Refining method of sulfide solid electrolyte

Through the synergistic action of alkane dispersant and oxygen-containing solvent and ball milling treatment, the problem of excessive particle size of sulfide electrolyte powder is solved, and the particle size refinement and dispersion are improved. It is suitable for all-solid battery electrolyte membranes preparation.

CN119009076APending Publication Date: 2024-11-22SHANGHAI FIRM LITHIUM NEW ENERGY TECH CO LTD
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202411264369.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to effectively refine sulfide solid electrolyte powder, resulting in too large particle size and cannot meet the needs of electrolyte membranes in all-solid batteries.

Method used

The synergistic effect of alkane dispersant and oxygen-containing solvent was adopted to refine the sulfide electrolyte powder by ball milling, combined with magnetic stirring and vacuum drying, and the particle size was controlled to be about 500nm.

Benefits of technology

The particle size of the sulfide electrolyte powder is significantly reduced, its dispersion and stability are improved, and it is suitable for the preparation of electrolyte membranes of all-solid batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009076A_ABST
    Figure CN119009076A_ABST
Patent Text Reader

Abstract

The invention relates to a refining method of sulfide solid electrolyte. The refining method comprises the following steps: S1, dispersing sulfide electrolyte powder in a mixed solution of an alkane dispersant and an oxygen-containing group solvent to obtain a powder dispersion liquid; and S2, carrying out ball milling treatment on the powder dispersion liquid in the step S1 to obtain refined sulfide electrolyte powder. The synergistic effect between the alkane dispersing agent and the oxygen-containing group solvent is utilized, the solvent is added to etch the powder, meanwhile, the dispersing agent enables the powder to be dispersed in the ball milling process and plays a role in protecting the powder so as to prevent the powder from being damaged due to over-etching, and the powder with the particle size being about 500 nm is obtained. The problem that coarse powder obtained in the prior art is too large in particle size is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of all-solid-state batteries and relates to a method for refining a sulfide solid electrolyte. Background Art

[0002] Sulfide solid electrolytes have received extensive attention from researchers due to their excellent properties such as high lithium ion conductivity and good electrolyte / electrode interface contact. In the assembly process of all-solid-state batteries, considering the demand for high energy density, the electrolyte needs to be mixed with a binder to prepare an electrolyte membrane, and the electrolyte membrane needs to be made as thin as possible, to about 30μm. However, since argyrodite-phase sulfide solid electrolytes are usually prepared by solid-phase reaction or solid-phase reaction + heat treatment process, their powder particle size is relatively large. If they are only crushed by mortar grinding, the maximum particle size will reach several hundred microns, which is difficult to meet the electrolyte membrane's demand for small electrolyte particle size.

[0003] The prior art often uses a first solvent to dissolve lithium sulfide, that is, to form lithium-related ions and sulfur-related ions, and then evaporates the first solvent due to the difference in boiling points between the first solvent and the second solvent, so that lithium sulfide crystals are precipitated. Although this method reduces the particle size of lithium sulfide to a certain extent, a small amount of impurities will be obtained; and this method is not suitable for sulfide electrolytes such as LPSX, which will cause the sulfide electrolyte to be unable to recrystallize and may increase the particle size of the sulfide electrolyte. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings and deficiencies of the prior art and provide a method for refining a sulfide solid electrolyte. In order to solve the problem that the particle size of the coarse sulfide solid electrolyte powder obtained in the prior art is too large, the present invention utilizes the synergistic effect between the alkane dispersant and the oxygen-containing group solvent, etches the powder by adding the oxygen-containing group solvent, and at the same time, the alkane dispersant disperses the powder during the ball milling process and protects the powder to avoid over-etching and damage to the powder, thereby obtaining a sulfide solid electrolyte powder with a particle size as low as about 500nm.

[0005] The purpose of the present invention can be achieved by the following scheme:

[0006] In a first aspect, the present invention provides a method for refining a sulfide solid electrolyte, the method comprising the following steps:

[0007] S1. dispersing sulfide electrolyte powder in a mixed solution of an alkane dispersant and an oxygen-containing group solvent to obtain a powder dispersion;

[0008] S2. The powder dispersion in step S1 is subjected to ball milling treatment and vacuum drying to obtain refined sulfide electrolyte powder.

[0009] As an embodiment of the present invention, the particle size D50 of the sulfide electrolyte powder is ≤500 μm; the particle size D50 of the refined sulfide electrolyte powder is <1 μm.

[0010] As an embodiment of the present invention, in step S1, the sulfide electrolyte includes LPSX, wherein L is Li, and X is one or more of Cl, Br, and I.

