Hard magnets without rare earth metals

By using a ternary intermetallic compound with the general formula The improvement of high coercivity, remanent magnetization and energy density is suitable for manufacturing high-performance permanent magnetic materials.

CN112136188BActive Publication Date: 2024-10-01MAX PLANCK GESELLSCHAFT ZUR FOERDERUNG DER WISSENSCHAFTEN EV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN201980032490.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-05-15
Filing Date
2019-05-08
Publication Date
2024-10-01
Estimated Expiration
2039-05-08

AI Technical Summary

Technical Problem

Existing hard magnetic materials that do not contain rare earth metals have problems with insufficient coercivity, residual magnetization, and energy density in their magnetic properties, and they cannot fully meet the requirements for corrosion stability and mechanical strength.

Method used

Using ternary intermetallic compounds with the general formula , forming compounds with high magnetic anisotropy.

Benefits of technology

The improvement in coercivity, remnant magnetization and energy density of hard magnetic materials without rare earth metals has been achieved. It is suitable for manufacturing high-performance permanent magnetic materials, and the crystal structure can be adjusted by controlling deposition parameters to optimize magnetic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112136188B_ABST
    Figure CN112136188B_ABST
Patent Text Reader

Abstract

The present invention relates to a hard magnet comprising a hard magnet having a general composition X a X' b Y c Z d An intermetallic compound of , wherein X and X' independently represent a 3d transition metal with unpaired electrons; Y is a 4d or 5d transition metal of Group 5, 8, 9 or 10; Z is a main group element of Group 13, 14 or 15; a and d independently represent a number between 0.1 and 2.0; and b and c independently represent a number between 0.0 and 2.0; such that a+b+c+d is between 3.0 and 4.0.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to materials having permanent magnetic properties, which are also called hard magnets.A good hard magnet or permanent magnet should generate a high magnetic field, should withstand external forces that would demagnetize it, and should be mechanically robust.

[0002] Permanently magnetic materials play an important role in many areas of life, for example in medical diagnostics, magnetic circuits and spintronics.

[0003] Typically, hard magnetic materials are ferromagnetic materials characterized by high remanent magnetization and high coercivity.

[0004] When a ferromagnetic material is magnetized in one direction, it will not decay to zero magnetization when the applied magnetizing field is removed. The amount of magnetization that a ferromagnetic material retains at zero applied field is called the remanent magnetization. In order to change the magnetization back to zero, a magnetic field in the opposite direction must be applied; the amount of opposite magnetic field required for demagnetization is called the coercivity. When an alternating magnetic field is applied to the material, its magnetization will follow a loop called a hysteresis loop. This hysteresis is related to the presence of magnetic domains ("Weiss domains"). Some ferromagnetic materials will retain an applied magnetization almost indefinitely, and can therefore be used as "permanent magnets".

[0005] In order to be considered as a potential permanent magnet, three intrinsic properties of a magnetic material are particularly important:

[0006] - Curie temperature (T C ), above which the cooperative magnetism of ferromagnetic or ferrimagnetic materials disappears.

[0007] - Saturation magnetization (Ms), which determines the energy density (BH) max ,and

[0008] -Uniaxial magnetocrystalline anisotropy, which is usually determined by the anisotropy field B a This indicates an upper limit on the potential coercivity of permanent magnets.

[0009] At present, the most commonly used high-performance permanent magnets are samarium and cobalt (Sm-Co) and neodymium, iron and boron (Nd-Fe-B such as Nd2Fe 14 B) a rare earth metal compound having a coercivity of about 1.2 T and a residual magnetization of about 1.2 T and a residual magnetization of about 400 kJm -3 Maximum energy density (BH) max However, dysprosium or praseodymium is needed to improve corrosion stability and intrinsic coercivity. These rare earth elements are "strategic materials" due to their limited resources. Their availability is subject to political constraints. In addition, since these materials are sensitive to corrosion, their service temperature is limited to less than 200°C.

