Solid electrolyte membrane, method for producing the same, and all-solid-state battery comprising the same

By pressing polymer electrolyte materials into porous polymer sheets, the problem of low strength of polymer solid electrolyte materials is solved, a solid-state battery electrolyte membrane with small thickness and high strength is realized, and the energy density and safety of the battery are improved. sex.

CN112074981BActive Publication Date: 2024-10-29LG ENERGY SOLUTION LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN201980027837.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-06
Publication Date
2024-10-29
Estimated Expiration
2039-12-06

AI Technical Summary

Technical Problem

Existing polymer solid electrolyte materials have low strength and are prone to tearing during the manufacturing process. In addition, the electrolyte membrane in lithium metal batteries may be damaged, leading to insulation failure and affecting the safety and energy density of solid-state batteries.

Method used

A composite of a porous polymer sheet and a polymer electrolyte material is used. The polymer resin and lithium salt are mixed in a solvent and dried to form a solid electrolyte membrane layer, and then pressed into the porous polymer sheet to form a composite to improve Mechanical strength and ionic conductivity.

Benefits of technology

The electrolyte membrane for solid-state batteries with small thickness and high strength has been realized, which improves the energy density and mechanical strength of the battery, reduces the porosity and resistance of the electrolyte membrane, and enhances the safety and processability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112074981B_ABST
    Figure CN112074981B_ABST
Patent Text Reader

Abstract

The present invention relates to a solid electrolyte membrane for an all-solid-state battery and a method for manufacturing the same, wherein the solid electrolyte membrane comprises a polymer electrolyte material and a porous polymer sheet, which form a composite with each other so that the pores of the porous polymer sheet are filled with the polymer electrolyte material. Since the porous polymer material and the solid electrolyte material form a composite with each other, a solid electrolyte membrane having excellent strength and a small thickness of 50 μm or less can be obtained, thereby improving the energy density of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrolyte membrane for a solid-state battery, a solid-state battery including the electrolyte membrane, and a method for producing the electrolyte membrane.

[0002] This application claims priority to Korean Patent Application No. 10-2018-0156424 filed in Korea on December 6, 2018, Korean Patent Application No. 10-2018-0156425 filed in Korea on December 6, 2018, and Korean Patent Application No. 10-2019-0052530 filed in Korea on May 3, 2019, the disclosures of which are incorporated herein by reference. Background Art

[0003] Lithium-ion batteries using liquid electrolytes have a structure in which the negative electrode and the positive electrode are defined by a separator, so when the separator is damaged by deformation or external impact, a short circuit may result, causing dangers such as overheating or explosion. Therefore, it can be said that the development of a solid electrolyte that can ensure safety is a very important issue in the field of lithium-ion secondary batteries.

[0004] The advantages of lithium secondary batteries using solid electrolytes are that they have enhanced safety, prevent leakage of electrolytes to improve battery reliability, and facilitate the manufacture of thin batteries. In addition, lithium metal can be used as a negative electrode to increase energy density. Therefore, in addition to compact secondary batteries, such lithium secondary batteries using solid electrolytes are expected to be applied to high-capacity secondary batteries for electric vehicles and are attracting much attention as next-generation batteries.

[0005] Generally, as solid electrolyte materials, polymer solid electrolytes, oxide solid electrolytes and sulfide solid electrolytes have been used. Among them, the advantages of polymer solid electrolytes include low cost, material flexibility, easy processability, battery safety, and improved energy density due to thin filmization of electrolyte layers and batteries.

[0006] However, the strength of this polymer solid electrolyte material is low. Therefore, when a thin film with a thickness of tens of microns is formed by the polymer solid electrolyte material, tearing may occur during the manufacturing process of the electrolyte membrane or the battery. In addition, when the polymer solid electrolyte material is used as an electrolyte membrane material for a lithium metal battery, the electrolyte membrane may be damaged by lithium dendrites formed from the negative electrode, resulting in insulation failure between the negative electrode and the positive electrode. Therefore, in order to achieve the excellent electrochemical properties of solid-state batteries, it is necessary to develop a solid electrolyte membrane using a polymer solid electrolyte with a new composition and a solid-state battery using the same.

[0007] Meanwhile, according to the prior art, polymer-based solid electrolyte materials are used in the form of slurry dispersed in a solvent. Since solid-state batteries do not use liquid electrolytes, the pores created by solvent evaporation can act as resistors. Summary of the invention

[0008] [Technical issues]

[0009] The present invention aims to solve the problems of the prior art, and therefore the present invention aims to provide a solid electrolyte membrane for a solid-state battery using a polymer-based solid electrolyte material, which has a small thickness and excellent strength, and a solid-state battery including the same.

[0010] The present invention also aims to provide a solid electrolyte membrane for solid-state batteries having improved ion conductivity compared with conventional solid electrolyte membranes.

[0011] In addition, the present invention aims to provide a method for manufacturing a solid electrolyte membrane having the above-mentioned characteristics and a method for manufacturing a solid-state battery comprising the solid electrolyte membrane. At the same time, these and other objects and advantages of the present invention can be understood from the following detailed description. Moreover, it is easy to understand that the objects and advantages of the present invention can be achieved by the means and combinations thereof shown in the attached claims.

[0012] [Technical solution]

[0013] In one aspect of the present invention, a solid electrolyte membrane for a solid-state battery as described in any one of the following embodiments is provided.

[0014] According to a first embodiment of the present invention, a solid electrolyte membrane for a solid-state battery is provided, which comprises a polymer electrolyte material and a porous polymer sheet, wherein the porous polymer sheet is a porous material comprising a plurality of pores, and the pores are penetrated by a fluid material; and the polymer electrolyte material forms a complex with the porous polymer sheet so that the pores of the porous polymer sheet are filled with the polymer electrolyte material.

[0015] According to a second embodiment of the present invention, there is provided a solid electrolyte membrane for a solid-state battery as defined in the first embodiment, wherein the polymer electrolyte material is a solid electrolyte membrane layer formed by drying a solvent in a polymer resin added to a solvated lithium salt, and exhibits a 1×10 -7 S / cm or above ionic conductivity.

[0016] According to a third embodiment of the present invention, there is provided the solid electrolyte membrane for a solid-state battery as defined in the second embodiment, wherein the polymer resin has a weight average molecular weight (Mw) of 5,000 to 5,000,000.

[0017] According to a fourth embodiment of the present invention, there is provided a solid electrolyte membrane for a solid-state battery as defined in any one of the first to third embodiments, wherein the porous polymer sheet is a nonwoven fabric.

[0018] According to a fifth embodiment of the present invention, there is provided a solid electrolyte membrane for a solid-state battery as defined in any one of the first to fourth embodiments, which has a thickness of 15 μm to 90 μm and a tensile strength of about 500 kgf / cm 2 Up to 2,000kgf / cm 2 .

[0019] According to a sixth embodiment of the present invention, there is provided the solid electrolyte membrane for a solid-state battery as defined in the fifth embodiment, the porosity of which is 15% or less.

[0020] According to a seventh embodiment of the present invention, there is provided a solid electrolyte membrane for a solid-state battery as defined in any one of the first to sixth embodiments, wherein the polymer electrolyte material includes at least one selected from a polyalkylene carbonate-based polymer resin and a polysiloxane-based polymer resin.

[0021] According to an eighth embodiment of the present invention, a solid electrolyte membrane for a solid-state battery as defined in any one of the first to seventh embodiments is provided, wherein the porous polymer sheet is provided with an ion channel comprising perforations, the porous polymer sheet is subjected to hydrophilic surface modification, and the polymer electrolyte material is filled in the ion channel of the porous polymer sheet and the pores of the porous polymer sheet, so that the polymer electrolyte material can form a complex with the porous polymer sheet.

[0022] According to a ninth embodiment of the present invention, there is provided a solid electrolyte membrane for a solid-state battery as defined in the eighth embodiment, wherein at least one of the surface, pores and ion channels of the porous polymer sheet is hydrophilically surface-modified.

[0023] According to a tenth embodiment of the present invention, there is provided a solid electrolyte membrane for a solid-state battery as defined in the eighth embodiment, wherein the porous polymer sheet is a polymer membrane including a polyolefin-based polymer resin, and the thickness of the polymer membrane is 5 μm to 50 μm.

[0024] In another aspect of the present invention, a method for manufacturing a solid electrolyte membrane for a solid-state battery as described in any one of the following embodiments is also provided.

[0025] According to an eleventh embodiment of the present invention, there is provided a method for manufacturing a solid electrolyte membrane for a solid-state battery, comprising the following steps:

[0026] (S10) preparing a porous polymer sheet and at least one solid electrolyte membrane layer;

[0027] (S20) disposing the solid electrolyte membrane layer on the surface of the porous polymer sheet; and

[0028] (S30) applying pressure to press the solid electrolyte membrane layer into the pores of the porous polymer sheet,

[0029] The solid electrolyte membrane layer comprises a solid electrolyte material formed by drying a solvent added to a polymer resin in a solvated lithium salt, and exhibits a 1×10 -7 S / cm or above ionic conductivity.

[0030] According to a twelfth embodiment of the present invention, there is provided a method for manufacturing a solid electrolyte membrane for a solid-state battery as defined in the eleventh embodiment, wherein the solid electrolyte membrane layer is heated before or simultaneously with step (S30).

[0031] According to a thirteenth embodiment of the present invention, a method for manufacturing a solid electrolyte membrane for a solid-state battery as defined in the eleventh or twelfth embodiment is provided, wherein the pressurizing in step (S30) is performed using at least one pressurizing member selected from a roller press, a clamp and a uniaxial press.

[0032] According to a fourteenth embodiment of the present invention, there is provided a method for producing a solid electrolyte membrane for a solid-state battery as defined in any one of the eleventh to thirteenth embodiments, wherein the pressurizing member is provided with a heating member.

[0033] According to a fifteenth embodiment of the present invention, there is provided a method for manufacturing a solid electrolyte membrane for a solid-state battery as defined in any one of the eleventh to fourteenth embodiments, wherein the polymer resin includes at least one selected from a polyalkylene carbonate polymer resin and a polysiloxane polymer resin, and the porous polymer sheet is a non-woven fabric.

[0034] In another aspect of the present invention, a method for manufacturing a solid electrolyte membrane for a solid-state battery as described in any one of the following embodiments is provided.

