Improved positive electrode design and related preparation methods for solid-state lithium-sulfur batteries
By using N-C-Co composite material and PEO conductive layer in lithium sulfur batteries, the problems of lithium polysulfide dissolution and shuttle effect are solved, the electrochemical performance and capacity retention rate of lithium sulfur batteries are improved, and high porosity and The low-impedance battery structure enhances the stability and energy density of the battery.
Patent Information
- Application Number
- CN201910314215.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-04-18
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2039-04-18
AI Technical Summary
During the discharge process, lithium sulfur batteries have an intermediate product lithium polysulfide dissolution and shuttle effect, resulting in low efficiency and capacity decay of battery curloss, and a conductive agent is required to enhance conductivity, but it will reduce energy density.
A modified positive electrode design for solid lithium-sulfur batteries was designed, using N-C-Co composite material as the conductive layer, combining polyethylene oxide (PEO) and lithium salt, and preparing sulfur positive electrodes by heating or freeze-drying to form high porosity and low impedance battery structure reduces the shuttle effect of lithium polysulfide and improves the utilization rate of active substances.
The high porosity, low impedance and stable cycling performance of lithium sulfur batteries are achieved, the capacity retention rate and energy density of the battery are improved, the loss of lithium polysulfide is reduced, and the electrochemical performance of the battery is enhanced.
Smart Images

Figure CN111834660B_ABST
Abstract
Description
Technical Field
[0001] This article discloses the positive electrode design and related preparation method of solid-state lithium-sulfur battery. Background Art
[0002] Lithium-sulfur secondary batteries are a new type of reversible battery that uses active sulfur and metallic lithium as positive and negative electrode materials respectively. When an electrochemical reaction occurs, two electrons are transferred on each sulfur atom. According to the calculation of the sulfur positive electrode, the specific capacity and energy density of the battery can theoretically reach 1675mAh / g and 2600Wh / kg, which is much higher than the existing lithium-ion batteries with transition metal oxides as positive electrodes. In addition, sulfur resources are abundant in the earth's crust, low in cost, and environmentally friendly. Therefore, lithium-sulfur batteries are considered to be a strong competitor for the next generation of new energy storage systems.
[0003] However, despite the outstanding advantages of lithium-sulfur batteries, their development and application still face many technical challenges. The most important factors restricting their development are: (1) The active substance sulfur and its discharge product lithium sulfide are both highly insulating materials for ions and electrons. Therefore, a conductive agent needs to be added when preparing the positive electrode to enhance its conductivity, which will inevitably reduce the energy density of the lithium-sulfur battery; (2) During the discharge process of lithium-sulfur batteries, there is an intermediate product lithium polysulfide. Lithium polysulfide can dissolve in the electrolyte and produce a shuttle effect. It can directly react with the negative electrode to cause corrosion of metallic lithium, loss of active substances, and battery overcharge. The "shuttle effect" is the main reason for the low coulombic efficiency and capacity decay of the battery.
[0004] This article discloses an improved positive electrode design for a solid-state lithium-sulfur battery and related synthesis and preparation methods. Summary of the invention
[0005] Specifically, the designed lithium-sulfur battery includes: a substrate, a sulfur positive electrode on the substrate, a coating layer on the sulfur positive electrode, a first intermediate layer on the coating layer, a solid electrolyte on the first intermediate layer, a second intermediate layer on the solid electrolyte, and a metal lithium sheet on the second intermediate layer, wherein the coating layer is evenly coated in the pores of the positive electrode and is in direct contact with the substrate.
[0006] On the one hand, in combination with other examples, the coating layer includes at least one of the following materials: carbon polysulfide (CS), polyethylene oxide (PEO), polyaniline (PANI), polypyrrole (PPY), poly(3,4-dioxyethylenethiophene) (PEDOT), sulfide polystyrene sulfonic acid (PSS), polyacrylonitrile (PAN), polyacrylic acid (PAA), polyallylamine hydrochloride (PAH), polyvinylidene fluoride-hexafluoropropylene (P(VDF-co-HFP)), poly(methyl methacrylate) (PMMA), polyvinylidene fluoride (PVDF), poly(diallyldimethylammonium) bis(trifluoromethylsulfonylimide) imide (TFSI) (PDDATFSI) or a combination thereof.
[0007] On the one hand, in combination with other examples, the coating layer includes at least one lithium salt listed below: lithium bis(trifluoromethane)sulfonyl imide (LiN(CF3SO2)2) (LiTFSI), lithium perchlorate, lithium bis(oxalate) borate (LiBOB), lithium bis(fluorosulfonyl)imide (LiFSI), lithium trifluoromethanesulfonate (LiCF3SO3) (LiTf), lithium (trifluoromethanesulfonamide) (Li(C2F5SO2)2N) (LiBETI) or a combination thereof.
[0008] In one aspect, in combination with other examples, the coating layer elements include at least: nitrogen, carbon, cobalt, titanium, tantalum, tungsten and combinations thereof.
[0009] In one aspect, in combination with other embodiments, the coating layer comprises a carbon-nitrogen-cobalt (NC-Co) composite material.
[0010] In one aspect, in combination with other examples, the coating layer comprises polyethylene oxide and at least one of LiTFSI, LiTf, LiBETI and NC-Co composite materials.
[0011] In one aspect, in conjunction with other embodiments, the NC-Co composite comprises a regular dodecahedral morphology and at least one dimension having a diameter in the range of 10-50 nm.
[0012] On the one hand, in combination with other examples, NC-Co composites contain mesoporous structures with a specific surface area ranging from 100 to 300 m 2 / g.
[0013] In one aspect, in combination with other embodiments, the total thickness of the sulfur cathode and the coating layer is less than 200 μm.
