Packaging material for organic electronic device and method for producing the same

Through the mechanical cutting process and the use of polyolefin adhesive resin, the problems of thermal deformation and offset in the laser cutting process are solved, the production efficiency and reliability of organic electronic device packaging materials are improved, and the service life is extended.

CN112349863BActive Publication Date: 2024-10-18INNOX ADVANCED MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202010788806.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-07
Publication Date
2024-10-18
Estimated Expiration
2040-08-07

AI Technical Summary

Technical Problem

Organic electronic device packaging materials manufactured by existing laser cutting processes have problems with thermal deformation, residue, burrs, and offset areas, resulting in long production times and shortened service life.

Method used

Mechanical cutting is used to manufacture packaging materials. Through the slitting and shearing technology of composite sheets, the cone angle and cone length of the cutting surface are controlled. A combination of polyolefin adhesive resin and metal layer is used to optimize the packaging resin layer and release layer. The structure reduces the initial peeling force and height deviation.

Benefits of technology

The production time is shortened by 30% to 50%, the bosses and burrs of the release layer are reduced, the reliability and service life of the packaging material are improved, and the initial peeling force and height deviation are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112349863B_ABST
    Figure CN112349863B_ABST
Patent Text Reader

Abstract

The present invention relates to an encapsulating material for an organic electronic device and a method for manufacturing the same, and more specifically, to an encapsulating material for an organic electronic device and a method for manufacturing the same that can solve the problems existing in the encapsulating material for an organic electronic device manufactured by conventional laser cutting and can be manufactured by introducing a mechanical cutting method that improves productivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an encapsulating material for an organic electronic device, which can solve the problems existing in an encapsulating material for an organic electronic device manufactured by conventional laser cutting and is manufactured by introducing a mechanical cutting method to improve productivity, and a method for manufacturing the same. Background Art

[0002] Organic light emitting diode (OLED) is a light emitting diode whose light emitting layer is composed of thin film organic compounds. It uses the phenomenon of electroluminescence, that is, it emits light by introducing current into fluorescent organic compounds. Usually, this organic light emitting diode realizes the main color through three-color (red, green, blue) independent pixel method, image conversion method (CCM), color filtering method, etc. Low molecular organic light emitting diode and high molecular organic light emitting diode are distinguished according to the amount of organic substance contained in the light emitting material used. In addition, passive driving method and active driving method can be distinguished according to the driving method.

[0003] Such organic light emitting diodes have the following advantages: they can display high-quality images by high efficiency of self-luminescence, low voltage driving, simple driving, etc. Moreover, they can be applied to flexible displays and organic electronic devices by utilizing the flexibility of organic materials.

[0004] Organic light-emitting diodes are manufactured by stacking organic compounds as light-emitting layers on a substrate in the form of a thin film. However, since the organic compounds used in organic light-emitting diodes are very sensitive to impurities, oxygen, and moisture, there is a problem that the characteristics can be easily degraded by external exposure or moisture and oxygen penetration. This organic degradation phenomenon not only affects the light-emitting characteristics of organic light-emitting diodes, but also shortens their service life. In order to prevent this phenomenon, a thin film encapsulation process can be used to prevent oxygen, moisture, etc. from flowing into the interior of the organic electronic device.

[0005] Although currently a desiccant for absorbing moisture is loaded in the groove in powder form by processing a metal can or glass into a lid shape with grooves, it is difficult for this method to simultaneously have the following advantages, namely, to remove moisture at a level for the purpose of moisture permeability through the encapsulated organic electronic device, to prevent moisture, impurities and other undesirable substances from entering the organic electronic device, to prevent interlayer delamination when removing moisture, and to produce excellent moisture resistance and heat resistance.

[0006] Furthermore, when manufacturing conventional encapsulation materials for organic electronic devices, carbon dioxide (CO 2) After the encapsulation resin layer and the release layer are cut for the first time by a laser cutting method, a fiber laser is used to cut the metal layer for the second time to manufacture the encapsulation material. However, this existing laser cutting method is complicated and changeable in the production process, so it takes a long production time, and a thermal deformation area will appear between the encapsulation resin layer and the release layer (a boss is formed on the upper part of the release layer, and residues are generated on the cut surfaces of the encapsulation resin layer and the release layer), which makes it difficult to remove the release layer. Burrs are generated on the cut section, and an off-set area is generated during the second cutting. Therefore, the service life of the organic electronic device will be shortened by the size of the off-set area.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent document 1: Korean Patent Publication No. 2006-0030718 (publication date: April 11, 2006);

[0010] Patent document 2: Japanese Patent Publication No. 2016-24240 (publication date: February 8, 2016). Summary of the invention

[0011] Problems to be solved by the invention

[0012] An object of the present invention to solve the above-mentioned problems is to provide a packaging material manufacturing method and a packaging material manufactured by the same, so as to improve the problems existing in the packaging material manufactured by the conventional laser process.

[0013] Solutions for solving problems

[0014] In order to solve the above problems, the encapsulation material for an organic electronic device according to the present invention comprises a composite sheet, wherein the composite sheet comprises a metal layer, an encapsulation resin layer and a release layer, and the composite sheet is a sheet having cut surfaces formed at a plurality of ends.

[0015] According to a preferred embodiment of the present invention, a layer having a different composition from the metal layer and the FSP may be included between the metal layer and the encapsulation resin layer, and a layer having a different composition from the encapsulation resin layer and the release layer may be included between the encapsulation resin layer and the release layer.

[0016] According to a preferred embodiment of the present invention, the taper angle of the above-mentioned cutting surface of the composite sheet including the metal layer, the encapsulation resin layer and the release layer can be 73 to 90 degrees. In this case, when observing from the side direction of the cutting surface of the tapered measurement object, the above-mentioned taper angle is the angle formed between the bottom surface end of the bottom layer of the cutting surface and the top surface end of the top layer of the cutting surface, with the bottom surface of the cutting surface as the reference.

[0017] According to a preferred embodiment of the present invention, the total thickness of the encapsulation material for an organic electronic device of the present invention can be 120 to 220 μm, and the taper length can be 60 μm or less. In this case, when observing from the side direction of the cut surface of the tapered measurement object, the taper length can be the difference in length between the bottom surface end of the bottom layer of the cut surface and the top surface end of the top layer.

[0018] According to a preferred embodiment of the present invention, the encapsulation material for an organic electronic device may be composed of a composite sheet including the metal layer and the encapsulation resin layer. In this case, the taper angle of the cut surface may be 67 to 90 degrees.

[0019] According to a preferred embodiment of the present invention, when the initial peeling force of the encapsulation material for an organic electronic device of the present invention is measured by the UTM method under the conditions that the descending speed and the ascending speed of the fixture are 1.0 mm / sec, the dwelling force is 800 gf, and the dwelling time is 10.0 sec, the initial peeling force of the release layer corner can be 200-400 gf.

[0020] According to a preferred embodiment of the present invention, in the packaging material for organic electronic devices of the present invention, the height deviation of the surface of the above-mentioned release layer calculated by the following mathematical formula 1 can be less than 4 μm. In this case, the height of the above-mentioned height deviation is the height in the vertical direction from the lower surface of the release layer at the bonding point between the packaging resin layer and the release layer to the upper surface corresponding to the lower surface of the above-mentioned release layer.

[0021] Mathematical formula 1: Height deviation = (maximum height of release layer edge - height of release layer center)

[0022] In Mathematical Formula 1, the edge of the release layer is a portion of the surface of the release layer that is 1 mm away from the cut surface along the inner direction of the release layer.

[0023] According to a preferred embodiment of the present invention, in the encapsulation material for an organic electronic device of the present invention, the cutting surface may be a cutting surface formed by slitting cutting or shearing cutting.

[0024] According to a preferred embodiment of the present invention, the composite sheet is a sheet including four ends and four cutting surfaces, the four cutting surfaces include two long-side cutting surfaces and two short-side cutting surfaces, and the two long-side cutting surfaces and the two short-side cutting surfaces can be cutting surfaces independently formed by slitting cutting or shearing cutting.

[0025] According to a preferred embodiment of the present invention, in the encapsulation material for an organic electronic device of the present invention, the taper angles of the cut surfaces may be different from each other.

[0026] According to a preferred embodiment of the present invention, the taper angles of the two long-side cutting surfaces and the two short-side cutting surfaces may be different from each other.

[0027] According to a preferred embodiment of the present invention, in the encapsulation material for an organic electronic device of the present invention, the encapsulation resin layer includes 1 to 3 pressure-reducing adhesive layers, and the pressure-reducing adhesive layers may include a polyolefin adhesive resin, a tackifier, and a moisture absorbent.

[0028] According to a preferred embodiment of the present invention, the polyolefin-based adhesive resin may include a poly(C 2 ~C 6 ) One or more of olefin resins and random copolymer resins obtained by copolymerization of ethylene, propylene and / or diene compounds.

[0029] According to a preferred embodiment of the present invention, the polyolefin-based adhesive resin may include a compound represented by the following Chemical Formula 1:

[0030] Chemical formula 1:

[0031] In the above chemical formula 1, R 1 A hydrogen atom or C 3 ~C 10 Straight chain alkenyl or C 4 ~C 10 wherein n is a rational number satisfying the weight average molecular weight of the compound represented by Chemical Formula 1 of 10,000 to 2,000,000.

[0032] According to a preferred embodiment of the present invention, the polyolefin-based adhesive resin may include a first adhesive resin and a second adhesive resin, the first adhesive resin may include a copolymer formed by copolymerization of ethylene, propylene and a diene compound, and the second adhesive resin may include a compound represented by the following Chemical Formula 1.

