Transparent conductive film
By adding dye to the nano-silver wire layer and adjusting the absorption peak ratio, the problem of yellowing of the nano-silver wire conductive film is solved, and the neutral color and high penetration of the transparent conductive film are achieved, which is suitable for the application of touch panels. .
Patent Information
- Application Number
- CN202010648899.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-07
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-07-07
AI Technical Summary
The surface plasma resonance effect generated by nano silver wires in the conductive film causes the absorption of ultraviolet light, causing the conductive film to be yellow, affecting the image color of the display panel, and it is necessary to reduce the yellowness and improve the visibility and penetration.
By forming a nano-silver wire layer on the substrate and adding a dye, such as cryptocrystal violet, adjusting the yellowishness to form an absorption peak within the UV spectrum 340nm-400nm and 500nm-650nm, the ratio of the first and second absorption peaks is controlled by controlling the ratio of the first and second absorption peaks, such as adding dyes, such as cryptocrystal violet, to adjust the yellowishness to form an absorption peak in the UV spectrum 340nm-400nm and 500nm-650nm. In the range of 2-5.5, a blue compensation layer is used to neutralize the yellow color, ensuring that the b* value of the conductive film in the CIELAB color space is within the range of ≤1.5 or ≤2.
The degree of yellowing of the nano silver wire layer is effectively reduced, so that the conductive film is neutral, the penetration rate and visibility are improved, the blue color shift caused by excessive compensation is avoided, and the resistance value of the conductive film is maintained.
Smart Images

Figure CN112037968B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a transparent conductive film, in particular to a transparent conductive film used for preparing a touch panel. Background Art
[0002] In recent years, the application scope of touch panels has become increasingly wider, and more electronic products have added touch panels to provide users with the function of directly operating or issuing commands. Among them, the demand for flexible touch panels is increasing. In order to meet this demand, many conductive materials that replace indium tin oxide (ITO) have emerged in recent years to provide good flexibility and excellent conductivity.
[0003] Among them, silver nanowires have high conductivity and excellent flexibility, and are excellent materials for the conductive layer of touch panels. However, since nanowires produce surface plasmon resonance effect, they absorb ultraviolet light in the wavelength range of 320nm to 420nm, so the conductive film prepared by silver nanowires will appear yellow. However, for touch panels combined with display panels, the yellow color presented by silver nanowires will affect the color of the image output by the display panel. Therefore, how to reduce the yellowness of the transparent conductive layer composed of silver nanowires and improve its visibility and transmittance is a technical problem that needs to be solved at present. Summary of the invention
[0004] In view of this, the present invention provides a novel transparent conductive film to achieve the purpose of reducing the yellowness of the conductive film containing nano silver wires.
[0005] The transparent conductive film of the present invention comprises: a substrate, comprising a first surface and a second surface opposite to the first surface; and a first nanosilver wire layer formed on the first surface of the substrate; wherein the transparent conductive film has a first absorption peak in the wavelength band region of 340nm-400nm of the UV spectrum, and a second absorption peak in the wavelength band region of 500nm-650nm, and the ratio of the maximum peak intensity of the first absorption peak to the maximum peak intensity of the second absorption peak is 2-5.5.
[0006] In one embodiment, the ratio of the spectrum integration area of the first absorption peak to the spectrum integration area of the second absorption peak of the transparent conductive film is 1.2-1.8.
[0007] In one embodiment, the transparent conductive film further includes a dye, and the dye is added into the substrate.
[0008] In one embodiment, the substrate includes a transparent base film and a first protective layer, the first protective layer is sandwiched between the transparent base film and the nano silver wire layer, and the dye is added to the first protective layer or the transparent body film.
[0009] In one embodiment, the absolute value of the b* value of the transparent conductive film in the CIELAB color space coordinates is ≤1.5.
[0010] In one embodiment, the transparent conductive film further includes a second nanosilver wire layer disposed on the second surface of the substrate.
[0011] In one embodiment, the substrate further includes a second protective layer sandwiched between the second nanosilver wire layer and the transparent base film, wherein the dye is added to the first protective layer and the second protective layer, or added to the transparent base film. At this time, the absolute value of the b* value of the transparent conductive film in the CIELAB color space coordinate is ≤2.
[0012] In one embodiment, the dye is at least one selected from the group consisting of alizarin blue, basic blue, alcohol blue, water-soluble aniline blue, azo blue, brilliant cresol blue, bromophenol blue, carazolyl blue, quinoline blue, indigo, resin phenol blue, methyl blue, methylene blue, phthalocyanine, resazurin, benzoazurine, Prussian blue, toluene cyanol, thymol blue, triphenyl blue, cryptocrystalline violet and mixtures thereof.
[0013] In one embodiment, the dye is added in an amount of 100-1000 ppm.