[0014] In one aspect, in combination with other embodiments, the solid electrolyte includes at least one of the following: Li 6.4 LqCy 1.4 Ta 0.6 O 12 (LLZTO),Li10 GeP2S 12 ,Li 1.5 Al 0.5 Ge 1.5 (PO4)3,Li 1.4 Al 0.4 Ti 1.6 (PO4)3,Li 0.55 La 0.35 TiO3, interpenetrating polymer networks of poly(ethyl acrylate) (IPN-PEA) electrolytes, three-dimensional ceramic / polymer networks, in situ plasticized polymers, composite polymers with well-aligned ceramic nanowires, PEO-based solid polymers, flexible polymers, polymer ionic liquids, in situ formed Li3PS4 and their combinations.
[0015] In one aspect, in combination with other embodiments, the positive electrode has a porosity of at least 30%.
[0016] In one aspect, in combination with other embodiments, the positive electrode has a porosity of at least 60%.
[0017] In one aspect, in combination with other embodiments, the diameter of the pores in the positive electrode ranges from 1 μm to 50 μm.
[0018] On the one hand, in combination with other examples, the battery configuration has at least the following data: impedance below 250Ω·cm 2 , reversible capacity is at least 500mA / hg S 1 , the capacity retention rate is at least 40%.
[0019] In an example, a lithium-sulfur battery comprises: a sulfur cathode on a substrate, and a coating layer on the sulfur cathode; wherein the coating layer is a polyethylene oxide (PEO)-based lithium ion conductive coating layer containing an NC-Co composite material, and the coating layer exists in pores in the cathode.
[0020] On the one hand, in combination with other examples, the coating layer includes at least one lithium salt listed below: lithium bis(trifluoromethane)sulfonyl imide (LiN(CF3SO2)2) (LiTFSI), lithium perchlorate, lithium bis(oxalate)borate (LiBOB), lithium bis(fluorosulfonyl)imide (LiFSI), lithium trifluoromethanesulfonate (LiCF3SO3) (LiTf), lithium (trifluoromethanesulfonamide) (Li(C2F5SO2)2N) (LiBETI) or a combination thereof.
[0021] In one aspect, in conjunction with other embodiments, the NC-Co composite comprises a regular dodecahedral morphology and at least one dimension having a diameter in the range of 10-50 nm.
[0022] On the one hand, in combination with other examples, NC-Co composites contain mesoporous structures with a specific surface area ranging from 100 to 300 m 2 / g.
[0023] In one aspect, in combination with other embodiments, the total thickness of the sulfur cathode and the coating layer is less than 200 μm.
[0024] On the one hand, in combination with other examples, the battery configuration has at least the following data: impedance below 250Ω·cm 2 , reversible capacity is at least 500mA / hg S 1 , the capacity retention rate is at least 40%. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The following detailed description, taken in conjunction with the accompanying illustrations, will provide a more complete understanding of this article, in which:
[0026] According to relevant examples, Figure 1 The specific structure of the designed solid-state lithium-sulfur battery is explained.
[0027] According to relevant examples, Figure 2 Methods for preparing positive electrodes for lithium-sulfur batteries by (a) heating drying and (b) freeze drying are described.
[0028] According to relevant examples, Figure 3a shows a transmission electron microscope (TEM) image of the prepared ZIF-67; Figure 3b shows a scanning electron microscope (SEM) image of the NC-Co composite material; Figure 3c shows a TEM image of the NC-Co composite material; Figure 3d shows a high-resolution TEM image of the NC-Co composite material; Figure 3e shows a field emission SEM image of the NC-Co composite material; Figures 3f-h show element distribution diagrams of the three elements C, N, and Co in the NC-Co composite material.
[0029] According to relevant examples, Figure 4 The adsorption phenomenon of NC-Co composite material on lithium polysulfide (Li2S6) solution was demonstrated.
[0030] According to relevant examples, Figure 5a shows the X-ray diffraction (XRD) patterns of ZIF-67 and NC-Co composites, Figure 5b gives the nitrogen adsorption-desorption isotherm of ZIF-67; Figure 5c gives the nitrogen adsorption-desorption isotherm of NC-Co composites.
[0031] According to the relevant examples, Figures 6a-c show the X-ray photoelectron spectra of C 1s (Figure 6a), N 1s (Figure 6b), and Co2p3 / 2 (Figure 6c) in the NC-Co composite material.
[0032] According to the relevant example, Figure 7a shows a cross-sectional SEM image of the modified CS positive electrode covered with the improved NC-Co / PEO coating layer; Figures 7b-g give the element distribution diagrams of C, S, F, Co, O and Al of the modified CS positive electrode.
[0033] 8a and 8b show the impedance spectra of the batteries of Example 8 and Comparative Sample 1 ( FIG. 8a ) and Comparative Sample 2 ( FIG. 8b ) before cycling, respectively.
[0034] Figures 9a and b show the cycle performance of the lithium-sulfur battery of Example 8 (Figure 9a) and Comparative Sample 1 (Figure 9b), respectively. DETAILED DESCRIPTION
[0035] Some specific embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings. Where possible, the same reference numerals will be used throughout the drawings to represent the same or similar parts. The components in the drawings are not necessarily to scale, but emphasize the principles of the illustrated examples. It should be understood that the present application is not limited to the details or methods described in the description or shown in the drawings. In addition, the terms are used for description only and should not be regarded as limiting terms.
[0036] In addition, any examples described in this specification are illustrative, but not limiting, and only illustrate some of the many possible embodiments of the claimed invention. Appropriate modifications and adjustments of various conditions and parameters commonly encountered in the art are common in the art and should be included in the scope of this specification.
[0037] The present invention relates to a solid-state lithium-sulfur battery design, and more specifically, to a sulfur-carbon (CS) positive electrode with an interface modification, wherein the CS positive electrode side facing the solid electrolyte in the interface is coated with a lithium ion conductive layer based on polyethylene oxide (PEO) containing an NC-Co composite material. The present invention also discloses a lithium-sulfur battery structure design with a modified positive electrode.
[0038] According to relevant examples, Figure 1 A schematic diagram of the solid-state lithium-sulfur battery structure is shown so that technicians will understand the preparation process described in this article and can apply the method to other configurations of solid-state lithium-sulfur batteries.