[0010] To date, there is no real commercial alternative to powerful rare earth permanent magnets, since they outperform all previously known systems due to their magnetic properties. They have a high magnetic anisotropy, since the electrons of the f-shell are shielded by the ligand field and thus the orbital momentum of this shell shows its advantage. In addition, they can exhibit a high local magnetic moment, which additionally allows a high saturation magnetization.

[0011] An alternative that does not contain rare earth metals is ferrite, which is already produced on a large scale and has a typical (BH) max <40kJm -3 Their use is limited to applications with low energy density, low cost and a maximum operating temperature of 250°C.

[0012] Another alternative is to have (BH) max About 80 kJm -3 ALNICO magnets. Relatively high (BH) for alloys without rare earth metals max is due to the high residual magnetization of about 1.1 T. However, μ0H c The relatively low coercive field strength of ∼0.14 T means that ALNICO magnets are subject to the risk of irreversible losses even at low magnetic field strengths. In addition, the bulk material is very brittle and therefore mechanically fragile. However, their high operating temperature of 550° C. maximum is very advantageous.

[0013] Magnets based on MnAl currently reach around 60 kJm -3 (BH) max with a Curie temperature of about 280°C. Their remanent magnetization and coercivity correspond to μ0M r is about 0.6T and μ0H c is about 0.4T. They do not contain "critical" elements and are therefore relatively cheap. In addition, the density is about 5gcm -3 , they are also relatively lightweight, but their coercivity of ≤0.5T is quite small.

[0014] MnBi can be used to prepare materials with up to (BH) max ~50kJm -3 The hard magnetic properties of MnBi are based on the uniaxial symmetry of the hexagonal crystal structure, its out-of-plane magnetization and the strong spin-orbit coupling of heavy Bi.

[0015] Binary compounds such as CoPt or FePt crystallized in tetragonal structure type L10 can exhibit a coercivity of 2 T. However, a high platinum content is economically disadvantageous.

[0016] In addition, some Heusler compounds are known to have hard magnetism. Heusler compounds are ternary intermetallic compounds with the formula X2YZ or XYZ, the latter also called half-Heusler compounds, in which X and Y are often transition metals and Z is a main group element. The class of Heusler alloys includes more than 1000 compounds, which can be ferromagnetic or ferrimagnetic, but the elements that compose them do not necessarily have such magnetic properties. Members of the tetragonal family of Heusler compounds can show high magnetocrystalline anisotropy due to the inherent uniaxial symmetry. Because tetragonal compounds are usually ferrimagnetic, they only show low saturation magnetization and therefore only low residual magnetization.

[0017] In addition to the further development and improvement of rare earth permanent magnets, new systems are being studied to close the gap between ferrites and Nd-Fe-B (which (BH) max Between 100 and 300 kJ·m -3 within the scope of ) is an important step for future technology.

[0018] It is therefore an object of the present invention to provide a hard magnetic material which does not contain rare earth metals but which at the same time exhibits a high coercivity, a high residual magnetization and a high energy density (compared to known hard magnets which do not contain rare earth metals).

[0019] The general formula is X a X' b Y c Z d The rare earth metal-free ternary intermetallic compounds with hexagonal or trigonal symmetry solve the above problems.

[0020] in

[0021] X and X' represent 3d transition metals with high total spin, i.e., with unpaired electrons, such as Mn, Fe, Co, and Ni;

[0022] Y is a 4d or 5d transition metal from Group 5, 8, 9 or 10, such as Ru, Rh, Pd, Pt, Ir, Ag, Au, Nb or Ta, characterized by high spin-orbit coupling (SOC);

[0023] Z is a main group element of Group 13, 14 or 15, such as Al, Ga, In, Ge, Sn, As, Sb or Bi, wherein the higher homologues of these elements (In, Sn, Sb or Bi) are also characterized by high spin-orbit coupling (SOC);

[0024] a and d represent numbers between 0.1 and 2.0; and

[0025] b and c represent numbers between 0.0 and 2.0;

[0026] Make a+b+c+d between 3.0 and 4.0.

[0027] Therefore, the total X a X' b Y c Z d It represents an intermetallic compound with a composition between that of a Heusler compound and a half-Heusler compound.