[0014] In one embodiment, the stain is preferably cryptocrystalline violet.
[0015] In addition, the term “on” in the present invention is only used to indicate a relative positional relationship. For example, a first nanosilver wire layer disposed “on” a substrate may include a situation where the first nanosilver wire layer is in direct contact with the substrate, or may also include a situation where there are other additional components between the first nanosilver wire layer and the substrate, such that the first nanosilver wire layer is not in direct contact with the substrate.
[0016] Furthermore, the "first" and "second" described in the present invention are only for convenience of explanation and have nothing to do with the quantity or arrangement order. For example, the "first nanosilver wire layer" and the "second nanosilver wire layer" can both be understood as nanosilver wire layers.
[0017] In the art, a dye is added to a transparent base film or a protective layer in a substrate as a blue compensation layer to adjust the yellowish nano silver wire layer to a neutral color. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 Schematic cross-sectional view of the transparent conductive film according to the first and second embodiments of the present invention.
[0019] Figure 2 2 is a schematic cross-sectional view of a transparent conductive film according to the third and fourth embodiments of the present invention.
[0020] Figure 3 It is the UV-VIS absorption spectrum in Test Example 1 of the present invention.
[0021] Description of reference numerals:
[0022] 1000, 2000 Transparent conductive film
[0023] 1 substrate
[0024] 11 Transparent basement membrane
[0025] 12. Protective layer
[0026] 121 First protective layer
[0027] 122 Second protective layer
[0028] 2 Nanosilver wire layer
[0029] 21 First nanosilver wire layer
[0030] 22 Second nanosilver wire layer DETAILED DESCRIPTION
[0031] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings.
[0032] First, the transparent conductive film 1000 of the first embodiment of the present invention is as follows Figure 1 As shown, it includes a substrate 1, a nano silver wire layer 2 and a dye. In the present invention, the substrate 1 includes a transparent base film 11 and a protective layer 12, and the protective layer 12 is between the nano silver wire layer 2 and the transparent base film 11. In this embodiment, the transparent base film 11 is made of PET, the protective layer 12 is a hard coating, and the dye is cryptocrystalline violet, which is added to the protective layer 12.
[0033] In other embodiments, the transparent base film 11 may be, for example, transparent materials commonly used in the art, such as glass, sapphire, acrylic (PMMA), polyvinyl chloride (PVC), polypropylene (PP), polyethylene terephthalate (PET), cycloolefin polymer (COP), polyethylene naphthalate (PEN), triacetate film (TAC), polycarbonate (PC), polystyrene (PS), polyimide, etc., but is not limited thereto.
[0034] In other embodiments, the silver nanowire layer 2 may further include a curing resin, and the slurry containing the silver nanowires and the curing resin are mixed in a ratio of 1: (0.8-1.2) and then coated on the substrate.
[0035] In other embodiments, the protective layer 12 may be a hardening layer or a coat layer formed on the surface of the transparent base film 11 , and may be made of any material currently available in the art as a hardening layer or a coat layer, without particular limitation.
[0036] In other embodiments, the dye can be selected from common dyes in the art, such as alizarin blue, basic blue, alcohol blue, water-soluble aniline blue, azo blue, brilliant cresol blue, bromophenol blue, carazol blue, quinoline blue, indigo, resin phenol blue, methyl blue, methylene blue, phthalocyanine, resazurin, benzazurol, Prussian blue, toluene blue, thymol blue, triphenyl blue, cryptocrystalline violet or a mixture thereof. Among them, cryptocrystalline violet is preferred.
[0037] The structure of the transparent conductive film in the second embodiment of the invention is substantially similar to the transparent conductive film 1000 in the first embodiment, except that the dye is added into the transparent base film 11 .
[0038] The transparent conductive film 2000 of the third embodiment of the present invention is as follows Figure 2 The illustrated embodiment includes a substrate 1, a first nanosilver wire layer 21, a second nanosilver wire layer 22, and a dye. In the present invention, the substrate 1 includes a transparent base film 11, a first protective layer 121, and a second protective layer 122. The first protective layer 121 is between the first nanosilver wire layer 21 and the transparent base film 11, and the second protective layer 122 is between the second nanosilver wire layer 22 and the transparent base film 11. In this embodiment, the transparent base film 11 is made of PET, the first protective layer 121 and the second protective layer 122 are a hard coating layer, and the dye 3 is cryptocrystalline violet, and is added to the first protective layer 121 and the second protective layer 122.
[0039] The structure of the transparent conductive film of the fourth embodiment of the present invention is substantially similar to the transparent conductive film 2000 of the third embodiment, except that the dye is added into the transparent base film 11 .