[0011] As an embodiment of the present invention, in step S1, the alkane dispersant includes at least one of xylene, n-hexane, n-heptane, and p-xylene. The alkane dispersant also includes an alkane dispersant of the above-mentioned alkane derivatives.

[0012] As an embodiment of the present invention, in step S1, the oxygen-containing group solvent includes one of esters, ethers and alcohols.

[0013] Preferably, the oxygen-containing group solvent is an ester solvent, that is, an ester-containing solvent.

[0014] In some embodiments, the ester solvent includes one of dimethyl carbonate and ethyl acetate. The oxygen with lone pair electrons in the ester group will attack the positive lithium on the surface of the sulfide electrolyte, thereby decomposing it to a certain extent, which is more conducive to more uniform and sufficient impact of the grinding ball on it, and the particle size of the sulfide electrolyte powder obtained by refinement is smaller.

[0015] As an embodiment of the present invention, in step S1, the mass ratio of sulfide electrolyte powder to alkane dispersant is 1:1-100, and the mass ratio of oxygen-containing group solvent to alkane dispersant is 1:10-200. If the dispersant ratio is too high, the slurry is too thin, which will lead to insufficient impact force of the grinding balls on the powder particles, affecting the refinement effect; if the dispersant ratio is too low, the powder cannot be fully dispersed; if the solvent ratio is too high, the powder is severely damaged; if the solvent ratio is too low, it will not have a significant effect.

[0016] As an embodiment of the present invention, in step S1, the dispersion method includes at least one of magnetic stirring, mechanical stirring, and ultrasonic dispersion. The dispersion is performed in a sealed container made of glass, quartz, or other materials that do not react with the solution used.

[0017] The dispersant and solvent used in the present invention are ultra-dry in purity, with a water content of less than 30 ppm.

[0018] As an embodiment of the present invention, in step S2, the ball milling treatment includes at least one of mechanical ball milling, vibration ball milling, roller milling, and ultrasonic grinding.

[0019] Furthermore, the ball milling treatment is first performed at 50-200 rpm min -1Low speed 360-degree all-round ball milling for 1-10h, then 300-600rpm min -1 In the present invention, the powder, grinding balls and solution in the ball mill are fully mixed and uniformly carried out by low-speed 360-degree all-round ball milling; and then high-speed ball milling is carried out to refine the powder.

[0020] In the present invention, the ball milling treatment comprises: transferring the dispersion to a ball milling jar, adding grinding balls, and sealing the jar and performing the treatment in a ball mill.

[0021] In some preferred embodiments, the grinding balls used in the ball milling process include at least one of zirconium oxide, aluminum oxide, agate, and stainless steel, the diameter of the grinding balls is 0.3-2 mm, and the ball-to-material ratio is 25-35:1. If the diameter of the grinding balls is too large, the gaps between the grinding balls will be too large, and the powder will not be ground sufficiently; if the diameter of the grinding balls is too small, the kinetic energy will be small, the impact force on the powder will be insufficient, and the refining effect will not be obvious. In addition, if the ball diameter is too small, it will also increase the difficulty of separating the balls from the powder.

[0022] As an embodiment of the present invention, in step S2, the ball milling is followed by drying, and the drying temperature is 20-250°C.

[0023] In a second aspect, the present invention provides a solid-state battery, comprising a sulfide solid electrolyte obtained by the refinement method.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The present invention adopts a wet ball milling refinement method combining solvent + dispersant. The oxygen with lone pair electrons in the ester group of the solvent will attack the positive lithium on the surface of the sulfide electrolyte, thereby etching the surface, and crushing and refining it under the impact of the grinding ball. The dispersant has a good dispersing effect on the crushed particles, and at the same time protects the surface of the particles to avoid electrolyte decomposition caused by over-etching. Compared with the use of solvent or dispersant alone, the present invention uses solvent and dispersant to synergistically improve the decomposition effect on sulfide electrolyte, so that its particle size can be reduced to about 500nm.

[0026] 2. The present invention unexpectedly discovered that, compared with other oxygen-containing groups, the ester group has the most suitable offensiveness to lithium on the surface of the sulfide electrolyte. It will neither completely decompose the sulfide electrolyte due to excessive reactivity, nor fail to achieve a dispersion effect due to lack of interaction with the electrolyte. It is more conducive to the subsequent uniform and sufficient impact of the grinding ball, thereby significantly refining the sulfide electrolyte powder. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0028] Figure 1 The microscopic morphology in Example 1;

[0029] Figure 2 It is the microscopic morphology in Example 2;

[0030] Figure 3 The microscopic morphology in Example 3;

[0031] Figure 4 It is the microscopic morphology in Example 4;

