Polymer electrolyte membrane, method for manufacturing the same, and membrane electrode assembly comprising the same

By adopting a stacked porous carrier structure and a specific impregnation process, the lack of performance of polymer electrolyte membranes under high temperature and low humidity conditions is solved, its mechanical and chemical durability is improved, and hydrogen permeability and dimensional stability are optimized.

CN112335083BActive Publication Date: 2024-11-08KOLON INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980043852.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-06-29
Filing Date
2019-06-28
Publication Date
2024-11-08
Estimated Expiration
2039-06-28

AI Technical Summary

Technical Problem

The existing polymer electrolyte membrane cannot achieve high performance under high temperature and low humidity conditions, and the hydrogen permeability and dimensional stability are insufficient, which affects its mechanical and chemical durability.

Method used

Using a laminated porous carrier structure, the proton conductivity and dimensional stability are improved by adding ionic conductors between the first porous carrier and the second porous carrier, and optimized by specific impregnation and drying processes to reduce hydrogen permeation and size. change.

Benefits of technology

The mechanical and chemical durability of the polymer electrolyte membrane is significantly improved, the long-term stability of the interface between the ionic conductor and the carrier is ensured, and the impregnation performance is optimized, reducing hydrogen permeability and dimensional changes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112335083B_ABST
    Figure CN112335083B_ABST
Patent Text Reader

Abstract

The present invention relates to a polymer electrolyte membrane, a method for manufacturing the polymer electrolyte membrane, and a membrane electrode assembly including the polymer electrolyte membrane, the polymer electrolyte membrane comprising: a first porous support having a first hole filled with a first ion conductor; a second porous support having at least one second hole filled with the first ion conductor and a third hole filled with a second ion conductor, wherein the first porous support and the second porous support are in contact with each other. The polymer electrolyte membrane has enhanced performance by improving impregnation performance, and has enhanced mechanical and chemical durability by minimizing hydrogen permeability and dimensional change. In addition, the interface between the ion conductor and the support in the polymer electrolyte membrane can be stably maintained for a long time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a polymer electrolyte membrane, a method for manufacturing the polymer electrolyte membrane, and a membrane electrode assembly including the polymer electrolyte membrane, and more specifically, to: a polymer electrolyte membrane configured so that impregnation of the polymer electrolyte membrane is improved, thereby improving the performance of the polymer electrolyte membrane, minimizing hydrogen crossover and dimensional changes of the polymer electrolyte membrane, thereby improving the mechanical and chemical durability of the polymer electrolyte membrane, and the interface between the ion conductor and the carrier is stably maintained for a long time; a method for manufacturing the polymer electrolyte membrane; and a membrane electrode assembly including the polymer electrolyte membrane. Background Art

[0002] A fuel cell is a battery that includes a power generation system for directly converting chemical reaction energy into electrical energy through oxidation / reduction reactions of hydrogen and oxygen contained in hydrocarbon fuels (such as methanol, ethanol or natural gas). Fuel cells have attracted attention as the next generation of clean energy that can replace fossil energy due to their environmentally friendly characteristics (such as high energy efficiency and reduced pollutant emissions).

[0003] The advantage of such a fuel cell is that the unit cells are stacked to form a battery stack, thereby providing various levels of power. In addition, the energy density of a fuel cell is 4 to 10 times that of a small lithium battery, so fuel cells have attracted attention as small power sources or mobile power sources.

[0004] A cell stack of a fuel cell that essentially generates electricity has the following structure: several to dozens of unit cells are stacked, each unit cell includes a membrane electrode assembly (MEA) and a separator (also called a bipolar plate), and the membrane electrode assembly is generally configured to have the following structure: an oxidation electrode (anode or fuel electrode) and a reduction electrode (cathode or air electrode) are formed on opposite sides of an electrolyte membrane with an electrolyte membrane set between them.

[0005] Fuel cells can be classified into alkaline electrolyte membrane fuel cells or polymer electrolyte membrane fuel cells (PEMFC) according to the state and type of electrolyte. Polymer electrolyte membrane fuel cells have attracted attention as mobile power sources, vehicle power sources, and household power sources due to their low operating temperature of less than 100°C, fast startup and response characteristics, and excellent durability.

[0006] Representative examples of polymer electrolyte membrane fuel cells may include a proton exchange membrane fuel cell (PEMFC) using hydrogen as fuel and a direct methanol fuel cell (DMFC) using liquid methanol as fuel.

[0007] The reactions occurring in the polymer electrolyte membrane fuel cell will be briefly described. First, when a fuel such as hydrogen is supplied to an oxidation electrode, protons (H + ) and electron (e - ). The generated protons are transferred to the reduction electrode via the polymer electrolyte membrane, and the generated electrons are transferred to the reduction electrode via an external circuit. Oxygen is supplied from the reduction electrode, and the oxygen is combined with the protons and the electrons, thereby generating water through the reduction reaction of oxygen.

[0008] At the same time, in order to realize the commercial use of polymer electrolyte membrane fuel cells, there are many technical problems to be solved, especially, the high performance, long life and low price of polymer electrolyte membrane fuel cells must be achieved. The element that has the greatest impact on it is the membrane electrode assembly, especially the polymer electrolyte membrane is one of the core factors that have the greatest impact on the performance and price of MEA.

[0009] The requirements for polymer electrolyte membranes required for operating polymer electrolyte membrane fuel cells include high proton conductivity, high mechanical and chemical stability, high heat resistance, low fuel permeability, high mechanical strength, low moisture content, and excellent dimensional stability. Conventional polymer electrolyte membranes often fail to properly achieve high performance under specific temperature and relative humidity conditions, particularly under high temperature / low humidity conditions. As a result, polymer electrolyte membrane fuel cells in which conventional polymer electrolyte membranes are applied are limited in the range in which the fuel cell can be used.

[0010] In order to ensure the performance, durability, mechanical properties and chemical properties of polymer electrolyte membranes at the same time, reinforced composite membrane type polymer electrolyte membranes in which reinforcing materials are applied have been developed. However, the disadvantage of polymer electrolyte membranes with high proton conductivity is that the moisture content is high, thereby reducing dimensional stability. Commercial fluorine-based electrolyte membranes have higher performance than hydrocarbon electrolyte membranes, but have the disadvantage that, due to their high hydrogen conductivity, the open circuit voltage (OCV) is reduced and the durability of the membrane is reduced.

[0011] Therefore, in order to commercialize polymer electrolyte membranes, it is necessary to improve their performance while increasing the dimensional stability of polymer electrolyte membranes during impregnation and drying, thereby improving their mechanical durability. To this end, it is necessary to ensure the optimal structure of the reinforced composite membrane and improve its impregnation. Summary of the invention

[0012] Technical issues

[0013] An object of the present disclosure is to provide a polymer electrolyte membrane, which is configured so that the impregnation of the polymer electrolyte membrane is improved, thereby the performance of the polymer electrolyte membrane is improved, the hydrogen permeation and dimensional change of the polymer electrolyte membrane are minimized, thereby the mechanical and chemical durability of the polymer electrolyte membrane is improved, and the interface between the ion conductor and the carrier is stably maintained for a long time.

[0014] Another object of the present disclosure is to provide a method for manufacturing a polymer electrolyte membrane.

[0015] Yet another object of the present disclosure is to provide a membrane electrode assembly including the polymer electrolyte membrane.

[0016] Technical Solution

[0017] According to one aspect of the present disclosure, there is provided a polymer electrolyte membrane, comprising: a first porous support having first pores filled with a first ion conductor; and a second porous support having at least one second pore filled with the first ion conductor and a third pore filled with the second ion conductor, wherein the first porous support and the second porous support are in contact with each other.

[0018] All pores of the first porous support may be filled with the first ion conductor.

[0019] The first porous support may further have at least one fourth pore filled with a second ion conductor.

[0020] Each of the first porous support and the second porous support can be an isotropic porous support, which is configured so that the machine direction (MD) tensile elongation and the transverse direction (TD) tensile elongation are equal to each other, or the higher of the MD tensile elongation and the TD tensile elongation is less than 1.5 times the lower one.

