Production method of collagen-laminoid matrix for treating human skin ulcers, burns, and wounds

By extracting type I collagen and human laminin from rat tails and combining them with HaCat cells, a cell-free three-dimensional collagen-laminin matrix was prepared, which solved the low tissue survival rate and the need for cell materials in the treatment of large-area burns. Big problem, achieve efficient skin regeneration and wound healing, simplify production and registration procedures.

CN112118860BActive Publication Date: 2024-10-18SHENESKE PRINTING GMBH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN201980032852.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-03-20
Publication Date
2024-10-18
Estimated Expiration
2039-03-20

AI Technical Summary

Technical Problem

Existing technologies face low tissue survival rate, immunogenicity, and transportation difficulties when using epidermal autografts to treat large-area burns. Moreover, treatment of large wounds requires a large amount of cell materials. The stability and biocompatibility of composite materials are insufficient, resulting in a complicated regeneration process. .

Method used

Type I collagen and human laminin extracted from rat tails are used, combined with HaCat cells, to prepare a cell-free three-dimensional collagen-laminin matrix through specific processing and fixation steps to form a highly immune-tolerant, Easily fabricated biocompatible collagen-laminin wound healing materials.

Benefits of technology

It achieves efficient skin regeneration and wound healing, simplifies production and registration procedures, and provides an easy-to-promote biocompatible collagen-laminin wound healing material with high wound healing efficiency and long shelf life.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to medical biotechnology, and more specifically to tissue engineering methods in regenerative medicine. The method is characterized in that, together with conservative treatment methods, an alternative therapy is provided for treating damaged skin through a polymer matrix, the organizational structure of which is similar to that of human tissue and includes bioactive agents of derived cells, especially collagen and laminin, which can promote the structural formation activity of the damaged site. A biodegradable wound healing composite material based on a combination of a polymer matrix and a product synthesized by human epithelial cells, although the material does not contain cellular components, is characterized in that the production process is relatively simple and the storage life is long, and, for example, in the case of large-area burns, trophic ulcers, etc., skin transplantation can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to medical biotechnology, in particular to cell technology and tissue engineering methods for solving regenerative medicine problems. According to this method, an alternative therapy for treating skin injuries is proposed, using a polymer matrix (histologically similar to human tissue) and bioactive agents (cell derivatives - collagen and laminin), which contribute to the function of the damaged area structure, together with conservative treatment methods.

[0002] The use of cell technology is the most important and rapidly developing field of modern regenerative medicine. The task of the collagen-laminin matrix is ​​to transplant living cells into the defect area, completely restore the structure and function of the skin, and also stimulate the regeneration process and create a microenvironment to realize the potential of own tissues and cells. Tissue engineering technology is applied to solve such problems. Tissue engineering aims to solve many problems of regenerative medicine, to achieve the extension of the life cycle of individuals and the improvement of their quality of life by restoring the lost structure and function of organs and tissues. The use of new materials created based on cell technology can become a prospective method for the treatment and restoration of tissues.

[0003] Methods based on dermotropic biomedical cell products are currently being developed to treat long-standing wounds (trophic ulcers, burns) and to restore or temporarily close large areas of skin. The use of cell technologies to stimulate tissue regeneration includes the use of cells of different types, (for example) biological matrices, and tissue-like structures in different variations and combinations thereof.

[0004] It is known that epidermal autografting is used to cover large burns. However, in the case of allogenic autografts, the use of epidermal layers to treat burn patients suffers from difficulties in terms of tissue survival due to immunogenicity and affordability. Various other cell types - dermal fibroblasts, mesenchymal bone marrow stem cells, induced pluripotent stem cells - have been successfully used in preclinical and clinical studies. However, such treatments usually require large amounts of cellular material. This is not a major problem in the treatment of small wounds, but may occur in the treatment of larger wounds.

[0005] Some approaches that effectively utilize dermophilic ingredients for skin regeneration (e.g., collagen gels, sponges, and collagen-based products) are modified from natural and synthetic polymers, but the regeneration process is complicated by low stability and biocompatibility.