[0039] In a related example, the battery 100 includes a substrate 102 (e.g., a current collector), a sulfur electrode 104 (e.g., a positive electrode) coated on the substrate, a coating layer 114 on the positive electrode, a first intermediate layer 106 on the coating layer, a solid electrolyte 108 on the intermediate layer, a second intermediate layer 110 on the solid electrolyte, and a lithium electrode 112 (e.g., a negative electrode) on the second intermediate layer. They can be relatively placed horizontally or vertically.
[0040] In a related example, substrate 102 may be a current collector comprising at least one of three-dimensional nickel (Ni) foam, carbon fiber, foil (e.g., aluminum, stainless steel, copper, platinum, nickel, etc.), or a combination thereof. In a related example, intermediate layers 106 and 110 may be at least one of the following materials: a carbon-based intermediate layer (e.g., interconnected independent, micro / mesoporous containing, functionalized, bio-derived), a polymer-based intermediate layer (e.g., PEO, polypyrrole (PPY), polyvinylidene fluoride, etc.), a metal-based intermediate layer (e.g., Ni foam, etc.), or a combination thereof. In a related example, at least one of intermediate layers 106 and 110 is PEO. 18 LiTFSI-10%SiO2-10%IL layer, the interlayer contains polyethylene oxide (PEO), bis(trifluoromethane)sulfonyl imide lithium salt (LIN(CF3SO2)2 or LITFSI), SiO2 nanoparticles and ionic liquid (IL). Adding SiO2 and IL to the middle layer can reduce the crystallinity of PEO and improve ionic conductivity.
[0041] In a related example, the solid electrolyte 108 can be used to solve common safety issues such as leakage, poor chemical stability, and flammability common in lithium batteries using liquid electrolytes. In addition, the solid electrolyte can also inhibit the shuttling of polysulfides from the positive electrode to the negative electrode, thereby improving the utilization of active materials in the positive electrode, discharge capacity, and energy density. In a related example, the solid electrolyte may include: Li 6.4 LqCy 1.4 Ta 0.6 O 12 (LLZTO),Li 10 GeP2S 12 ,Li 1.5 Al 0.5 Ge 1.5 (PO4)3,Li 1.4 Al 0.4 Ti 1.6 (PO4)3,Li 0.55 La 0.35 TiO3, interpenetrating polymer networks of poly(ethyl acrylate) (IPN-PEA) electrolytes, three-dimensional ceramic / polymer networks, in situ plasticized polymers, composite polymers with well-aligned ceramic nanowires, PEO-based solid polymers, flexible polymers, polymer ionic liquids, in situ formed Li3PS4 and their combinations.
[0042] In a related example, the negative electrode 112 may include metallic lithium (Li). In some examples, the battery may include at least one negative electrode protective agent, such as an electrolyte additive (e.g., lanthanum nitrate, lanthanum nitrate, copper acetate, P2S5, etc.), an artificial interface layer (e.g., Li3N, (CH3)3SiCl, Al2O3, LiAl, etc.), a composite metal (e.g., Li7B6, Li-rGO (reduced graphene oxide), layered Li-rGO, etc.) or a combination thereof.
[0043] A description of the sulfur cathode 104, the coating layer 114, and the method of making them is as follows.
[0044] Figure 2 A schematic diagram 200 of a scheme for the positive electrode of a designed lithium-sulfur battery by (a) heating drying and (b) freeze drying methods is shown. In the first step of the positive electrode preparation scheme, a sulfur-containing battery slurry containing a binder 202 and a sulfur composite material 204 is coated on a substrate current collector 206. The slurry layer is synthesized as follows: First, a metal carbide, a carbon material, and a sulfur material are mixed in a solvent to form a sulfur slurry precursor. The metal carbide can be a carbide containing at least one of tungsten (W), iron (Fe), chromium (Cr), manganese (Mn), cobalt (Co), nickel (Ni), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), molybdenum (Mo), sodium (Na), calcium (Ca), or a combination thereof. The carbon material can be at least one of nanoparticles, nanowires, nanofibers, nanorods, nanotubes, nanospheres, graphene, carbon black (e.g., Ketjen Black), or a combination thereof. The sulfur material is elemental sulfur. The solvent can be any known compatible solvent, such as at least one of water, hexane, octane, acetone, tetrahydrofuran, 2-butanone, toluene, xylene, ethanol, methanol, isopropanol, benzene or a combination thereof. In a related example, the mixing can be performed by at least one of ball milling, ultrasound, magnetic mixing, vortex mixing, and the like.
[0045] Subsequently, the sulfur slurry precursor may be ground (e.g., dry grinding, etc.) to form a sulfur composite material, which is then mixed and stirred with a binder to form a sulfur-based slurry. In some examples, the binder includes at least one of styrene-butadiene rubber, carboxymethyl cellulose, polyacrylic acid (PAA), sodium alginate, or a combination thereof. In some examples, the binder includes styrene-butadiene rubber and carboxymethyl cellulose. In some examples, the binder includes water. Subsequently, the slurry having the sulfur composite material 204 and the binder 202 is applied to the substrate 206 by at least one of spin coating, dip coating, layer-by-layer deposition, sol-gel deposition, inkjet printing, or a combination thereof.
[0046] Subsequently, depending on the desired electrochemical properties of the battery, the sulfur-based slurry layer can be applied as follows: Figure 2 Heat drying is performed as shown in route (a) in the embodiment of the present invention, or as shown in the embodiment of the present invention. Figure 2 In some examples, route (a) can be carried out in a vacuum at 50°C to 150°C, 50°C to 100°C, 50°C to 75°C, 100°C to 150°C, 125°C to 150°C, or any temperature value or range disclosed therein, for a time range of 1 hour to 24 hours, 2 hours to 20 hours, or 3 hours to 16 hours, or 4 hours to 16 hours, or 8 hours to 16 hours, or any time or range disclosed herein. In some embodiments, during the thermal drying process, the filling structure 208 formed after the solvent in route (a) is dried has a porosity of at least 50%, or at least 45%, or at least 40%, or at least 35%, or at least 30%, or at least 25%, or at least 20%, or any value or range disclosed therein.