[0021] The first porous support and the second porous support may be stacked such that directions in which the first porous support and the second porous support are stretched are perpendicular to each other.

[0022] According to another aspect of the present disclosure, a polymer electrolyte membrane is provided, comprising a porous support and an ion conductor, wherein the pores of the porous support are filled with the ion conductor, wherein, at a temperature of 80°C and a relative humidity (RH) of 50%, the polymer electrolyte membrane has an in-plane (IP) proton conductivity of 0.046S / cm to 0.1S / cm and a through-plane (TP) proton conductivity of 0.042S / cm to 0.1S / cm, and after the polymer electrolyte membrane is immersed in distilled water at room temperature for 12 hours and then dried at 50°C under a vacuum state for 24 hours, each of the MD swelling ratio and the TD swelling ratio of the polymer electrolyte membrane calculated by the following Formulas 1 and 2 is less than 2%.

[0023] [Formula 1]

[0024] △L(MD)=[(L 湿润 (MD)–L 干燥 (MD)) / L 干燥 (MD)]×100

[0025] [Formula 2]

[0026] △L(TD)=[(L 湿润 (TD)–L 干燥 (TD)) / L 干燥 (TD)]×100

[0027] Among them, △L(MD) is the MD swelling ratio, △L(TD) is the TD swelling ratio, L 湿润 (MD) and L 湿润 (TD) are the MD length and TD length measured just before drying, L 干燥 (MD) and L 干燥 (TD) are MD length and TD length measured immediately after drying, respectively.

[0028] The TP proton conductivity and the IP proton conductivity of the polymer electrolyte membrane may be equal to each other, or the higher of the TP proton conductivity and the IP proton conductivity may be 1.5 times or less the lower one thereof.

[0029] The TP swelling ratio and the MD swelling ratio may be equal to each other, or the higher of the TP swelling ratio and the MD swelling ratio may be 1.5 times or less the lower one thereof.

[0030] The polymer electrolyte membrane can have a thermal conductivity of 7×10 -5 cm 2 / sec or less hydrogen permeability.

[0031] The MD tensile strength and the TD tensile strength of the polymer electrolyte membrane may be equal to each other, or the higher of the MD tensile strength and the TD tensile strength may be 1.5 times or less the lower one thereof.

[0032] The MD tensile elongation and TD tensile elongation of the polymer electrolyte membrane may be equal to each other, or the higher of the MD tensile elongation and the TD tensile elongation may be 1.5 times or less the lower thereof.

[0033] According to another aspect of the present disclosure, a method for manufacturing a polymer electrolyte membrane is provided, the method comprising: casting a first mixed solution containing a first ion conductor; placing a first porous carrier in a dry state on the first mixed solution so that the first porous carrier is completely in a wet state; immediately after the first porous carrier is completely in a wet state, adding a second porous carrier in a dry state to the first porous carrier so that the first porous carrier and the second porous carrier are in contact with each other; applying a second mixed solution containing a second ion conductor to the second porous carrier so that the second porous carrier is completely in a wet state; and drying the first porous carrier and the second porous carrier in a wet state.

[0034] According to another aspect of the present disclosure, there is provided a membrane electrode assembly including an anode and a cathode disposed opposite to each other and a polymer electrolyte membrane located between the anode and the cathode.

[0035] According to yet another aspect of the present disclosure, a fuel cell including a membrane electrode assembly is provided.

[0036] Beneficial Effects

[0037] According to the present disclosure, impregnation of the polymer electrolyte membrane is improved, so that the performance of the polymer electrolyte membrane is improved, hydrogen permeation and dimensional change of the polymer electrolyte membrane are minimized, thereby improving the mechanical and chemical durability of the polymer electrolyte membrane, and the interface between the ion conductor and the support is stably maintained for a long time. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 is an exploded perspective view showing a state in which porous supports according to the present disclosure are stacked in intersecting directions.

[0039] Figure 2 yes Figure 1 Coupling perspective view.

[0040] Figure 3 is a cross-sectional view schematically showing an example of a polymer electrolyte membrane according to an embodiment of the present disclosure.

[0041] Figure 4 and Figure 5The following are scanning electron microscope (SEM) images of polymer electrolyte membranes manufactured according to Example 1 and Comparative Example 1 of the present disclosure, respectively. DETAILED DESCRIPTION

[0042] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the accompanying drawings so that those skilled in the art to which the present disclosure belongs can easily implement the embodiments of the present disclosure. However, the present disclosure can be implemented in various different forms and is not limited to the embodiments described herein.

[0043] According to an embodiment of the present disclosure, a polymer electrolyte membrane includes: a first porous support having first pores filled with a first ion conductor; a second porous support having at least one second pore filled with the first ion conductor and a third pore filled with the second ion conductor, wherein the first porous support and the second porous support are in contact with each other.

[0044] Alternatively, the polymer electrolyte membrane according to the present disclosure may further include one or more porous supports stacked on any one of the first porous support and the second porous support. That is, the polymer electrolyte membrane according to the present disclosure includes a stacked porous support having a structure in which two or more porous supports are stacked.

[0045] According to the present disclosure, the individual porous carriers constituting the stacked porous carrier are in close contact with each other. Unless the types of the individual porous carriers are different from each other so as to be distinguished from each other, the interface between them may not be visually recognizable, and the stacked porous carrier may not be an obvious single porous carrier. Therefore, when viewed from the perspective of the final product rather than from the perspective of the manufacturing process, the stacked porous carrier according to the present invention can be regarded as a single porous carrier, depending on the circumstances.

[0046] However, the use of a stacked porous support and the features associated therewith related to the manufacturing method according to the present disclosure provide various advantages in various physical properties of the polymer electrolyte membrane compared to the case of using a single porous support having the same thickness as the stacked porous support, which will be described in detail below.

[0047] In an embodiment of the present disclosure, all pores of the first porous support may be filled with the first ion conductor. Alternatively, the first porous support may further have at least one fourth pore filled with the second ion conductor.

[0048] Each of the first porous carrier and the second porous carrier can be an isotropic porous carrier, which is configured so that the machine direction (machine-direction, MD) tensile elongation (hereinafter referred to as "MD tensile elongation") and the transverse direction (transverse-direction, TD) tensile elongation (hereinafter referred to as "MD tensile elongation") are equal to each other, or the higher of the MD tensile elongation and the TD tensile elongation is less than 1.5 times the lower one.

[0049] The first porous support and the second porous support may be stacked such that directions in which the first porous support and the second porous support are stretched are perpendicular to each other.

[0050] The thickness of the laminated porous support may be more than 50% of the total thickness of the polymer electrolyte membrane, specifically 50% to 90%. In the case where the thickness of the laminated porous support is less than 50% of the total thickness of the polymer electrolyte membrane, the improvement effect of the dimensional stability and mechanical durability of the reinforced composite membrane having the laminated porous support as a reinforcing material may be negligible. In the case where the thickness of the laminated porous support is greater than 90% of the total thickness of the polymer electrolyte membrane, the thickness of the ion conductive layer located on the upper surface or the lower surface of the laminated porous support may be too small, and thus the surface resistance may increase.

[0051] A stacked porous carrier is formed by stacking a plurality of porous carriers, and the surface area of ​​the stacked porous carrier in direct contact with the ion conductor during the impregnation process is increased compared to the case of using a single porous carrier having the same thickness as the stacked porous carrier, thereby improving the wetting of the stacked porous carrier caused by the solution containing the ion conductor. In addition, when the pores of the porous carrier are filled with ion conductors, the air in the pores can be more easily discharged therefrom, thereby minimizing the generation of microscopic bubbles, and thus the impregnation can be improved. This improvement in wetting and impregnation improves the ionic conductivity of the polymer electrolyte membrane according to the present disclosure. In addition, the area capable of buffering dimensional changes can be increased, thereby improving dimensional stability.