[0028] These new compounds are characterized by a high uniaxial magnetocrystalline anisotropy; they are therefore suitable for the production of rare-earth-free permanent magnetic materials with a high coercive field.

[0029] BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 shows the growth of 22 nm thin Mn films on the (001) surface of a sapphire support (Al2O3) at different temperatures. 1.5 PtGa and 44nm thin Mn 1.08 Fe 0.58 Pt 1.19 Room temperature X-ray powder diffraction patterns of Ga layer: a) 200°C, b) 300°C, c) 400°C, d) 300°C.

[0031] Figure 2 shows a) for Mn on sapphire (001) as substrate 1.5 Temperature dependence of magnetization at 0.05 T for a PtGa thin layer upon cooling; b) out-of-plane (OP) and in-plane (IP) hysteresis curves at 20 K; c) out-of-plane (OP) and in-plane (IP) hysteresis curves at 200 K; d) 22 nm thin Mn deposited on sapphire substrate at various temperatures (20, 50, 100, 150 and 200 K). 1.5 Out-of-plane hysteresis curve of the PtGa layer.

[0032] Figure 3 shows that the 44nm thick Mn 1.08 Fe 0.58 Pt 1.19 Ga thin layer applied on a sapphire (001) support at 300 °C; a) temperature dependence of the magnetization upon cooling in an external magnetic field of 0.1 T; b) out-of-plane (OP) hysteresis curves at 50 K and 300 K.

[0033] DETAILED DESCRIPTION OF THE INVENTION

[0034] The ternary intermetallic compounds according to the invention possess a hexagonal or trigonal crystal structure. This is an important feature, since a crystal structure of this symmetry satisfies the criteria of crystal anisotropy due to the inherent uniaxial symmetry. This crystal anisotropy is combined with the significant spin-orbit coupling of the 4d and 5d elements (transition metals or main group elements) in the compounds of the invention. The result is that these compounds exhibit strong magnetic anisotropy even in the absence of shape anisotropy caused by magnetocrystalline anisotropy.

[0035] The intermetallic compound of the present invention has the general formula composition X a X' b Y c Z d The composition is therefore between the Heusler compounds and the semi-Heusler compounds.

[0036] Heusler compounds are intermetallic compounds with the general composition X2YZ and crystallize with the L21 structure type (Pearson's Handbook of Crystallographic Data for Intermetallic Phases, ASM International, The Materials Information Society, 1991). Intermetallic compounds are usually the following compounds

[0037] a) Between two or more true metals (T1 and T2)

[0038] b) between one or more true metals and one or more true metals of subgroup B

[0039] c) between two or more metals of subgroup B

[0040] When moving from a) to c), the properties of these compounds become less metallic and more and more similar to true chemical compounds. The classification of true metals and elements of the B subgroup is shown in Table 13.1 from RCEvans (Introduction to Crystal Chemistry, Walter de Gruyter Verlag Berlin New York 1976 p. 276):

[0041]

[0042] Metals of the lanthanides and actinides belong to category T2. In the Heusler compound X2YZ, X and Y are mainly transition metals (T2 in the table above), and sometimes Y is also a rare earth element. Z is a nonmagnetic metal or nonmetal (B1 or B2).

[0043] The intermetallic compound of the present invention has the general formula composition X a X' b Y c Z d In these Hosler and semi-Hosler compounds,

[0044] X and X' represent 3d transition metals with high total spin, i.e., with unpaired electrons, preferably Mn, Fe, Co or Ni;

[0045] Y is a 4d or 5d transition metal of Group 5, 8, 9 or 10 characterized by high spin-orbit coupling (SOC), preferably Ru, Rh, Pd, Pt, Ir, Ag, Au, Nb or Ta;

[0046] Z is a main group element of group 13, 14 or 15, preferably Al, Ga, In, Ge, Sn, As, Sb or Bi, wherein the higher homologues of these elements (In, Sn, Sb or Bi) are also characterized by high spin-orbit coupling (SOC);

[0047] a and d represent numbers between 0.1 and 2.0; and

[0048] b and c represent numbers between 0.0 and 2.0;

[0049] Make a+b+c+d between 3.0 and 4.0.