[0035] According to a sixteenth embodiment of the present invention, there is provided a method for manufacturing a solid electrolyte membrane for a solid-state battery, comprising the following steps:

[0036] (T10) preparing a porous polymer sheet;

[0037] (T11) forming an ion channel including perforations in the thickness direction of the porous polymer sheet;

[0038] (T13) performing hydrophilic surface modification on the porous polymer sheet;

[0039] (T14) disposing a solid electrolyte membrane layer on the upper surface of the resultant product of step (T13) to obtain a laminated structure; and

[0040] (T15) pressurizing the stacked structure so that the ion channels and pores of the porous polymer sheet can be filled with the solid electrolyte membrane layer,

[0041] The solid electrolyte membrane layer comprises a solid electrolyte material formed by adding a polymer resin to a solvated lithium salt and is formed by drying a solvent in the solid electrolyte material and exhibits a 1×10 -7 S / cm or above ionic conductivity.

[0042] According to a seventeenth embodiment of the present invention, there is provided a method for manufacturing a solid electrolyte membrane for a solid-state battery as defined in the sixteenth embodiment, wherein the volume of the ion channel is 5 volume % to 90 volume % based on 100 volume % of the total volume of the porous polymer sheet.

[0043] According to an eighteenth embodiment of the present invention, there is provided a method for manufacturing a solid electrolyte membrane for a solid-state battery as defined in the sixteenth or seventeenth embodiment, wherein the diameter of the perforations is 50 nm to 1 mm.

[0044] According to a nineteenth embodiment of the present invention, there is provided a method for manufacturing a solid electrolyte membrane for a solid-state battery as defined in any one of the sixteenth to eighteenth embodiments, wherein the surface modification is performed using any one of UV irradiation, plasma, acid treatment and ozone treatment.

[0045] [Beneficial Effects]

[0046] The solid electrolyte membrane of the present invention can reduce manufacturing costs by using a polymer solid electrolyte and allows easy deformation, so it can be applied to various types of batteries. In addition, the solid electrolyte membrane of the present invention includes a composite of a porous polymer sheet (such as a non-woven fabric) and a solid electrolyte material, so it can be formed into a film with a thickness of less than 50 μm while providing high strength. Therefore, the solid electrolyte membrane of the present invention is conducive to improving the energy density of the battery.

[0047] In addition, since the polymer electrolyte material is used in a form after drying the solvent, the formation of pores that may function as resistance may be reduced after drying the solvent. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] The accompanying drawings illustrate preferred embodiments of the present invention and are used together with the foregoing disclosure to provide a further understanding of the technical features of the present invention. Therefore, the present invention is not to be construed as being limited to the accompanying drawings. At the same time, the shapes, sizes, scales or proportions of some constituent elements in the accompanying drawings may be exaggerated for a clearer description.

[0049] Figure 1 1 is a schematic flow chart showing a method for producing a solid electrolyte membrane of the present invention.

[0050] Figure 2 is a schematic cross-sectional view showing a conventional solid electrolyte membrane.

[0051] Figure 3 This is a schematic flow chart showing a method for producing a solid electrolyte membrane according to one embodiment of the present invention.

[0052] Figure 4 Schematic diagram showing a solid electrolyte membrane according to one embodiment of the present invention. DETAILED DESCRIPTION

[0053] Hereinafter, the preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. Before the description, it should be understood that the terms used in the specification and the appended claims should not be interpreted as limited to the general meaning and dictionary meaning, but should be interpreted based on the principle that the inventor is allowed to appropriately define the terms for the best interpretation, based on the meaning and concept corresponding to the technical aspects of the present invention. Therefore, the descriptions presented herein are only preferred examples for illustrative purposes and are not intended to limit the scope of the present invention, so it should be understood that other equivalent substitutions and modifications may be made thereto without departing from the scope of the present invention.

[0054] Throughout the specification, the expression “a part “comprising” an element” does not exclude the existence of any other elements but means that the part may further include other elements.

[0055] As used herein, the terms "about" or "substantially" and the like are used to mean extending in both directions from the stated numerical value, indicating acceptable manufacturing and material errors unique to the stated meaning, and for the purpose of preventing unscrupulous infringers from improperly using the disclosed content containing exact or absolute numerical values, which are provided to aid in the understanding of the present invention.

[0056] As used herein, the expression "A and / or B" means "A, B, or both."

[0057] Specific terms used in the following description are for illustrative purposes only and are not intended to be limiting. Terms such as "right," "left," "upper surface," and "lower surface" indicate directions in the drawings to which they refer. Terms such as "inwardly" and "outwardly" indicate directions toward the geometric center of the corresponding device, system, and components thereof, and directions away from the center, respectively. "Front," "rear," "upper," and "lower," and related words and expressions indicate positions and orientations in the drawings to which they refer, but should not be limited. Such terms include the words listed above, their derivatives, and words of similar meaning.

[0058] The present invention relates to a solid electrolyte membrane for a solid-state battery and a solid-state battery comprising the same. The present invention also relates to a method for manufacturing the electrolyte membrane. The solid electrolyte membrane for a solid-state battery of the present invention can be formed into a thin film having a thickness of about 100 μm or less, and thus has high ion conductivity and can provide a battery with increased energy density. In addition, the solid electrolyte membrane is thin but strong, and therefore is less damaged during its manufacturing process or during the use of the battery.

[0059] Figure 1 1 is a schematic diagram showing a solid electrolyte membrane and a method for manufacturing the solid electrolyte membrane according to an embodiment of the present invention. Hereinafter, the present invention will be described in detail with reference to the accompanying drawings.

[0060] The solid electrolyte membrane 100 for a solid-state battery of the present invention includes a polymer electrolyte material 11 and a porous polymer sheet 12 having a plurality of pores, wherein the pores of the polymer sheet are filled with a polymer-based solid electrolyte.

[0061] In the solid electrolyte membrane, the polymer electrolyte material forms a complex in the porous polymer sheet, thereby causing an increase in mechanical strength. At the same time, the polymer electrolyte material can transport lithium ions, thereby providing an electrolyte membrane with improved ion conductivity.

[0062] The polymer electrolyte material is formed by drying the solvent in the polymer resin added to the solvated lithium salt, and exists in the form of a solid electrolyte membrane layer after the solvent is dried. It can be easily handled and used in the form of a membrane layer from which the solvent has been dried to prevent the formation of pores that may serve as resistance.

[0063] The polymer sheet is a porous material containing a plurality of pores and includes a polymer material. According to one embodiment of the present invention, the polymer sheet may include: a polymer film formed by dry melting, extruding and extending a polymer material, a polymer film obtained by wet extracting a plasticizer to form pores, a non-woven fabric obtained by melting, spinning and compressing a polymer material, a laminated sheet including two or more layers thereof, and the like. For example, the polymer sheet may be a non-woven fabric.

[0064] In the porous polymer sheet, a plurality of holes are formed, wherein the holes are interconnected and penetrate the substrate from one surface to another surface, so that the fluid material can pass through these holes. As the material for forming the porous polymer sheet, any organic material or inorganic material with electrical insulation can be used. According to one embodiment of the present invention, the polymer sheet may include at least one polymer resin, such as polyolefin, polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide and polyethylene naphthalate.

[0065] According to one embodiment of the present invention, the thickness of the porous sheet may be about 5 to 90 μm. Considering the thickness and strength of the finished electrolyte membrane, the thickness may be appropriately selected within the above range. If the thickness of the porous sheet is less than the above range, it is difficult to obtain the desired level of strength of the solid electrolyte membrane. If the thickness of the sheet is too large, it is difficult to control the thickness to the desired level even if a pressurization process is applied.

[0066] In addition, according to one embodiment of the present invention, the porosity of the porous polymer sheet can be about 10% to 90%, and the pore size can be appropriately controlled within the range of 50nm to 100μm. The porosity range and the pore size range can be appropriately selected within the above range so that the porous polymer sheet can retain a sufficient amount of electrolyte membrane layer to function as an electrolyte membrane, and will not hinder the electrolyte membrane layer with low fluidity from being pressed into the sheet while maintaining appropriate ionic conductivity and mechanical strength. In other words, as the porosity increases, the ionic conductivity can be improved, but the mechanical strength may decrease. In addition, as the pore size increases, the electrolyte membrane layer is easier to press into.

[0067] Meanwhile, according to the present invention, the polymer solid electrolyte is a composite of a lithium salt and a polymer resin, that is, a polymer electrolyte material formed by adding a polymer resin to a solvated lithium salt and drying the solvent. The ionic conductivity of the polymer solid electrolyte can be about 1x10 -7 S / cm or more, preferably about 1x10 -5 S / cm or more.

[0068] According to one embodiment of the present invention, the weight average molecular weight (Mw) of the polymer resin may be about 5,000 to 5,000,000. As the molecular weight decreases, fluidity increases to facilitate the pressing process.

[0069] As described below, the solid electrolyte membrane of the present invention is obtained by forming a polymer electrolyte into a membrane layer shape and pressing the polymer electrolyte membrane layer into a porous sheet. When the above conditions are met, the pressing process can be easily performed.

[0070] According to one embodiment of the present invention, the polymer resin is a polymer resin that satisfies the above conditions, and may include a thermoplastic polymer resin. Non-limiting examples of polymer resins may include polyether polymers, polycarbonate polymers, acrylate polymers, polysiloxane polymers, phosphazene polymers, polyethylene derivatives, alkylene oxide derivatives (e.g., polyethylene oxide), phosphate polymers, poly-stirring lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, or polymers containing ionic dissociation groups, etc. According to one embodiment of the present invention, the solid polymer electrolyte may include the following materials as polymer resins: branched copolymers, comb polymers, or cross-linked polymer resins, etc., comprising a polyethylene oxide (PEO) main chain copolymerized with a comonomer containing an amorphous polymer (e.g., PMMA, polycarbonate, polysiloxane (PDMS) and / or phosphazene).