[0032] Figure 5 It is the microscopic morphology in Example 5;

[0033] Figure 6 It is the microscopic morphology in Comparative Example 1;

[0034] Figure 7 It is the microscopic morphology in Comparative Example 2;

[0035] Figure 8 It is the microscopic morphology in Comparative Example 3;

[0036] Fig. 9 This is the microscopic morphology in Comparative Example 4. DETAILED DESCRIPTION

[0037] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. The following examples are implemented on the premise of the technical solution of the present invention, provide detailed implementation methods and specific operation processes, and will help those skilled in the art to further understand the present invention. It should be pointed out that the protection scope of the present invention is not limited to the following embodiments, and several adjustments and improvements made under the premise of the concept of the present invention all belong to the protection scope of the present invention.

[0038] Example 1

[0039] This embodiment prepares a sulfide electrolyte nanopowder, and the specific steps are as follows:

[0040] 1) Weigh 5 g of LPSCl powder (D50 = 30 μm) in a glove box and transfer it to a zirconia ball mill;

[0041] 2) Add 25 g of xylene dispersant and 2 g of dimethyl carbonate solvent into a quartz sealed container, stir magnetically, and then add into a ball mill;

[0042] 3) Add 150 g of 1 mm diameter zirconium oxide grinding balls into the ball mill;

[0043] 4) Seal the ball mill jar and transfer it to the ball mill for ball milling. First, perform 100 rpm min -1The ball mill was performed at a low speed of 360 degrees for 6 hours, and then at 450 rpm min. -1 High-speed horizontal ball mill for 6 hours;

[0044] 5) After the ball milling is completed, transfer the ball mill jar to a vacuum drying oven in the glove box;

[0045] 6) Dry under vacuum at 60°C, transfer the powder to a sieving machine for sieving, and obtain electrolyte powder. Figure 1 As shown, the average particle size of the electrolyte powder is about 300 nm.

[0046] Example 2

[0047] 1) Weigh 5 g of LPSCl powder (D50 = 30 μm) in a glove box and transfer it to a zirconia ball mill;

[0048] 2) Add 25 g of xylene dispersant and 2 g of anisole solvent into a quartz sealed container, stir magnetically, and then add to a ball mill;

[0049] 3) Add 150 g of 1 mm diameter zirconium oxide grinding balls into the ball mill;

[0050] 4) Seal the ball mill jar and transfer it to the ball mill for ball milling. First, perform 100 rpm min -1 The ball mill was performed at a low speed of 360 degrees for 6 hours, and then at 450 rpm min. -1 High-speed horizontal ball mill for 6 hours;

[0051] 5) After the ball milling is completed, transfer the ball mill jar to a vacuum drying oven in the glove box;

[0052] 6) Dry under vacuum at 60°C, transfer the powder to a sieving machine for sieving, and obtain electrolyte powder. Figure 2 As shown, the average particle size of the electrolyte powder is about 1 μm.

[0053] Example 3

[0054] 1) Weigh 5 g of LPSCl powder (D50 = 30 μm) in a glove box and transfer it to a zirconia ball mill;

[0055] 2) Add 25 g of n-hexane dispersant and 2 g of dimethyl carbonate solvent into a quartz sealed container, stir magnetically, and then add into a ball mill;

[0056] 3) Add 150 g of 1 mm diameter zirconium oxide grinding balls into the ball mill;

[0057] 4) Seal the ball mill jar and transfer it to the ball mill for ball milling. First, perform 100 rpm min -1 The ball mill was performed at a low speed of 360 degrees for 6 hours, and then at 450 rpm min.-1 High-speed horizontal ball mill for 6 hours;

[0058] 5) After the ball milling is completed, transfer the ball mill jar to a vacuum drying oven in the glove box;

[0059] 6) Dry under vacuum at 60°C, transfer the powder to a sieving machine for sieving, and obtain electrolyte powder. Figure 3 As shown, the average particle size of the electrolyte powder is about 500 nm.

[0060] Example 4

[0061] This embodiment prepares a sulfide electrolyte nanopowder, and the specific steps are as follows:

[0062] 1) Weigh 5 g of LPSCl powder (D50 = 30 μm) in a glove box and transfer it to a zirconia ball mill;

[0063] 2) Add 25 g of xylene dispersant and 2 g of ethyl acetate solvent into a quartz sealed container, stir magnetically, and then add into a ball mill;

[0064] 3) Add 150 g of 1 mm diameter zirconium oxide grinding balls into the ball mill;

[0065] 4) Seal the ball mill jar and transfer it to the ball mill for ball milling. First, perform 100 rpm min -1 The ball mill was performed at a low speed of 360 degrees for 6 hours, and then at 450 rpm min. -1 High-speed horizontal ball mill for 6 hours;

[0066] 5) After the ball milling is completed, transfer the ball mill jar to a vacuum drying oven in the glove box;

[0067] 6) Dry under vacuum at 60°C, transfer the powder to a sieving machine for sieving, and obtain electrolyte powder. Figure 4 As shown, the average particle size of the electrolyte powder is about 500 nm.