[0033] In a preferred embodiment of the present invention, in the encapsulation material for an organic electronic device of the present invention, the metal layer may include a metal sheet, and the metal sheet includes one or more selected from iron (Fe), bismuth (Bi), tin (Sn), indium (In), silver (Ag), copper (Cu), zinc (Zn), antimony (Sb), nickel (Ni), chromium (Cr), aluminum (Al), cobalt (Co), manganese (Mn), titanium (Ti), molybdenum (Mo), silicon (Si), magnesium (Mg), tungsten (W) and alloys thereof.

[0034] Another object of the present invention is to provide a method for manufacturing a packaging material for an organic electronic device, which can be manufactured by executing a process comprising the following steps: a first step of preparing a composite sheet comprising a metal layer, a packaging resin layer and a release layer; a second step of performing mechanical cutting such as slitting cutting or shearing cutting on both sides of the long side direction of the above-mentioned composite sheet; and a third step of performing mechanical cutting such as slitting cutting or shearing cutting on the slit composite sheet along the short side direction.

[0035] According to a preferred embodiment of the present invention, according to the manufacturing method of the present invention, the composite sheet in the first step can be manufactured by a roll laminator, and the roll laminator includes a curling roller control system having a fixed roller, a supporting curling roller, a first curling roller, a second curling roller, an upper end roller laminator, and a lower end roller laminator.

[0036] According to a preferred embodiment of the present invention, with the bonding point of the upper roller laminator and the lower roller laminator as a reference, the center height of the support roller of the roll-type laminator with a curling roller control system is located at a place equal to or lower than the height of the above-mentioned bonding point, the height of the center of the first curling roller and the center of the second curling roller are located at a place lower than the height of the center of the above-mentioned support roller, and when bonding, the metal sheet is supplied from the direction of the lower roller laminator, and the packaging sheet is supplied from the direction of the upper roller laminator.

[0037] According to a preferred embodiment of the present invention, in the manufacturing method of the present invention, the mechanical cutting in the second step and the third step can be performed by different mechanical cutting methods.

[0038] According to a preferred embodiment of the present invention, after the slitting is performed in the second step or the third step, a wet cleaning process may be continuously performed on the slitting long side portions of the composite sheet.

[0039] According to a preferred embodiment of the present invention, the shearing can be performed by a shearing machine, which includes an upper knife with a blade angle (slope) of 0.140 to 0.300 degrees and a lower knife with a blade angle of less than 3 degrees.

[0040] According to a preferred embodiment of the present invention, the third step may further include a process of passing the composite sheet through a dry cleaning-free process after the mechanical cutting.

[0041] Another object of the present invention is to provide an organic electronic device, comprising: a substrate; an organic electronic device formed on at least one side of the substrate; and an encapsulation material for an organic electronic device, used to encapsulate the organic electronic device.

[0042] The term "cone angle" used in this specification refers to the angle formed between the bottom surface end of the cut surface of the lower layer (or lower sheet) of the composite sheet and the top surface end of the cut surface of the upper layer (or upper sheet) of the composite sheet, with the bottom surface of the lower layer (or lower sheet) of the composite sheet as the reference, when viewed from the side direction of the cut surface of the conical measurement object (refer to Figure 7 ).

[0043] The term "comb pattern" used in this specification refers to a pattern formed in an oblique direction.

[0044] The term "cone length" used in this specification refers to the difference in length between the bottom surface end of the lower layer (or lower sheet) and the top surface end of the upper layer (or upper sheet) of the cut surface of the composite sheet when viewed from the side direction of the cut surface of the conical measurement object (refer to Figure 7 ).

[0045] Effects of the Invention

[0046] The packaging material for organic electronic devices of the present invention is manufactured by a mechanical cutting method instead of using the existing laser cutting method. Compared with laser cutting with a complex production process, the time for the cutting process can be shortened by 30% to 50%. Since the existing laser cutting has the following problems, namely, due to the thermal deformation of the cutting part, a boss is generated on the cutting surface of the release layer, and residues and burrs and offset (pff-set) areas are generated on the cutting surface. Therefore, when a large amount of packaging materials with excellent reliability and low initial peeling force are stacked for preservation (or storage), there is no space loss caused by the boss on the surface of the release layer, which is beneficial to the storage of the product and makes the dimensional tolerance of the short side smaller. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 Part (a) and part (b) of FIG. 1 are simplified cross-sectional views showing an organic electronic device encapsulation material according to a preferred embodiment of the present invention.

[0048] Figure 2 A simplified diagram showing the cutting.

[0049] Figure 3a and Figure 3b To illustrate a schematic diagram of shearing and the upper and lower knives used therefor, Figure 3c A simplified diagram is shown for explaining the cut surface of a composite sheet.

[0050] Figure 4 The figure shows the SEM measurement of the long side cut surface of the cut.

[0051] Figure 5 The figure shows SEM measurement of the cut surface sheared by the upper knife and the lower knife.

[0052] Figure 6 The figures and schematic diagrams show SEM measurements of the cut surface of the laser-cut composite sheet.

[0053] Figure 7 This is a schematic diagram showing an example of explaining the taper length and the taper angle.

[0054] Figure 8 The following is a photograph showing an apparatus for measuring the initial peeling force of the release sheet of the composite sheet carried out in Experimental Example 2 and the results of the test.

[0055] Fig. 9 The following are the results of measuring the initial peeling force of the release sheet of the composite sheet implemented in Experimental Example 2.

[0056] Figure 10a to Figure 10e The diagram shows the cut surfaces of the long sides of the slit composite sheets observed under an optical microscope with different upper blade side pressures.

[0057] Fig.11a This is a diagram showing a SEM measurement of a cut surface cut by a lower knife. Fig.11b This is a diagram showing the confirmation of the floating of PET generated in the inner direction from the end of the release sheet. DETAILED DESCRIPTION

[0058] The present invention is described in further detail below.

[0059] After the composite sheet is manufactured, the long side and the short side of the composite sheet may be cut by a mechanical cutting method to manufacture the encapsulation material for an organic electronic device of the present invention.

[0060] As a preferred example, the encapsulation material for an organic electronic device of the present invention (hereinafter referred to as "encapsulation material") is as follows: Figure 1 As shown in the schematic diagram of part (a), the composite sheet 10 may include a metal layer 14, an encapsulating resin layer 15 and a release layer 13, or the composite sheet may include a metal layer 14 and an encapsulating resin layer 15 from which the release layer is peeled off.

[0061] Furthermore, the composite sheet is a sheet having cutting surfaces formed at a plurality of ends, and preferably may include four ends. The composite sheet may be a sheet having cutting surfaces formed at each end.

[0062] Between the metal layer and the encapsulation resin layer of the above-mentioned composite sheet, there may also be a layer with a different composition from the metal layer and the encapsulation resin layer and / or a layer (or sheet) that plays a different role; between the encapsulation resin layer and the release layer, there may also be a layer with a different composition from the encapsulation resin layer and the release layer and / or a layer (or sheet) that plays a different role.

[0063] Moreover, if Figure 1 As shown in the simplified diagram of parts (a) and (b), the encapsulation resin layer may include a single-layer pressure-reducing adhesive layer or more than two layers of a multi-layer pressure-reducing adhesive layer. When the encapsulation resin layer is composed of multiple layers of pressure-reducing adhesive layers, each layer in the pressure-reducing adhesive layer may be composed of pressure-reducing adhesive components with different composition components and / or composition ratios.

[0064] According to the packaging material of the present invention, each of the above-mentioned cutting surfaces is a cutting surface formed by a mechanical cutting method, and the cone angle of each of the above-mentioned cutting surfaces can be 73 to 90 degrees, preferably, 75 to 90 degrees, and the cone angle of each cutting surface can be the same or different. Moreover, the cone length of each of the above-mentioned cutting surfaces can be less than 60 μm, preferably, less than 50 μm, and more preferably, 0 to 30 μm. Relative to the cutting surface formed by the laser cutting method, this cone angle and cone length belong to a higher cone angle and a shorter cone length, because the offset (off-set) area formed by the laser cutting method does not appear or appears with a lower probability on the cutting surface of the mechanical cutting method.

[0065] Furthermore, the packaging material for the above-mentioned organic electronic device may be composed of a composite sheet without the release layer and including a metal layer and an encapsulation resin layer. In this case, the taper angle of each cutting surface of the composite sheet can be 67 to 90 degrees, preferably 68 to 89 degrees. When the composite sheet is manufactured by using a metal layer and an encapsulation resin layer with the same thickness and composition, the composite sheet without the release layer may have a lower taper angle than the composite sheet including the release layer.

[0066] The packaging material of the present invention comprises four ends, and a cutting surface can be formed at each end, and the four cutting surfaces can all be cutting surfaces formed by the same mechanical cutting method. Moreover, the cone angles of the cutting surfaces can be different from each other.

[0067] Furthermore, when the packaging material is in the form of a sheet having long sides and short sides, it may include two long side ends and two short side ends. When a cut surface is formed in each end, the two long side cut surfaces and the two short side cut surfaces may be formed by slitting cutting or shearing cutting. In this case, the taper angles of the two long side cut surfaces and the two short side cut surfaces may be different from each other.

[0068] Comb patterns are formed on the surface of the cut surface, and the cut surface can form a linear pattern along the vertical direction.

[0069] Moreover, the cutting surface of shearing and the cutting surface of slitting can satisfy the following equation 1.