[0040] The effect of regulating the yellowing degree of the nano silver wire layer in the following test examples is mainly to use the L*a*b* color model established by CIE as the standard for measuring color. The Lab* color model consists of three elements, where L* represents brightness, L*=0 is black, and L*=100 is white; a* represents the position between red / green, a* indicates green when it is negative, and red when it is positive; b* is the position between yellow / blue, b* indicates blue when it is negative, and yellow when it is positive. Therefore, in the following test examples, the b* value can represent the yellowing degree of the transparent conductive film and the indicator of reducing the yellowing degree after adding a dye.
[0041] Test Example 1
[0042] First, this test case uses Figure 1 The transparent conductive film 100 shown is used to measure the UV absorption spectrum of the transparent conductive film 1000 including the nano silver wire layer 2 with different concentrations of cryptocrystalline violet. The parameters of Examples 1-3 and Comparative Examples 1-2 and their transmittance, haze, b* value, and a* value are shown in Table 1.
[0043] Table 1
[0044]
[0045] The UV absorption spectra of Examples 1 to 3 and the comparative example in this test example are as follows: Figure 3 As shown by Figure 3 It can be observed from the UV-Vis absorption spectrum that each group has a first absorption peak in the wavelength range of 340-400nm (blue), and the embodiment with cryptocrystalline violet added has a second absorption peak in the wavelength range of 500-650nm (yellow). The maximum peak intensity and spectrum integration area of the first absorption peak and the second absorption peak are shown in Table 2 and Table 3 respectively:
[0046] Table 2
[0047]
[0048] Table 3
[0049]
[0050] From the above test results, it can be seen that in the group with cryptocrystalline violet added to the protective layer 12, the absolute value of the b* value is reduced, making the b* value closer to 0, indicating that the yellowing degree of the transparent conductive film 1000 is significantly improved. In addition, the ratio of the maximum peak intensity of the first absorption peak (340-400nm) and the second absorption peak (500-650nm) of the UV-Vis absorption spectrum must be within the range of 2-5.5, so that the yellowness of the transparent conductive film can be effectively compensated and present a neutral color, and will not be over-compensated and present a blue color.
[0051] Test Example 2
[0052] This test example tests the addition of different concentrations of cryptocrystalline violet to the protective layer 12 and measures the transmittance, haze, and b* value of the transparent conductive film 1000 formed therefrom to evaluate the effect of the concentration of cryptocrystalline violet added on adjusting the yellowing degree of the nanosilver wire layer 2. Among them, the resistance value of the nanosilver wire layer of Examples 4 to 7 and Comparative Examples 2 to 3 is about 65Ω / square, and the concentration of cryptocrystalline violet is 0-2000ppm, that is, the results are shown in Table 4:
[0053] Table 4
[0054]
[0055] From the test results in Table 4, it can be seen that the absolute values of the b* values of Examples 4 to 7 are all ≤1. Within this appropriate range, the yellowing degree of the transparent conductive film can be effectively controlled. However, the b* value of Comparative Example 2 is -3.52, which is too low, making the overall transparent conductive film appear bluish. Therefore, if the concentration of cryptocrystalline violet is added too high (the concentration of cryptocrystalline violet in Comparative Example 2 is 2000 ppm), the color presented by the transparent conductive film cannot be effectively adjusted. Therefore, the results of this test example confirm that the concentration of cryptocrystalline violet in the range of 125-1000 ppm (i.e., Examples 4 to 7) can effectively reduce the yellowing degree of the nanosilver wire layer 2.
[0056] Test Example 3
[0057] Based on the results of the previous test example, this test example tests the concentration of cryptocrystalline violet added to the protective layer 12 in the range of 125-1000 ppm, and measures the transmittance, haze, and b* value of the transparent conductive film formed therefrom to evaluate the effect of cryptocrystalline violet on the yellowing degree of the nanosilver wire layer 2 with different resistance values. Among them, the resistance value of the nanosilver wire layer 2 of Example 8-Example 11 and Comparative Example 4 is approximately 30-35Ω / square, and the test results are shown in Table 5. The resistance value of the nanosilver wire layer 2 of Example 12-Example 15 and Comparative Example 5 is approximately 50-55Ω / square, and the test results are shown in Table 6. The resistance value of the nanosilver wire layer 2 of Example 16-Example 19 and Comparative Example 6 is approximately 70-75Ω / square, and the test results are shown in Table 7.
[0058] Table 5
[0059]
[0060] Table 6
[0061]
[0062] Table 7
[0063]
[0064]
[0065] From the experimental results in Tables 5 to 7, it can be seen that the addition of cryptocrystalline violet can effectively control the yellowing degree of the silver nanowire layer 2 with different resistance values and maintain the absolute value of its b* value within ≤1.5.
