a base layer, and the polyester yarn and the base layer are knitted at the same time to form a first polyester yarn layer 1 and a second extension layer 5, a second polyester yarn layer 2 and a first extension layer 3 respectively inserted on both sides of the base layer. The structures and needle threading methods of the first polyester yarn layer 1 and the second extension layer 5, the second polyester yarn layer 2 and the first extension layer 3 are as described above and will not be repeated. After knitting, the grey cloth of the fabric is obtained and stored;

[0076] The grey cloth is scourged and bleached in a high temperature and high pressure liquid flow dyeing machine at a temperature of 90-110°C, a bleaching time of 30-60 minutes, and a bath ratio of 1:8-1:15;

[0077] For the first shaping, positive overfeeding process is adopted, the cloth feeding speed is greater than the speed of the stenter or shaping machine, the temperature is 180-220℃, and the cloth feeding speed is 15-30m / min;

[0078] Dyeing, adding dyes, moisture absorbing quick-drying aids and antibacterial agents for dyeing, and after dyeing, using a soaping-hot washing-neutralization process for post-treatment;

[0079] The second shaping process uses a positive overfeeding process to obtain medical fabrics after shaping.

[0080] In the warping step, the polyester yarn is warped at a warping speed of 300 to 700 m / min and a warping tension of 0.15 to 0.25 cn / dtex;

[0081] For the warping of cotton yarn, the warping speed is 200-600 m / min and the warping tension is 0.15-0.20 cn / dtex to ensure the stability of the weaving tension.

[0082] During the warp knitting process, three or more combs are used to complete the weaving of the grey cloth. Different raw materials are woven into different layers according to their characteristics, and their respective organizational forms and yarn threading methods are interwoven to form fabrics of different styles and textures. The multi-comb design ensures the anti-see-through nature of the fabric and makes the product comfortable to wear.

[0083] The present invention adopts 3 or more combs for production, the outer layer (first polyester filament layer 1 and second extension layer 5) is polyester filament, and the comb is mainly DTY; the middle layer (base layer 4) is cotton yarn and conductive yarn, the inner layer (second polyester filament layer 2 and first extension layer 3) is polyester filament, and the comb is DTY or FDY.

[0084] The multi-layer structure design makes the fabric thicker, increases the shielding and structural stability, and makes the fabric more durable. At the same time, the conductive yarn is woven into the fabric using the weft insertion structure to reduce the extreme bending of the conductive yarn. This not only greatly reduces the frequency of yarn breakage during the weaving process, but also avoids mechanical damage to the conductive yarn caused by severe washing during use.

[0085] The invention changes the style or texture of the product by selecting the raw material variety and specification, designing different comb numbers, organizational structures and threading methods. The relative positions of the loop forming parts must be adjusted on the machine, and the tension compensation setting must be adjusted according to the product, so that the warp tension is controlled at 15-20cN to ensure smooth weaving.

[0086] The key to weaving cotton yarn and conductive yarn is to weave them into the inside in the form of weft insertion to reduce the influence of yarn knots and uneven yarn on the appearance quality of the fabric.

[0087] The key to long-lasting antistatic properties is that the proportion of conductive yarn used is not less than 0.1% to ensure compliance with corresponding technical indicators while controlling production costs.

[0088] In the scouring and bleaching step of the grey cloth, 3-5 g / L of hydrogen peroxide and 3-5 g / L of sodium hydroxide are added as bleaching aids. This bleaching is to remove the colloidal impurities in the cotton yarn, improve the whiteness of the cotton yarn, and facilitate uniform coloring and color control.

[0089] The first shaping is the core process of the product, which directly affects the dimensional stability of the final product. In the production process of the product, the present invention undergoes two processes: scouring and bleaching of the grey cloth and the first shaping. In the first shaping step, the temperature is selected to be 180-220°C and the speed is 15-30m / min. In addition, the positive overfeeding process is adopted, which can improve the longitudinal stability of the fabric, so that the dimensional stability of the final product can reach a dimensional change rate of ±3% after boiling in boiling water for 30 times.

[0090] The first setting before dyeing uses a high temperature of 180℃ to 220℃ to fully heat the fabric, and under tension, the internal molecules of the fabric melt and recrystallize, and maintain a high dimensional stability below this temperature; when entering the dyeing process, since the dyeing temperature is only around 130℃, which is far below the setting temperature, the dimensional stability of the fabric after dyeing is very high and the dimensional change rate is very small.