[0052] In order to improve the dimensional stability of the enhanced composite electrolyte membrane manufactured using only a single porous support, it is necessary to increase the thickness of the porous support. However, as the thickness of the porous support increases, the wetting and impregnation of the porous support decrease, thereby reducing the ionic conductivity of the electrolyte membrane. On the other hand, when the thickness of the porous support is reduced, the ionic conductivity of the electrolyte membrane can be improved due to the improvement of wetting and impregnation; however, the function as a support cannot be properly exerted, so the dimensional stability of the electrolyte membrane is reduced. That is, in the enhanced composite electrolyte membrane manufactured using only a single porous support, ionic conductivity and dimensional stability are physical properties with a trade-off relationship between them.

[0053] In the present disclosure, a laminated porous support is used, and an impregnation process and an add-on process unique to the present disclosure are simultaneously performed, thereby making it possible to improve both the ion conductivity and the dimensional stability of the polymer electrolyte membrane.

[0054] Specifically, a polymer electrolyte membrane manufactured using the manufacturing method according to the present disclosure includes a porous support and an ion conductor, wherein the pores of the porous support are filled with the ion conductor, wherein (i) at a temperature of 80° C. and a relative humidity (RH) of 50%, the polymer electrolyte membrane has an in-plane (IP) proton conductivity of 0.046 S / cm to 0.1 S / cm (hereinafter referred to as “IP proton conductivity”) and a through-plane (TP) proton conductivity of 0.042 S / cm to 0.1 S / cm (hereinafter referred to as “TP proton conductivity”), and (ii) after the polymer electrolyte membrane is immersed in distilled water at room temperature for 12 hours and then dried at 50° C. under a vacuum state for 24 hours, each of the machine direction (MD) swelling ratio (hereinafter referred to as “MD swelling ratio”) and the transverse direction (TD) swelling ratio (hereinafter referred to as “TD swelling ratio”) of the polymer electrolyte membrane calculated by the following Formulas 1 and 2 is 2% or less.

[0055] [Formula 1]

[0056] △L(MD)=[(L 湿润 (MD)–L 干燥 (MD)) / L 干燥 (MD)]×100

[0057] [Formula 2]

[0058] △L(TD)=[(L 湿润 (TD)–L 干燥 (TD)) / L 干燥 (TD)]×100

[0059] Among them, △L(MD) is the MD swelling ratio, △L(TD) is the TD swelling ratio, L 湿润 (MD) and L 湿润 (TD) are the MD length and TD length measured just before drying, L 干燥 (MD) and L 干燥 (TD) are MD length and TD length measured immediately after drying, respectively.

[0060] The machine direction (MD) as the length direction refers to the direction in which the roller travels when the polymer electrolyte membrane is continuously produced in a roll-to-roll manner, or the direction in which the manufactured polymer electrolyte membrane is wound, and the transverse direction (TD) as the width direction refers to the direction perpendicular to the machine direction.

[0061] In addition, the thickness T of the polymer electrolyte membrane in a wet state can be measured in a similar manner to the method of measuring the MD swelling ratio and the TD swelling ratio. 湿润 and the thickness T of the polymer electrolyte membrane in the dry state 干燥 , and substitute it into the following formula 3 to calculate the thickness swelling ratio.

[0062] [Formula 3]

[0063] (T 湿润 -T 干燥 / T 干燥 )×100=△T(thickness swelling ratio, %)

[0064] The TD swelling ratio and the MD swelling ratio of the polymer electrolyte membrane may be equal to each other, or the higher of the TD swelling ratio and the MD swelling ratio may be 1.5 times or less of the lower one. When the higher of the TD swelling ratio and the MD swelling ratio is greater than 1.5 times of the lower one, the swelling resistance is different from each other in two directions, and thus, the mechanical durability of the polymer electrolyte membrane is sharply reduced due to repeated moisturizing and drying.

[0065] In addition, when the impregnation of the laminated porous support is improved, a water channel along which protons can move can be successfully formed in the through-plane direction of the laminated porous support, whereby the performance of the laminated porous support can be improved. In addition, the flow channel along which hydrogen can move may be complicated, so that resistance may increase when hydrogen moves, and thus hydrogen permeability may decrease. Therefore, in the case of using a laminated porous support, chemical durability can be ensured while ensuring high performance.

[0066] Therefore, the polymer electrolyte membrane according to the embodiment of the present disclosure can have an IP proton conductivity of 0.046 S / cm to 0.1 S / cm and a TP proton conductivity of 0.042 S / cm to 0.1 S / cm at a temperature of 80° C. and a relative humidity (RH) of 50%, and can have a 7×10 -5 cm 2 / sec or less. In the case where the IP and TP proton conductivities of the polymer electrolyte membrane are less than the above ranges, it is impossible to ensure the basic function as a polymer electrolyte membrane. In the case where the hydrogen permeability of the polymer electrolyte membrane is greater than 7×10 -5 cm 2 / sec, the OCV may be reduced and the long-term chemical durability may be greatly reduced. As long as the polymer electrolyte membrane meets the proton conductivity of a predetermined level or higher, the hydrogen permeability is preferably low. However, when considering the current technical limitations, the lower limit of the hydrogen permeability of the polymer electrolyte membrane may be 1×10 -8 cm2 / sec.

[0067] In addition, the TP proton conductivity and IP proton conductivity of the polymer electrolyte membrane may be equal to each other, or the higher of the TP proton conductivity and the IP proton conductivity may be less than 1.5 times, specifically 1.0 to 1.1 times, of the lower one. That is, the stacked porous supports of the polymer electrolyte membrane may be in close contact with each other to the extent that the interface between the supports cannot be visually identified, so that impregnation may be improved, and therefore, a through-plane (TP) water channel along which protons can move may be more successfully formed than with other methods. This may be represented by the ratio between the IP proton conductivity and the TP proton conductivity.

[0068] The in-plane (IP) direction of the polymer electrolyte membrane, which is a planar direction perpendicular to the through-plane (TP) direction, may refer to one or both of a machine direction (MD) and a transverse direction (TD) perpendicular to the machine direction.

[0069] The IP proton conductivity can be calculated using the membrane resistance at a relative humidity of 50% after measuring the membrane resistance at a temperature of 80°C and a relative humidity of 30% to 95% using a magnetic suspension balance (Bell Japan). The TP proton conductivity can be measured by coating the opposite surface of the polymer electrolyte membrane with Pt catalyst ink, placing and fastening the gas diffusion layer thereon, measuring the membrane resistance at a temperature of 80°C and a relative humidity of 50%, and dividing the measured membrane resistance by the thickness of the polymer electrolyte membrane. At this time, the following formulas 4 and 5 can be used.

[0070] [Formula 4]

[0071] Membrane resistance (R) = (R1-R2) × (effective area of ​​membrane)

[0072] Here, R1 is the resistance [Ω] when the film is poured, and R2 is the resistance [Ω] when the film is not poured.

[0073] [Formula 5]

[0074] Proton conductivity (S / cm) = 1 / R × t

[0075] Where R is the membrane resistance [Ω·cm 2 ], t is the thickness of the film [cm].

[0076] The ratio between the IP proton conductivity and the TP proton conductivity can be calculated by dividing the higher of the IP proton conductivity and the TP proton conductivity by the lower thereof. For example, when the IP proton conductivity is less than the TP proton conductivity, the TP proton conductivity can be divided by the IP proton conductivity to obtain the ratio. On the other hand, when the TP proton conductivity is less than the IP proton conductivity, the IP proton conductivity can be divided by the TP proton conductivity to obtain the ratio.

[0077] If the ratio of the IP proton conductivity to the TP proton conductivity is greater than 1.5, the performance of the membrane electrode assembly may be reduced, and the amount of hydrogen permeation through the non-impregnated region may increase.