[0066] Test Example 4
[0067] This test example uses a transparent conductive film 1000 composed of a transparent base film 11 of different materials, and measures the transmittance, haze and b* value of the transparent conductive film 1000 composed of a dye (cryptocrystalline violet) added to the protective layer 12 to evaluate the effect of cryptocrystalline violet on the yellowing degree of the nano silver wire layer 2 with different resistance values. The test results are shown in Table 8. Among them, the substrate 1 used in Example 20 includes a transparent base film 11 composed of cycloolefin polymer (COP) and a protective layer 12 added with 250 ppm of cryptocrystalline violet, and the nanosilver wire layer 2 is formed on the protective layer 12, and its resistance value is about 30-35Ω / square. The substrate 1 of Comparative Example 7 also uses a transparent base film 11 composed of cycloolefin polymer, but does not have the protective layer 12 added with cryptocrystalline violet, and the nanosilver wire layer 2 is directly formed on the transparent base film 11; The substrate used in Example 21 includes a transparent base film 11 composed of PET and a protective layer 12 added with 250 ppm of cryptocrystalline violet, and the nanosilver wire layer 2 is formed on the protective layer 12, and its resistance value is about 30-35Ω / square. The substrate 1 of Comparative Example 8 also uses a transparent base film 11 composed of PET, does not have the protective layer 12 added with cryptocrystalline violet, and the nanosilver wire layer 2 is directly formed on the transparent base film 11.
[0068] Table 8
[0069] Penetration rate (%) Haze(%) b* value Embodiment 20 91.3 1.32 0.26 Comparative Example 7 91.7 1.36 1.08 Embodiment 21 91.1 1.42 0.72 Comparative Example 8 91.2 1.64 1.49
[0070] From the above test results, it can be seen that the b* value of Example 20 is 0.26, which is 76% lower than the b* value of 1.08 of Comparative Example 7 without adding cryptocrystalline violet; and the b* value of Example 21 is 0.72, which is 51% lower than the b* value of 1.49 of Comparative Example 8 without adding cryptocrystalline violet. Therefore, this test example confirms that for substrates of different materials, adding a dye can still effectively control the yellowing degree caused by the nano silver wire layer 2, making the b* value of the transparent conductive film close to 0, and maintaining a certain high transmittance and low haze.
[0071] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A transparent conductive film, characterized in that: include: A substrate having a first surface and a second surface opposite to the first surface; as well as A first nanosilver wire layer is formed on the first surface of the substrate; a dye added to the substrate; The transparent conductive film has a first absorption peak in the wavelength band of 340 nm-400 nm and a second absorption peak in the wavelength band of 500 nm-650 nm, and the ratio of the maximum peak intensity of the first absorption peak to the maximum peak intensity of the second absorption peak is 2-5.
5.
2. The transparent conductive film according to claim 1, characterized in that: The ratio of the maximum peak intensity of the first absorption peak to the maximum peak intensity of the second absorption peak is 3.23-5.
35.
3. The transparent conductive film according to claim 1 or 2, characterized in that: The ratio of the spectrum integration area of the first absorption peak to the spectrum integration area of the second absorption peak of the transparent conductive film is 1.2-1.
8.
4. The transparent conductive film according to claim 1, wherein: The substrate comprises a transparent base film and a first protection layer, wherein the first protection layer is sandwiched between the transparent base film and the first nano silver wire layer.
5. The transparent conductive film according to claim 4, characterized in that: The dye is added into the first protective layer or the transparent base film.
6. The transparent conductive film according to claim 4, characterized in that: The absolute value of the b* value of the transparent conductive film in the CIELAB color space coordinates is ≤1.
5. 7 . The transparent conductive film as claimed in claim 4 , further comprising a second nanosilver wire layer disposed on the second surface of the substrate.
8. The transparent conductive film according to claim 7, characterized in that: The substrate also includes a second protective layer, which is sandwiched between the second nano silver wire layer and the transparent base film, wherein the dye is added to the first protective layer and the second protective layer, or added to the transparent base film.
9. The transparent conductive film according to claim 8, characterized in that: The absolute value of the b* value of the transparent conductive film in the CIELAB color space coordinates is ≤2.
10. The transparent conductive film according to claim 1, wherein: The dye is at least one selected from the group consisting of alizarin blue, basic blue, alcohol blue, water-soluble aniline blue, azo blue, brilliant cresol blue, bromophenol blue, carazolyl blue, quinoline blue, indigo, resin phenol blue, methyl blue, methylene blue, phthalocyanine, resazurin, benzoazurine, Prussian blue, toluene cyanol, thymol blue, triphenyl blue, cryptocrystalline violet and a mixture thereof.
11. The transparent conductive film according to claim 10, wherein: The dye is added in an amount of 100-1000ppm.
12. The transparent conductive film according to claim 11, characterized in that: The stain is cryptocrystalline violet.