[0071] According to one embodiment of the present invention, the polymer resin may include at least one selected from a polyalkylene carbonate polymer resin and a polysiloxane polymer resin, which is combined with the above-mentioned polymer resin or is independent of the above-mentioned polymer resin. For example, the polyalkylene carbonate resin may include at least one of polyethylene carbonate, polyethylene carbonate copolymer, polypropylene carbonate and polypropylene carbonate copolymer. In terms of ionic conductivity and oxidative stability, polypropylene carbonate (PPC) is preferably used. In addition, according to one embodiment of the present invention, the weight average molecular weight (Mw) of the polyalkylene carbonate polymer resin may be about 5,000 to 1,000,000.

[0072] According to one embodiment of the present invention, the polymer resin may include a polysiloxane polymer, which is combined with the above-mentioned polymer resin or is independent of the above-mentioned polymer resin. Although the polysiloxane polymer resin has high ionic conductivity, it has low strength, so it is difficult to use it in a solid electrolyte membrane. However, when a polysiloxane polymer is used as a solid electrolyte material of the present invention, ionic conductivity and mechanical properties can be ensured at the same time. According to one embodiment of the present invention, the polysiloxane polymer resin contains a structure represented by [Chemical Formula 1] in the polymer chain, and may be selected from at least one of polyalkylsiloxane, polyarylsiloxane, polyorganosiloxane and a copolymer containing at least one thereof. Non-limiting examples of polysiloxane polymer resins include polymethylhydrogensiloxane (PMHS) and polydimethylsiloxane (PDMS). In addition, the weight average molecular weight (Mw) of the polysiloxane polymer resin may be about 1,000 to 1,000,000.

[0073] [Chemical formula 1]

[0074]

[0075] Wherein, R1 and R2 each independently represent H or a C1-C30 straight chain, branched, monocyclic or polycyclic saturated or unsaturated hydrocarbon group containing or not containing heteroatoms.

[0076] According to one embodiment of the present invention, in terms of ionic conductivity and physical strength, the polymer electrolyte material may include at least one of a polyalkylene carbonate-based polymer resin and a polysiloxane-based polymer resin in an amount of 80 wt % or more, or 90 wt % or more, based on 100 wt % of the polymer resin.

[0077] Meanwhile, according to one embodiment of the present invention, the polymer electrolyte material may further include a plasticizer in an amount of 0.1 to 20 weight percent based on 100 weight percent of the polymer electrolyte material. The plasticizer can improve the flexibility and fluidity of the electrolyte membrane layer, thereby facilitating the introduction of the electrolyte membrane layer into the porous sheet during the press-in process as described below. With regard to the manufacturing process of the solid electrolyte membrane, the higher the content of the plasticizer, the better. However, in this case, the content of the solid electrolyte material will decrease. Therefore, with regard to strength, the content of the plasticizer is preferably limited within the above range.

[0078] In terms of its composition, the plasticizer that can be used in this article is not particularly limited, and suitable plasticizer can be selected according to the specific type of the solid electrolyte material used. The non-limiting examples of plasticizers include ethylene carbonate (EC), propylene carbonate (PC), vinylene carbonate (VC), dioctyl phthalate (DOP), diisodecyl phthalate (DIDP), diisononyl phthalate (DINP), trioctyl trimellitate (TOTM) or triisononyl trimellitate (TINTM) etc. At least one. After being pressed into, the plasticizer can remain in the solid electrolyte membrane or can be removed by a drying process.

[0079] Meanwhile, the inventors of the present invention have found that when a solid electrolyte membrane containing a solid electrolyte is formed into a thin film, there is a problem of reduced mechanical strength. It has also been found that since the solid electrolyte membrane acts as an ion channel between the positive electrode and the negative electrode, high ion conductivity is still required.

[0080] In order to solve the above problems, according to the present invention, a solid electrolyte membrane for a solid-state battery is also provided, which has improved mechanical strength and ion conductivity and low resistance by using a porous polymer sheet provided with an ion channel having perforations of a predetermined size, performing hydrophilic surface modification on the porous polymer sheet, and applying a polymer solid electrolyte material in the solid electrolyte membrane for the solid-state battery. The solid electrolyte membrane of the present invention includes a porous polymer sheet forming a composite with a solid electrolyte material, has excellent strength and can be formed into a thin film with a thickness of 50 μm or less, and is therefore conducive to improving the energy density of the battery.

[0081] Figure 2 is a schematic cross-sectional view showing a conventional solid electrolyte membrane. Figure 3 Schematic diagram showing a solid electrolyte membrane according to an embodiment of the present invention and a method for producing the solid electrolyte membrane according to an embodiment of the present invention. Figure 4 Schematic diagram showing a solid electrolyte membrane of one embodiment of the present invention. Hereinafter, the present invention will be explained in more detail with reference to the accompanying drawings.

[0082] refer to Figure 2 When the solid electrolyte membrane 21 is controlled to have a large thickness of about 100 μm in order to improve the mechanical strength of the solid electrolyte membrane, the energy density is reduced and the processability is also deteriorated. In addition, even if the thickness is increased, the strength of the solid electrolyte membrane itself is low, so the membrane itself is damaged by lithium dendrites formed by the lithium metal negative electrode 22, thereby undesirably causing a short circuit. The inventors of the present invention have studied a method of forming a composite of a porous polymer sheet and a solid electrolyte material to solve the above-mentioned problems.

[0083] However, conventional polymer sheets have a low porosity of 20% to 50% and a small average pore size of 20nm to 500nm. Therefore, it is difficult to press the solid electrolyte material into the polymer sheet. Even if the solid electrolyte material is filled in the polymer sheet, there is a problem of low ion conductivity due to the tortuosity in the porous polymer sheet.

[0084] In order to solve the above problems, the solid electrolyte membrane for solid-state batteries according to an embodiment of the present invention includes a polymer solid electrolyte material and a porous polymer sheet having multiple pores, wherein the pores of the polymer sheet are filled with the polymer solid electrolyte material, and in particular, the polymer sheet is provided with ion channels having perforations of a predetermined diameter and has undergone hydrophilic surface modification.

[0085] The solid electrolyte membrane of the embodiment of the present invention can use a porous polymer sheet to improve mechanical strength. In addition, since a polymer-based solid electrolyte material is used, it is possible to facilitate the incorporation of the solid electrolyte material into the ion channels in the porous polymer sheet and the pores of the porous polymer sheet. Therefore, the dead zone can be reduced and the ion conductivity can be significantly improved.

[0086] In another aspect of the present invention, a solid electrolyte membrane for a solid-state battery is provided, which comprises a polymer electrolyte material and at least one porous polymer sheet, wherein the porous polymer sheet is provided with an ion channel comprising perforations, the porous polymer sheet is subjected to hydrophilic surface modification, and the polymer electrolyte material is filled in the ion channel of the porous polymer sheet and the pores of the porous polymer sheet, so that the polymer electrolyte material can form a complex with the porous polymer sheet.

[0087] The porous polymer sheet is a porous material containing a plurality of pores and includes a polymer resin. The porous polymer sheet of the present invention may be provided with ion channels containing through holes having a diameter of 50 nm to 1 mm, 100 nm to 700 μm, or 1 μm to 500 μm.

[0088] Ion channels can be penetrated by the fluid material in the thickness direction. Therefore, lithium ions can be transferred more smoothly between the positive and negative electrodes of the battery.

[0089] In particular, unlike conventional porous polymer sheets, the porous polymer sheet of the present invention is provided with large-diameter ion channels in the thickness direction, so that the tortuosity of lithium ions is low, so that lithium ions can form a flow in a specific direction toward the positive electrode or the negative electrode. Therefore, the lithium ion migration length is minimized and the ion conductivity is improved.

[0090] At this time, the diameter of the above-mentioned perforation is very large compared with the holes in the conventional porous polymer sheet, and is not limited to any specific shape. For example, the perforation can have a circular, elliptical or polygonal shape. From the perspective of reducing the dead zone when pressing the polymer-based solid electrolyte membrane layer, the perforation can have a circular or elliptical shape.

[0091] According to one embodiment of the present invention, the perforations may be formed at intervals of 0.1 to 10 mm, 0.5 to 7 mm, 0.75 to 5 mm, or 1 to 2 mm. When the intervals between the perforations are controlled as described above, the volume of the ion channels in the solid electrolyte membrane may be controlled. Within the above range, a solid electrolyte membrane having high ion conductivity and controlled mechanical strength may be provided.

[0092] The volume of the ion channel may be 5 to 90%, 10 to 80%, or 20 to 60% based on 100% by volume of the entire porous polymer sheet. Within the above range, a solid electrolyte membrane having high ion conductivity and high mechanical strength can be provided.

[0093] Ion channels can be formed by physical drilling.

[0094] According to one embodiment of the present invention, the tortuosity of the ion channel may be 1-2.

[0095] In other words, according to the present invention, the pore tortuosity (ie, straightness) that enables lithium ions to be smoothly transferred in the solid electrolyte membrane can be ensured by means of the ion channel.

[0096] As used herein, "tortuosity" is an index indicating how tortuosity an ion channel has, and can be calculated by dividing the actual migration length of lithium ions in the ion channel by the length of a straight line between the same points. In other words, in the case where the tortuosity is 1, it refers to an ion channel where the migration length of lithium ions is a straight line. As the tortuosity increases to greater than 1, the pore has a greater tortuosity.

[0097] According to one embodiment of the present invention, the tortuosity of the ion channel is preferably 1 to 2. Within the above range, smooth transmission of lithium ions can be ensured. In other words, the ion channel in the solid electrolyte membrane of the embodiment of the present invention can be formed into a tubular shape with little or no tortuosity.

[0098] Such an ion channel structure enables lithium ions to be transported smoothly, thereby improving the ionic conductivity of the solid electrolyte membrane and reducing the resistance.

[0099] The porous polymer sheet of the present invention is hydrophilically modified. Specifically, at least one of the pores, surfaces and ion channels in the porous polymer sheet can be hydrophilically modified. Therefore, the solid electrolyte membrane of the embodiment of the present invention allows the polymer solid electrolyte material to be incorporated into the pores and ion channels of the porous polymer sheet, and the polymer solid electrolyte and the hydrophilically modified porous polymer sheet can form a composite more firmly physically or chemically.

[0100] More specifically, improving the compatibility between the hydrophilic polymer-based solid electrolyte material and the hydrophilic porous polymer sheet makes it possible to increase the density of the polymer-based solid electrolyte material incorporated into the ion channels or pores, thereby improving the ion conductivity.