[0070] Equation 1: The average cone angle of the sheared cutting surface is ≤ the average cone angle of the cut

[0071] In Equation 1, when observing from the side direction of the cut surface of the conical measurement object, with the bottom surface of the lower layer (or lower sheet) of the cut surface as a reference, the above-mentioned cone angle is the angle formed between the end of the bottom surface of the lower layer (or lower sheet) of the cut surface and the end of the top surface of the upper layer (or upper sheet) of the cut surface.

[0072] Furthermore, the two cutting surfaces and the two shearing cutting surfaces may satisfy the following equation 2.

[0073] Equation 2: The cone angle deviation of the cutting surface of the slitting is less than the cone angle deviation of the cutting surface of the shearing.

[0074] In equation 2, the cone angle deviation of the long side cutting surface is the difference between the cone angles of the two cut cutting surfaces, and the cone angle deviation of the sheared cutting surface is the difference between the cone angles of the two sheared cutting surfaces.

[0075] In the case of a composite sheet including a metal layer, an encapsulation resin layer and a release layer, the taper angle of the cut surface of the slitting can be 83 to 90 degrees, preferably 85 to 90 degrees. In addition, in the case of a composite sheet including a metal layer and an encapsulation resin layer without the release layer, the taper angle of the cut surface of the slitting can be 80 to 90 degrees, preferably 81 to 89 degrees.

[0076] Furthermore, the taper length of the long-side cut surface is 20 μm or less, and the scrap generated by shearing of the long-side cut surface can be eliminated by a scrap winder.

[0077] Furthermore, in the case of a composite sheet including the above-mentioned metal layer, encapsulation resin layer and release layer, the sheared cutting surface may have a first cutting surface formed by the lower blade of the shearing knife and a second cutting surface formed by the upper blade of the shearing knife, and the taper angle of the above-mentioned first cutting surface is 73 to 90 degrees (or 0 to -17 degrees), and the taper angle of the above-mentioned second cutting surface may be 73 to 90 degrees. Moreover, in this case, the taper length of the above-mentioned first cutting surface may be 0 to +60 μm, preferably, 0 to +50 μm, and the taper length of the second cutting surface may be 0 to +60 μm (or 0 to -60 μm), preferably, 0 to +50 μm (or 0 to -50 μm).

[0078] Furthermore, in the case of a composite sheet including a metal layer and an encapsulation resin layer after removing the release layer, the taper angle of the first cutting surface can be 67 to 90 degrees (or 0 to -23 degrees), and the taper angle of the second cutting surface can be 68 to 88 degrees. In this case, the taper length of the first cutting surface can be 0 to +60 μm, preferably 0 to +50 μm, and the taper length of the second cutting surface can be 0 to +60 μm (or 0 to -60 μm), preferably 0 to +50 μm (or 0 to -50 μm).

[0079] To give a preferred example, in order to process the composite sheet 10 including the metal layer 14, the encapsulation resin layer 15 and the release layer 13 into an appropriate size, when mechanical cutting is performed, the long side direction (length direction) of the composite sheet is processed by slitting, and the short side direction can be processed by shearing. The packaging material manufactured in this way has 4 ends and 4 cutting surfaces, and the long side cutting surfaces and the short side cutting surfaces have different cutting surface surface morphologies, taper angles, and taper lengths. The first short side cutting surface formed by the lower knife of the shearing knife of the short side cutting surface and the second short side cutting surface formed by the upper knife of the shearing knife can have different taper angles and taper lengths.

[0080] Furthermore, the thickness of the metal layer may be 60 to 150 μm, preferably 70 to 120 μm, and more preferably 75 to 105 μm.

[0081] Furthermore, the thickness of the encapsulation resin layer may be 30 to 100 μm, preferably 40 to 80 μm, and more preferably 45 to 75 μm.

[0082] Moreover, the thickness of the release layer may be 15 to 75 μm, preferably 25 to 60 μm, and more preferably 35 to 55 μm.

[0083] The total thickness of the packaging material of the present invention may be 120 to 280 μm, preferably 125 to 220 μm, and more preferably 128 to 200 μm.

[0084] When the initial peeling force of the packaging material of the present invention is measured by the UTM method under the conditions of the descending speed and ascending speed of the fixture being 1.0 mm / sec, the dwelling force being 800 gf and the dwelling time being 10.0 sec, the initial peeling force of the corner of the release layer can be 200 to 400 gf, preferably, 250 to 380 gf, and more preferably, 300 to 370 gf. When compared with the initial peeling force of the packaging material manufactured by laser cutting being 500 gf or more, the initial peeling force value of this packaging material is a relatively small value, because there is a difference in the residues generated and formed on the cut surface of the release layer and the packaging resin layer in the case of laser cutting.

[0085] In the encapsulation material of the present invention, the height deviation of the release layer surface calculated by the following mathematical formula 1 is 4 μm or less, preferably 2 μm or less, and more preferably 0 to 1.5 μm, and there is almost no height deviation. The height of the height deviation is the height in the vertical direction from the lower surface of the release layer at the bonding portion between the encapsulation resin layer and the release layer to the upper surface corresponding to the lower surface of the release layer.

[0086] Mathematical formula 1: Height deviation = (maximum height of the release layer edge) - (height of the release layer center)

[0087] In Mathematical Formula 1, the edge of the release layer is a portion of the surface of the release layer that is 1 mm away from the cut surface along the inner direction of the release layer.

[0088] When compared with the packaging material manufactured by laser cutting with a higher deviation, that is, compared with the height deviation of the boss formed at the end portion of the release layer by thermal fusion, the packaging material of the present invention can have a very low height deviation or no height deviation because such a boss does not occur.

[0089] Metal layer

[0090] In the encapsulation material for an organic electronic device of the present invention, the metal layer may include one or more selected from iron (Fe), bismuth (Bi), tin (Sn), indium (In), silver (Ag), copper (Cu), zinc (Zn), antimony (Sb), nickel (Ni), chromium (Cr), aluminum (Al), cobalt (Co), manganese (Mn), titanium (Ti), molybdenum (Mo), silicon (Si), magnesium (Mg), tungsten (W) and alloys thereof.

[0091] As a preferred example, the metal sheet includes a stainless steel metal material containing bismuth (Bi), tin (Sn), indium (In), silver (Ag), copper (Cu), zinc (Zn), antimony (Sb), nickel (Ni), chromium (Cr), etc. More preferably, it can be a metal sheet including an alloy containing 34 to 38 weight percent of nickel and the remainder of iron (Fe) (including essential impurities in addition to nickel and iron).

[0092] Encapsulation resin layer

[0093] Furthermore, in the encapsulation material for an organic electronic device of the present invention, the encapsulation resin layer can be prepared by a reduced-pressure adhesive composition comprising a polyolefin-based adhesive resin, wherein the polyolefin-based adhesive resin can comprise a poly(C) selected from polyethylene, polypropylene, polypropylene, polyisobutylene, etc. 2 ~C 6 ) one or more of olefin resins and random copolymer resins copolymerized with ethylene, propylene and / or diene compounds.

[0094] As a preferred example, the polyolefin-based binder resin may include a compound represented by the following Chemical Formula 1.

[0095] Chemical formula 1:

[0096] In the above chemical formula 1, R 1 A hydrogen atom or C 3 ~C 10 Straight chain alkenyl or C 4 ~C 10 Preferably, R 1 It can be a hydrogen atom or a C 4 ~C 8 Straight chain alkenyl or C 4 ~C 8 The branched alkenyl group, and the above n can be a rational number that satisfies the weight average molecular weight of the compound represented by Chemical Formula 1 of 10000 to 2000000, preferably, it can be a rational number that satisfies the weight average molecular weight of 30000 to 1550000, and more preferably, it can be a rational number that satisfies the weight average molecular weight of 40000 to 1500000. When the weight average molecular weight is less than 10000, the plate sag phenomenon caused by the low modulus may occur, and it may lead to the reduction of heat resistance, the reduction of hygroscopic filling, the reduction of reliability, the reduction of mechanical properties, and, with the reduction of elasticity, the floating phenomenon between the substrate caused by the volume expansion of the hygroscopic agent may occur. And, when the weight average molecular weight is greater than 2000000, the bonding force between the substrate and the substrate may be reduced due to the reduction of wettability, and the bonding property to the plate may be reduced due to the increase of modulus.

[0097] When the compound represented by the above Chemical Formula 1 is measured by the following measurement method, the crystallization temperature may be 100 to 140°C, preferably 110 to 130°C, and more preferably 115 to 125°C.

[0098] Determination method

[0099] When the temperature is cooled from 200°C to -150°C at a rate of 10°C / min, the crystallization temperature (T) is determined by analyzing the peak of the cooling curve of the heat flow measured by differential scanning calorimetry (DSC). c ).

[0100] Furthermore, the polyolefin adhesive resin may include a copolymer formed by copolymerization of ethylene, propylene and diene compounds. In this case, ethylene and propylene are randomly copolymerized at a weight ratio of 1:0.3 to 1.4, preferably at a weight ratio of 1:0.5 to 1.2. When the weight ratio of the copolymerized ethylene and propylene is less than 1:0.3, the increase in modulus and hardness will cause poor board bonding, thereby causing problems of reduced bonding strength with the substrate and reduced physical properties under low temperature conditions. As the elastic modulus decreases, it has an adverse effect on the volume expansion of the hygroscopic agent. When the weight ratio exceeds 1:1.4, the decrease in modulus and hardness will cause board sagging, and the reduction in mechanical properties will lead to a reduction in the mechanical properties of the product. Since it is difficult to achieve high filling of the hygroscopic agent, the problem of reduced reliability may occur. Furthermore, relative to the total weight of the copolymer formed by copolymerization of ethylene, propylene and diene compounds, 2 to 15 weight percent of diene compounds may be included, preferably 7 to 11 weight percent of diene compounds may be included. When the diene compound is less than 2 weight percent, the lower curing speed and curing density may lead to plate sagging due to reduced modulus and reduce heat resistance. As the elasticity decreases, floating between the substrate and the substrate may occur due to the volume expansion of the hygroscopic agent. When it exceeds 15 weight percent, the high curing density leads to insufficient wettability, resulting in reduced adhesion to the substrate, reduced compatibility between resins, and reduced plate bonding due to high modulus, which may lead to yellowing caused by heat.