[0091] In the dyeing process, the dyeing temperature is 125-135℃, the dyeing time is 30-60min, and the bath ratio is 1:8-1:15. A large number of experiments have proved that at this temperature, the molecular gap is fully opened, and the addition of moisture-absorbing quick-drying additives and antibacterial agents at this stage can ensure that the effective molecules of the additives are firmly combined with polyester, which is also the essential reason why the product can achieve long-lasting functionality. It ensures the sweat absorption and antibacterial functions, and ensures the core functionality of continuous durability. Taking antibacterial as an example, it can reach antibacterial AAA level after 50 washings. The choice of dyeing time and bath ratio ensures sufficient dyeing and improves the overall aesthetics of the fabric.

[0092] If you want to produce a high-quality dark product, you need to focus on maintaining color fastness, which can be achieved by adding a soaping process to wash away the floating color on the surface.

[0093] In the second shaping step, the temperature is selected to be 180-200°C, the speed is 15-30m / min, and a resin finishing agent is added to improve the feel. Since this process ultimately determines the dimensional stability of the product, a smaller width setting is selected as much as possible during the shaping process. In this process, the shaping temperature and speed determine the degree to which the product is subjected to heat in the shaping machine. The higher the degree, the slower the speed, the higher the degree of heat action, and the better the shaping effect. However, too high a temperature will cause the product to change color, and too slow a speed will also cause the product to change color. Too fast a speed will cause the shaping effect to deteriorate and reduce the dimensional stability. The present invention has been determined through a large number of experiments that when the temperature is 180-200°C and the speed is 15-30m / min, the shaping effect is good, the product has strong stability, and the feel is also improved. At the same time, the positive overfeeding process is still used in the second shaping to improve the stability of the fabric.

[0094] The invention not only has relatively good elasticity and dimensional stability, but also has good air permeability and wrinkle resistance, and at the same time has multiple durable composite functions such as antibacterial, antistatic, moisture absorption and quick drying, easy decontamination, etc. The medical professional clothing made of it is more comfortable due to its good elasticity, durable and non-shrinking due to its good dimensional stability, not stuffy due to its good air permeability, and not wrinkled after washing due to its good wrinkle resistance. It meets the use of medical staff in various occasions such as instrument rooms, wards and offices. While effectively improving the comprehensive protection performance, it also protects the privacy of medical staff and maintains the professional dignity of medical staff.

[0095] It should be noted that the above embodiments are all preferred embodiments, and the relevant functional components can be replaced by other components, and the units and modules involved are not necessarily required for this application. The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same and similar parts between the various embodiments can be referenced to each other.

[0096] The above is a detailed introduction to a medical fabric and a preparation method thereof provided by the present application. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method and core idea of ​​the present application; at the same time, for general technicians in this field, according to the idea of ​​the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A medical fabric with high dimensional stability, characterized in that: Including the following settings: The first polyester yarn layer is formed by stringing polyester yarns in sequence into loops in a full-threading manner; The second polyester yarn layer is formed by stringing polyester yarns in sequence into loops in a full-threading manner; The first stretching layer is formed by full-threading polyester yarns in sequence and is continuous with the second polyester yarn layer; The base layer is formed by full-threading of the first cotton yarn and the conductive yarn, wherein the conductive yarn is formed by paralleling the conductive silk and the second cotton yarn, and the distance between any two conductive yarns is 1.5 cm to 2.1 cm; The second stretching layer is formed by full-threading polyester yarns in sequence and is continuous with the first polyester yarn layer; The first polyester filament layer includes a plurality of first yarns, each of which completes a reciprocating lateral movement in front of two adjacent knitting needles to form a first coil; The second polyester filament layer includes a plurality of second yarns, each of which moves back and forth in front of two knitting needles to form a second coil; The first extension layer includes a plurality of third yarns, the third yarns are continuous with the second yarns, and each of the third yarns completes a reciprocating transverse movement on the back of two knitting needles to form an inner layer extension line; The second extension layer includes a plurality of fourth yarns, the fourth yarns are continuous with the first yarns, and each of the fourth yarns completes a reciprocating transverse movement on the backs of two adjacent knitting needles to form an outer extension line; In the base layer, the twist of the conductive yarn is 250 to 350 twists / meter, and the ratio of the conductive yarn to the first cotton yarn is 1:20 to 1:

35.