[0101] According to one embodiment of the present invention, the porous polymer sheet may be a polymer film including a polyolefin-based polymer resin.

[0102] Here, the polyolefin-based polymer resin may include any one or two or more of the following: polyethylene; polypropylene; polybutene; polypentene; polyhexene; polyoctene; and copolymers of two or more of ethylene, propylene, butene, pentene, 4-methylpentene, hexene and octene.

[0103] According to one embodiment of the present invention, the polyolefin polymer resin can be a hydrophilic polymer resin. For example, the polyolefin polymer resin can be a hydrophilic polymer resin including polyethylene, polypropylene, polyvinyl alcohol, polylactic acid, poly(allylamine hydrochloride), polyamide, polysilane, polysiloxane, polyimide, polyacetate or two or more thereof. When using a hydrophilic polymer resin, hydrophilicity is enhanced by a hydrophilic surface treatment described below. Therefore, a complex can be formed more firmly with a hydrophilic polymer solid electrolyte.

[0104] In particular, the polyolefin-based polymer resin may be hydrophilically surface-modified using polyethylene oxide, polyacrylonitrile, polyacrylic acid, polyacrylate, or two or more thereof.

[0105] According to one embodiment of the present invention, the thickness of the polymer film may be about 5 μm to 50 μm. Within the above range, the solid electrolyte membrane not only achieves a desired strength level but also achieves a high energy density.

[0106] According to the present invention, the polymer-based solid electrolyte material is filled in the pores of the porous polymer sheet, so that the polymer-based solid electrolyte material can form a composite with the porous polymer sheet.

[0107] As described below, the solid electrolyte member is obtained by forming a solid electrolyte containing a solid electrolyte material into a film layer shape and pressing the film layer into a porous polymer sheet. Since the solid electrolyte material is pressed into the porous polymer sheet from this film layer shape, the dead space in the solid electrolyte membrane can be reduced.

[0108] In the electrolyte of the present invention, the lithium salt is an ionizable lithium salt and can be composed of Li + X - The anion of lithium salt (X - ) is not particularly limited, but may include F - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - PF6 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 - CF3CF2SO3 - 、(CF3SO2)2N - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、(SF5)3C - 、(CF3SO2)3C - CF3(CF2)7SO3 - CF3CO2 - 、CH3CO2- 、SCN - or (CF3CF2SO2)2N - wait.

[0109] Since the polymer electrolyte is filled in the porous sheet, the solid electrolyte membrane can be formed into a thin film without reducing the strength of the solid electrolyte membrane. According to the present invention, the thickness of the solid electrolyte membrane is about 100 μm or less, preferably about 15 to 90 μm. Within the above range, the solid electrolyte membrane can have a suitable thickness in consideration of ionic conductivity, physical strength, or energy density applied to the battery, etc. For example, in terms of ionic conductivity or energy density, the thickness can be 80 μm or less, 70 μm or less, 60 μm or less, or 50 μm or less. At the same time, in terms of physical strength, the thickness can be more than 20 μm, more than 30 μm, or more than 40 μm. In addition, the solid electrolyte membrane can have a strength of about 500 to 2,000 kgf / cm 2 The solid electrolyte membrane may have a porosity of 15% or less or about 10% or less.

[0110] According to one embodiment of the present invention, a solid electrolyte membrane can be obtained as follows: an electrolyte membrane layer is formed using a polymer electrolyte material, the electrolyte membrane layer is disposed on the surface of a polymer sheet, and pressurized so that the electrolyte membrane layer can be pressed into the polymer sheet and the pores of the polymer sheet can be filled with a polymer electrolyte.

[0111] Will refer to Figure 1 The method for manufacturing the electrolyte membrane of the present invention is explained in more detail. First, an electrolyte membrane layer is prepared (S10). The electrolyte membrane layer can be prepared as follows. A polymer electrolyte is mixed with a solvent to prepare a slurry for forming an electrolyte membrane layer ( Figure 1 (a)). The solvent may be appropriately selected according to the polymer electrolyte used. For example, when an alkylene oxide electrolyte (e.g., polyethylene oxide (PEO)) is used as the polymer resin, acetonitrile may be used as the solvent. According to one embodiment of the present invention, the solid content of the slurry may be about 5 to 15 wt %. At this time, the uniform mixing of the polymer electrolyte and the solvent may be promoted by increasing the temperature of the slurry to 40° C. to 60° C.

[0112] Next, the slurry is coated on a release sheet such as a terephthalate film and formed into a film layer shape having a predetermined thickness. The coating and forming can be performed by a known coating method (e.g., doctor blade coating). Then, the slurry is dried to remove the solvent and obtain an electrolyte membrane layer ( Figure 1 (b)).

[0113] The obtained electrolyte membrane layer is disposed on the surface of a porous polymer sheet (eg, nonwoven fabric), and pressure is applied to press the electrolyte membrane layer into the sheet (S20) ( Figure 1 (c)). At this time, in order to protect the surface of the electrolyte membrane layer and prevent the electrolyte material from contaminating the surface of the pressurized member, a release film (e.g., a terephthalate film) may be disposed on the surface of the electrolyte membrane layer. Pressurization may be performed using at least one device (e.g., a roller press, a uniaxial press, or a fixture). At this time, by controlling process conditions (e.g., a press, a roller, a fixture gap, an applied pressure, and a temperature), the electrolyte membrane may have a suitable thickness and / or porosity.

[0114] According to one embodiment of the present invention, pressurization can be performed using a suitable pressurizing member selected from known pressurizing members (e.g., a uniaxial press, a hot press, a roller press, and a clamp). In this case, the pressurizing member may be further provided with a separate heating member so that the surface of the member facing the electrolyte membrane layer can be heated. Since the electrolyte membrane layer has increased ductility by being heated by the pressurizing member, it can be easily pressed into the sheet even under low pressure conditions.

[0115] Meanwhile, according to one embodiment of the present invention, after preparing the electrolyte membrane layer and before introducing it into the press-in process, the electrolyte membrane layer may be heated to room temperature (25°C) to 180°C, thereby facilitating the introduction of the material into the pores of the polymer sheet by increasing the ductility of the material. Such a heating method is not limited to a specific method. However, the membrane layer may be heated by allowing it to stand for several hours in an oven heated to a predetermined temperature. At this point, fluidity can be more easily ensured near the glass transition temperature of the solid electrolyte material. However, the addition of lithium salts may result in a decrease in the glass transition temperature.

[0116] According to one embodiment of the present invention, before the porous polymer sheet is introduced into the pressing process, it can be surface modified to improve the hydrophilicity or hydrophobicity of the surface. For example, when PEO is used as the electrolyte membrane layer, the porous polymer sheet can be subjected to hydrophilic surface modification to improve the affinity with PEO. By improving the affinity with the electrolyte material, it is possible to promote the electrolyte membrane layer to be pressed into the porous sheet, and to improve the adhesion between the electrolyte membrane layer and the porous sheet. The hydrophilic surface modification method is not limited to a specific method. For example, the surface modification method can be appropriately selected from known methods, such as UV irradiation, plasma treatment, acid treatment and ozone treatment.

[0117] In still another aspect of the present invention, a method for manufacturing a solid electrolyte membrane according to the following embodiment is provided.

[0118] In the following, reference will be made to Figure 3 The method of manufacturing the solid electrolyte membrane 300 of the embodiment is explained in more detail.

[0119] First, a porous polymer sheet 32 ​​is prepared (T10) ( Figure 3 (a)). The porous polymer sheet may be a polymer film including a polyolefin-based polymer resin, and the thickness of the polymer film may be 5 to 100 μm. In step (T10), the porous polymer sheet may have a low porosity of 20% to 50% and a small pore size of 20 nm to 500 nm.

[0120] The porous polymer sheet may be a polymer film formed by dry-melting, extruding, and extending a polymer material, or a polymer film formed by wet-extracting a plasticizer to form pores.

[0121] Next, an ion channel (T11) including through holes 33 with a diameter of 50 nm to 1 mm is formed in the thickness direction of the porous polymer sheet ( Figure 3 (b)).

[0122] Specifically, the diameter of the perforation may be 50 nm to 1 mm, 100 nm to 700 μm, or 1 μm to 500 μm. Within the above range, a solid electrolyte membrane having high ion conductivity and excellent mechanical strength can be provided.

[0123] In this case, ion channels comprising perforations can be formed by physical perforation.

[0124] For example, a die cutter having a perforation pattern with perforations having a diameter of 500 μm and a perforation interval of 1.5 mm may be used to form ion channels having perforations in the thickness direction of the porous polymer sheet.

[0125] Then, the porous polymer sheet and the ion channels are subjected to hydrophilic surface modification (T13).

[0126] In other words, at least one of the surface, pores and ion channels of the porous polymer sheet is surface modified. As described below, the surface modification is performed before the polymer solid electrolyte material is pressed into the sheet, and the hydrophilicity of the surface can be improved by the surface modification. By improving the affinity of the polymer solid electrolyte material to the porous polymer sheet, it is possible to facilitate the pressing of the electrolyte membrane layer into the porous sheet and improve the adhesion between the electrolyte membrane layer and the porous polymer sheet.

[0127] At this time, the surface modification may be performed by any one method selected from UV (ultraviolet) irradiation, plasma treatment, acid treatment, and ozone treatment.

[0128] According to one embodiment of the present invention, the plasma may be argon, nitrogen, oxygen or a mixed gas plasma containing a mixture of two or more thereof. The plasma may be a low temperature or high temperature plasma, and the plasma generated at low temperature may be particularly preferred. The porous polymer sheet may be treated with plasma to obtain a hydrophilically modified surface, pores and ion channels, thereby firmly forming a composite with the polymer solid electrolyte material.

[0129] Specifically, the polyolefin polymer resin may be subjected to hydrophilic surface modification by plasma using oxygen or ozone. The hydrophilic surface modified polyolefin polymer resin has a hydroxyl or carboxyl functional group, and thus exhibits hydrophilicity.

[0130] According to one embodiment of the present invention, UV irradiation may be performed by exposing the porous polymer sheet to UV having a wavelength of 150 to 300 nm in air to increase compounds containing hydroxyl groups, carbonyl groups, and oxygen groups and to achieve hydrophilic surface modification.