[0006] Epidermal and dermal equivalents have been used with positive clinical results in closing smaller wounds, including bovine collagen with human neonatal fibroblasts (Apligraf) and allogeneic fibroblasts from neonatal foreskin on a synthetic matrix (Dermagraft). However, in these variants, three-dimensional collagen gels with fibroblasts have encountered challenges in terms of infection, immunogenicity, storage, and transportation of tissue-engineered constructs.

[0007] The claimed method is performed as follows. Type I collagen is obtained from rat tail tendons. This requires adult Wistar rats (or similar animals) weighing equal to or greater than 300 grams under laboratory feeding conditions (excluding infection, parasites, etc.). Rat tails after animal euthanasia can be frozen and stored at -20°C for several years. Before separating collagen, the tail is washed with a standard detergent and sterilized with 70% ethanol for 24 hours before extracting collagen. All operations are performed under sterile conditions (in a laminar flow cabinet with a biosafety level of level 1 or 2). The skin is removed from the tail with a scalpel and tweezers, and the tail is cut into small pieces of 2-3 cm. The resulting tail fragments are incubated again in 70% ethanol for 15 minutes. The tendon is then removed from the tail with tweezers, the tendon is split into fine fibers, and placed in a container containing a sterile solution of 0.1% glacial acetic acid. Collagen begins to be extracted into the solution almost immediately, and the solution becomes viscous and appears as a blue milky mist. To obtain the correct concentration and solution strength, a whole tail tendon should be dissolved in 100-150 ml of solution. The solution is then incubated at +4°C for one month. If possible, the bottle with the solution should be removed daily and the precipitate stirred. The result is a viscous liquid with insoluble precipitate at the bottom. The collagen solution is then centrifuged (rotated at 1500g to 4000rpm for 1 hour at room temperature with a rotor radius of 10 cm) to precipitate the undissolved collagen fibers. The supernatant is drained into a sterile storage container. The concentration of the solution can be calculated by evaporating the water in a dry air thermostat and weighing the resulting precipitate. Collagen concentrations at a concentration of not less than 1 mg / ml (usually 3-5 mg / ml) can be considered acceptable collagen solutions.

[0008] For collagen polymerization, the acidic solution of acetic acid should be neutralized. To do this, pour the collagen solution into a sterile Petri dish (if necessary, with a radius of 3 cm, 6 cm or 10 cm) and add the appropriate amount of 0.1 M NaOH solution under stirring to form a solution with a pH of about 7.0 to 7.2. The acidity of this solution can be easily determined by adding Ml 99 formula containing phenol red dye, the color of which depends on the pH value. The desired color of the solution is dark red. By varying the amount of collagen solution, matrices of different depths can be produced. The polymerization of collagen occurs within 3-5 minutes, so all steps must be carried out quickly, preferably on ice. After adding all the necessary ingredients and mixing, place the Petri dish with the collagen gel in an incubator at +37°C for several hours (one day is optimal).

[0009] On the second day, HaCat cells were implanted on the collagen gel at a density of 10,000-40,000 cells per square centimeter. HaCat cells are immortalized human keratinocytes with good proliferation capacity and are widely used in scientific research. The required amount of complete growth medium of HaCaT cells was added from above, and the composition was further incubated for several days until a dense and superdense cell monolayer was achieved. During this time, HaCat cells synthesized the laminin layer of the basement membrane on the surface of the gel.

[0010] After reaching the desired cell density, the resulting matrix is ​​fixed with 4% paraformaldehyde at 4°C for 1 day. Thus, all proteins in the composition fuse together to form an insoluble single complex and the cells are inactivated. After fixation, the grafts are washed from the formaldehyde with a sterile solution of sterile phosphate-salt buffer (PBS), shaking 3 times for 15 minutes each time on an orbital shaker. The matrix then undergoes a decellularization phase at +4°C in SDS detergent and 0.1% Triton-X-100 detergent over 1 day. During this process, lipids, bonds between lipids and proteins are broken, all intracellular components are released and washed away, and DNA and RNA cells are degraded. After decellularization, the grafts are washed from the detergent with sterile phosphate-buffered saline (PBS), shaking 6 times for 1 hour each time on an orbital shaker. The final washing phase is performed at +4°C for 1 day. The matrix can then be stored in a PBS solution at +4°C for one month or dried in a freezer at -20°C for two years.