[0101] Considering the physical property improvement level such as increasing elastic force, the above-mentioned polyolefin-based binder resin can be used by mixing two kinds of binder resins. As a preferred example thereof, it can include the above-mentioned disregarded copolymer (first binder resin) formed by copolymerization of ethylene, propylene and diene compounds and the compound represented by the above-mentioned chemical formula 1 (second binder resin). Preferably, the weight ratio of the first binder resin to the second binder resin can be 1:0.1 to 10, more preferably, it can be 1:1 to 9, and more preferably, it can be 1:1.1 to 5. In this case, when the weight ratio is greater than 1:10, the problem of reduced elastic force will occur. Therefore, the first binder resin and the second binder resin can be mixed and used without departing from the above range.

[0102] In addition to the polyolefin adhesive resin described above, the reduced pressure adhesive composition used for preparing the encapsulating resin layer may further include additives such as a tackifier, a moisture absorbent, a curing agent, a photoinitiator, and an antioxidant.

[0103] The above-mentioned tackifier in the additive can be used as long as it is a bonding resin commonly used in the bonding composition for organic electronic device packaging materials, without any special restrictions. Preferably, it can include one or more selected from hydrogenated petroleum resin, hydrogenated rosin resin, hydrogenated rosin ester resin, hydrogenated terpene resin, hydrogenated terpene phenol resin, polymerized rosin resin and polymerized rosin ester resin. Moreover, the amount of tackifier used is 50 to 300 parts by weight, preferably 80 to 280 parts by weight, relative to 100 parts by weight of the polyolefin bonding resin. Relative to 100 parts by weight of the mixed resin, when the tackifier is less than 50 parts by weight, it is difficult to ensure moisture resistance. When it is greater than 300 parts by weight, the problem of reduced durability and moisture resistance may occur as the elasticity decreases (Brittle).

[0104] The above-mentioned desiccant in the additive can be used without any particular limitation as long as it is a desiccant commonly used for encapsulation of organic electronic devices. Preferably, it includes one or more of a desiccant containing zeolite, titanium dioxide, zirconium oxide or montmorillonite as a component, a metal salt and a metal oxide, and more preferably, it may include a metal oxide.

[0105] The metal oxide may include silicon dioxide (SiO 2 ), aluminum oxide (Al 2 O 3 ), lithium oxide (Li 2 O), sodium oxide (Na 2 O), barium oxide (BaO), calcium oxide (CaO) or magnesium oxide (MgO) and other metal oxides, organic metal oxides and phosphorus pentoxide (P 2 O 5 )

[0106] The metal salt may include lithium sulfate (Li 2 SO 4 ), sodium sulfate (Na 2 SO 4 ), calcium sulfate (CaSO 4 ), magnesium sulfate (MgSO 4 ), cobalt sulfate (CoSO 4 ), gallium sulfate (Ga 2 (SO 4 ) 3 ), titanium sulfate (Ti(SO 4 ) 2 ) or nickel sulfate (NiSO 4 ) and other sulfates; calcium chloride (CaCl 2 ), magnesium chloride (MgCl 2 ), Strontium chloride (SrCl 2 ), yttrium chloride (YCl 3 ), copper chloride (CuCl 2 ), cesium fluoride (CsF), tantalum fluoride (TaF 5 ), niobium fluoride (NbF 5 ), lithium bromide (LiBr), calcium bromide (CaBr 2 ), cesium bromide (CeBr 3 ), Selenium bromide (SeBr 4 ), vanadium bromide (VBr 3 ), magnesium bromide (MgBr 2 ), barium iodide (BaI 2 ) or magnesium iodide (MgI 2 ) and other metal halides; and barium perchlorate (Ba(ClO 4 ) 2 ) or magnesium perchlorate (Mg(ClO 4 ) 2 ) or more of metal chlorates.

[0107] It is preferred to use a moisture absorbent having a purity of 95% or more. When the purity is less than 95%, not only the moisture absorption function is reduced, but also the substances contained in the moisture absorbent may cause defects in the adhesive film as impurities, which may affect the organic electronic device, but is not limited to this.

[0108] When a desiccant is used, the appropriate amount used may be 10 to 550 parts by weight, preferably 20 to 520 parts by weight, relative to 100 parts by weight of the polyolefin adhesive resin. When the amount of the desiccant used is less than 10 parts by weight, the adhesive film for the purpose of reducing the durability of the organic electronic device and significantly reducing the water removal effect cannot be embodied. When the amount of the desiccant used is greater than 550 parts by weight, the adhesive film and the organic electronic device are poorly bonded due to insufficient wettability, such as adhesion and bonding, resulting in reduced reliability of the organic electronic device. In the case of absorbing moisture, the floating phenomenon caused by excessive volume expansion occurs, and the service life of the organic electronic device is shortened.

[0109] The above-mentioned curing agent in the additive can be used as long as it is a substance commonly used as a curing agent, and there is no special restriction. Preferably, it can include a substance that ensures sufficient cross-linking density of the adhesive film by acting as a cross-linking agent. More preferably, it can include one or more selected from urethane acrylate curing agents with a weight average molecular weight of 100 to 1500 and acrylate curing agents with a weight average molecular weight of 100 to 1500. When the weight average molecular weight of the curing agent is less than 100, the board bonding and the bonding force between the board and the substrate decrease with the increase of hardness, thereby causing the problem of gas leakage (Outgas) of the unreacted curing agent. When the weight average molecular weight is greater than 1500, the problem of reduced mechanical properties caused by increased softening (Softness) can occur. Moreover, relative to 100 parts by weight of the polyolefin adhesive resin, the appropriate amount of the curing agent used can be 2 to 50 parts by weight, preferably, 5 to 40 parts by weight. When the amount of curing agent used is less than 2 parts by weight, it is difficult to achieve the desired setting rate and modulus and the problem of reduced elastic force may occur. When it is greater than 50 parts by weight, the high modulus and high hardness may cause poor board joining and reduced adhesion due to reduced wettability.

[0110] The above-mentioned photoinitiator in the additive can be used as long as it is a substance commonly used as a photoinitiator, without any particular limitation. For example, it can include one or more selected from monoacylphosphine, bisacylphosphine, α-hydroxyketone, α-aminoketone, phenylglyoxylate, and dimethylbenzylketal. Moreover, the appropriate amount of the photoinitiator used can be 0.1 to 10 parts by weight, preferably 0.5 to 8 parts by weight, relative to 100 parts by weight of the polyolefin-based binder resin. When the amount of the photoinitiator used is less than 0.1 parts by weight, the problem of reduced heat resistance due to poor curing may occur, and when it is greater than 10 parts by weight, the problem of reduced heat resistance due to reduced curing density may occur.

[0111] The viscosity of the above-mentioned decompression adhesive composition used to manufacture the encapsulation resin layer can be 100000-300000 Pa·s (50°C), preferably, the viscosity can be 120000-280000 Pa·s (50°C). When the viscosity is less than 100000 Pa·s (50°C), due to the increase of adhesion (Tack), the processability is not good, so that the problem of being unable to peel off the release layer (or release sheet) may occur. When the viscosity is greater than 300000 Pa·s (50°C), due to the decrease of adhesion (Tack), the problem of too low adhesion between the substrate and the substrate may occur.

[0112] As described above, the encapsulating resin layer can be manufactured into a single or multi-layered decompression adhesive layer using the decompression adhesive composition. A preferred example is described below, but it is only an example for understanding the present invention and does not limit the present invention.

[0113] When the encapsulation resin layer is a single-layer structure of a decompression adhesive layer, the glass bonding force can be 1500gf / 25mm or more, preferably, 1600gf / 25mm or more. In this case, the bonding force can be measured by laminating a bonding force measuring tape (7475, TESA) on the bonding film by a hand roller (2Kg Hand Roller), cutting the sample with a width of 25mm and a length of 120mm, laminating the bottom of the bonding film on the glass at 80°C, placing the prepared sample at room temperature for 30 minutes, and measuring the glass bonding force at a speed of 300mm / minute.

[0114] Moreover, the bonding force of the metal layer to the density resin layer can be 1000 gf / 25 mm or more, preferably, 1100 gf / 25 mm or more. In this case, under the condition of 80° C., the bonding force to the metal layer is measured by laminating a nickel (Ni) alloy having a thickness of 80 μm on the top of the bonding film, and laminating a bonding force measuring tape (7475, TESA) under the bonding film by a hand roller (2 Kg Hand Roller), cutting the sample with a width of 25 mm and a length of 120 mm, placing the prepared sample at room temperature for 30 minutes, and measuring the bonding force at a speed of 300 mm / min.

[0115] And, if Figure 1 As shown in the schematic diagram of part (b) of FIG. 1 , the encapsulating resin layer may be formed as a pressure-reducing adhesive layer having a double-layer structure of a first pressure-reducing adhesive layer 11 and a second pressure-reducing adhesive layer 12 .