[0131] Then, a solid electrolyte membrane layer 31 including a polymer-based solid electrolyte material is disposed on at least one surface of the hydrophilic surface-treated porous polymer sheet to obtain a laminated structure (T14) ( Figure 3 (c)).

[0132] At this time, the solid electrolyte membrane layer containing a polymer solid electrolyte material can be prepared as follows. The solid electrolyte material is mixed with a solvent to prepare a slurry for forming a solid electrolyte membrane layer. The solvent can be appropriately selected according to the solid electrolyte material used. For example, when an alkylene oxide electrolyte (such as polyethylene oxide) is used as a solid polymer material, acetonitrile can be used as a solvent. According to one embodiment of the present invention, the solid content of the slurry can be about 5% to 15% by weight. At this time, the uniform mixing of the polymer electrolyte and the solvent can be promoted by raising the temperature of the slurry to 40°C to 60°C.

[0133] Then, the slurry is coated on a release sheet (e.g., terephthalate film) and formed into a film shape having a predetermined thickness. Coating and forming can be performed by known coating methods, such as blade coating. Then, the slurry is dried to remove the solvent and obtain a solid electrolyte film layer. In the solid electrolyte film layer, the solvent has been dried. Therefore, unlike coating and drying the solid electrolyte forming slurry on the electrode, this reduces the formation of holes that play a role in resistance.

[0134] The obtained polymer-based solid electrolyte membrane layer is provided on at least one surface of the heat-treated porous polymer sheet to obtain a laminated structure.

[0135] Finally, the stacked structure of step (T14) is pressurized so that the pores and ion channels of the surface-treated porous polymer sheet can be filled with the polymer solid electrolyte material, thereby forming a composite of the polymer solid electrolyte material and the porous polymer sheet (T15) ( Figure 3 (d)).

[0136] Pressurization can be performed using a suitable pressurizing member selected from known pressurizing members (e.g., a uniaxial press, a hot press, a roller press, and a clamp). At this time, by controlling process parameters (e.g., a press, a roller, a clamp gap, an applied pressure, and a temperature), the electrolyte membrane can have a suitable thickness and / or porosity. At this time, the pressurizing member may be further provided with a separate heating member so that the surface of the member facing the electrolyte membrane layer can be heated. Since the electrolyte membrane layer has increased ductility due to being heated by the pressurizing member, it can be easily pressed into the sheet even under low pressure conditions.

[0137] Meanwhile, according to one embodiment of the present invention, before the electrolyte membrane layer is introduced into the press-in process, the electrolyte membrane layer may be heated to room temperature (25° C.) to 180° C., thereby facilitating the introduction of the material into the pores of the polymer sheet by increasing the ductility of the material. Such a heating method is not limited to a specific method. However, the membrane layer may be heated by allowing it to stand for several hours in an oven heated to a predetermined temperature.

[0138] In another aspect of the present invention, a solid-state battery comprising the above-mentioned solid electrolyte membrane is provided. The solid-state battery comprises a positive electrode, a negative electrode and a solid electrolyte membrane. According to one embodiment of the present invention, the solid electrolyte membrane may include a carbon sheet embedded in the solid electrolyte membrane on at least one surface, wherein the electrolyte membrane may be arranged so that the carbon sheet may face the positive electrode.

[0139] According to the present invention, the positive electrode and the negative electrode may include a current collector and an electrode active material layer formed on at least one surface of the current collector, respectively, wherein the active material layer may include a plurality of electrode active material particles and a solid electrolyte. In addition, if necessary, the electrode active material layer may further include at least one of a conductive material and a binder resin. In addition, in order to supplement or improve the physicochemical properties of the electrode, the electrode active material layer may further include various additives.

[0140] According to the present invention, in the case of the negative electrode, the electrode active material may be any material conventionally used as a negative electrode active material for lithium ion secondary batteries. For example, the negative electrode active material may include at least one selected from the following materials: carbon, such as non-graphitizable carbon or graphite carbon, etc.; metal composite oxides, such as Li x Fe2O3(0≤x≤1), Li x WO2(0≤x≤1), Sn x Me1-x Me y O z (Me: Mn, Fe, Pb or Ge; Me': Al, B, P, Si, an element of Group 1, Group 2 or Group 3 in the periodic table, or a halogen; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8); lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4 or Bi2O5, etc.; conductive polymers such as polyacetylene; Li-Co-Ni-based materials; titanium oxides; and lithium titanium oxides, etc. According to an embodiment of the present invention, the negative electrode active material may include a carbonaceous material and / or Si.

[0141] In the case of the positive electrode, the electrode active material may be any material conventionally used as the positive electrode active material of a lithium ion secondary battery. For example, the positive electrode active material may include, but is not limited to: layered compounds such as lithium cobalt oxide (LiCoO2) and lithium nickel oxide (LiNiO2), or these compounds substituted with one or more transition metals; lithium manganese oxides such as lithium manganese oxide represented by the chemical formula Li 1+x Mn 2-x O4 (where x is from 0 to 0.33), LiMnO3, LiMn2O3 and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5 or Cu2V2O7; nickel-site type lithium nickel oxide represented by the chemical formula LiNi 1-x M x O2 (where M is Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x is from 0.01 to 0.3); lithium manganese composite oxide represented by the chemical formula LiMn 2-x M x O2 (where M = Co, Ni, Fe, Cr, Zn or Ta, x = 0.01 to 0.1) or Li2Mn3MO8 (where M = Fe, Co, Ni, Cu or Zn); lithium manganese composite oxide having a spinel structure and represented by the formula LiNi x Mn 2-x O4; LiMn2O4 partially substituted with alkaline earth metal ions; disulfides; or Fe2(MoO4)3, etc.

[0142] According to the present invention, the current collector includes a metal plate having conductivity and can be appropriately selected according to the polarity of the electrode known in the field of secondary batteries.

[0143] According to the present invention, the amount of the conductive material added is generally 1 to 30% by weight based on the total weight of the mixture containing the electrode active material. The conductive material is not particularly limited as long as it does not cause chemical changes in the corresponding battery and has conductivity. For example, the conductive material includes any one selected from the following materials: graphite, such as natural graphite or artificial graphite; carbon black, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black or thermal black; conductive fibers, such as carbon fibers or metal fibers; metal powders, such as fluorocarbons, aluminum or nickel powders; conductive whiskers, such as zinc oxide or potassium titanate; conductive metal oxides, such as titanium oxide; and conductive materials such as polyphenylene derivatives, or mixtures of two or more thereof.

[0144] According to the present invention, the binder resin is not particularly limited as long as it is a component that contributes to the combination of the electrode active material and the conductive material and the combination with the current collector. Specific examples of binder resins include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber or various copolymers. Typically, based on 100% by weight of the electrode active material layer, the amount of the binder resin used can be 1 to 30% by weight, or 1 to 10% by weight.

[0145] Meanwhile, according to the present invention, the electrode active material layer may include at least one additive, such as an oxidation stabilizing additive, a reduction stabilizing additive, a flame retardant, a heat stabilizer, an antifogging agent, or the like, if necessary.

[0146] According to the present invention, the solid electrolyte may further include at least one of a polymer-based solid electrolyte, an oxide-based solid electrolyte, and a sulfide-based solid electrolyte.

[0147] According to the present invention, different solid electrolytes can be used for the positive electrode, the negative electrode and the solid electrolyte membrane. In one variation, the same solid electrolyte can be used for at least two battery elements. For example, in the case of the positive electrode, as a solid electrolyte, a polymer solid electrolyte with excellent oxidation stability can be used. In addition, in the case of the negative electrode, as a solid electrolyte, a polymer solid electrolyte with excellent reduction stability is preferably used. However, the scope of the present invention is not limited thereto. Since the solid electrolyte mainly plays the role of transporting lithium ions in the electrode, a solid electrolyte with high ion conductivity (e.g., 10 -7 S / cm or more, 10 -5 S / cm or more) without particular limitation.

[0148] According to the present invention, the polymer-based solid electrolyte may be a solid polymer electrolyte formed by adding a polymer resin to a lithium salt, wherein the polymer resin and the lithium salt are solvated independently of each other. In one variation, the polymer-based solid electrolyte may be a polymer gel electrolyte formed by impregnating a polymer resin with an organic electrolyte containing an organic solvent and a lithium salt.

[0149] According to the present invention, the polymer-based solid electrolyte may be the same as described above with respect to the solid electrolyte membrane.

[0150] Sulfide-based solid electrolytes contain sulfur (S), have conductivity of metal ions belonging to Group 1 or Group 2 of the periodic table, and may include Li-PS glass or Li-PS glass ceramics. Non-limiting examples of sulfide-based solid electrolytes include at least one of Li2S-P2S5, Li2S-LiI-P2S5, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2O5, Li2S-P2S5-SiS2, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S-GeS2, or Li2S-GeS2-ZnS, etc.

[0151] In addition, the oxide-based solid electrolyte contains oxygen (O) and has conductivity of metal ions belonging to Group 1 or Group 2 of the periodic table. Non-limiting examples of the oxide-based solid electrolyte include LLTO compounds, Li6La2CaTa2O 12 、Li6La2ANb2O 12 (where A is Ca or Sr), Li2Nd3TeSbO 12 、Li3BO 2.5 N 0.5 、Li9SiAlO8、LAGP compound、LATP compound、Li 1+x Ti 2-x Al x Si y (PO4) 3-y (where 0≤x≤1, 0≤y≤1), LiAl x Zr 2-x (PO4)3 (where 0≤x≤1, 0≤y≤1), LiTi x Zr 2-x At least one of (PO4)3 (wherein 0≤x≤1, 0≤y≤1), a LISICON compound, a LIPON compound, a perovskite compound, a NASICON compound and a LLZO compound.

[0152] In another aspect of the present invention, a secondary battery comprising the above-mentioned solid electrolyte membrane is provided. A battery module comprising the secondary battery as a unit cell, a battery pack comprising the battery module, and a device comprising the battery pack as a power source are also provided. At this time, specific examples of the device may include, but are not limited to: a power tool driven by a motor; an electric vehicle, including an electric vehicle (EV), a hybrid electric vehicle (HEV), or a plug-in hybrid electric vehicle (PHEV), etc.; an electric power-assisted vehicle, including an electric bicycle (E-bike) and an electric scooter (E-scooter); an electric golf cart; or a power storage system, etc.