[0068] Example 5

[0069] This embodiment prepares a sulfide electrolyte nanopowder, and the specific steps are as follows:

[0070] 1) Weigh 5 g of LPSCl powder (D50 = 30 μm) in a glove box and transfer it to a zirconia ball mill;

[0071] 2) Add 25 g of xylene dispersant and 2 g of ethanol solvent into a quartz sealed container, stir magnetically, and then add into a ball mill;

[0072] 3) Add 150 g of 1 mm diameter zirconium oxide grinding balls into the ball mill;

[0073] 4) Seal the ball mill jar and transfer it to the ball mill for ball milling. First, perform 100 rpm min -1 The ball mill was performed at a low speed of 360 degrees for 6 hours, and then at 450 rpm min. -1 High-speed horizontal ball mill for 6 hours;

[0074] 5) After the ball milling is completed, transfer the ball mill jar to a vacuum drying oven in the glove box;

[0075] 6) Dry under vacuum at 60°C, transfer the powder to a sieving machine for sieving, and obtain electrolyte powder. Figure 5 As shown, the average particle size of the electrolyte powder is about 2 μm.

[0076] Comparative Example 1

[0077] This comparative example prepares a sulfide electrolyte powder, and the specific steps are as follows:

[0078] 1) Weigh 5 g of LPSCl powder (D50 = 30 μm) in a glove box and transfer it to a zirconia ball mill;

[0079] 2) Add 25 g of xylene dispersant and 2 g of dimethyl carbonate solvent into a quartz sealed container, stir magnetically, and then add into a ball mill;

[0080] 3) Add 150 g of 3 mm diameter zirconium oxide grinding balls into the ball mill;

[0081] 4) Seal the ball mill jar and transfer it to the ball mill for ball milling. First, perform 100 rpm min -1 The ball mill was performed at a low speed of 360 degrees for 6 hours, and then at 450 rpm min. -1 High-speed horizontal ball mill for 6 hours;

[0082] 5) After the ball milling is completed, transfer the ball mill jar to a vacuum drying oven in the glove box;

[0083] 6) Dry under vacuum at 60°C, transfer the powder to a sieving machine for sieving, and obtain electrolyte powder. Figure 6 As shown, the average particle size of the electrolyte powder is about 1 μm.

[0084] The results of Comparative Example 1 and Example 1 show that if the diameter of the grinding balls is too large, the powder particle size will be larger and the powder particles will stick together, resulting in a poor refining effect.

[0085] Comparative Example 2

[0086] This comparative example prepares a sulfide electrolyte powder, and the specific steps are as follows:

[0087] 1) Weigh 5 g of LPSCl powder (D50 = 30 μm) in a glove box and transfer it to a zirconia ball mill;

[0088] 2) Add 25 g of xylene dispersant to a quartz sealed container, stir magnetically, and then add it to a ball mill;

[0089] 3) Add 150 g of 1 mm diameter zirconium oxide grinding balls into the ball mill;

[0090] 4) Seal the ball mill jar and transfer it to the ball mill for ball milling. First, perform 100 rpm min -1 The ball mill was performed at a low speed of 360 degrees for 6 hours, and then at 450 rpm min. -1 High-speed horizontal ball mill for 6 hours;

[0091] 5) After the ball milling is completed, transfer the ball mill jar to a vacuum drying oven in the glove box;

[0092] 6) Dry under vacuum at 60°C, transfer the powder to a sieving machine for sieving, and obtain electrolyte powder. Figure 7 As shown, the average particle size of the electrolyte powder is about 1.5 μm.