[0116] The first decompression adhesive layer 11 as a layer directly contacting the organic electronic device may include a first mixed resin 11b, a tackifier and a first moisture absorbent 11a. In this case, the first mixed resin 11b may include a first adhesive resin and a second adhesive resin. The tackifier may include a first tackifier and may also include a second tackifier.

[0117] The polyolefin adhesive resin 11b of the first pressure-reducing adhesive layer may include the above-mentioned first adhesive resin and the above-mentioned second adhesive resin. Moreover, the tackifier of the first pressure-reducing adhesive layer 11 may include one or two tackifiers (the first tackifier and the second tackifier). In this case, the types described above may be used as tackifiers, and preferably, hydrogenated petroleum resins with different softening points may be included. As an example, when hydrogenated petroleum resins with different softening points are included, the softening point of the first tackifier may be lower than the softening point of the second tackifier, and the weight ratio of the mixed use amount of the first tackifier and the second tackifier may be 1:0.5 to 1.5, preferably, 1:0.6 to 1.4. When the weight ratio of the first tackifier and the second tackifier is less than 1:0.5, the problem of reduced heat resistance maintenance rate may occur, and when the weight ratio is greater than 1:1.5, the problem of reduced bonding force with the substrate due to reduced bonding and wettability may occur.

[0118] Furthermore, the first moisture absorbent 11a used for manufacturing the first pressure-reducing adhesive layer can be used without limitation as long as it is a substance commonly used as a moisture absorbent. Preferably, a substance having a BET specific surface area of ​​2 to 20 m 2 / g of silica, more preferably, a silica having a BET specific surface area of ​​3 to 14 m 2 / g of silica, more preferably, a silica with a BET specific surface area of ​​4 to 8 m 2 / g of silicon dioxide. Silicon dioxide can be used as the first moisture absorbent 11a, thereby improving the water removal performance, preventing the separation of the organic electronic device and the packaging material, and significantly improving the durability of the organic electronic device.

[0119] The reduced pressure adhesive composition used to manufacture the second reduced pressure adhesive layer 12 may include a polyolefin adhesive resin 12b, a tackifier, and a second hygroscopic agent 12a. In this case, the polyolefin adhesive resin 12b may include a first adhesive resin and a second adhesive resin, and unlike the first reduced pressure adhesive layer in which the first tackifier and the second tackifier are mixed as two tackifiers, only the first tackifier may be used as the tackifier. Moreover, as the hygroscopic agent, the same hygroscopic agent as that used to manufacture the first reduced pressure adhesive layer may be used, and preferably, calcium oxide may be used.

[0120] Release layer

[0121] In the packaging material for an organic electronic device of the present invention, the release sheet (liner sheet) material used as the release layer can use a release sheet material commonly used in the relevant field. For example, a preferred example can include one or more selected from polyethylene terephthalate (PET), paper, polyimide (PI) and polyester (PE).

[0122] The method for producing the encapsulating material for an organic electronic device of the present invention described above is as follows.

[0123] The encapsulation material for organic electronic devices of the present invention can be manufactured by executing a process comprising the following steps: a first step of preparing a composite sheet; a second step of mechanically cutting both sides of the composite sheet in the long side direction; and a third step of mechanically cutting the cut composite sheet along the short side direction.

[0124] As described above, the composite sheet in the first step includes a metal layer, an encapsulation resin layer and a release layer. In addition to these layers, a layer having a different composition and / or a layer having a different function from the metal layer and the encapsulation resin layer may be included between the metal layer and the encapsulation resin layer, and a layer having a different composition and / or a layer having a different function from the encapsulation resin layer and the release layer may be included between the encapsulation resin layer and the release layer. Moreover, the components, physical properties, characteristics, etc. of the metal layer, the encapsulation resin layer and the release layer are as described above.

[0125] The mechanical cutting in the second step and the third step can be slitting cutting or shearing cutting. The mechanical cutting in the second step and the third step can be performed by the same cutting method or different cutting methods. Preferably, different cutting methods are used. More preferably, slitting is performed in the second step and shearing is performed in the third step.

[0126] like Figure 2 As shown in the schematic diagram, in the mechanical cutting method, the above-mentioned slitting can be performed by a slitting machine, and the above-mentioned slitting machine includes an upper knife in the form of a rotating blade and a lower knife formed with an insertion portion for inserting the upper knife. Moreover, in order to ensure excellent cutting quality, preferably, the above-mentioned upper knife is made of high-speed steel and the lower knife is made of superhard material. In addition, the land values ​​of the above-mentioned upper knife and the lower knife are 0.10 to 0.30 mm, preferably 0.15 to 0.25 mm, and more preferably 0.18 to 0.22 mm. When the land value is less than 0.10 mm, problems with the durability of the knife may occur, and when the land value is greater than 0.30 mm, problems with the cutting quality may occur.

[0127] When slitting, the side pressure applied to the upper knife is 0.5 to 2.5 kgf / cm 2 Preferably, the side pressure is 0.5 to 1.8 kgf / cm 2 More preferably, the side pressure is 0.8 to 1.2 kgf / cm 2 In this case, when the side pressure is less than 0.5kgf / cm 2 When the side pressure is greater than 2.5kgf / cm 2 When the offset is larger, the problem of increasing the area where the offset occurs may occur.

[0128] Moreover, when performing the above-mentioned slitting, the insertion depth of the upper knife relative to the lower knife is 0.3 to 2.0 mm, preferably 0.5 to 1.5 mm, and more preferably 0.6 to 1.3 mm. In this case, when the insertion depth is 0.3 mm, the problem of uncut parts may occur. When the insertion depth is greater than 2.0 mm, the problem of loosening (collapse) of the decompression adhesive layer may occur.

[0129] Furthermore, preferably, when slitting is performed, the rotation speed of the rotating blade as the upper knife is the same as the moving speed of the composite sheet.

[0130] like Figure 3a and Figure 3bAs shown in the schematic diagram, in the mechanical cutting method, the shearing can be performed by a shearing machine, wherein the shearing machine is composed of an upper knife and a lower knife, and the upper knife forms a blade angle (slope), and the blade angle of the lower knife is less than 0.30 degrees, preferably, the blade angle is less than 0.005 degrees. The blade angle of the upper knife is 0.140 to 0.300 degrees, preferably 0.143 to 0.287 degrees, and more preferably 0.143 to 0.225 degrees. In this case, when the blade angle is less than 0.140 degrees, the damage (Damage) of the FSPM may be aggravated. When the blade angle of the upper knife is greater than 0.300 degrees, the cutting surface may be squeezed, thereby causing a problem of dimensional consistency.

[0131] Furthermore, the gap between the upper blade and the lower blade is 0.5 μm to 50 μm, preferably 1 μm to 25 μm, and more preferably 2 μm to 10 μm. When the gap is greater than 50 μm, the release sheet may be lifted.

[0132] Furthermore, the shearing speed can be adjusted by the moving speed of the composite sheet and the size of the composite sheet to be produced, and is preferably 150 to 300 mm / sec, and more preferably 180 to 250 mm / sec.

[0133] Furthermore, after the slitting is performed in the second step or the third step, a step of continuously wet-cleaning the slit long side portions of the composite sheet may be performed.

[0134] Furthermore, after the mechanical cutting in the third step, preferably, a process of continuously performing dry cleaning-free treatment on the composite sheet can be performed.

[0135] The present invention is further described in detail below by way of examples. However, the following examples do not limit the scope of the present invention and should be interpreted as being helpful for understanding the present invention.

[0136] Example

[0137] Preparation Example 1-1: Production of an Adhesive Sheet for Organic Electronic Device Encapsulation Material

[0138] 1. Preparation of polyolefin adhesive resin

[0139] The polyolefin-based binder resin was prepared by mixing a copolymer (first binder resin) obtained by copolymerizing ethylene, propylene and a diene-based compound and a compound (second binder resin) represented by the following Chemical Formula 1 at a weight ratio of 1:2.33.

[0140] The first bonding resin is prepared by copolymerizing ethylene and propylene monomers in a weight ratio of 1:0.85, and is prepared by copolymerizing a diene compound at a weight percentage of 9% relative to the total weight of the random copolymer, wherein the diene compound is a random copolymer having a weight average molecular weight of 500,000 prepared by ethylidene norbornene.

[0141] Chemical formula 1:

[0142] In the above chemical formula 1, the above R 1 isoprene, and n is a rational number satisfying the weight average molecular weight of the compound represented by Chemical Formula 1 of 400,000.

[0143] The first binder resin and the second binder resin were cooled at a rate of 10°C / min from 200°C to -150°C, and the crystallization temperature (T) was determined by analyzing the peak of the cooling curve of the heat flow measured by differential scanning calorimetry (DSC). c ), and as a result, the crystallization temperature was not measured for the first binder resin, but the measurement result for the second binder resin was 120°C.

[0144] 2. Manufacture of adhesive sheets for encapsulation materials of organic electronic devices

[0145] For 100 parts by weight of the above-prepared polyolefin adhesive resin (first adhesive resin), 80 parts by weight of the first tackifier (SU-90, Cologne Industries) and 50 parts by weight of the second tackifier (SU-100, Cologne Industries), 11 parts by weight of methyl acrylate (M200, Meiyuan Special Chemicals) with a weight average molecular weight of 226 as a curing agent, 3 parts by weight of a photoinitiator (photoinitiator TP0, Ciba) and 24 parts by weight of silica with an average particle size of 0.5 μm are added for stirring. After the stirred mixture is passed through a capsule filter to remove foreign matter, it is coated on a heavy peelable release polyethylene terephthalate (REL382, Torayadvance Materials) with a thickness of 38 μm using a slit coater, and then dried at 120°C to form a first pressure-reducing adhesive layer with a final thickness of 10 μm after removing the solvent.