[0153] Hereinafter, the embodiments will be described more fully so that the present invention can be easily understood. However, the following embodiments are for illustrative purposes only, and the scope of the present invention is not limited thereto.

[0154] [Test Example 1]

[0155] In Examples 1 to 7, a solid electrolyte membrane for a solid-state battery was obtained in which the polymer electrolyte material formed a composite with the porous polymer sheet so that the pores of the porous polymer sheet were filled with the polymer electrolyte material. Comparative Examples 1 to 5 were used for comparison with Examples 1 to 7.

[0156] Example 1

[0157] Polyethylene oxide (PEO, Mw 600,000) was prepared and mixed with LiTFSI to obtain a polymer electrolyte material. In the polymer electrolyte material, PEO and LiTFSI were mixed in a molar ratio of 9:1. The polymer electrolyte material and acetonitrile were stirred at 60°C overnight to prepare a polymer solution with a concentration of about 10 wt%. Next, the polymer solution was coated on a terephthalate release film using a scraper at room temperature and dried naturally at room temperature to obtain an electrolyte membrane layer with a thickness of about 50 μm.

[0158] Then, a nonwoven fabric substrate (polyethylene terephthalate (PET), 10 μm thick, 50% porosity) was prepared, and the electrolyte membrane layer obtained as described above was arranged on the surface of the substrate to prepare a laminate. The laminate was introduced into a roller press, and pressurization was performed 4 times by successively reducing the gap between the rollers. In this way, the electrolyte membrane layer was pressed into the nonwoven fabric substrate. Finally, a solid electrolyte membrane with a thickness of about 30 μm was obtained.

[0159] Example 2

[0160] A laminate was prepared in the same manner as in Example 1. The laminate was heated to 60° C. and introduced into a roll press, and pressurized twice by successively reducing the gap between the rolls, thereby obtaining a solid electrolyte membrane having a thickness of 30 μm.

[0161] Example 3

[0162] A laminate was prepared in the same manner as in Example 1. The laminate was introduced into a roll press heated to 60° C. and pressed once by controlling the gap between the rolls to obtain a solid electrolyte membrane having a thickness of 30 μm. The other conditions were the same as in Example 1.

[0163] Example 4

[0164] A laminate was prepared in the same manner as in Example 1. The laminate was introduced into a roll press heated to 60° C. and once pressed by controlling the gap between the rolls to obtain a solid electrolyte membrane having a thickness of 20 μm. Other conditions were the same as in Example 1.

[0165] Example 5

[0166] A laminate was prepared in the same manner as in Example 1. The laminate was introduced into a roll press heated to 40° C. and pressed twice by successively reducing the gap between the rolls to obtain a solid electrolyte membrane having a thickness of 20 μm. Other conditions were the same as in Example 1.

[0167] Example 6

[0168] A laminate was prepared in the same manner as in Example 1. The laminate was introduced into a uniaxial press heated to 60° C. and pressed once to obtain a solid electrolyte membrane having a thickness of 20 μm. The other conditions were the same as in Example 1.

[0169] Example 7

[0170] Two electrolyte membrane layers were prepared in the same manner as in Example 1. One electrolyte membrane layer was stacked on each surface of the nonwoven fabric, and the resultant was introduced into a uniaxial press heated to 60° C. and pressed once, thereby obtaining a solid electrolyte membrane having a thickness of 30 μm. The nonwoven fabric was the same as that used in Example 1.

[0171] The process conditions of each example are shown in Table 1 below.

[0172] [Table 1]

[0173]

[0174] Comparative Example 1

[0175] Polyethylene oxide (PEO, Mw 600,000) was prepared and mixed with LiTFSI to obtain a polymer electrolyte material. In the polymer electrolyte material, PEO and LiTFSI were mixed in a molar ratio of 9:1. The polymer electrolyte material and acetonitrile were stirred at 60°C overnight to prepare a polymer solution with a concentration of about 10 wt%. Next, the polymer solution was coated on a terephthalate release film using a scraper at room temperature and dried naturally at room temperature to obtain an electrolyte membrane layer with a thickness of about 50 μm.

[0176] Comparative Example 2

[0177] An electrolyte membrane layer was obtained in the same manner as in Comparative Example 1, except that the thickness of the solid electrolyte membrane layer was 30 μm.

[0178] Comparative Example 3

[0179] An electrolyte membrane layer having a thickness of 50 μm was obtained in the same manner as in Comparative Example 1. Then, the electrolyte membrane layer was introduced into a roll press at 60° C. and pressed once so that the thickness of the electrolyte membrane layer could be 30 μm.

[0180] Comparative Example 4

[0181] A polymer solution was prepared in the same manner as in Comparative Example 1. The polymer solution was applied onto a nonwoven fabric using a doctor blade and dried to obtain a solid electrolyte membrane having a thickness of about 50 μm.

[0182] Comparative Example 5

[0183] The solid electrolyte membrane obtained from Comparative Example 4 was introduced into a roll press heated to 60° C. and pressed once to obtain a solid electrolyte membrane having a thickness of about 30 μm.

[0184] Determination of porosity

[0185] The solid electrolyte membranes of the examples and comparative examples were cut into 1.7671 cm 2 The size of each solid electrolyte membrane is measured, and the weight and volume of each solid electrolyte membrane are measured (the apparent density is determined), and the apparent density is compared with the designed value (true density) to calculate the porosity. In other words, the true density of each solid electrolyte membrane is calculated from the composition ratio of the components in each solid electrolyte membrane and the density of each component, and then the porosity is calculated from the difference between the apparent density and the true density.

[0186] Determination of ionic resistance

[0187] The solid electrolyte membranes of the examples and comparative examples were cut into 1.7671 cm2 Then, the solid electrolyte membrane was placed between two pieces of stainless steel (SUS) to obtain a coin cell. The electrochemical impedance of the coin cell was determined using an impedance analyzer (VMP3, Bio logicscience instrument) at 60°C, with an amplitude of 10 mV and a scanning range of 500 kHz to 0.1 mHz.

[0188] Tensile Strength

[0189] The solid electrolyte membranes of the examples and comparative examples were cut into a size of 15 mm×50 mm, respectively. In order to minimize the damage of the solid electrolyte membrane caused by the tweezers, tapes were attached to both ends of each sample, and the tensile strength was determined using a UTM device.

[0190] Discharge capacity

[0191] First, NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 O2), vapor-grown carbon fiber (VGCF) as a conductive material, and a polymer solid electrolyte (a mixture of PEO and LiTFSI (CF3SO2NLiSO2CF3), the molar ratio of PEO:LiTFSI = 9:1) are mixed in a weight ratio of 80:3:17, and the resulting mixture is introduced into acetonitrile, followed by stirring to provide an electrode slurry. An aluminum current collector with a thickness of 20 μm is prepared. The electrode slurry is applied to the current collector using a scraper, and the resulting product is vacuum dried at 120°C for 4 hours. Then, a roller press is used to press to obtain an electrode loading of 3 mAh / cm 2 , an electrode (positive electrode) having an electrode active material layer thickness of 86 μm and a porosity of 16%. Then, the electrode was cut into pieces with an area of ​​1.4875 cm 2 In addition, a circular shape with an area of ​​1.7671 cm 2 The negative electrode includes lithium metal having a thickness of 40 μm bonded to the surface of a current collector made of copper and having a thickness of 10 μm.

[0192] The solid electrolyte membranes obtained in Examples 4 and 7 and Comparative Examples 1 and 5 were cut into 1.7671 cm 2 The size of the battery was placed between the positive electrode and the negative electrode to obtain a battery. The battery was charged / discharged at about 60° C. to evaluate the initial discharge capacity.

[0193] -Charging conditions: constant current (CC) / constant voltage (CV), (4.0V, 0.005C current cutoff)

[0194] -Discharge conditions: constant current (CC), 3V

[0195] After evaluation, Example 4 and Example 7 provided high discharge capacities of 130 mAh / g and 133 mAh / g, respectively. In contrast, Comparative Examples 1 and 5 provided discharge capacities of 126 mAh / g and 124 mAh / g, respectively, which were lower than Examples 4 and 7.

[0196] [Table 2]

[0197] Example Porosity (%) Ionic resistance (ohm) <![CDATA[Tensile strength (kgf / cm 2 )]]> 1 9 24 688 2 9 24 712 3 7 22 695 4 7 15 732 5 8 16 744 6 7 16 735 7 7 20 698

[0198] [Table 3]

[0199] Comparative Example Porosity (%) Ionic resistance (ohm) <![CDATA[Tensile strength (kgf / cm 2 )]]> 1 13 25 407 2 15 19 388 3 10 18 393 4 18 45 607 5 15 26 650

[0200] It can be seen from Tables 2 and 3 that in the case of the electrolyte membranes pressed into the electrolyte membrane layer of the embodiments, they show excellent tensile strength compared to the electrolyte membranes of the comparative examples while being formed into a thin film with a thickness of 20 μm or 30 μm. In addition, the electrolyte membranes of the embodiments have low porosity and small thickness, and thus show excellent ionic resistance characteristics. At the same time, compared with the embodiments, the electrolyte membranes of Comparative Examples 2 and 3 show lower ionic resistance characteristics, but have greater thickness, higher porosity and lower strength. At the same time, in the batteries using the electrolyte membranes of the embodiments and comparative examples, the batteries using the electrolyte membranes of the embodiments show higher discharge capacity than the batteries using the electrolyte membranes of the comparative examples.