[0093] Comparative Example 3

[0094] This comparative example prepares a sulfide electrolyte powder, and the specific steps are as follows:

[0095] 1) Weigh 5 g of LPSCl powder (D50 = 30 μm) in a glove box and transfer it to a zirconia ball mill;

[0096] 2) Add 2 g of dimethyl carbonate solvent into a quartz sealed container, stir magnetically, and then add it into a ball mill;

[0097] 3) Add 150 g of 1 mm diameter zirconium oxide grinding balls into the ball mill;

[0098] 4) Seal the ball mill jar and transfer it to the ball mill for ball milling. First, perform 100 rpm min -1 The ball mill was performed at a low speed of 360 degrees for 6 hours, and then at 450 rpm min. -1 High-speed horizontal ball mill for 6 hours;

[0099] 5) After the ball milling is completed, transfer the ball mill jar to a vacuum drying oven in the glove box;

[0100] 6) Dry under vacuum at 60°C, transfer the powder to a sieving machine for sieving, and obtain electrolyte powder. Figure 8 As shown, the average particle size of the electrolyte powder is greater than 10 μm. As can be seen from Comparative Examples 2-3, the use of a single oxygen-containing group solvent or alkane dispersant cannot produce a synergistic effect, thereby significantly reducing the decomposition effect on the sulfide electrolyte, resulting in a higher particle size of the electrolyte powder.

[0101] Comparative Example 4

[0102] This comparative example prepares a sulfide electrolyte powder, and the specific steps are as follows:

[0103] 1) Weigh 5 g of LPSCl powder (D50 = 30 μm) in a glove box and transfer it to a zirconia ball mill;

[0104] 2) Add 25 g of xylene dispersant and 20 g of dimethyl carbonate solvent into a quartz sealed container, stir magnetically, and then add into a ball mill;

[0105] 3) Add 150 g of 1 mm diameter zirconium oxide grinding balls into the ball mill;

[0106] 4) Seal the ball mill jar and transfer it to the ball mill for ball milling. First, perform 100 rpm min -1 The ball mill was performed at a low speed of 360 degrees for 6 hours, and then at 450 rpm min. -1 High-speed horizontal ball mill for 6 hours;

[0107] 5) After the ball milling is completed, transfer the ball mill jar to a vacuum drying oven in the glove box;

[0108] 6) Dry under vacuum at 60°C, transfer the powder to a sieving machine for sieving, and obtain electrolyte powder.

[0109] like Fig. 9 As shown, the electrolyte powder has almost no individual particles and is aggregated into blocks of several tens of micrometers. Comparison of Comparative Example 4 with Example 1 shows that excessive dimethyl carbonate causes serious damage to the powder, and the powder is obviously aggregated.

[0110] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A method for refining a sulfide solid electrolyte, characterized in that: The refinement method comprises the following steps: S1. Dispersing sulfide electrolyte powder in a mixed solution of an alkane dispersant and an oxygen-containing group solvent to obtain a powder dispersion; the oxygen-containing group solvent is an ester solvent; S2. The powder dispersion in step S1 is subjected to ball milling treatment and vacuum drying to obtain refined sulfide electrolyte powder.

2. The thinning method according to claim 1, characterized in that: The particle size D50 of the sulfide electrolyte powder is ≤500 μm; the particle size D50 of the refined sulfide electrolyte powder is <1 μm.

3. The thinning method according to claim 1, characterized in that: In step S1, the sulfide electrolyte includes LPSX, wherein L is Li, and X is one or more of Cl, Br, and I.

4. The thinning method according to claim 1, characterized in that: In step S1, the alkane dispersant includes at least one of xylene, n-hexane, n-heptane, and p-xylene.

5. The thinning method according to claim 1, characterized in that: The ester solvent includes one of dimethyl carbonate and ethyl acetate.

6. The thinning method according to claim 1, characterized in that: In step S1, the mass ratio of the sulfide electrolyte powder to the alkane dispersant is 1:1-100, and the mass ratio of the oxygen-containing group solvent to the alkane dispersant is 1:10-200.

7. The thinning method according to claim 1, characterized in that: In step S2, the ball milling treatment includes at least one of mechanical ball milling, vibration ball milling, roller milling, and ultrasonic crushing; the grinding balls used in the ball milling treatment include at least one of zirconium oxide, aluminum oxide, agate, and stainless steel, and the diameter of the grinding balls is 0.3-2 mm; the ball-to-material ratio of the ball milling treatment is 25-35:

1.

8. A solid-state battery, characterized in that: It comprises a sulfide solid electrolyte obtained by the refinement method as described in any one of claims 1 to 7.

Citation Information

Cited By

  • Solid electrolyte refining method based on pi-pi stacking self-assembly composite aprotic solvent and application of solid electrolyte refining method

    CN119994162A

  • Sulfide solid electrolyte, preparation method thereof and all-solid-state battery

    CN121307166A

  • High-dispersity sulfide solid electrolyte composite material, preparation method thereof and all-solid-state battery

    CN122118049A

  • Roller milling-sanding combined preparation method of submicron sulfide solid electrolyte

    CN122638598A

  • Solid-state battery cell, battery device, electric device, modified sulfide electrolyte and preparation method therefor

    WO2026200232A1