[0146] Next, for 100 parts by weight of the above-prepared polyolefin adhesive resin (second adhesive resin), 150 parts by weight of the first tackifier (SU-90, Cologne Industry), 17 parts by weight of methyl acrylate (M200, Meiyuan Special Chemicals) with a weight average molecular weight of 226 as a curing agent, 3 parts by weight of a photoinitiator (photoinitiator TP0, Ciba) and 100 parts by weight of calcium oxide with an average particle size of 3 μm are added for stirring. At 20° C., the viscosity of the stirred mixture is adjusted to 800 cps and foreign matter is removed by a capsule filter, and then it is coated on a light peeling release polyethylene terephthalate (TG65R, SKC) with a thickness of 36 μm using a slit coater, and then dried at 120° C., thereby forming a second pressure-reducing adhesive layer with a final thickness of 40 μm after removing the solvent.

[0147] The second pressure-reducing adhesive layer was attached to the first pressure-reducing adhesive layer so that they were opposite to each other, and the adhesive sheet for an organic electronic device encapsulation material was manufactured by a laminar roll at 70° C. (refer to Figure 1 (b) of the Regulations).

[0148] Preparation Example 1-2: Production of an Adhesive Sheet for Organic Electronic Device Encapsulation Material

[0149] An adhesive sheet for an encapsulating material of an organic electronic device is manufactured by the same method as in the above-mentioned preparation example 1-1, but only the second adhesive resin is used to prepare the polyolefin adhesive resin, and the polyolefin adhesive resin is used as the polyolefin adhesive resin of the first pressure-reducing adhesive layer and the second pressure-reducing adhesive layer. Furthermore, when manufacturing the first pressure-reducing adhesive layer, the first pressure-reducing adhesive layer is formed by replacing the silicon dioxide with the same calcium oxide as used in manufacturing the second pressure-reducing adhesive layer, and then the adhesive sheet for an encapsulating material of an organic electronic device is manufactured by laminating the first pressure-reducing adhesive layer with the second pressure-reducing adhesive layer.

[0150] Preparation Example 2: Preparing Metal Sheet (Face Seal Metal)

[0151] A metal sheet including about 36 weight percent of nickel (Ni) and the balance of iron (Fe) (including essential impurities), having a density (d) of 8.1, a hardness of 200 HV, and an average thickness of 80 μm was prepared.

[0152] Preparation Example 3-1: Production of Composite Sheet (FSPM Sheet) 1

[0153] After manufacturing a FSPM sheet as a composite sheet by bonding the encapsulation sheet of Preparation Example 1-1 and the metal sheet of Preparation Example 2, a FSPM sheet (composite sheet) having a three-layer structure (metal layer (80 μm)-encapsulation resin layer (50 μm)-release layer (38 μm)) is manufactured by rolling the bonded sheets.

[0154] Preparation Example 3-2: Production of Composite Sheet (FSPM Sheet) 2

[0155] A rolled composite sheet was manufactured by the same method as in the above-mentioned Preparation Example 3-1, by using the encapsulating sheet of Preparation Example 1-2 instead of the encapsulating sheet of Preparation Example 1-1 to manufacture a rolled composite sheet (hereinafter, referred to as "FSPM sheet").

[0156] Example 1: Manufacturing of organic electronic device encapsulation material by slitting and shearing (SSC) process

[0157] The automated equipment for slitting and shearing (SSC) the FSPM sheet which is the composite sheet rolled in Preparation Example 3-1 includes a cutting object supplying section, a slitting section, an edge cleaner section, an automatic size inspection section, a shearing section, and a dry cleaning-free section.

[0158] 1. Slitting cutting process

[0159] like Figure 2 As shown in the simplified diagram, the cutting portion includes an upper knife and a lower knife. The upper knife is a rotating blade for cutting, and is a circular knife (Knife) with a diameter of 150 mm. The lower knife is a circular knife with a diameter of 150 mm. The upper knife is made of high-speed steel, and the lower knife is made of superhard material. The land values ​​of the upper knife and the lower knife are 0.2 mm respectively.

[0160] The rolled composite sheet supplied from the cutting object supply section is cut at the same time on both long sides in the longitudinal direction of the above-mentioned cutting section. When cutting, the release layer of the FSPM sheet faces the upper knife direction. In addition, the side pressure applied to the rotating blade for cutting is 1.0kgf / cm 2 When cutting, the surface of the lower blade is used as a reference, and the cutting is performed under the condition that the depth of the rotating blade of the upper blade is 0.8 mm. In addition, the scrap (scrap) produced by shearing is removed by a scrap winder (scrap winder).

[0161] 2. Shearing cutting process

[0162] After the position value of the FSPM sheet to be cut is confirmed by a camera and an automatic inspection is performed for size correction, a shearing process is performed to cut the short side of the FSPM sheet.

[0163] like Figure 3a and Figure 3b As shown in the schematic diagram, the upper knife is cut by moving up and down. When the shearing process is performed, the interval between the lower knife and the upper knife is 5μm, the blade angle (Slope) of the upper knife is 0.143 degrees, and the lower knife has no angle (Slope). In addition, the material of the upper knife is high-speed steel, the material of the lower knife is superhard material, and the cutting speed is 200mm / second.

[0164] Figure 4 The figure shows the SEM measurement of the cut surface (long side) of the manufactured encapsulating material for an organic electronic device.

[0165] When observing the cut surface after slitting, comb lines were formed on the cut surface, which could be judged to be formed by the rotating blade.

[0166] and, Figure 5 The figure shows SEM measurement of the cut surface of the encapsulating material for an organic electronic device manufactured by shearing with a lower blade and an upper blade.

[0167] When the packaging material is manufactured by the slitting and shearing process of the present invention, when viewed from the moving direction of the composite sheet (FSPM sheet), the front short side is cut by the lower blade, and the rear short side is cut by the upper blade. Figure 5 As shown, the shearing cut surface is different from the slitting cut surface, and there is no comb pattern, and a line pattern is formed in the vertical direction. It can also be confirmed that the cross-sectional morphology of the upper knife cutting surface and the lower knife cutting surface are different, and the lower knife cutting surface of the short side hardly forms an offset area, and the morphological difference occurs in the offset area of ​​the upper knife cutting surface of the short side.

[0168] Example 2: Manufacturing organic electronic device encapsulation material through slitting and shearing processes

[0169] An organic electronic device encapsulation material was manufactured through a slitting and shearing process in the same manner as in Example 1, by using the rolled composite sheet of Preparation Example 3-2 instead of the rolled composite sheet of Preparation Example 3-1 and using a slitting and shearing automated equipment.

[0170] Comparative Example 1

[0171] The same composite sheet (FSPM sheet) as the roll-pressed composite sheet of Preparation Example 3 was prepared.

[0172] Next, the encapsulation resin layer and the release layer in the composite sheet are cut for the first time by means of carbon dioxide laser cutting.

[0173] Then, the metal layer of the composite sheet is cut a second time by a fiber laser, thereby manufacturing the packaging material by laser cutting.

[0174] In this case, carbon dioxide (CO 2 ) The power of laser cutting is about 140W / cm 2 , The power of fiber laser cutting is 170W / cm 2 .

[0175] Figure 6 To show the SEM measurement time of the manufactured packaging material, Figure 7 This is a conceptual diagram showing the boss formed at the end of the release layer, the residue existing in the release layer and the encapsulating resin layer, and the off-set area confirmed from the SEM image.

[0176] Reference Figure 4 , Figure 5 It can be confirmed that, unlike Example 1 which has no bosses and residues and no offset area or is minimized, in the case of Comparative Example 1 manufactured by laser cutting, bosses are formed on the upper surface of the release layer, and residues are formed on the release layer and the encapsulation resin layer, thereby forming a large offset area. This is due to thermal deformation of the release layer and the encapsulation resin layer caused by heat generated during laser cutting.

[0177] Experimental Example 1: Cone Angle Measurement

[0178] 1. Measurement of taper angle of packaging materials produced by laser cutting process

[0179] After preparing a composite sheet having the thickness shown in Table 1 below, it was laser cut in the same manner as in Comparative Example 1 to prepare a packaging material. In this case, the composite sheet was prepared by changing the thickness of the metal layer and the release layer, respectively.

[0180] When the tapered measurement target cut surface is viewed from the side, the taper length is the difference between the bottom surface end of the metal layer and the top surface end of the release layer of the cut surface (the longest length of the offset region).

[0181] Furthermore, when observing from the side direction of the cut surface of the conical measurement object, the cone angle is the angle formed between the end of the bottom surface of the metal layer of the cut surface and the end of the top surface of the release layer of the cut surface, with the bottom surface of the metal layer of the cut surface as the reference. For ease of understanding, Figure 6 (Comparative Example 1) and Figure 5 The schematic diagram of (upper knife shear cut surface of Example 1) shows the taper length and taper angle.

[0182] Furthermore, 10 packaging materials produced by the laser process were randomly selected, and the measurement results of their average taper lengths and taper angles are shown in Table 1 below.

[0183] Table 1

[0184]

[0185] From Table 1, it can be confirmed that the taper angle tends to increase with increasing FSPM sheet thickness and tends to decrease with increasing taper length. Furthermore, it can be confirmed that when the thickness of the encapsulating material is 168 to 200 μm, the encapsulating material cut by laser cutting has a taper angle in the range of 33.9 to 84.30 degrees.