[0078] In addition, when a stacked porous carrier is manufactured by stacking porous carriers, the porous carriers are not bonded to each other using an adhesive, and the porous carriers are not bonded to each other by thermal compression. If the stacked porous carrier includes an adhesive layer or is formed by thermal compression, the proton conductivity is reduced, thereby reducing the performance. Therefore, when manufacturing a stacked porous carrier, one of the porous carriers is added to another porous carrier while wetting each of the multiple porous carriers with a solution containing an ion conductor, so that the interface where the ion conductors are joined to each other is located in any one of the porous carriers, and thus the bonding strength is improved. Therefore, one of the porous carriers can be added to another porous carrier with high bonding strength without causing the problem of performance degradation that may otherwise occur due to the additional bonding layer.

[0079] Therefore, the ratio of the tensile strength in the machine direction (MD) of the polymer electrolyte membrane to the tensile strength in the transverse direction (TD) can be 1.0 to 1.5, specifically 1.0 to 1.2. The ratio of the tensile elongation in the machine direction (MD) of the polymer electrolyte membrane to the tensile elongation in the transverse direction (TD) can be 1.0 to 1.5, specifically 1.0 to 1.2.

[0080] A 3 cm thick film can be stretched in the machine direction (MD) or transverse direction (TD) using a 1 kN load cell at a crosshead speed of 500 mm / sec. 2 The tensile strength and tensile elongation were measured by stretching the polymer electrolyte membrane in the machine direction to measure the MD tensile strength and MD tensile elongation, and by stretching the polymer electrolyte membrane in the transverse direction to measure the TD tensile strength and TD tensile elongation.

[0081] The ratio of MD tensile strength to TD tensile strength and the ratio of MD tensile elongation to TD tensile elongation can be calculated by dividing the larger of the two by the smaller of the two.

[0082] If the ratio of the MD tensile strength to the TD tensile strength and the ratio of the MD tensile elongation to the TD tensile elongation of the polymer electrolyte membrane are greater than 1.5, the mechanical durability of the polymer electrolyte membrane may not be sufficiently improved due to the anisotropy of the polymer electrolyte membrane.

[0083] As an example, the porous support may include a highly fluorinated polymer, preferably a perfluorinated polymer, that is highly resistant to thermal and chemical decomposition. For example, the porous support may be polytetrafluoroethylene (PTFE) or tetrafluoroethylene and CF2=CFC n F 2n+1 (n is a real number from 1 to 5) or CF2=CFO-(CF2CF(CF3)O) m C n F 2n+1 (m is a real number of 0 to 15, and n is a real number of 1 to 15).

[0084] PTFE is commercially available and can be suitably used as a porous support. In addition, expanded polytetrafluoroethylene (e-PTFE) having a polymer fibril microstructure or a microstructure in which nodes are connected to each other by fibrils can also be suitably used as a porous support, and a membrane having a polymer fibril microstructure without nodes can also be suitably used as a porous support.

[0085] A porous support including a perfluorinated polymer is formed by extruding a dispersed polymerized PTFE onto a belt and stretching it in the presence of a lubricant. Therefore, a porous support with higher porosity and higher strength can be manufactured. In addition, e-PTFE can be heat-treated at a temperature exceeding the melting point of PTFE (about 342°C), thereby increasing the amorphous content ratio of PTFE. The e-PTFE membrane manufactured using the above method can have micropores and porosity including various diameters. The e-PTFE membrane manufactured using the above method can have a porosity of at least 35%, and the diameter of each micropore can be about 0.01 μm to 1 μm. In addition, the thickness of the porous support including a perfluorinated polymer can be changed differently. As an example, the thickness of the porous support can be 2 μm to 40 μm, preferably 5 μm to 20 μm. In the case where the thickness of the porous support is less than 2 μm, the mechanical strength of the porous support may be significantly reduced. On the other hand, in the case where the thickness of the porous support is greater than 40 μm, the resistance loss of the porous support may increase, the weight of the porous support may increase, and the integrity of the porous support may deteriorate.

[0086] As another example of a porous support, the porous support may be a nonwoven web including a plurality of randomly oriented fibers.

[0087] Nonwoven webs are sheets that are interlayered but have a structure of individual fibers or filaments rather than the same structure as woven fabrics. Nonwoven webs can be manufactured using a method selected from the group consisting of carding, garneting, air-laid, wet-laid, melt-blown, spunbonded, and stitch bonding.

[0088] The fiber may comprise one or more polymer materials. Generally, any fiber-forming polymer material may be used. Specifically, hydrocarbon-based fiber-forming polymer materials may be used. For example, the fiber-forming polymer material may include, but is not limited to, polyolefins (e.g., polybutylene, polypropylene, or polyethylene); polyesters (e.g., polyethylene terephthalate or polybutylene terephthalate); polyamides (nylon 6 or nylon 6,6); polyurethanes; polybutylenes; polylactic acid; polyvinyl alcohol; polyphenylene sulfide; polysulfones; liquid crystal polymers; polyethylene-co-vinyl acetate; polyacrylonitrile; cyclic polyolefins; polyoxymethylene; polyolefin-based thermoplastic elastomers; and combinations thereof.

[0089] As another example of the porous support having a nonwoven fiber web form, the porous support may include a nanoweb in which nanofibers are integrated in the form of a nonwoven fabric including a plurality of pores.

[0090] The polymer based on hydrocarbon shows high chemical resistance and hydrophobicity, thereby preventing the polymer based on hydrocarbon from being deformed due to moisture in a high humidity environment, and the polymer based on hydrocarbon is preferably used as nanofiber. Specifically, the polymer based on hydrocarbon can be selected from the group consisting of nylon, polyimide, polyaramid, polyetherimide, polyacrylonitrile, polyaniline, polyethylene oxide, polyethylene naphthalate, polybutylene terephthalate, styrene-butadiene rubber, polystyrene, polyvinyl chloride, polyvinyl alcohol, polyvinylidene fluoride, polyethylene butene, polyurethane, polybenzoxazole, polybenzimidazole, polyamide-imide, polyethylene terephthalate, polyphenylene sulfide, polyethylene, polypropylene, its copolymer and its mixture. Wherein, it is preferred to use the polyimide showing higher heat resistance, chemical resistance and shape stability.

[0091] Nanonet is the aggregate of nanofiber, and the nanofiber manufactured by electrospinning is randomly arranged. At this time, considering the porosity and thickness of nanonet, when using scanning electron microscope (JSM6700F, JEOL) to measure the diameter of 50 fibers and calculate the mean value of fiber diameter, preferably nanofiber has an average diameter of 40nm to 5000nm. In the case where the average diameter of nanofiber is less than 40nm, the mechanical strength of porous support may be reduced. On the other hand, in the case where the average diameter of nanofiber is greater than 5000nm, the porosity of porous support may be significantly reduced, and the thickness of porous support may increase.

[0092] The thickness of the nonwoven web may be 3 μm to 50 μm, specifically 3 μm to 20 μm. When the thickness of the nonwoven web is less than 3 μm, the mechanical strength of the nonwoven web may be reduced. On the other hand, when the thickness of the nonwoven web is greater than 50 μm, the resistance loss of the nonwoven web may increase, the weight of the nonwoven web may increase, and the integration of the nonwoven web may deteriorate.

[0093] The basic weight of the nonwoven web can be 3 g / m 2 Up to 20g / m 2 In the range of nonwoven fiber web, the basic weight is less than 3g / m 2 In the case of the nonwoven web, visible holes are formed in the nonwoven web, and thus it may be difficult to realize the function as a porous carrier. When the basic weight of the nonwoven web is greater than 20 g / m 2 In some cases, the nonwoven web may be manufactured in the form of a paper or fabric having few or no holes formed therein.

[0094] The porosity of the porous carrier may be 45% or more, specifically 60% or more. At the same time, the porosity of the porous carrier is preferably 90% or less. In the case where the porosity of the porous carrier is greater than 90%, the shape stability of the porous carrier may deteriorate, so that subsequent processes may not be carried out smoothly. The porosity of the porous carrier can be calculated using the following formula 6 based on the ratio of the volume of air to the total volume of the porous carrier. At this time, the total volume of the porous carrier can be calculated by manufacturing a rectangular sample and measuring the length, width, and thickness of the sample, and the volume of the air can be obtained by subtracting the volume of the polymer calculated by back-calculating its density after measuring the mass of the sample from the total volume of the porous carrier.