2. A medical fabric with high dimensional stability according to claim 1, characterized in that: The conductive thread is made by blending or composite spinning conductive microparticles and high molecular polymers, and the specification of the conductive thread is 20-30D.

3. The medical fabric with high dimensional stability according to claim 1, characterized in that: The first cotton yarn is a single-ply combed pure cotton yarn of 28 to 60 counts or a double-ply combed pure cotton yarn of 56 to 120 counts, with a usage ratio of 10 to 20%.

4. The medical fabric with high dimensional stability according to claim 1, characterized in that: The polyester yarn is full-dull yarn, and the content of titanium dioxide in the polyester yarn is greater than or equal to 2.5%.

5. The medical fabric with high dimensional stability according to claim 1, characterized in that: The first cotton yarn and the second cotton yarn are replaced by the first polyester yarn and the second polyester yarn respectively.

6. A method for preparing a medical fabric with high dimensional stability as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: Prepare conductive yarn for standby use, and parallel the conductive yarn with the second cotton yarn / polyester yarn to form the conductive yarn; Warping, on a warping machine, respectively warping the first cotton yarn, the conductive yarn and the polyester yarn, and controlling the finished product spacing between any two adjacent conductive yarns to be 1.5 cm to 2.1 cm; Warp weaving, weaving the warped conductive yarn and the first cotton yarn in the form of weft insertion to form a base layer, weaving the polyester yarn and the base layer at the same time to form a first polyester yarn layer and a second extension layer, a second polyester yarn layer and a first extension layer respectively inserted on both sides of the base layer, and obtaining the grey cloth of the fabric after weaving, and storing it; The grey cloth is scourged and bleached in a high temperature and high pressure liquid flow dyeing machine at a temperature of 90 to 110°C, a bleaching time of 30 to 60 minutes, and a bath ratio of 1:8 to 1:15; For the first shaping, positive overfeeding process is adopted, the cloth feeding speed is greater than the speed of the stenter or shaping machine, the temperature is 180-220°C, and the cloth feeding speed is 15-30m / min; Dyeing, adding dyes, moisture absorbing quick-drying aids and antibacterial agents for dyeing, and after dyeing, using a soaping-hot washing-neutralization process for post-treatment; The second shaping process uses positive overfeeding technology to obtain medical fabrics after shaping; The first polyester filament layer includes a plurality of first yarns, each of which completes a reciprocating lateral movement in front of two adjacent knitting needles to form a first coil; The second polyester filament layer includes a plurality of second yarns, each of which moves back and forth in front of two knitting needles to form a second coil; The first extension layer includes a plurality of third yarns, the third yarns are continuous with the second yarns, and each of the third yarns completes a reciprocating transverse movement on the back of two knitting needles to form an inner layer extension line; The second extension layer includes a plurality of fourth yarns, which are continuous with the first yarns. Each of the fourth yarns completes a reciprocating lateral movement on the backs of two adjacent knitting needles to form an outer extension line.

7. The preparation method according to claim 6, characterized in that: In the warping step, the polyester yarn is warped at a warping speed of 300 to 700 m / min and a warping tension of 0.15 to 0.25 cn / dtex; For the warping of cotton yarn, the warping speed is 200-600 m / min and the warping tension is 0.15-0.20 cn / dtex.

8. The preparation method according to claim 6, characterized in that: In the step of scouring and bleaching the grey cloth, 3-5 g / L of hydrogen peroxide and 3-5 g / L of sodium hydroxide are added as bleaching aids.

9. The preparation method according to claim 6, characterized in that: In the first shaping step, the temperature is selected to be 180-220°C and the speed is 15-30 m / min.

10. The preparation method according to claim 6, characterized in that: In the dyeing step, the dyeing temperature is 125-135° C., the dyeing time is 30-60 min, and the bath ratio is 1:8-1:

15.

11. The preparation method according to claim 6, characterized in that: In the second shaping step, a temperature of 180-200°C and a speed of 15-30 m / min are selected, and a resin finishing agent is added.

Citation Information

Patent Citations

  • Dyeing and finishing process of antibacterial antistatic highly-comfortable type warp-knitted fabric

    CN109385790A

  • Antistatic warp-knitted face fabric

    CN1804178A

  • Medical fabric with high dimensional stability

    CN212477055U