[0186] 2. Measurement of the taper angle of the packaging material of Example 1 manufactured by the slitting and shearing process

[0187] After manufacturing the FSPM sheet having the thickness shown in Table 2 below, the packaging material was manufactured by slitting and shearing in the same manner as in Example 1. In this case, the FSPM sheet was manufactured by changing the thickness of the metal layer and the release layer respectively. Furthermore, the taper length and taper angle of the lower knife and upper knife cutting surface of the short side of the sheared packaging material were measured in the same manner as in Table 1 above, and the results are shown in Table 2 below.

[0188] Furthermore, 10 packaging materials produced by automatic processes such as slitting and shearing processes were randomly selected, and the measurement results of their average taper lengths and taper angles are shown in Tables 2 and 3 below.

[0189] Table 2

[0190]

[0191] Table 3

[0192]

[0193] and, Figure 6 (Comparative Example 1) and Figure 5 (Example 1) SEM measurement images of the side surface direction of the long side cut surface of the packaging material manufactured in Example 1 and Comparative Example 1 are respectively shown.

[0194] Reference Figure 6It was confirmed that, in the case of manufacturing by laser cutting, burrs were generated and offset regions existed in Comparative Example 1, whereas in Example 1, there were no burrs and no offset regions on the cut surface of the long side.

[0195] Furthermore, as shown in Table 2 above, when the packaging material is manufactured through the slitting and shearing process, since the cutting surfaces of the upper knife and the lower knife on the short side have no or only a very short taper length which is the length of the offset area, it can be confirmed that the taper angle is 73 to 90 degrees. It can be confirmed that, unlike the packaging material manufactured through laser cutting, the packaging material manufactured through the slitting and shearing process has a very low offset area.

[0196] And, refer to Figure 7 The upper knife area of ​​the long side cutting surface will be sheared out, and the resulting scrap (Scrap) is removed by a scrap winder, thereby manufacturing a packaging material with a cutting surface of the lower knife, and the taper angle of the slitting cutting surface is shown in the above Table 3. The angle at this time is smaller than the taper angle of the short side, that is, it is within the tolerance range of 83 to 90 degrees.

[0197] 3. Measurement of the taper angle of the packaging material of Example 2 manufactured by the slitting and shearing process

[0198] The taper angle was measured by the same method as in 2 above, using the packaging material manufactured in Example 2 instead of the packaging material in Example 1 to measure the taper angle, and the results are shown in the following Table 4. In addition, the slitting and shearing processes were performed by an automatic process, so that 10 packaging materials were randomly selected from the manufactured packaging materials, and the measurement results of their average taper length and taper angle are shown in the following Tables 4 and 5.

[0199] Table 4

[0200]

[0201]

[0202] Table 5

[0203]

[0204] By referring to the cone angle measurement results in Table 4 and Table 5 and the cone angle measurement results in Table 2 and Table 3, it can be confirmed that almost similar or identical results are obtained, that is, when the encapsulation resin layer has the same thickness, the composition of the encapsulation sheet has no effect on the cone angle.

[0205] 4. Measurement of the cone angle after the release sheet of the packaging material of Example 1 is removed

[0206] After removing the release sheet of the packaging material manufactured and measured in Example 1, the taper angles of the long and short side cut surfaces of the packaging material (metal sheet-packaging sheet) were measured. The results are shown in Tables 6 and 7 below.

[0207] Table 6

[0208]

[0209]

[0210] Table 7

[0211]

[0212] The taper angles in Tables 6 and 7 above tend to be relatively reduced compared to those in Tables 2 to 5 above due to the removal of the release sheet.

[0213] Furthermore, it was confirmed that the taper angle of the shearing cut surface was 67 to 90 degrees, and the taper angle of the cleaving cut surface was 80 to 90 degrees.

[0214] Experimental Example 2: Determination of initial peeling force of release layer

[0215] The composite sheets (FSPM sheets) produced in Example 1 and Comparative Example 1 were respectively prepared.

[0216] Next, the initial peeling force of the liner films at four corners of the FSPM sheets in Example 1 and Comparative Example 1 was measured by UTM and a probe tack test.

[0217] The specific measuring method is as follows: the lowering speed and the rising speed of the clamp are 1.0 mm / sec, the dwell force (applied pressure) is 800 gf, and the dwell time (applied pressure maintenance time) is 10 seconds.

[0218] Figure 8 Parts A and B of FIG8 are the equipment used in the experiment and the photos of the experiment. Part C of FIG8 is a schematic diagram showing that the ball-shaped fixture approaches the edge of the sheet and maintains contact and separates the release layer. Fig. 9 Part A and Part B of FIG. 1 are diagrams showing the initial peel force measurement results of Example 1 and Comparative Example 1. Fig. 9 Part C of FIG. 1 is a graph showing the average value of the initial peel force (gf). Fig. 9 In Part A and Part B of , L / C-1 to L / C-5 and SSC-1 to SSC-5 are packaging materials prepared in Example 1 and / or Comparative Example 1 and their initial peeling forces are measured by randomly selecting packaging materials.

[0219] Reference Fig. 9 When the encapsulation material (Comparative Example 1) is manufactured by laser cutting, the initial peeling force of the encapsulation resin layer of the release layer is 500-500 gf, whereas when the encapsulation material (Example 1) is manufactured by slitting and shearing, the initial peeling force of the encapsulation resin layer of the release layer is 300-350 gf, thereby confirming the difference in initial peeling force. The factors causing this difference are as follows, namely, in the case of Comparative Example 1, when laser cutting is performed, the release layer and / or the encapsulation resin layer are thermally deformed, and residues are formed on the cut surface of the release layer and the encapsulation resin layer, thereby increasing the initial peeling force.

[0220] Example 3: Manufacturing of Slitting-Slitting Packaging Material

[0221] After cutting the long side (length direction) of the FSPM sheet using the same conditions and methods as in Example 1, the short side of the FSPM sheet having the three-layer structure (metal layer (80 μm) - packaging resin layer (50 μm) - release layer (38 μm)) of the above-mentioned preparation example 3-1 is also cut using the same conditions and methods to produce a packaging material with evenly cut long and short sides.

[0222] When compared with Example 1, the tension of the manufactured packaging material was not good, and there were broken portions in the initial portion of cutting, and the production speed was reduced compared with Example 1.

[0223] Example 4: Fabrication of Shear-Shear Packaging Material

[0224] After cutting the long side (length direction) of the FSPM sheet under the same conditions and methods as in Example 1, the short side of the FSPM sheet having the three-layer structure (metal layer (80 μm) - packaging resin layer (50 μm) - release layer (38 μm)) of the above-mentioned preparation example 3-1 is also cut under the same conditions and methods to produce a packaging material with both the long and short sides cut.

[0225] When compared with Example 1, since the process for cutting the long sides of the manufactured packaging material becomes complicated, the production speed is also reduced, and therefore, there is actually a problem that it is difficult to apply shearing and cutting to an automated process.

[0226] Example 5

[0227] (1) The rolled composite sheet (FSPM sheet) of Preparation Example 3-1 was manufactured into an organic electronic device encapsulation material by using a slitting and shearing (SSC) automated equipment in the same manner as in Example 1. As shown in Table 8 below, when slitting, the long side of the composite sheet was cut by changing the side pressure and the insertion depth of the upper blade. Figure 10a to Figure 10e The figure shows the SEM measurement of the cut surface of the long side of the cut. The letter symbols in the following Table 5 mean the figure measured under an optical microscope. In this case, the lower layer in the figure of FIG. 10 is a metal layer.

[0228] Table 2

[0229]

[0230] Reference Figures 10a to 10e It was confirmed that when the upper blade was inserted to a depth of 2.2 mm, which is greater than 2.0 mm, the decompression adhesive layer loosened, and the distinction between the layers became unclear, and the cutting quality was also reduced. In addition, when the side pressure applied to the upper blade was 2.7 kgf, which is greater than 2.5 kgf, an excessively large taper was generated, and the uniformity was also reduced, resulting in a problem of reduced quality.

[0231] (2) Cone angle based on upper tool condition

[0232] The taper angle of the cut surface of the slit cut relative to the cut surface of the lower blade was measured using the upper blade insertion depth and side pressure conditions in Table 8. The results are shown in Table 9. The letters in Table 9 mean the upper blade conditions in Table 8.

[0233] Table 9

[0234]

[0235] Referring to Table 9, it can be confirmed that when the upper blade insertion depth is 2.2 mm, which is greater than 2.0 mm, or when the side pressure applied to the upper blade is greater than 2.5 kgf, the taper angle tends to decrease as the taper length (offset region) increases.

[0236] Example 6

[0237] (1) The rolled composite sheet (FSPM sheet) of Preparation Example 3-1 was manufactured into an organic electronic device encapsulation material by the same method as in Example 1 using a slitting and shearing (SSC) automated equipment. When shearing the short side, the intervals between the upper blade and the lower blade were 5 μm, 12.5 μm, 25 μm, and 50 μm, respectively. Fig.11aThis is a diagram showing the measurement of the cut surface sheared by the lower knife using an optical microscope. Fig.11b This is a diagram showing whether or not PET of a composite sheet floats as measured by an optical microscope. Fig.11b The average value (Avg.Average) is the average value of the floating amount of PET generated from the end of the release sheet along the inner direction. It can be confirmed by a microscope whether the FSPM sheet cut on the release layer has floating phenomenon. Fig.11b It was confirmed that the floating phenomenon of the release sheet tended to increase as the distance between the upper knife and the lower knife increased (see Table 10).

[0238] Table 10

[0239]

[0240] (2) When shearing, the taper angle of the cutting surface of the upper knife is adjusted by the blade angle of the upper knife.