[0050] In the Heusler compounds of the present invention the parameters a, b, c and d can be independently selected from numbers between 0.1 and 2.0 (for a and d) and between 0.0 and 2.0 (for b and c). Preferably a is 1 or 2, more preferably a is 1 when b is 1 and a is 2 when b is 0. Preferably d is 1. Preferably b is 0 or (when a is 1) b is preferably 1. Preferably c is 1.

[0051] Typically the sum of a, b, c and d is between 3.0 and 4.0, preferably 3.0 or 4.0.

[0052] Manufacturing method

[0053] Sputtering technology is used for producing the compounds according to the invention. This allows the production of thin layers (films) of the compounds. For this purpose, elemental metals and / or alloys of two metals are used as targets in sputtering. The base pressure of the vacuum receiver is preferably ≤10 -6 mbar, preferably ≤10 -7 mbar and most preferably ≤10 -8 mbar and deposition preferably occurs at 0.1 × 10 -3 mbar to 10×10 -3 mbar, more preferably 1×10 -3 mbar to 5×10-3 mbar, and most preferably at 3×10 -3 mbar, and in a temperature range of preferably 100°C to 500°C, more preferably 150°C to 450°C and most preferably 200°C to 400°C. The growth rate of the thin layer is about 0.03 to 0.04 nm / s. After deposition, the thin layer on the substrate in the receiver is preferably vacuum annealed for preferably 5 to 25 minutes, more preferably 10 to 20 minutes and most preferably about 15 minutes, and then slowly cooled to room temperature. A 2 to 3 nm aluminum protective layer is then preferably deposited to pre-coat the thin metal layers to protect them from oxidation.

[0054] The crystal structure of the deposited material can be influenced by changing the deposition parameters. It was found that at low deposition temperatures of about 200° C., hexagonal structures are preferentially formed, while the proportion of tetragonal half-Hossler compounds increases with increasing temperature (at about 400° C.). In a further preferred embodiment, the compound can be obtained by epitaxially growing a thin film on a predetermined substrate with a desired crystal structure, such as a sapphire substrate (along 0001) or on MgO (along 001) as a substrate. It was observed that the hexagonal compounds of the present invention preferentially grow on sapphire in a crystallographic

[001] direction perpendicular to the substrate surface. In principle, hexagonal Ru or Co can also be used as the substrate surface. However, these substrates have a high lattice mismatch compared to the hexagonal compounds of the present invention and are therefore less preferred. Another but equally less preferred alternative is hexagonal SiC (2H) and trigonal (SiO2) as substrates; thin layers grown on these types of substrates show poor crystallinity.

[0055] Manufacturing magnets for use

[0056] In order to be used as a magnet, the compound of the present invention can be sintered as a raw material or bonded with a suitable binder material, for example. Sintered magnets are generally stronger and anisotropic but limited in shape. They are made by a heating process followed by pressure molding of the raw material. Bonded magnets are not as strong as sintered magnets, but are less expensive and can be made into almost any size and shape. For bonded magnets, the raw material (compound according to the present invention) is mixed with 5 to 90% by weight, preferably 10 to 60% by weight, more preferably 20-40% by weight of a binder, compacted and cured at an elevated temperature (e.g., at 50-350°C, preferably at 80-280°C, more preferably at 100-200°C, depending on the temperature stability of the binder and the magnetic compound used). They are isotropic, i.e., they can be magnetized in any direction. The molding method can be, for example, injection molding or a compression bonding method. Typical binder types are nylon, polyamide, polyphenylene sulfide (PPS) and nitrile rubber (NBR). Example

[0057] Equipment and measurement methods

[0058] By using Cu-K α X-ray diffraction (XRD) measurements with a source (Philips PANanalytical X'pert Pro) were used to examine the crystal structure and thickness of the films. Energy dispersive X-ray spectroscopy (EDX) measurements were performed on a QUANTA 200FEG I to determine the composition of the films. The StrataGEM software package was used to obtain the film thickness. A Quantum Design superconducting quantum interference device vibrating sample magnetometer (MPMS-3) was used to study the magnetic properties of the films.