[0047] In some examples, after the sulfur-based slurry layer is coated on the substrate, the slurry layer can be freeze-dried, as described in route (b), to form a sulfur-based composite layer 210 having a porosity in the range of 50%-99% or 60%-99% or 60%-80% or any value or range disclosed herein. The structure of the sulfur cathode can be maintained by freezing the solvent in the slurry layer under low temperature conditions before drying. When the frozen solvent sublimates during the drying process, pores are formed in the composite layer (i.e., the pores remain at the locations where the solvent was originally located). That is, during the freeze-drying process, the internal volume space of the composite layer occupied by the solvent can be retained, thereby avoiding shrinkage of the composite layer. Compared with traditional thermal drying, freeze drying can increase the porosity of the composite layer by 3-5 times.
[0048] In some instances, the size of the pores in the composite layer may be in the range of 1 μm-50 μm. In some instances, the size of the pores may be in the range of 2 μm-10 μm. In some instances, freeze drying is performed at a temperature range of -50°C-0°C, or in the range of -35°C--10°C, or in the range of -25°C--15°C. In some instances, freezing is performed at a temperature of -20°C. In some instances, freezing is performed for a period of time in the range of 1-12 hours, or in the range of 2-9 hours, or in the range of 4-7 hours. In some examples, the freezing time is 6 hours. In some instances, freezing is performed at a temperature of -20°C for 6 hours. In some instances, drying is performed in a freeze dryer for a time range of 1-24 hours, or 6-18 hours, or 9-15 hours. In some instances, drying lasts for 12 hours.
[0049] In some examples, the filler structure 208 or the composite layer 210 includes 5-40 wt.%, 10-30 wt.%, or 15-25 wt.% of carbon material. In some examples, the filler structure 208 or the composite layer 210 includes 1-20 wt.%, 3-17 wt.%, or 5-15 wt.% of metal carbide. The carbon material and the metal carbide are conductive phases uniformly distributed in the final sulfur positive electrode, which helps to adsorb polysulfides (i.e., minimize polysulfide migration) to improve sulfur utilization (i.e., minimize the loss of positive electrode active materials).
[0050] Subsequently, conductive layer 212 is coated on top of composite layer 210 or filling structure 208 (not shown) and within the pores of composite layer 210 or filling structure 208 by at least one of spin coating, dip coating, layer-by-layer deposition, sol-gel deposition, inkjet printing, or a combination thereof to achieve a final structure 214 including sulfur cathode 218 and coating 216.
[0051] In some examples, the conductive layer includes at least one of carbon polysulfide (CS), polyethylene oxide (PEO), polyaniline (PANI), polypyrrole (PPY), poly(3,4-ethylenedioxythiophene) (PEDOT), polyterephthalate sulfonic acid (PSS), polyacrylonitrile (PAN), polyacrylic acid (PAA), polyamine hydrochloride (PAH), polyvinylidene fluoride-hexafluoropropylene (P(VDF-CO-HFP)), polymethyl methacrylate (PMMA), polyvinylidene fluoride (PVDF), poly(diallyldimethylammonium) bis(trifluoromethylsulfonylimide)imide (TFSI) (PDDATFSI), or a combination thereof, and at least one lithium salt (e.g., bis(trifluoromethane)sulfonylimide lithium salt (LiN(CF3SO2)2) (LiTFSI), lithium perchlorate, lithium bis(oxalate)borate (LiBOB), lithium bis(fluorosulfonyl)imide (LiFSI), lithium trifluoromethanesulfonate (LiCF3SO3) (LiTf ), lithium trifluoromethanesulfonamide) (Li(C2F5SO2)2N) (LiBETI) or a combination thereof. In some examples, the conductive layer may further include at least one or at least two or at least three elements of nitrogen, carbon, cobalt, titanium, tantalum and tungsten. In some examples, the conductive layer comprises a NC-Co composite material, and it has at least one dimension in the range of 1-100nm, 5-50nm, or 10-50nm, or 10-25nm, or any value or range disclosed therein. In some examples, the conductive layer comprises a NC-Co composite material having a size in the range of 50-500nm 2 / g, 100-400m 2 / g, or 50-250m 2 / g, or 100-300m 2 / g, or 300-500m 2 / g, or 50-200m 2 / g, or a Brunauer-Emmett-Teller (BET) surface area within any value or range disclosed therein.
[0052] In some examples, the conductive layer comprises polyethylene oxide. In some examples, the conductive layer comprises polyethylene oxide and at least one lithium salt of LITFSI, LITF and LIBETI. In some examples, the conductive layer comprises polyethylene oxide, LITFSI, LITF and LIBETI, and three elements of nitrogen, carbon and cobalt (e.g., NC-Co composite material). Due to the holes present inside the composite layer and / or the filling structure, after the conductive layer slurry is applied to the surface of the composite layer and / or the filling structure, a portion of the conductive layer slurry can penetrate into the interior through its porous structure. This penetration phenomenon between the coating surface and the cathode enhances the interfacial compatibility and improves the ionic conductivity of the prepared sulfur electrode. In some examples, the combined thickness of the sulfur cathode 218 and the coating 216 is less than 200 μm, less than 180 μm, less than 160 μm, less than 140 μm, less than 120 μm, less than 100 μm, or any value or range disclosed therein.
[0053] Example
[0054] Example 1 - Preparation of CS cathode using scheme (a)
[0055] CS composite materials were prepared by conventional melting method. Sulfur-ketjen black (S-KB) with a mass ratio of 3:1 was mixed evenly and placed in a high-temperature oven and heated at 155°C for 12 hours. Subsequently, the obtained S-KB powder, conductive carbon (such as Super P), sodium hydroxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) were dispersed in an appropriate amount of water solvent according to a mass ratio of 8:1:0.5:0.5, and the electrode slurry with uniform dispersion of each component was obtained after ball milling for 6 hours. The uniform slurry was coated on an aluminum foil substrate and then dried at 60°C under vacuum for 12 hours.