[0095] [Formula 6]

[0096] Porosity (%) = (volume of air in porous carrier / total volume of porous carrier) × 100

[0097] The polymer electrolyte membrane is a reinforced composite membrane type polymer electrolyte membrane in which pores in a porous support are filled with ion conductors.

[0098] The porous supports constituting the stacked porous support may be of the same type, or may be of different types.

[0099] At this time, each porous support may be an isotropic porous support having a ratio of MD tensile elongation to TD tensile elongation of 1.0 to 1.5, specifically 1.0 to 1.2.

[0100] When isotropic porous supports are stacked, the deviation in the ratio of machine direction tensile elongation to transverse direction tensile elongation and the dimensional change of the stacked porous supports can be minimized, thereby overcoming the shortcomings of porous supports manufactured using the stretching method and further improving impregnation properties and dimensional stability.

[0101] The tensile elongation is measured by stretching a porous support having a width of 1 cm and a length of 5 cm in the machine direction (MD) or transverse direction (TD) at a crosshead speed of 500 mm / sec using a 1 kN load cell. The ratio of the MD tensile elongation to the TD tensile elongation is calculated by dividing the larger of the two by the smaller.

[0102] In addition, the porous supports may be stacked in the same direction, or may be stacked in intersecting directions. For example, each of the porous supports may be stretched in either the machine direction (MD) or the transverse direction (TD) to have directionality, and the porous supports may be stacked so that the directions in which the porous supports are stretched intersect each other perpendicularly.

[0103] Figure 1 is an exploded perspective view showing a state where porous supports are stacked in intersecting directions, Figure 2 yes Figure 1 Coupling perspective view. Figure 1 and Figure 2 , the first porous support 11 has been stretched in direction A, and the second porous support 12 has been stretched in direction B. At this time, the stacked porous support 10 is configured such that the first porous support 11 and the second porous support 12 are stacked in such a manner that direction A and direction B perpendicularly intersect each other.

[0104] In addition, each of the porous supports may have higher mechanical properties such as tensile strength and tensile elongation in any one of the machine direction and the transverse direction, and the porous supports may be stacked such that directions in which their mechanical properties are higher perpendicularly intersect each other.

[0105] As described above, in the case where the porous supports are stacked in the intersecting directions, even if the above-mentioned isotropic porous supports are not used, the deviation of the ratio of the tensile elongation in the machine direction to the tensile elongation in the transverse direction of the stacked porous supports and the dimensional change can be minimized, thereby overcoming the disadvantages of the porous supports manufactured using the stretching method and further improving the impregnation property and dimensional stability. More specifically, although the ratio of the tensile elongation in MD to the tensile elongation in TD of each porous support stacked in the intersecting directions may be greater than 1.5, as a result of the intersecting stacking, the ratio of the tensile elongation in MD to the tensile elongation in TD of the stacked porous supports may be 1.0 to 1.5.

[0106] Figure 3 is a cross-sectional view schematically showing an example of a polymer electrolyte membrane. Figure 3 The stacked porous carrier 10 includes a first porous carrier 11 and a second porous carrier 12, wherein the first pores of the first porous carrier 11 are filled with the first ion conductor 20, and the third pores of the second porous carrier 12 are filled with the second ion conductor 30. In addition, the first ion conductor layer 21 is located on the outer surface of the first porous carrier 11, and the second ion conductor layer 13 is located on the outer surface of the second porous carrier 12.

[0107] The interface at which the first ion conductor 20 and the second ion conductor 30 are bonded to each other may be located in any one of the porous supports 11 and 12. Figure 3 , the interface where the first ion conductor 20 and the second ion conductor 30 are bonded to each other is shown to be located in the second porous support 12. That is, the second porous support 12 has at least one second pore filled with the first ion conductor 20.

[0108] The polymer electrolyte membrane according to the present disclosure has improved bonding strength between porous supports because, at the time of manufacturing, one porous support is added on another porous support while the one porous support is wetted with a solution containing an ion conductor, whereby the ion conductor can penetrate into the other porous support.

[0109] In addition, according to the present disclosure, the polymer electrolyte membrane does not include an ion conductor layer between the stacked porous supports.

[0110] That is, the polymer electrolyte membrane includes a stacked porous support manufactured by adding one porous support to another porous support while the porous support has been wetted with a solution containing an ion conductor. Therefore, the polymer electrolyte membrane according to the present disclosure is different from a stacked polymer electrolyte membrane manufactured by respectively wetting porous supports with solutions containing ion conductors, drying them respectively to manufacture a plurality of polymer electrolyte membranes, and then stacking them in that an ion conductor layer is not included between the stacked porous supports.

[0111] That is, in the stacked polymer electrolyte membrane, when stacking the polymer electrolyte membrane, the first ion conductor layer formed on the surface of the first porous support and the second ion conductor layer formed on the surface of the second porous support are brought into contact with each other and laminated, thereby forming a thick ion conductor layer between the porous supports. On the other hand, in the case of the polymer electrolyte membrane according to the present disclosure, the porous supports are in direct contact with each other.

[0112] Therefore, the impregnation of the polymer electrolyte membrane according to the present disclosure can be improved, thereby successfully forming a water channel along which protons can move in the through-plane direction of the laminated porous support, and thus the performance of the polymer electrolyte membrane can be improved. In addition, the flow channel along which hydrogen can move may be complicated, thereby the resistance may increase when hydrogen moves, and thus the hydrogen permeability may decrease. However, in the case of a laminated polymer electrolyte membrane, the flow channel along which hydrogen can move is not complicated, thereby not obtaining the effect of reducing hydrogen permeability due to increased resistance when hydrogen moves.

[0113] Each of the first ion conductor and the second ion conductor may independently be a cation conductor having a cation exchange group capable of transferring cations such as protons, or an anion conductor having an anion exchange group capable of transferring anions such as hydroxide ions, carbonates, or bicarbonates.

[0114] The cation exchange group may be any one selected from the group consisting of sulfonic acid group, carboxyl group, boric acid group, phosphoric acid group, imide group, sulfonimide group, sulfonamide group, sulfonic acid fluoride group and a combination thereof. Typically, the cation exchange group may be a sulfonic acid group or a carboxyl group.

[0115] The cation conductor may be: a fluorine-based polymer having a cation exchange group and including fluorine in its main chain; a hydrocarbon-based polymer such as benzimidazole, polyamide, polyamideimide, polyimide, polyacetal, polyethylene, polypropylene, acrylic resin, polyester, polysulfone, polyether, polyetherimide, polyester, polyethersulfone, polyetherimide, polycarbonate, polystyrene, polyphenylene sulfide, polyetheretherketone, polyetherketone, polyaryl ether sulfone, polyphosphazene or polyphenylquinoxaline; a partially fluorinated polymer such as polystyrene-graft-ethylene tetrafluoroethylene copolymer or polystyrene-graft-polytetrafluoroethylene copolymer; or sulfonimide.

[0116] More specifically, in the case where the cation conductor is a proton conductor, each of the polymers may include, in a side chain thereof, a cation exchange group selected from the group consisting of a sulfonic acid group, a carboxylic acid group, a phosphoric acid group, a phosphonic acid group, and derivatives thereof. As specific examples, the cationic conductor may be, but is not limited to, fluorine-based polymers including poly(perfluorosulfonic acid), poly(perfluorocarboxylic acid), copolymers of tetrafluoroethylene and fluorovinyl ether containing a sulfonic acid group, defluorinated polyetherketone sulfide, and mixtures thereof; or hydrocarbon-based polymers including sulfonated polyimide (S-PI), sulfonated polyarylethersulfone (S-PAES), sulfonated polyetheretherketone (SPEEK), sulfonated polybenzimidazole (SPBI), sulfonated polysulfone (S-PSU), sulfonated polystyrene (S-PS), sulfonated polyphosphazene, sulfonated polyquinoxaline, sulfonated polyketone, sulfonated polyphenylene oxide, sulfonated polyethersulfone, sulfonated polyetherketone, sulfonated polyphenylenesulfone, sulfonated polyphenylene sulfide, sulfonated polyphenylene sulfide sulfonate sulfonated polyphenylene sulfide The invention relates to sulfonated polyarylene ether nitrile, sulfonated polyarylene ether nitrile, sulfonated polyarylene ether ether nitrile, sulfonated polyarylene ether ether nitrile, sulfonated polyarylene ether sulfone ketone and mixtures thereof.