[0059] Examples 1 and 2

[0060] Mn 1.5 PtGa and Mn 1.08 Fe 0.58 Pt 1.19 Ga

[0061] Mn was prepared by epitaxial growth on the sapphire surface (0001) as a substrate. 1.5 PtGa and Mn 1.08 Fe 0.58 Pt 1.19 Since sapphire (Al2O3) crystallizes in the trigonal system, i.e., has a hexagonal metric, the structure of the sapphire surface supports Mn 1.5 PtGa and Mn 1.08 Fe 0.58 Pt 1.19 Epitaxial growth of Ga layer.

[0062] Alloys of elemental manganese, platinum, iron and composite MnGa are used as sputtering targets. The base pressure of the vacuum receiver is ≤10 - 8 mbar, and within the temperature range of 200°C to 300°C within 3×10 -3 The deposition on the substrate takes place at 400 mbar. The growth rate of the thin layer is about 0.03 to 0.04 nm / s. After deposition, the thin layer on the substrate in the receiver is vacuum annealed for 15 minutes and then slowly cooled to room temperature. A 2 to 3 nm aluminum protective layer is then deposited to protect the thin metal layer from oxidation.

[0063] Figure 1 shows that in the 22nm Mn 1.5 PtGa thin layer and 44nm Mn 1.08 Fe 0.58 Pt 1.19X-ray powder diffraction pattern at room temperature using "out-of-plane" geometry on a Ga thin layer. The Bragg reflections of the hexagonal structure are marked as H(0002) and H(0004). The thin layer grown at 300°C (Figure 1b) shows better crystallinity than the layer applied at 200°C (Figure 1a). At deposition temperatures greater than 300°C (Figure 1c), a decrease in the Bragg intensity and additional weak reflections (marked with *) are observed. It can be assumed that the additional reflections are caused by tetragonal semi-Hossler compounds as a minor phase. Similar behavior was also observed in bulk samples. As shown in Figure 1d, partial substitution of Mn by Fe maintains the hexagonal structure. Regardless of the deposition temperature, all films deposited on sapphire (0001) exhibit texture. Epitaxial growth on the surface of a trigonal substrate respectively causes hexagonal Mn 1.5 PtGa and Mn 1.08 Fe 0.58 Pt 1.19 Ga is deposited with a preferential orientation in the crystallographic

[001] direction, which is perpendicular to the surface of the substrate and thus parallel to the crystallographic c-axis of sapphire.

[0064] The crystal structure of the deposited material can be influenced by means of different deposition parameters. It was observed that at low deposition temperatures a hexagonal structure is preferentially formed, while with increasing temperature the proportion of tetragonal half-Hossler compounds increases. The lattice parameters of the hexagonal crystal structure are 1.5 For PtGa and and for Mn 1.08 Fe 0.58 Pt 1.19 For Ga and This corresponds to the a-axis relative to the sapphire substrate. The a-axis lattice mismatch is about 8.2% and 8.6%. Despite the relatively large lattice mismatch, Mn was observed on the sapphire surface (0001) of the substrate. 1.5 PtGa and Mn 1.08 Fe 0.58 Pt 1.19 Epitaxial growth of Ga.

[0065] In Figure 2, well-crystallized Mn deposited on a sapphire (0001) surface at 300 °C is shown. 1.5Magnetic properties of PtGa thin layers. Figure 2a illustrates the variation of magnetization with temperature measured using field cooling mode (FC) at a field strength of 0.05T. At the Curie temperature (Tc) of about 241K, a ferromagnetic to paramagnetic phase transition is observed. The corresponding M(H) curves for 20K and 200K for the "in-plane" (IP) and "out-of-plane" (OP) directions are shown in Figures 2b and 2c, respectively. The data shown correspond to the raw data after deducting the substrate contribution for each temperature. The sample shows a coercive field strength H for the "out-of-plane" orientation at 20K. c At 1.5 T, but at 200 K only a vanishing coercivity (0.18 T) is shown (due to the temperature dependence of the magnetic anisotropy). Figure 2d shows a systematic decrease in the coercivity with increasing temperature. The measured values ​​of the coercivity in the "out-of-plane" direction show a strong magnetic anisotropy compared to the "in-plane" measurements. At 20 K and 5 T, a total magnetization of 400 kA / m was measured. According to the equation K U =(μ0M S xH a ) / 2, which results in 3.3MJ / m 3 As the anisotropy constant (K U ) value. S is the saturation magnetization and H a is the anisotropy field. An estimate of the latter is obtained by using the intersection of the “in-plane” and “out-of-plane” curves. 1.5 PtGa thin layer shown at 20K (BH) max About 30 kJm -3 . As the temperature increases, (BH) max The energy density is reduced and approaches the Curie temperature at 200K, which is only 4 kJm -3 .