[0056] Example 2 - Preparation of CS positive electrode using scheme (b)
[0057] Sulfur, tungsten carbide (WC) and vapor-grown carbon fiber (VGCF) were ball-milled in an ethanol solvent at a mass ratio of 6:2:2. After ball milling for 4 hours, the resulting mixed powder was filtered and dried. After dry milling (e.g., dry milling) for 24 hours, the mixed powder was sieved to finally obtain a sulfur-carbon composite. A mixture of the previously prepared sulfur-carbon composite material, tungsten carbide (WC), vapor-grown carbon fiber (VGCF), styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) was mixed in a mass ratio of 80:5:5:5:5 by ball milling or stirring to prepare an electrode slurry. Subsequently, the slurry was coated on an aluminum foil having a thickness of 100 μm. The slurry-coated aluminum foil was frozen at -20°C for about 6 hours and then placed in a freeze dryer for about 12 hours to remove moisture from the slurry. After freeze drying, the electrode was cut into a disc with a diameter of 12 mm. The sulfur content of the resulting positive electrode was measured to be approximately 1.78 mg / cm 2 .
[0058] Example 3 - Preparation of ZIF-67 and NC-Co composites
[0059] 4mmol Co(NO3)2·6H2O and 16mmol 2-methylimidazole were dissolved in 50ml methanol respectively. Subsequently, the methanol solution of 2-methylimidazole was slowly added to the methanol solution of Co(NO3)2·6H2O and stirred continuously. After stirring for 1h, the mixed solution was allowed to stand at room temperature for 24h. The precipitate obtained after standing was centrifuged, washed several times with methanol and deionized water respectively, and dried at 65℃ for 12h. The bright purple sample finally obtained was ZIF-67. ZIF-67 was heat treated at 600℃ for 8h in a tubular furnace with a heating rate of 1℃ / min and a protective atmosphere of N2. Finally, the heat-treated product was used to remove part of the metal cobalt using 2M hydrochloric acid to obtain the NC-Co composite material.
[0060] Example 4- NC-Co / PEO material coating on CS positive electrode
[0061] The CS positive electrode prepared in Example 1 or Example 2 was used.
[0062] PEO powder and at least one lithium salt (e.g., LITFSI, lithium perchlorate, LIBOB, LIFSI, LITF, LIBETI or a combination thereof) are mixed in an EO / Li +The molar ratio is (6 to 20): 1 and dissolved in acetonitrile. 10-20% ionic liquid (e.g., n-butyl, methylpyrrolidine bis(trifluoromethylsulfonyl)imide, 1-butyl-3-methylimidazole bis(trifluoromethyl)sulfonyl]imide, 1-ethyl-3-methylimidazole bis(trifluoromethyl)sulfonyl]imide, etc.) and 5-50wt.% of the NC-Co composite prepared in Example 3 are added to the PEO / Li acetonitrile solution and stirred thoroughly. The solution is then coated on the surface of a common CS positive electrode and then vacuum dried at 60°C (to volatilize the solvent) to obtain a composite positive electrode containing a NC-CO / PEO coating (i.e., see Figure 1 104th and 114th floors and Figure 2 216 and 218 in the positive electrode). The coating thickness is 20 μm to 80 μm. To ensure sufficient ionic and electronic conductive networks in the positive electrode, the thickness of the positive electrode containing the NC-CO / PEO coating is designed to be less than 200 μm.
[0063] The resulting composite sulfur cathode is then assembled into a battery with other components (e.g., interlayer, electrolyte, and metallic lithium anode).
[0064] Example 5 - Preparation of Intermediate Layer
[0065] PEO powder and lithium salt (as disclosed herein) were mixed in an EO / Li + The molar ratio is (6-20): 1 and dissolved in acetonitrile. 10-20% ionic liquid (such as Example 4) is added to the PEO / Li acetonitrile solution and mixed thoroughly with 10wt.% ceramic filler (such as SiO2, Al2O3, CuO, etc.). In some examples, the concentration of the ceramic filler is in the range of 1wt.% to 15wt.%, which is mainly determined by the size of the silica particles. Ceramic fillers help to reduce the crystallinity of PEO and improve lithium ion conductivity. The slurry is cast in a polytetrafluoroethylene (PTFE) mold and then vacuum dried.
[0066] The intermediate layer between the positive electrode and the electrolyte reduces the interfacial impedance of the battery. In order to avoid reducing the mass energy density and volume energy density of the solid-state battery, the thickness of the intermediate layer is controlled as thin as possible. In some examples, the thickness of the intermediate layer can be in the range of 5-50 μm, or in the range of 5-150 μm.
[0067] Example 6-Preparation of garnet solid electrolyte
[0068] Using LiOH·H2O(Ar), La2O3(99.99%), ZrO2(Ar), and Ta2O5(99.99%) as precursor powders, cubic Li 6.4 LqCy1.4 Ta 0.6 O 12 . 2 wt% excess LiOH·H2O was added to compensate for the loss of lithium during sintering. Heat treatment was performed at 900°C for about 12 hours to remove trace moisture and adsorbed carbon dioxide in La2O3. The raw materials were mixed by wet grinding process using yttrium-stabilized zirconia (YSZ) balls and isopropyl alcohol (IPA) as grinding media. The mixture was dried and calcined in an alumina crucible at 950°C for 6 hours, mixed twice, and calcined again at 950°C for 6 hours to obtain pure cubic garnet phase ceramic powder. These powders were pressed into green blanks (d ~ 16 mm), and then covered with LLZTO powder containing 10 wt.% excess Li and sintered at 1250°C in a platinum crucible for 10 hours. The well-sintered ceramic sheets were polished to a thickness of 0.8 mm.
[0069] In some examples, one side of the LLZTO ceramic wafer was subjected to a 10-minute gold vapor deposition treatment by ion sputtering. The sample was then transferred to an argon-filled glove box. A certain amount of metallic lithium was heated to at least 250°C and poured onto the gold-deposited surface of the LLZTO ceramic wafer.