[0117] Anion conductors are polymers capable of transporting anions such as hydroxide ions, carbonate or bicarbonate. Anion conductors are commercially available in the form of hydroxides or halides (usually chlorides) and can be used in industrial water purification, metal separation or catalyst processes.

[0118] Polymers doped with metal hydroxides can generally be used as anion conductors. Specifically, poly(ether sulfone), polystyrene, vinyl polymers, poly(vinyl chloride), poly(vinylidene fluoride), poly(tetrafluoroethylene), poly(benzimidazole) or poly(ethylene glycol) doped with metal hydroxides can be used as anion conductors.

[0119] Meanwhile, any one selected from the group consisting of the laminated porous support, the first ion conductor layer, and the second ion conductor layer may further contain an antioxidant.

[0120] Since the reduction reaction of oxygen on the cathode of the polymer electrolyte membrane fuel cell is performed by hydrogen peroxide (H2O2), hydrogen peroxide may be generated on the cathode, or hydroxyl radicals (OH - ). In addition, at the anode of the polymer electrolyte membrane fuel cell, hydrogen peroxide or hydroxyl radicals may also be generated at the anode as oxygen molecules permeate the polymer electrolyte membrane. The generated hydrogen peroxide or hydroxyl radicals degrade the polymer containing sulfonic acid groups contained in the polymer electrolyte membrane or the catalyst electrode.

[0121] Therefore, an antioxidant capable of decomposing peroxides or free radicals may be included to suppress the generation of free radicals from peroxides or free radicals generated by decomposition, thereby preventing degradation of the polymer electrolyte membrane or the catalyst electrode, thereby improving the chemical durability of the polymer electrolyte membrane.

[0122] The type of antioxidant capable of decomposing peroxides or free radicals is not particularly limited, and any type of antioxidant can be used in the present disclosure, as long as it can rapidly decompose peroxides (specifically, hydrogen peroxide) or free radicals (specifically, hydroxyl radicals) generated during the operation of the polymer electrolyte membrane fuel cell. Specifically, for example, the antioxidant capable of decomposing peroxides or free radicals can be configured in the form of a transition metal capable of decomposing peroxides or free radicals, a noble metal capable of decomposing peroxides or free radicals, an ion thereof, a salt thereof, or an oxide thereof.

[0123] Specifically, the transition metal capable of decomposing peroxides or free radicals can be any one selected from the group consisting of cerium (Ce), nickel (Ni), tungsten (W), cobalt (Co), chromium (Cr), zirconium (Zr), yttrium (Y), manganese (Mn), iron (Fe), titanium (Ti), vanadium (V), molybdenum (Mo), lanthanum (La) and neodymium (Nd).

[0124] Furthermore, the noble metal capable of decomposing peroxides or radicals may be any one selected from the group consisting of silver (Au), platinum (Pt), ruthenium (Ru), palladium (Pd), and rhodium (Rh).

[0125] In addition, the ions of the transition metal or noble metal capable of decomposing peroxides or free radicals may be any one selected from the group consisting of cerium ions, nickel ions, tungsten ions, cobalt ions, chromium ions, zirconium ions, yttrium ions, manganese ions, iron ions, titanium ions, vanadium ions, platinum ions, lanthanum ions, neodymium ions, silver ions, platinum ions, ruthenium ions, palladium ions and rhodium ions. Specifically, in the case of cerium, trivalent cerium ions (Ce 3+ ) or tetravalent cerium ion (Ce 4+ ).

[0126] In addition, the oxide of a transition metal or a noble metal capable of decomposing peroxides or free radicals may be any one selected from the group consisting of cerium oxide, nickel oxide, tungsten oxide, cobalt oxide, chromium oxide, zirconium oxide, yttrium oxide, manganese oxide, iron oxide, titanium oxide, vanadium oxide, molybdenum oxide, lanthanum oxide and neodymium oxide.

[0127] In addition, the transition metal or noble metal salt capable of decomposing peroxide or free radical can be any one selected from the group consisting of carbonate, acetate, chloride salt, fluoride salt, sulfate, phosphate, tungstate, hydrate, ammonium acetate, ammonium sulfate and acetylacetonate of the transition metal or noble metal. Specifically, in the case of cerium, cerium carbonate, cerium acetate, cerium chloride, cerium nitrate, cerium sulfate, ammonium cerium (II) nitrate or ammonium cerium (IV) sulfate can be used, and cerium acetylacetonate can be used as an organic metal complex salt.

[0128] Meanwhile, in order to prevent elution of the antioxidant during operation of the fuel cell, an organic-based second antioxidant capable of fixing the antioxidant may be included.

[0129] The organic-based second antioxidant may be a compound including a resonance structure based on a double bond of carboxylic acid, hydroxyl group and carbon. The organic-based second antioxidant having such a structure has a molecular size larger than the ion clusters and channels in the polymer electrolyte membrane, thereby preventing elution due to the molecular size that cannot use the elution path and by hydrogen bonding between a large amount of carboxylic acid and hydroxyl groups contained in the organic-based second antioxidant and the polymer in the polymer electrolyte membrane.

[0130] Specific examples of the organic-based second antioxidant may be any one selected from the group consisting of syringic acid, vanillic acid, protocatechuic acid, coumaric acid, caffeic acid, ferulic acid, chlorogenic acid, cynarine, gallic acid, and a mixture thereof.

[0131] In the case where the antioxidant includes both the first antioxidant and the second antioxidant, the second antioxidant may be included in an amount of 0 to 200 parts by weight, specifically 30 to 100 parts by weight, based on 100 parts by weight of the first antioxidant. In the case where the content of the second antioxidant is less than 30 parts by weight, it is possible to achieve an anti-oxidation similar to that of the case where only the first antioxidant is used, thereby making it difficult to obtain the effect of introducing the second antioxidant. In the case where the content of the second antioxidant is greater than 200 parts by weight, the dispersibility of the polymer in the polymer electrolyte membrane may deteriorate, thereby reducing the uniformity of the entire polymer electrolyte membrane.

[0132] A method for manufacturing a polymer electrolyte membrane according to another embodiment of the present disclosure includes: a step of casting a first mixed solution containing a first ion conductor; a step of placing a first porous carrier in a dry state on the first mixed solution so that the first porous carrier is completely in a wet state; a step of adding a second porous carrier in a dry state to the first porous carrier immediately after the first porous carrier is completely in a wet state so that the first carrier and the second carrier are in contact with each other; a step of applying a second mixed solution containing a second ion conductor to the second porous carrier so that the second porous carrier is completely in a wet state; and a step of drying the first porous carrier and the second porous carrier in a wet state.

[0133] The step of applying the second mixed solution containing the second ion conductor to the second porous support so that the second porous support is completely in a wet state can be performed by: (i) if the first ion conductor and the second ion conductor are the same, adding the second porous support to the first porous support, and then immersing or dipping the first porous support and the second porous support in or with the second mixed solution, or (ii) coating the exposed surface of the second porous support with the second mixed solution. The coating with the second mixed solution can be performed by rod coating, comma coating, slot die coating, screen printing, spray coating, doctor blade coating or lamination.