[0066] Figure 3 shows that 44 nm Mn deposited at 300 °C 1.08 Fe 0.58 Pt 1.19 The magnetization intensity of Ga film varies with temperature. The magnetization intensity measured by field cooling mode (FC) at a field intensity of 0.1 T ( Figure 3a ) shows a ferromagnetic to paramagnetic phase transition at about 312K. Figure 3b The hysteresis curves measured in the out-of-plane geometry at 50 and 300 K are shown in Figure 2. The low temperature measurement results show a coercive field strength of 0.87 T close to T C The coercive field strength of the measured results is 0.02T.

[0067] The two examples illustrate that materials with a hexagonal crystal structure can exhibit significant coercivity and remanent magnetization in the presence of elements with abundant unpaired electrons, such as manganese or iron, and elements with significant spin-orbit coupling, such as platinum. 1.08 Fe 0.58 Pt 1.19 The Ga system also showed that the Curie temperature and magnetic moment can be further increased in the quaternary system. Similar results can also be achieved in the MnCoPtGa system.

Claims

1. A hard magnet comprising an intermetallic compound X having the following general formula a X' b Y c Z d in X and X' independently represent a 3d transition metal with unpaired electrons; Y is a 4d or 5d transition metal of Group 5, 8, 9 or 10; Z is a main group element of Group 13, 14 or 15; a and d independently represent numbers between 0.1 and 2.0; b represents a number between 0.0 and 2.0; and c is 1; Make a+b+c+d between 3.0 and 4.0; The intermetallic compound has hexagonal or trigonal crystal symmetry; and The hard magnet has a coercive force B c ≥0.05T.

2. The hard magnet according to claim 1, wherein X and X' are independently selected from Mn, Fe, Co or Ni.

3. The hard magnet according to claim 1 or 2, wherein Y is Ru, Rh, Pd, Pt, Ir, Ag, Au, Nb or Ta.

4. A hard magnet according to claim 1, 2 or 3, wherein Z is Al, Ga, In, Ge, Sn, As, Sb or Bi.

5. The hard magnet according to claim 1, wherein a is 1 or 2, more preferably When b is 1, a is 1 and When b is 0, a is 2. 6 . The hard magnet according to claim 1 , wherein d is 1.

7. A hard magnet according to one of claims 1 to 6, wherein b is 0 or When a is 1 b is 1.

8. The hard magnet according to claim 1, wherein the sum of a, b, c and d is 3.0 or 4.

0.

9. The hard magnet according to one of claims 1 to 8, wherein the intermetallic compound has magnetocrystalline anisotropy.

10. The hard magnet according to one of claims 1 to 9, wherein the hard magnet is sintered.

11. The hard magnetic body according to one of claims 1 to 9, wherein the hard magnetic body further comprises a binder.

12. Use of intermetallic compounds with the following general formula as hard magnets a X' b Y c Z d in X and X' represent 3d transition metals with unpaired electrons; Y is a 4d or 5d transition metal of Group 5, 8, 9 or 10; Z is a main group element of Group 13, 14 or 15; a and d independently represent a number between 0.1 and 2.0; and b and c independently represent numbers between 0.0 and 2.0; Make a+b+c+d between 3.0 and 4.0.

Citation Information

Patent Citations

  • Magnetic resistance device

    EP1560231A2

  • Magneto-optical material

    JP1988079253A

  • Resin coupled permanent magnet material and magnetization thereof as well as encoder using the same

    JP2000040611A