[0070] Example 7 - Battery Assembly
[0071] The lithium-sulfur battery obtained by the preparation method adopted in this article has the following structure: a sulfur positive electrode 104 coated with NC-Co / PEO, PEO-based intermediate layers 106 and 110, a solid electrolyte LLZTO ceramic 108 and a metal lithium negative electrode 112. The assembly of the solid-state lithium-sulfur battery is carried out in an argon-filled glove box. A structure of a lithium-sulfur battery is as follows Figure 1 shown.
[0072] In some examples, the assembled cells exhibited a relative humidity of less than 250 Ω·cm 2 , or less than 225Ω·cm 2 , or less than 200Ω·cm 2 , or less than 175Ω·cm 2 , or less than 150Ω·cm 2 , or less than 125Ω·cm 2 or any value or range of electrochemical impedance disclosed therein. In some examples, the assembled battery exhibits at least 500 mA / hg in the first week. S 1 , or at least 600mA / hg S 1 , or at least 700mA / hg S 1 , or at least 800mA / hg S 1, or at least 900mA / hg S 1 , or at least 1000mA / hg S 1 Or a reversible capacity of any value or range disclosed therein. In some examples, the assembled battery exhibits a capacity retention rate of at least 40%, or at least 50%, or at least 60%, or at least 70%, or at least 80%, or at least 90%, or at least 95%, or at least 99% or any value or range disclosed therein after 50 cycles.
[0073] Example 9-CS positive electrode preparation
[0074] The sulfur-ketjen black (S-KB) mixed powder with a mass ratio of 3:1 was ball-milled with ethanol as solvent for 4 hours. Subsequently, the mixed powder was sieved and dried at 60°C, and then further ground and heated in an oven at 155°C for 12 hours. The obtained S-KB powder, conductive carbon (such as Super P), sodium hydroxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) were dispersed in an appropriate amount of water solvent according to a mass ratio of 8:1:0.5:0.5, and the electrode slurry with uniform dispersion of each component was obtained after ball milling for 6 hours. The uniform slurry was coated on an aluminum foil substrate with a thickness of 100μm, and then dried at 60°C for 12 hours under vacuum conditions. The electrode was cut into a disc with a diameter of 12 mm. The sulfur content of the electrode was calculated to be 1.58mg / cm 2 .
[0075] PEO powder and LITFSI according to EO / Li + The molar ratio of 18:1 was dissolved in acetonitrile. Subsequently, an ionic liquid containing 10wt.% NC-Co composite material was added and stirred thoroughly in the acetonitrile solution to obtain a slurry with uniform components. The solid content of the obtained slurry was about 5%. 5ml of the mixed slurry was poured on the surface of the CS electrode and dried in vacuum at 60℃.
[0076] The coated CS positive electrode was used in button cell assembly, and the other components of the battery were prepared using the methods listed in Examples 5 to 7. The thickness of the PEO electrolyte intermediate layer was about 100 μm.
[0077] Comparative Example 1-Preparation of CS positive electrode
[0078] The CS cathode was prepared as described in Example 8, but without the NC-Co composite in the PEO infiltration layer.
[0079] Comparative Example 2-Preparation of CS positive electrode
[0080] The CS cathode was prepared as described in Example 8, but without the partially infiltrated NC-Co / PEO layer and the interlayer.
[0081] Characterization of Example 8, Comparative Example 1 and Comparative Example 2
[0082] Morphology analysis
[0083] Scanning electron microscope images were obtained by a scanning electron microscope (Hitachi JSM 6700). Elemental mapping images were characterized by an energy dispersive spectrometer (EDS) attached to a Hitachi scanning electron microscope.
[0084] Electrochemical impedance spectroscopy
[0085] Electrochemical impedance spectroscopy (EIS) was performed on an Autolab electrochemical workstation (EcoChemie BV, The Netherlands) with a frequency response analyzer.
[0086] Electrochemical performance
[0087] The charge and discharge curves of solid-state lithium-sulfur batteries were measured using a Land CT2001A battery test system (China) with a voltage range of 3-1 V and a current density of 0.1 mA / cm 2 The battery test temperature is 60°C. Before the battery test, the battery is kept at 70°C for 12 hours.
[0088] Regarding the images shown, according to some embodiments, Figure 3a illustrates a transmission electron microscope (TEM) image of the prepared ZIF-67; Figure 3b illustrates a scanning electron microscope (SEM) image of the NC-Co composite material; Figure 3c illustrates a TEM image of the NC-Co composite material; Figure 3d illustrates a high-magnification TEM image of the NC-Co composite material; Figure 3e inset draws a field emission scanning electron microscope image of the NC-Co composite material; Figures 3f-3h show the elemental distribution diagrams of carbon, nitrogen and cobalt in the NC-Co composite material, respectively.
[0089] Figures 3a-3h show the SEM images, TEM images and corresponding element distribution of the synthesized NC-Co composites. As a metal organic framework (MOF) compound, ZIF-67 framework is composed of Co 2+ The transition metal ions and N-containing 2-methylimidazole ligands can form a special framework similar to the zeolite topology through organic crosslinking. As shown in Figures 3a and 3c, the diameter of the synthesized ZIF-67 particles is about 350nm and the size is relatively uniform, with a rhombic dodecahedral morphology. After carbonization under a nitrogen atmosphere, the obtained NC-Co sample inherits the unique shape of ZIF-67 (Figure 3b) and has a porous structure (Figure 3d). TEM images clearly show that cobalt nanocrystals (indicated by the arrows in Figure 3d) are uniformly embedded in the carbon polyhedrons, and the size of the cobalt nanoparticles is about 20 nanometers (Figures 3c and 3d).
[0090] In order to further confirm the element distribution in the NC-Co composite material, the SEM images and element distribution of the heat-treated samples were characterized (as shown in Figures 3e and 3h). The organic ligands were carbonized to generate a nitrogen-doped carbon skeleton, and there were uniformly distributed metal Co nanoparticles in the skeleton (as shown in Figure 3h).