[0201] As can be seen from the above test results, the use of a porous substrate can significantly improve the strength of the solid electrolyte membrane. Therefore, when the release film is removed or the solid electrolyte membrane is cut into the desired size, the processability is improved, in particular, the deformation (damage) of the solid electrolyte membrane is reduced and the short circuit generation is also reduced, resulting in an increase in yield. On the contrary, when a porous substrate is added, the ionic conductivity may be reduced due to tortuosity. However, by forming a solid electrolyte membrane with a smaller thickness, the ionic resistance can be maintained at an appropriate level. Therefore, the discharge capacity of the positive electrode can be improved. In addition, since the thickness of the solid electrolyte membrane is small, the energy density of the battery can be significantly improved. In addition, in the case of a conventional solid electrolyte membrane obtained by impregnating a porous substrate with a polymer solution, due to the compatibility difference between the polymer solution and the porous substrate and the evaporation of the solvent during the drying step, a large number of pores may remain in the solid electrolyte membrane obtained as a product of a composite formation of a solid electrolyte and a porous substrate. On the contrary, since the solid electrolyte membrane of the present invention is obtained by pressing a solid electrolyte membrane layer into a porous substrate, the porosity of the solid electrolyte membrane can be significantly reduced and the ionic resistance can be improved. In addition, the fluidity of the electrolyte membrane layer can be improved by heat treatment before pressing or by heating during pressing, thereby reducing the number of processing times and making the solid electrolyte membrane have a uniform surface state. In addition, after the membrane layer is pressed into the porous substrate by various methods of Examples 1 to 7, all methods can provide excellent electrochemical characteristics compared with the comparative example. In other words, it can be seen that when the electrolyte membrane layer is pressed into the porous substrate, the surface of the solid electrolyte membrane can be improved and the ion resistance can be reduced, regardless of any specific single step or method.

[0202] [Test Example 2]

[0203] In Examples 8 to 11, at least one selected from a polyalkylene carbonate-based polymer resin and a polysiloxane-based polymer resin is used as the polymer electrolyte material. Comparative Examples 1 to 5 are used for comparison with Examples 8 to 11.

[0204] Example 8

[0205] Polyethylene oxide (PEO, Mw 600,000) was prepared and mixed with LiTFSI to obtain a polymer electrolyte material. In the polymer electrolyte material, PEO and LiTFSI were mixed in a molar ratio of 9:1. The polymer electrolyte material and acetonitrile were stirred at 60°C overnight to prepare a polymer solution with a concentration of about 10 wt%. Next, the polymer solution was coated on a terephthalate release film using a scraper at room temperature and naturally dried at room temperature to obtain an electrolyte membrane layer with a thickness of about 50 μm.

[0206] Then, a nonwoven fabric substrate (polyethylene terephthalate (PET), 10 μm thick, 50% porosity) was prepared, and the electrolyte membrane layer obtained as described above was disposed on the surface of the substrate to prepare a laminate. The laminate was heated to 60° C., introduced into a roll press, and pressurized so that the electrolyte membrane layer could be pressed into the nonwoven fabric substrate. Finally, a solid electrolyte membrane having a thickness of about 20 μm was obtained.

[0207] Example 9

[0208] A solid electrolyte membrane having a thickness of 2 μm was obtained in the same manner as in Example 8, except that a mixture of polymethylhydrogensiloxane (PMHS) and LiTFSI (LiTFSI 30 wt %) was used as the polymer electrolyte material.

[0209] Example 10

[0210] A solid electrolyte membrane having a thickness of 20 μm was obtained in the same manner as in Example 8, except that a mixture of PEO, polymethylhydrogensiloxane (PMHS) and LiTFSI was used as the polymer electrolyte material. In the mixture, the content of LiTFSI was 30 wt % based on 100 wt % of the polymer electrolyte material. In addition, PEO and polymethylhydrogensiloxane (PMHS) were used in a weight ratio of 1:1.

[0211] Embodiment 11

[0212] A solid electrolyte membrane having a thickness of 20 μm was obtained in the same manner as in Example 8, except that a mixture of PEO, polypropylene carbonate (PPC) and LiTFSI (molar ratio of PPC:Li=20:1) was used as the polymer electrolyte material. Here, PEO and PPC were used in a weight ratio of 1:1.

[0213] [Table 4]

[0214] Porosity (%) Ionic resistance (ohm) <![CDATA[Tensile strength (kgf / cm 2 )]]> Example 8 7 15 695 Example 9 7 15 732 Example 10 5 12 699 Embodiment 11 6 13 714

[0215] It can be seen from the above test results that the use of a porous substrate can significantly improve the strength of the solid electrolyte membrane, resulting in improved processability and increased yield. On the contrary, when a porous substrate is added, the ionic conductivity may be reduced due to tortuosity. However, a solid electrolyte membrane with a small thickness can be obtained, so the solid electrolyte membrane exhibits excellent ionic resistance characteristics. Therefore, the discharge capacity of the positive electrode can be improved. In addition, since the thickness of the solid electrolyte membrane is small, the energy density of the battery can be significantly improved. In addition, in the case of a conventional solid electrolyte membrane obtained by impregnating a porous substrate with a polymer solution, due to the compatibility difference with the porous substrate and the evaporation of the solvent during the drying step, pores may be fully formed in the solid electrolyte membrane. Since the solid electrolyte membrane is incorporated into the porous substrate according to the present invention, the porosity can be significantly reduced and the ionic resistance can be improved compared with the conventional solid electrolyte membrane. In addition, it can be seen that the ionic resistance of the solid electrolyte membrane can be reduced regardless of the solid electrolyte material.

[0216] Evaluation of initial discharge capacity and continuous charge

[0217] Battery Manufacturing(1)

[0218] The performance of the batteries of Examples 9 to 11 and Comparative Example 1 was evaluated as follows. First, NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 O2), vapor-grown carbon fiber (VGCF) as a conductive material, and a polymer solid electrolyte (a mixture of PEO and LiTFSI (CF3SO2NLiSO2CF3), the molar ratio of PEO:LiTFSI = 9:1) are mixed in a weight ratio of 80:3:17, and the resulting mixture is introduced into acetonitrile, followed by stirring to provide an electrode slurry. An aluminum current collector with a thickness of 20 μm is prepared. The electrode slurry is applied to the current collector with a scraper, and the resulting product is vacuum dried at 120°C for 4 hours. Then, a roller press is used to press to obtain an electrode loading of 3 mAh / cm 2 , an electrode (positive electrode) having an electrode active material layer thickness of 86 μm and a porosity of 16%. Then, the electrode was cut into pieces with an area of ​​1.4875 cm 2 In addition, a circular shape with an area of ​​1.7671 cm 2 The negative electrode includes a lithium metal having a thickness of 40 μm bonded to the surface of a copper current collector having a thickness of 10 μm. The solid electrolyte membranes obtained from Examples 9 to 11 and Comparative Example 1 were cut into 1.7671 cm 2 of size and placed between the positive and negative electrodes to obtain a battery.

[0219] The batteries obtained by the battery preparation (1) were each charged / discharged at about 60° C. to evaluate the initial discharge capacity.

[0220] -Charging conditions: constant current (CC) / constant voltage (CV), (4.0V, 0.005C current cutoff)

[0221] -Discharge conditions: constant current (CC), 3V (0.05C)

[0222] At the same time, the batteries of Examples 9 to 11 and Comparative Example 1 were respectively continuously charged to test the side reaction time in the electrode. The test was performed by charging to 4.205V in CC mode at 0.05C at 60°C and then continuously applying current under CV conditions. In each battery, the current enhancement time caused by the side reaction in the battery was determined. The results are shown in Table 5.

[0223] [Table 5]

[0224]

[0225] As can be seen from Tables 3 and 4, the electrolyte membrane pressed into the electrolyte membrane layer of the embodiment exhibits high physical strength (e.g., tensile strength) and allows the formation of a thin film. In addition, it can be seen that the electrolyte membrane of the embodiment has a low porosity and a small thickness, thereby providing excellent ionic resistance characteristics, thereby improving the discharge capacity. In particular, the ionic conductivity of polysiloxane electrolytes is high, but the mechanical strength is unexpectedly low. However, this polysiloxane electrolyte improves the applicability to batteries through the method of the present invention. At the same time, polycarbonate polymers with high known oxidative stability can be used to increase the current enhancement time, thereby improving the stability of the battery.

[0226] [Test Example 3]

[0227] In Examples 12 to 16, a porous polymer sheet having ion channels including through holes was used, and the porous polymer sheet was hydrophilically surface-modified. Comparative Examples 6 to 10 were used for comparison with Examples 12 to 16.

[0228] Example 12

[0229] A polyethylene porous polymer sheet (porosity 37%, pore diameter 43 nm) having a thickness of 6.8 μm was prepared.

[0230] Next, an ion channel including perforations with a diameter of 500 μm was formed in the thickness direction of the porous polymer sheet using a die cutter. At this time, the perforations were spaced 1 mm apart.

[0231] Then, the porous polymer sheet was treated with O2 plasma (SPI Plasma Prep II, 50 watts). Specifically, O2 plasma was flowed at a flow rate of 100 sccm for 1 minute. In this way, the surface, pores and ion channels of the porous polymer sheet were hydrophilically modified.

[0232] Meanwhile, polyethylene oxide (PEO, Mw 600,000) was prepared and mixed with LiTFSI to obtain a polymer electrolyte material. In the polymer electrolyte material, PEO and LiTFSI were mixed in a molar ratio of 9:1. The polymer electrolyte material and acetonitrile were stirred at 60°C overnight to prepare a polymer solution having a concentration of about 10 wt%. Next, the polymer solution was coated onto a terephthalate release film using a scraper at room temperature and dried naturally at room temperature to obtain a solid electrolyte membrane layer having a thickness of about 50 μm.

[0233] Then, the electrolyte membrane layer prepared as described above is arranged on one surface of the surface-treated porous polymer sheet to obtain a laminated structure. The laminated structure is introduced into a roller press and pressurized 4 times by successively reducing the gap between the rollers. In this way, the polymer electrolyte membrane layer is pressed into the pores of the surface-treated porous polymer sheet. Finally, a solid electrolyte membrane for a solid-state battery having a thickness of about 50 μm is obtained.

[0234] Example 13

[0235] A solid electrolyte membrane was obtained in the same manner as in Example 12, except that the interval of the perforations was 0.75 mm.

[0236] Embodiment 14

[0237] A polyethylene porous polymer sheet (porosity 37%, pore diameter 43 nm) having a thickness of 6.8 μm was prepared.

[0238] Next, an ion channel including perforations with a diameter of 500 μm was formed in the thickness direction of the porous polymer sheet using a die cutter. At this time, the perforations were spaced 1 mm apart.

[0239] Then, the porous polymer sheet was subjected to hydrophilic surface modification using polyethylene glycol (PEG, Sigma-Aldrich Co., weight average molecular weight 400) by spin coating.