[0134] The first mixed solution / the second mixed solution may be a solution or a dispersion containing the first ion conductor / the second ion conductor. Meanwhile, an antioxidant may be further added to the first mixed solution and / or the second mixed solution. The description of the antioxidant is the same as the above description, so its repeated description will be omitted.

[0135] The solvent or dispersion medium used to prepare the first mixed liquid and the second mixed liquid may be water, a hydrophilic solvent, an organic solvent, or a mixture of two or more thereof.

[0136] The hydrophilic solvent may have at least one functional group selected from the group consisting of alcohol, isopropanol, ketone, aldehyde, carbonate, carboxylate, carboxylic acid, ether and amide, each of which includes as its main chain a linear or branched saturated or unsaturated hydrocarbon having a carbon number of 1 to 12. Each of which may include an alicyclic or aromatic cyclic compound as at least a part of its main chain.

[0137] The organic solvent may be selected from N-methylpyrrolidone, dimethyl sulfoxide, tetrahydrofuran and mixtures thereof.

[0138] Meanwhile, the step of filling the pores in the stacked porous carrier with the first ion conductor or the second ion conductor may be affected by various factors such as temperature and time. For example, the filling step may be affected by the thickness of the stacked porous carrier, the concentration of the mixed solution containing the first ion conductor or the second ion conductor, and the type of solvent / dispersion medium. However, the process can be carried out at a temperature equal to or higher than the freezing point of the solvent / dispersion medium and equal to or less than 100°C. More generally, the process can be carried out at a temperature of room temperature (20°C) to 70°C for about 5 to 30 minutes. Here, the above temperature must be lower than the melting point of each porous carrier.

[0139] Finally, in the step of drying the first porous support and the second porous support to which the first porous support is added, primary drying may be performed at 60°C to 150°C for 15 minutes to 1 hour, and then secondary drying may be performed at 150°C to 190°C for 3 minutes to 1 hour. Specifically, the primary drying may be performed at 60°C to 120°C for 15 minutes to 1 hour, and the secondary drying may be performed at 170°C to 190°C for 3 minutes to 1 hour. If the primary drying is performed at a temperature below 60°C for less than 15 minutes, the solvent may not be discharged first, so that the porous support may not have the form of a high-density membrane. If the secondary drying is performed at a temperature above 190°C for more than 1 hour, the sulfonic acid group may decompose, so that the performance of the membrane may be reduced.

[0140] According to another embodiment of the present disclosure, a membrane electrode assembly and a fuel cell including the membrane electrode assembly are provided.

[0141] Specifically, the membrane electrode assembly includes an anode and a cathode disposed opposite to each other and a polymer electrolyte membrane located between the anode and the cathode. Except for using the polymer electrolyte membrane according to the present disclosure as the polymer electrolyte membrane, the membrane electrode assembly is the same as a general membrane electrode assembly for a fuel cell, so its detailed description will be omitted in this specification.

[0142] In addition, the fuel cell is the same as a general fuel cell except that it includes the membrane electrode assembly, and therefore, a detailed description thereof will be omitted in this specification.

[0143] Hereinafter, examples of the present disclosure will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily implement the examples of the present disclosure. However, the present disclosure can be implemented in various different forms and is not limited to the examples described herein.

[0144] [Manufacturing Example 1: Manufacture of polymer electrolyte membrane]

[0145] (Example 1)

[0146] The first porous support (e-PTFE, pore size: 0.10 μm to 0.15 μm, thickness: 6 μm, ratio of MD tensile elongation to TD tensile elongation: 1.1) was wetted in a first ion conductor dispersion (the first ion conductor dispersion contained 20 wt% of a highly fluorinated polymer with an equivalent weight (EW) of 800 g / eq).

[0147] When the first porous support had been wetted, a second porous support (e-PTFE, pore size: 0.10 μm to 0.15 μm, thickness: 6 μm, ratio of MD tensile elongation to TD tensile elongation: 1.1) was added on the first porous support.

[0148] While the second porous support was placed on the first porous support, a second ion conductor dispersion containing 20 wt% of a highly fluorinated polymer having an equivalent weight (EW) of 800 g / eq was additionally applied to the second porous support.

[0149] Subsequently, the first porous support and the second porous support were dried at 60° C. for 1 hour and then dried at 150° C. for 30 minutes to manufacture a polymer electrolyte membrane.

[0150] (Example 2)

[0151] The first porous support (e-PTFE, pore size: 0.10 μm to 0.15 μm, thickness: 6 μm, ratio of MD tensile elongation to TD tensile elongation: 1.2) was wetted in a first ion conductor dispersion containing 20 wt% of a highly fluorinated polymer having an equivalent weight (EW) of 800 g / eq.

[0152] When the first porous support was wetted, a second porous support (e-PTFE, pore size: 0.10 μm to 0.15 μm, thickness: 6 μm, ratio of MD tensile elongation to TD tensile elongation: 1.2) was added to the first porous support. At this time, the first e-PTFE support and the second e-PTFE support were stacked so that the direction in which the first e-PTFE support was stretched and the direction in which the second e-PTFE support was stretched were perpendicular to each other.

[0153] While the second porous support was placed on the first porous support, a second ion conductor dispersion containing 20 wt % of a highly fluorinated polymer having an equivalent weight (EW) of 800 g / eq was additionally applied to the second porous support.

[0154] Subsequently, the first porous support and the second porous support were dried at 60° C. for 1 hour and then dried at 150° C. for 30 minutes to manufacture a polymer electrolyte membrane.

[0155] (Comparative Example 1)

[0156] Two porous supports (e-PTFE, pore size: 0.10 μm to 0.15 μm, thickness: 6 μm, ratio of MD tensile elongation to TD tensile elongation: 1.1) were impregnated with an ion conductor dispersion containing 20 wt% of a highly fluorinated polymer having an equivalent weight (EW) of 800 g / eq. Subsequently, the two porous supports were dried at 60°C for 1 hour and then at 120°C for 30 minutes to produce two polymer electrolyte membranes.

[0157] The two manufactured polymer electrolyte membranes were heat-pressed under the conditions of 160° C. and 1.2 tons to manufacture a laminated polymer electrolyte membrane.

[0158] (Comparative Example 2)

[0159] A polytetrafluoroethylene adhesive was applied between two porous supports (e-PTFE, pore size: 0.10 μm to 0.15 μm, thickness: 6 μm, ratio of MD tensile elongation to TD tensile elongation: 1.1), and then the two porous supports were heated and pressed at a temperature of 340°C and a pressure of 0.27 MPA for 30 seconds so that the two porous supports were bonded to each other to produce a bonded porous support.

[0160] The manufactured bonded porous support was impregnated with an ion conductor dispersion containing 20 wt % of a highly fluorinated polymer having an equivalent weight (EW) of 800 g / eq. Subsequently, the bonded porous support was dried at 60° C. for 1 hour and then at 150° C. for 30 minutes to manufacture a polymer electrolyte membrane.

[0161] (Comparative Example 3)

[0162] The porous support (e-PTFE, pore size: 0.10 μm to 0.15 μm, thickness: 15 μm, MD tensile elongation to TD tensile elongation ratio: 1.5) was impregnated with a highly fluorinated ion conductor dispersion containing 20 wt % of an equivalent weight (EW) of 800 g / eq. Subsequently, the porous support was dried at 60° C. for 1 hour and then at 150° C. for 30 minutes to produce a polymer electrolyte membrane.

[0163] [Experimental Example 1: Measurement of Characteristics of Produced Polymer Electrolyte Membrane]

[0164] Scanning electron microscope photographs of the polymer electrolyte membranes manufactured according to Example 1 and Comparative Example 1 are shown in Figure 4 and Figure 5 middle.

[0165] Reference Figure 4 , it can be seen that the polymer electrolyte membrane manufactured according to Example 1 is well bonded to such an extent that not only the interface between the first ion conductor and the second ion conductor but also the interface between the first porous support and the second porous support is not visible.

[0166] Furthermore, it can be seen that the first porous support and the second porous support are in contact with each other, and there is no layer consisting only of an ion conductor between them.