[0091] According to some examples, Figure 4 The adsorption test phenomenon of NC-Co composite and lithium polysulfide (Li2S6) is illustrated. The color change of Li2S6 solution (left) after adding NC-Co composite confirms that NC-Co composite has strong adsorption effect on polysulfide.
[0092] Figure 5a illustrates an X-ray diffraction (XRD) pattern of ZIF-67 and NC-Co composites; Figure 5b illustrates an N2 adsorption-desorption isotherm analysis of ZIF-67; Figure 5c illustrates an N2 adsorption-desorption isotherm analysis of NC-Co composites according to some embodiments. After heat treatment, the characteristic peak of ZIF-67 completely disappears (Figure 5a), and three characteristic peaks of cobalt nanoparticles are found at 44.2°, 51.6° and 75.9°, corresponding to the (111), (200) and (220) crystal planes of cobalt, respectively.
[0093] The specific surface area and corresponding pore size distribution of ZIF-67 (Figure 5b) and NC-Co composites (Figure 5c) were analyzed by N2 adsorption-desorption isotherm measurement. The BET surface area of ZIF-67 was calculated to be 1392.3 m 2 / g, and the BET surface area of the NC-Co composite is 232.5 m 2 / g. In addition, the pore diameter of ZIF-67 is 1.96nm, while the pore diameter of NC-Co composite is mainly distributed in 4.81nm and 6.36nm, indicating that the mesoporous structure is formed during the carbonization of 2-methylimidazole organic ligand and the acid treatment of metal cobalt. The high surface area and rich mesoporous structure make it suitable for the intermediate product Li2S x It has strong physical absorption capacity.
[0094] According to some examples, 6a-6c tested the X-ray photoelectron spectroscopy of NC-Co composites. Since the precursor ZIF-67 is cross-linked by divalent cobalt ions and nitrogen-containing organic ligands, after heat treatment, the nitrogen-containing organic ligands will eventually pyrolyze to form C=N double bonds (285.8eV) and C=C double bonds (284.8eV). The surface of this N-doped carbon material can act as a conductive Lewis acid "catalyst", which can further enhance the Li2S xAs shown in Figure 6b, the form of nitrogen in the NC-Co composite is determined by the XPS spectrum of N1s, and the fitted peaks at 398.9eV, 400.4eV and 401.3eV correspond to pyridinic nitrogen, pyrrolic nitrogen and graphitic nitrogen, respectively. Pyrrolic nitrogen and pyridinic nitrogen can affect the Co-N x The presence of. From the N1s fitting peak results, it can be seen that the NC-Co composite material has a high content of pyridinic nitrogen. Pyridinic nitrogen belongs to p-type doped nitrogen, which can act as a conductive Lewis acid matrix to improve the electrochemical performance of the battery. This result is consistent with the previous C1s peak fitting results. The XPS spectrum of Co2p3 / 2 in Figure 6c can be fitted into two characteristic peaks, at 778.5eV and 780.3eV. The two peaks respectively determine the presence of elemental metal cobalt and the Co-N chemical bonds formed by the embedding of cobalt nanoparticles into the N-doped carbon skeleton.
[0095] Figure 7a shows a scanning electron microscope image of a cross section of a CS positive electrode modified with an NC-Co / PEO coating layer, wherein the cathode is provided with an NC-Co / PEO coating and filtered in the CS cathode; Figures 7b-7g show the element distribution of carbon, sulfur, fluorine, cobalt, oxygen and aluminum of the modified CS positive electrode. As shown in Figure 7a, the thickness of the modified CS positive electrode is about 150 μm, and the thickness of the NC-Co / PEO coating is about 30 μm. In particular, the element distribution map of Co in Figure 7e clearly shows that the NC-Co / PEO coating is uniformly infiltrated into the CS positive electrode layer. In some instances, the NC-Co coating penetrates and can directly contact the substrate current collector.
[0096] Figures 8a and 8b show the electrochemical impedance spectra of the lithium-sulfur battery before cycling of Example 8, Comparative Example 1 (as shown in Figure 8a), and Comparative Example 2 (as shown in Figure 8b). Example 8 shows the lowest impedance of about 203Ω·cm 2 The impedance of comparative example 1 (excluding the PEO layer) under the same conditions is about 249Ω·cm 2 , which shows that NC-Co / PEO has the function of reducing the internal impedance of the battery. PEO polymer (containing LiTFSI) is a good lithium ion conductor. By infiltrating NC-Co / PEO into the positive electrode, it can penetrate deeply into the CS positive electrode to build a well-connected lithium ion conduction network, thereby reducing the internal impedance of the battery, and adding NC-Co composite materials can further help lithium ion diffusion and reduce battery impedance. The battery impedance of Comparative Example 2 is very large, exceeding 10000Ω·cm 2, under such a large internal resistance, the battery cannot be normally charged and discharged. The PEO intermediate layer on both sides of the positive and negative electrodes of the solid electrolyte strengthens the contact between the positive and negative electrodes and the solid electrolyte, effectively reducing the interface impedance inside the battery.
[0097] Figures 9a and 9b show the lithium-sulfur batteries of Example 8 and Comparative Example 1 at 60°C and 0.1 mA / cm 2 Cycling performance under current density conditions. The lithium-sulfur battery in Example 8 can release 920 mA / hg in the first week. S 1 The discharge specific capacity of the battery is 50% after 50 cycles. The capacity retention rate of the battery in Example 1 is only 24% after 50 cycles. The improvement in capacity retention in Example 8 is mainly attributed to the effect of the NC-Co composite material. As explained before, the NC-Co composite material can improve the ability to reuse lithium polysulfide. The reduction of lithium polysulfide in the electronic and ion conductive skeleton is the main reason for the battery capacity decay.