[0240] A solid electrolyte membrane was obtained in the same manner as in Example 13, except that the surface-treated porous polymer sheet obtained as described above was used.

[0241] Embodiment 15

[0242] After preparing the same porous polymer sheet as in Example 13, the polymer-based solid electrolyte membrane layer was pressed into the porous polymer sheet to obtain a solid electrolyte membrane having a thickness of 20 μm.

[0243] Example 16

[0244] A solid electrolyte membrane was obtained in the same manner as in Example 12, except that a polymer-based solid electrolyte solution was used instead of the polymer-based solid electrolyte membrane layer.

[0245] The process conditions and test data of the embodiment are shown in Table 6.

[0246] Comparative Example 6

[0247] A solid electrolyte membrane was obtained in the same manner as in Example 12, except that no ion channels were formed in the porous polymer sheet and no hydrophilic surface treatment was performed.

[0248] Comparative Example 7

[0249] A solid electrolyte membrane was obtained in the same manner as in Example 12, except that ion channels were formed in the porous polymer sheet but the porous polymer sheet was not subjected to a hydrophilic surface treatment.

[0250] Comparative Example 8

[0251] A solid electrolyte membrane was obtained in the same manner as in Example 12, except that no ion channels were formed in the porous polymer sheet, but the porous polymer sheet was subjected to a hydrophilic surface treatment.

[0252] Comparative Example 9

[0253] A polyethylene porous polymer sheet (porosity 37%, pore size 43 nm) with a thickness of 6.8 μm was prepared. Next, an ion channel including perforations with a diameter of 500 μm was formed in the thickness direction of the porous polymer sheet using a die cutter. At this time, the perforations were spaced 0.75 mm apart. The porous polymer sheet was not subjected to a hydrophilic surface treatment.

[0254] Next, an oxide-based solid electrolyte slurry was obtained as follows: Specifically, LAGP, PEO, and LiTFSI were introduced into acetonitrile (AN) at a weight ratio of 75:18:7 to obtain a slurry having a solid content of 40 wt %.

[0255] Then, a porous polymer sheet without surface treatment was impregnated with the oxide-based solid electrolyte slurry to obtain a solid electrolyte membrane with a thickness of 90 μm.

[0256] Comparative Example 10

[0257] A polyethylene porous polymer sheet (porosity 37%, pore diameter 43 nm) having a thickness of 6.8 μm was prepared.

[0258] Next, an ion channel including perforations with a diameter of 500 μm was formed in the thickness direction of the porous polymer sheet using a die cutter. At this time, the perforations had an interval of 0.75 mm.

[0259] Next, the porous polymer sheet was treated with O2 plasma (SPI Plasma Prep II, 50 watts). Specifically, O2 plasma was flowed at a flow rate of 100 sccm for 1 minute. In this way, the surface, pores and ion channels of the porous polymer sheet were hydrophilically modified.

[0260] Thereafter, an oxide-based solid electrolyte slurry was obtained as follows: Specifically, LAGP, PEO, and LiTFSI were introduced into xylene at a weight ratio of 75:18:7 to obtain a slurry having a solid content of 40 wt %.

[0261] Then, the surface-treated porous polymer sheet was impregnated with the oxide-based solid electrolyte slurry to obtain a solid electrolyte membrane having a thickness of 90 μm.

[0262] Test Method

[0263] Determination of porosity

[0264] The porosity was determined in the same manner as above.

[0265] Determination of air permeability

[0266] The time required for 100 mL of air to pass through the solid electrolyte membrane was determined using an air permeability tester.

[0267] Tensile Strength

[0268] The tensile strength was determined in the same manner as above.

[0269] Determination of thickness

[0270] The thickness of each solid electrolyte membrane of Examples and Comparative Examples was determined using a thickness analyzer available from Mouser Co.

[0271] Determination of ionic resistance

[0272] The ionic resistance was determined in the same manner as above.

[0273] Discharge capacity measurement

[0274] The discharge capacity was determined in the same manner as above.

[0275] [Table 6]

[0276]

[0277] As shown in Table 6, when perforations are further introduced into the porous polymer sheet, the porosity of the solid electrolyte membrane increases. With the added pores, the solid electrolyte membrane exhibits improved air permeability. In addition, since the solid electrolyte material is incorporated into the pores and ion channels of the solid electrolyte membrane, the ionic resistance is reduced. In addition, when the porous polymer sheet is hydrophilically treated, the compatibility between the porous polymer sheet and the polymer-based solid electrolyte material increases, resulting in a further reduction in ionic resistance.

[0278] In contrast, it can be seen from Comparative Examples 9 and 10 that when the porous polymer sheet is impregnated with an oxide-based solid electrolyte material, which is an inorganic solid electrolyte material, incorporation of the polymer-based solid electrolyte material is limited and thin film formation is difficult.

[0279] [Explanation of Reference Numerals]

[0280] 100: Solid electrolyte membrane for solid-state batteries

[0281] 11: Polymer electrolyte materials

[0282] 12: Porous polymer sheet

[0283] 21: Conventional solid electrolyte membrane

[0284] 22: Lithium metal anode

[0285] 300: Solid electrolyte membrane for solid-state batteries

[0286] 31: Solid electrolyte membrane layer

[0287] 32: Porous polymer sheet

[0288] 33: Perforation

Claims

1. A solid electrolyte membrane for a solid-state battery, comprising a polymer electrolyte material and a porous polymer sheet, in, The porous polymer sheet is a porous material comprising a plurality of pores and the pores can be penetrated by a fluid material, the porous polymer sheet is further provided with an ion channel comprising perforations, the diameter of the perforations is larger than the diameter of the pores, and the porous polymer sheet is subjected to hydrophilic surface modification; wherein the polymer electrolyte material is a solid electrolyte membrane layer formed by drying a solvent in a polymer resin added to a solvated lithium salt; and The polymer electrolyte material forms a composite with the porous polymer sheet, and the composite is formed by pressurizing the solid electrolyte membrane layer disposed on the surface of the porous polymer sheet to press the solid electrolyte membrane layer into the ion channels and the pores of the porous polymer sheet, so that the ion channels and the pores of the porous polymer sheet are filled with the polymer electrolyte material.

2. The solid electrolyte membrane for a solid-state battery according to claim 1, wherein The polymer electrolyte material exhibits a 1×10 -7 S / cm or above ionic conductivity.

3. The solid electrolyte membrane for solid-state batteries according to claim 2, wherein: The polymer resin has a weight average molecular weight (Mw) of 5,000 to 5,000,000.

4. The solid electrolyte membrane for solid-state batteries according to claim 1, which has a thickness of 15 μm to 90 μm and a tensile strength of 500 kgf / cm 2 Up to 2,000 kgf / cm 2 .

5. The solid electrolyte membrane for solid-state batteries according to claim 4, wherein the porosity is 15% or less.

6. The solid electrolyte membrane for solid-state batteries according to claim 1, wherein The polymer electrolyte material includes at least one selected from a polyalkylene carbonate-based polymer resin and a polysiloxane-based polymer resin.

7. The solid electrolyte membrane for a solid-state battery according to claim 1, wherein The diameter of the through-holes is 1 μm to 500 μm.

8. The solid electrolyte membrane for a solid-state battery according to claim 1, wherein At least one of the surface, pores and ion channels of the porous polymer sheet is subjected to hydrophilic surface modification.

9. The solid electrolyte membrane for a solid-state battery according to claim 1, wherein The porous polymer sheet is a polymer film including a polyolefin-based polymer resin, and the thickness of the polymer film is 5 μm to 50 μm.

10. The solid electrolyte membrane for solid-state batteries according to claim 1, wherein The porous polymer sheet is a nonwoven fabric in which a plurality of pores are interconnected and penetrate from one surface to another.

11. A method for manufacturing a solid electrolyte membrane for a solid-state battery, comprising the following steps: (T10) preparing a porous polymer sheet, wherein the porous polymer sheet is a porous material comprising a plurality of pores, and the pores can be penetrated by a fluid material; (T11) forming an ion channel including a perforation in the thickness direction of the porous polymer sheet, wherein the diameter of the perforation is larger than the diameter of the pore; (T13) performing hydrophilic surface modification on the porous polymer sheet; (T14) disposing a solid electrolyte membrane layer on the upper surface of the resultant product of step (T13) to obtain a laminated structure; and (T15) pressurizing the stacked structure so that the ion channels and pores of the porous polymer sheet are filled with the solid electrolyte membrane layer, The solid electrolyte membrane layer comprises a solid electrolyte material formed by adding a polymer resin to a solvated lithium salt and is formed by drying a solvent in the solid electrolyte material and exhibits a 1×10 -7 S / cm or above ionic conductivity.

12. The method for producing a solid electrolyte membrane for a solid-state battery according to claim 11, wherein: The volume of the ion channel is 5 volume % to 90 volume % based on 100 volume % of the total volume of the porous polymer sheet.

13. The method for producing a solid electrolyte membrane for a solid-state battery according to claim 11, wherein: The diameter of the perforation is 50 nm to 1 mm.

14. The method for producing a solid electrolyte membrane for a solid-state battery according to claim 11, wherein: The surface modification is performed by any one of UV irradiation, plasma, acid treatment, and ozone treatment.

15. The method for producing a solid electrolyte membrane for a solid-state battery according to claim 11, wherein: The solid electrolyte membrane layer is heated before or simultaneously with step (T15).

16. The method for producing a solid electrolyte membrane for a solid-state battery according to claim 11, wherein: The pressing in step (T15) is performed using at least one pressing member selected from a roll press, a jig, and a uniaxial press.

17. The method for producing a solid electrolyte membrane for a solid-state battery according to claim 16, wherein: The pressurizing member is provided with a heating member.

18. The method for producing a solid electrolyte membrane for a solid-state battery according to claim 11, wherein: The polymer resin includes at least one selected from a polyalkylene carbonate-based polymer resin and a polysiloxane-based polymer resin, and the porous polymer sheet is a nonwoven fabric.

Citation Information

Patent Citations

  • Method for controlling data transmission of cameras for monitoring, and remotely monitoring system

    KR1020190052530A

  • Solid electrolyte structure and preparation method thereof, and lithium battery

    CN108336401A

  • Solid electrolyte sheet and manufacturing method thereof, and all-solid battery and manufacturing method thereof

    JP2017103146A