[0167] On the other hand, refer to Figure 5 In the case of the polymer electrolyte membrane manufactured according to Comparative Example 1, a layer composed only of an ion conductor existed between the first porous support and the second porous support, and the thickness of the layer was 2 μm.

[0168] [Experimental Example 2: Measurement of Physical Properties of Produced Polymer Electrolyte Membrane]

[0169] The IP proton conductivity, TP proton conductivity, swelling ratio, tensile strength, and tensile elongation of each of the polymer electrolyte membranes manufactured according to the Examples and Comparative Examples were measured, and the results are shown in Table 1 below.

[0170] The IP proton conductivity can be calculated using the membrane resistance at a relative humidity of 50% after measuring the membrane resistance at a temperature of 80°C and a relative humidity of 30% to 95% using a magnetic suspension balance (Bell Japan). At this time, the effective area of ​​the membrane is 0.75 cm 2 .

[0171] TP proton conductivity was measured by coating opposite surfaces of the fabricated polymer electrolyte membrane with Pt catalyst ink, placing and fastening a gas diffusion layer (GDL) thereon, measuring the membrane resistance at a temperature of 80°C and a relative humidity (RH) of 50%, and dividing the measured membrane resistance by the thickness of the polymer electrolyte membrane.

[0172] Regarding the swelling ratio, the manufactured polymer electrolyte membrane was immersed in distilled water at room temperature for 12 hours, the polymer electrolyte membrane in a wet state was taken out from the distilled water, and the thickness, machine direction (MD) length, and transverse direction (TD) length of the wet polymer electrolyte membrane were measured, the polymer electrolyte membrane was dried at 50° C. for 24 hours in a vacuum state, the thickness, machine direction (MD) length, and transverse direction (TD) length of the dried polymer electrolyte membrane were measured, and the thickness T of the polymer electrolyte membrane in a wet state was measured. 湿润 and length L 湿润 and the thickness T of the polymer electrolyte membrane in the dry state 干燥 and length L 干燥 Substitute into the above formula 1 and formula 2 to calculate the thickness swelling ratio and length swelling ratio.

[0173] The sample was stretched in the machine direction (MD) or transverse direction (TD) with a 3 cm diameter by using a 1 kN load cell at a crosshead speed of 500 mm / sec. 2 The tensile strength and elongation of the polymer electrolyte membrane were measured.

[0174] [Table 1]

[0175]

[0176] Referring to Table 1 above, it can be seen that in the case of the polymer electrolyte membrane manufactured according to each example, the surface area of ​​the porous support in direct contact with the ion conductor increases when the porous support is impregnated with the ion conductor, thereby improving the wettability of the porous support due to the solution containing the ion conductor, and when the pores of the porous support are filled with the ion conductor, the air in the pores is more easily discharged therefrom, thereby minimizing the generation of micro bubbles, and thus the impregnation is improved. Therefore, it can be seen that the ratio of IP proton conductivity to TP proton conductivity is close to 1.

[0177] In addition, in the case of the polymer electrolyte membrane manufactured according to each example, since the laminated porous support is included, the area capable of buffering the dimensional change increases, and thus the dimensional stability is also improved. In addition, when the change in dimensional stability is observed, it can be seen that there is no substantial difference in MD / TD change, that is, the polymer electrolyte membrane is isotropic.

Claims

1. A polymer electrolyte membrane comprising: a first porous support having first pores filled with a first ion conductor; as well as a second porous support having at least one second pore filled with the first ion conductor and third pores filled with a second ion conductor, such that an interface between the first ion conductor and the second ion conductor is located in the second porous support, wherein The first porous support and the second porous support are in contact with each other, and After the polymer electrolyte membrane is immersed in distilled water at room temperature for 12 hours and then dried at 50° C. under vacuum for 24 hours, each of the MD swelling ratio and the TD swelling ratio of the polymer electrolyte membrane calculated by the following Formulas 1 and 2 is 2% or less, [Formula 1] △L(MD)=[(L 湿润 (MD)–L 干燥 (MD)) / L 干燥 (MD)]×100 [Formula 2] △L(TD)=[(L 湿润 (TD)–L 干燥 (TD)) / L 干燥 (TD)]×100 Among them, △L(MD) is the MD swelling ratio, △L(TD) is the TD swelling ratio, L 湿润 (MD) and L 湿润 (TD) are the MD length and TD length measured just before drying, L 干燥 (MD) and L 干燥 (TD) are MD length and TD length measured immediately after drying, respectively.

2. The polymer electrolyte membrane according to claim 1, wherein All pores of the first porous support are filled with the first ion conductor.

3. The polymer electrolyte membrane according to claim 1, wherein Each of the first porous carrier and the second porous carrier is an isotropic porous carrier, and the isotropic porous carrier is configured so that the tensile elongation in the machine direction and the tensile elongation in the transverse direction are equal to each other, or the higher of the tensile elongation in the machine direction and the tensile elongation in the transverse direction is less than 1.5 times the lower of the tensile elongation in the machine direction and the tensile elongation in the transverse direction, the machine direction is MD, and the transverse direction is TD.

4. The polymer electrolyte membrane according to claim 1, wherein The first porous support and the second porous support are stacked such that directions in which the first porous support and the second porous support are stretched are perpendicular to each other.

5. The polymer electrolyte membrane according to claim 1, wherein At a temperature of 80° C. and a relative humidity of 50%, the polymer electrolyte membrane has an in-plane proton conductivity of 0.046 S / cm to 0.1 S / cm and a through-plane proton conductivity of 0.042 S / cm to 0.1 S / cm, wherein the relative humidity is RH, the in-plane proton conductivity is IP proton conductivity, and the through-plane proton conductivity is TP proton conductivity.

6. The polymer electrolyte membrane according to claim 5, wherein The TP proton conductivity and the IP proton conductivity of the polymer electrolyte membrane are equal to each other, or the higher of the TP proton conductivity and the IP proton conductivity is 1.5 times or less the lower of the TP proton conductivity and the IP proton conductivity.

7. The polymer electrolyte membrane according to claim 1, wherein The TD swelling ratio and the MD swelling ratio are equal to each other, or a higher one of the TD swelling ratio and the MD swelling ratio is 1.5 times or less a lower one of the TD swelling ratio and the MD swelling ratio.

8. The polymer electrolyte membrane according to claim 1, wherein The polymer electrolyte membrane has a 7×10 -5 cm 2 / sec or less, the relative humidity is RH.

9. The polymer electrolyte membrane according to claim 1, wherein The MD tensile strength and the TD tensile strength of the polymer electrolyte membrane are equal to each other, or the higher of the MD tensile strength and the TD tensile strength is 1.5 times or less the lower of the MD tensile strength and the TD tensile strength.

10. The polymer electrolyte membrane according to claim 1, wherein The polymer electrolyte membrane has an MD tensile elongation and a TD tensile elongation that are equal to each other, or a higher one of the MD tensile elongation and the TD tensile elongation is 1.5 times or less a lower one of the MD tensile elongation and the TD tensile elongation.

11. A method for manufacturing a polymer electrolyte membrane, the method comprising: Casting a first mixed solution including a first ion conductor; Placing a first porous carrier in a dry state on the first mixed liquid so that the first porous carrier is completely wetted; Immediately after the first porous carrier is completely in the wet state by the first mixed liquid, a second porous carrier in a dry state whose pores are not filled with any ion conductor is added to the first porous carrier, so that the first porous carrier and the second porous carrier are in contact with each other; applying a second mixed solution containing a second ion conductor to the second porous support so that the second porous support is completely wetted; as well as The first porous support and the second porous support in a wet state are dried so that an interface between the first ion conductor and the second ion conductor appears in the second porous support.

12. A membrane electrode assembly comprising: an anode and a cathode disposed opposite to each other; as well as The polymer electrolyte membrane according to claim 1, wherein the polymer electrolyte membrane is located between the anode and the cathode.

13. A fuel cell comprising the membrane electrode assembly according to claim 12.