[0098] Therefore, as described herein, the present invention is a design for a solid-state lithium-sulfur battery, specifically, a design (and related methods) for coating a CS positive electrode with a PEO / NC-Co ion-conducting layer in a lithium-sulfur battery containing a ceramic electrolyte. Its advantages include: (1) NC-Co / PEO can penetrate into the CS electrode, so that the active material has good contact with the ion-conducting network, thereby improving the utilization rate of the active material; (2) the NC-Co / PEO coating can absorb and reuse lithium polysulfide during the cycle, thereby reducing the shuttle effect of lithium polysulfide; (3) the PEO-based coating and the intermediate layer help to improve the interfacial stress and interfacial impedance of the solid-state lithium battery; (4) compared with the lithium-sulfur battery with a conventional positive electrode, the solid-state lithium battery containing the modified CS positive electrode disclosed herein has a higher battery specific capacity and stable cycle performance.
[0099] Reducing stress / strain and establishing a robust electronic and ion conducting pathway between the carbon-sulfur cathode and the solid electrolyte are key challenges to improving the reaction kinetics of lithium-sulfur batteries. The poor contact between the electronic conductor, active materials, and lithium-ion conductors hinders the practical application of lithium-sulfur batteries. As described in this article, the modified coating that penetrates into the cathode can provide a conductive network within the cathode and provide good contact between the components inside the battery.
[0100] Therefore, compared with the conventional lithium-sulfur battery, the positive electrode prepared by the positive electrode preparation method described in this article has a higher battery reversible specific capacity (e.g., more than 920 mA / hg) after the battery is assembled. S 1 ), lower battery internal resistance and more stable battery cycle performance.
[0101] As used herein, the terms "about," "approximately," "substantially," and similar terms are intended to be broadly defined and consistent with common and recognized usage by those of ordinary skill in the art to which the subject matter of the present invention pertains. It should be understood by those skilled in the art who review the present invention that these terms are intended to allow for certain features to be described and claimed without limiting the scope of such features to the precise numerical ranges provided. Accordingly, these terms should be interpreted as indicating that insubstantial or insubstantial modifications or alterations of the subject matter described and claimed are considered to be within the scope of the invention as described in the appended claims.
[0102] As used herein, "optional" or "optionally" means that the described event or situation may or may not occur, and the described event or situation includes both occurrence and non-occurrence. Unless otherwise specified, the words "a" or "an" and their corresponding words "said" as used herein refer to at least one or more.
[0103] References to element positions herein (e.g., "upper," "lower," "upper," "lower," etc.) are only used to describe the orientation of various elements in the figures. It should be noted that the orientation of different elements may be different according to other examples, and the present invention is intended to cover these variations.
[0104] For the use of any plural and / or singular terms in the art, those skilled in the art can translate from plural to singular and / or from singular to plural according to the context and / or application. For clarity, various singular / plural arrangements may be explicitly described herein.
[0105] It will be apparent to those skilled in the art that various modifications and variations may be made without departing from the spirit or scope of the subject matter. Accordingly, the claimed subject matter is not to be limited except in accordance with the appended claims and their equivalents.
Claims
1. A lithium-sulfur battery comprising: substrate; A sulfur cathode on a substrate; A coating layer on the positive electrode; a first intermediate layer on the coating layer; a solid electrolyte on the first intermediate layer; a second intermediate layer on the solid electrolyte; and a metallic lithium negative electrode on the second intermediate layer, wherein the coating layer is uniformly coated on the surface of the positive electrode and penetrates into the pores of the positive electrode and directly contacts the substrate, Wherein, the coating layer comprises polyethylene oxide, Wherein, the coating layer comprises NC-Co composite material, Wherein, the coating layer comprises one of the following lithium salts: lithium bis(trifluoromethane)sulfonyl imide, lithium perchlorate, lithium bis(oxalate)borate, lithium bis(fluorosulfonyl)imide, lithium trifluoromethanesulfonate, lithium di(trifluoromethanesulfonamide) or a combination thereof, wherein the NC-Co composite material comprises a regular dodecahedral morphology and at least one dimension having a diameter in the range of 10-50 nm, wherein the positive electrode has a porosity of at least 30%, The diameter of the pores of the positive electrode is in the range of 1-50 μm.
2. The battery according to claim 1, wherein The applied coating layer comprises one of the following materials: carbon polysulfide, polyaniline, polypyrrole, poly(3,4-dioxyethylenethiophene), sulfide polystyrene sulfonic acid, polyacrylonitrile, polyacrylic acid, polyallylamine hydrochloride, polyvinylidene fluoride-hexafluoropropylene, poly(methyl methacrylate), polyvinylidene fluoride, poly(diallyldimethylammonium)bis(trifluoromethylsulfonylimide)imide or a combination thereof.
3. The battery according to claim 1, wherein The coating layer contains at least one of nitrogen, carbon, cobalt, titanium, tantalum and tungsten.
4. The battery according to claim 1, wherein The first intermediate layer and the second intermediate layer each further include a ceramic filler.
5. The battery as claimed in claim 1, wherein the NC-Co composite material has a mesoporous structure and a specific surface area in the range of 100-300 m 2 / g.
6. The battery according to claim 1, wherein the total thickness of the sulfur positive electrode and the coating layer is less than 200 μm.
7. The battery as claimed in claim 1, wherein the solid electrolyte comprises one of the following: The solid electrolyte may include: Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 (LLZTO), Li 10 GeP2S 12 , Li 1.5 Al 0.5 Ge 1.5 (PO4)3, Li 1.4 Al 0.4 Ti 1.6 (PO4)3, Li 0.55 La 0.35 TiO3, interpenetrating polymer networks of poly(ethyl acrylate) electrolytes, three-dimensional ceramic / polymer networks, in situ plasticized polymers, composite polymers with well-aligned ceramic nanowires, PEO-based solid polymers, flexible polymers, polymer ionic liquids, in situ formed Li3PS4 and their combinations.
8. The battery of claim 1, wherein the positive electrode has a porosity of at least 60%.
9. The battery of claim 1, wherein the configuration exhibits at least one of the following parameters: Impedance less than 250 Ω•cm 2 ; Reversible capacity of at least 500 mA / hgs 1 ;or The capacity retention rate is at least 40%.