[0011] The resulting matrix is ​​a protein composition consisting of two main components, type I collagen and basement membrane laminin, which are completely similar to the structure of human skin in terms of tissue structure. Collagen forms the matrix of the graft, and laminin covers the matrix in the form of a basement membrane. The matrix is ​​sterile, immunotolerant (because collagen is a highly conserved, immunotolerant protein, and laminin is human-derived), and does not have any cellular components, which makes it a medical product and greatly simplifies the registration process.

[0012] Various additives (antibiotics, growth factors, cytokines) can be added to the final matrix composition, making it a convenient base model with great development potential. The HaCat cell line can be merged into other immortalized epithelial cell lines producing other types of laminins, thus making it possible to use the matrix to treat other epithelial-mesenchymal defects (ureteric urothelium, laryngeal epithelium, intestinal epithelium, etc.).

[0013] Studies carried out in vitro with the help of cell-based techniques and the application of biopolymeric matrices made it possible to obtain data on the possibility of stable tissue-engineered tissue-type compositions based on collagen matrices extracted in the form of gel films with acellular laminin surfaces. Immunohistochemical fluorescence analysis identified the expression of complex proteins such as type I collagen and laminin, as well as the epithelial cell marker pan-cytokeratin.

[0014] The proposed variant of the three-dimensional matrix is ​​a protein composition consisting of two main components, namely type I collagen and basement membrane laminin, which have a complete histological similarity to the structure of human skin. Collagen and laminin are the two most common types of human skin proteins. Collagen is the basis of the interstitial component of the dermis of the skin and provides mechanical strength and elasticity. Laminin is the basis of any basement membrane of an organ, including the basement membrane of the skin.

[0015] The results of a 21-day controlled study of the dynamics of simulated wound processes in a patchwork musculocutaneous wound model in male Wistar rats showed that the area of ​​wound defects was reduced at an accelerated rate in the group using collagen-laminin matrix on days 7 and 14. The growth of granulation tissue was observed from the bottom of the wound, and vascularization was observed in the tumor of connective tissue.

[0016] The data obtained on the restoration of skin integrity indicate that the resulting repair composition has a high wound healing efficiency due to the directional growth of the regenerated tissue that maintains the vascularization process. The biocompatible collagen-laminin wound healing material developed based on the combination of a polymer matrix and a synthetic product of human keratinocytes, although free of cellular components, is characterized by its ease of manufacture and long shelf life, so that the present design can be promoted in practice.

Claims

1. A method for producing a collagen-laminin matrix for treating human skin ulcers, burns and wounds, characterized in that: The invention comprises obtaining a tissue-engineered wound surface composition by using a combination of the following methods: Collagen was extracted from rat tail tendons to form a collagen matrix. Cultivating immortalized keratinocytes of HaCaT skin on the collagen matrix, With the help of detergents SDS and Triton-X-100 solution, the formed collagen membrane is stripped of cell membranes, cells are removed from the final product, and laminin is retained on its surface. In this process, lipids, bonds between lipids and proteins are broken, all intracellular components are released and washed away, and DNA and RNA cells are degraded; The laminin is a major protein of the basement membrane and is synthesized by HaCaT cells; The collagen-laminin matrix is ​​sterile, immunologically tolerable, and free of any cellular components.

2. The method according to claim 1, characterized in that After removal of cells, the collagen-laminin matrix was washed from the detergent with sterile phosphate-buffered saline, shaking on an orbital shaker for 6 times, each for 1 hour; the final washing phase was carried out at +4°C for 1 day; The matrix was then stored in PBS solution at +4°C for one month or dried in a freezer at -20°C for two years.

3. An acellular collagen-laminin matrix, characterized in that: The matrix comprises collagen and laminin, and the acellular collagen-laminin matrix is ​​prepared by the method of claim 2.

Citation Information

Patent Citations

  • Wound healing composition for skin external application comprising mycosporine-like amino acid and method for preparing the same

    CN107019690A

  • External preparation for skin

    JP2004262861A

  • Implantable medical articles having pro-healing coatings

    US20080243243A1

  • Tissue-equivalent and method for preparation thereof

    US4485096A