[0241] The rolled composite sheet (FSPM sheet) of Preparation Example 3-1 was manufactured into an organic electronic device packaging material using slitting and shearing (SSC) automated equipment in the same manner as in Example 1. When shearing the short side, the cutting angle of the upper knife was changed to perform shearing. The results of measuring the cone angle of the cut surface of the upper knife of the sheared short side are shown in Table 11 below.

[0242] Table 11

[0243]

[0244] With reference to Table 11, it can be confirmed that when the blade angle of the upper blade is less than 0.140 degrees or greater than 0.300 degrees, the taper angle tends to decrease sharply.

[0245] (3) When shearing, the taper angle of the upper knife cutting surface is

[0246] 1) The rolled composite sheet (FSPM sheet) of Preparation Example 3-1 was manufactured into an organic electronic device encapsulation material by the same method as in Example 1 using a slitting and shearing (SSC) automated equipment. When shearing the short side, the face value of the upper blade was changed to perform shearing, and the results of measuring the taper angle of the cut surface of the upper blade of the sheared short side are shown in the following Table 14. In this case, the face value of the lower blade was fixed to 0.50 mm.

[0247] 2) Durability test of shear blade

[0248] Since a shear blade actually used in a cutting process cuts a composite sheet including a high-strength metal sheet tens to millions of times, the long-term durability and stability of the blade is very important.

[0249] Since the durability of the shear blade cannot be measured by actually cutting it tens to millions of times, the durability of the shear upper blade was determined by using a sheet having high mechanical strength as a cutting object instead of the composite sheet of the present invention.

[0250] Specifically, a sheet of martensitic stainless steel SUS431 (100 μm, Brinell hardness of approximately 400 to 400 Hb) having a hardness approximately 2.5 to 3 times higher than that of the metal sheet of Preparation Example 2 (thickness 80 μm, Vickers hardness 200 HV) is prepared, and then shearing is performed by the same method as in 3 above using a shearing machine composed of upper knives having different face values ​​in the following Table 12.

[0251] Then, after the SUS431 sheet was sheared 10,000 times, the durability was evaluated by using a scanning electron microscope to determine whether fine cracks were generated on the blade surface of the upper blade.

[0252] Table 12

[0253]

[0254] Referring to Table 12, it can be confirmed that the taper angle decreases as the face value of the upper blade increases. When the face value of the upper blade is 2.20 mm, which is greater than 2.0 mm, there is a problem that the taper angle is less than 73 degrees, and when the face value of the upper blade is 0.08 mm, which is less than 0.10 mm, there is a large taper angle. Although the upper blade with a face value of 0.08 mm has very good cutting power, it is not suitable for a shearing blade for shearing a composite sheet including a metal sheet due to its poor blade durability.

[0255] Example 7 to Example 9

[0256] The FSPM sheet of the rolled composite sheet of Preparation Example 3-1 was slit at both sides of the long side direction of the composite sheet by using a slitting and shearing (SSC) automated equipment and by shearing the short sides in the same manner as in Example 1 to produce an organic electronic device encapsulation material, and the upper and lower knives used for shearing were cut with the materials shown in Table 13 below. In this case, although the upper and lower knives used for shearing in Examples 7 to 9 were the same as those in Example 1 only in terms of the materials, the conditions of the upper and lower knives (upper knife face value = 1.20 mm, upper knife blade angle = 0.143 degrees, lower knife blade angle = 89 degrees, interval between the upper and lower knives = 5 μm, cutting speed = 200 mm / sec) were the same.

[0257] (1) Furthermore, the taper angles of the cut surfaces in the longitudinal direction of the cut pieces were measured. The results are shown in Table 14 below.

[0258] Table 13

[0259] distinguish upper knife lower knife Example 1 High speed steel material Super hard steel material Example 7 High speed steel material High speed steel material Example 8 Super hard steel material Super hard steel material Example 9 Super hard steel material High speed steel material

[0260] Table 14

[0261]

[0262] Referring to the measurement results in Table 14, when super-hard steel is introduced as the material of the upper blade and / or the lower blade, the taper angle shows a relatively higher result than that of high-speed steel.

[0263] (2) The conditions of the upper blade and the lower blade (upper blade face value = 1.20 mm, upper blade blade angle = 0.143 degrees, interval between the upper blade and the lower blade = 5 μm, cutting speed = 200 mm / sec) were the same, and the durability of the blade was measured by using different materials for the upper blade and the lower blade as shown in Table 15. The durability measurement was performed by the same method as the durability stability measurement of the shear blade in Example 6 to confirm whether fine cracks were generated in the upper blade.

[0264] Table 15

[0265]

[0266] Although microcracks did not occur in Examples 1 and 7, microcracks occurred in Examples 8 and 9, indicating a decrease in durability stability.

[0267] By referring to Tables 14 and 15 above, it can be confirmed that in terms of ensuring an appropriate taper angle and durable stability, it is optimal to introduce high-speed steel material into the upper cutter and super-hard steel material into the lower cutter.

[0268] Through the above-mentioned embodiments and experimental examples, it can be confirmed that the packaging material for organic electronic devices provided by the present invention can solve the problems existing in the packaging material manufactured by the laser process, such as the generation of bosses on the cut surface of the release layer, the generation of residues and burrs on the cut surface, and the generation of a large number of off-set areas.

Claims

1. A packaging material for an organic electronic device, characterized in that: The composite sheet includes a metal layer, an encapsulation resin layer and a release layer. The composite sheet is a sheet formed by four ends and four cut surfaces, wherein the four cut surfaces are composed of two long-side cut surfaces formed by slitting and two short-side cut surfaces formed by shearing. When the slitting is performed, the release layer of the composite sheet faces the upper blade of the slitting machine, and the side pressure applied to the upper blade is 0.5 to 2.5 kgf / cm 2 When cutting, the insertion depth of the upper knife relative to the lower knife is 0.3 to 2.0 mm. The taper angles of the long side cutting surface and the short side cutting surface are 67 to 90 degrees respectively. The taper angle is the angle formed between the bottom surface end of the bottom layer of the cut surface and the top surface end of the top layer of the cut surface, with the bottom surface of the cut surface as a reference, when viewed from the side of the tapered cut surface to be measured.

2. A packaging material for an organic electronic device, characterized in that: The composite sheet includes a metal layer, an encapsulation resin layer and a release layer. The composite sheet is a sheet formed by four ends and four cut surfaces, wherein the four cut surfaces are composed of two long-side cut surfaces formed by slitting and two short-side cut surfaces formed by shearing. When the slitting is performed, the release layer of the composite sheet faces the upper blade of the slitting machine, and the side pressure applied to the upper blade is 0.5 to 2.5 kgf / cm 2 When cutting, the insertion depth of the upper knife relative to the lower knife is 0.3 to 2.0 mm. The long side cutting surface and the short side cutting surface satisfy the following equation 1, Equation 1: The average cone angle of the short-side cutting surface ≤ the average cone angle of the long-side cutting surface, In Equation 1, when viewed from the side of the tapered measurement target cut surface, the taper angle is the angle formed between the bottom surface end of the bottom layer of the cut surface and the top surface end of the top layer of the cut surface, with the bottom surface of the cut surface as a reference.

3. The encapsulation material for an organic electronic device according to claim 1 or 2, characterized in that: The total thickness of the packaging material is 120 to 220 μm, and the taper length is less than 60 μm. The taper length is the difference in length between the bottom surface end of the bottom layer and the top surface end of the top layer of the cut surface when viewed from the side of the tapered measurement target cut surface.

4. The encapsulation material for an organic electronic device according to claim 1 or 2, characterized in that: When the initial peeling force was measured by the UTM method under the conditions of a lowering speed and an ascending speed of the clamp of 1.0 mm / sec, a dwelling pressure of 800 gf, and a dwelling time of 10.0 sec, the initial peeling force of the corner of the release layer was 200-400 gf.

5. The encapsulation material for an organic electronic device according to claim 1 or 2, characterized in that: The composite sheet is a composite sheet formed by sequentially stacking a metal layer, an encapsulation resin layer and a release layer. The height deviation of the release layer surface calculated by the following mathematical formula 1 is 4 μm or less. The height deviation is the height in the vertical direction from the lower surface of the release layer at the bonding portion between the encapsulating resin layer and the release layer to the upper surface corresponding to the lower surface of the release layer. Mathematical formula 1: Height deviation = (maximum height of the release layer edge) - (height of the release layer center), In Mathematical Formula 1, the edge of the release layer is a portion of the surface of the release layer that is 1 mm away from the cut surface along the inner direction of the release layer.

6. The encapsulation material for an organic electronic device according to claim 1, characterized in that: The taper angles of the two long-side cut surfaces and the two short-side cut surfaces are different from each other.

7. The encapsulation material for an organic electronic device according to claim 1 or 2, characterized in that: The encapsulation resin layer includes 1 to 3 layers of pressure-reducing adhesive layers. The pressure-reducing adhesive layer includes a polyolefin adhesive resin, a tackifier, and a moisture absorbent.

8. The encapsulation material for an organic electronic device according to claim 7, characterized in that: The polyolefin-based binder resin includes one or more selected from polyolefin resins and random copolymer resins obtained by copolymerization of ethylene, propylene and / or diene compounds.

9. The encapsulation material for an organic electronic device according to claim 7, characterized in that: The polyolefin-based binder resin includes a compound represented by the following Chemical Formula 1: Chemical formula 1: In the above chemical formula 1, R 1 A hydrogen atom or a C3~C 10 Straight-chain alkenyl or C4~C 10 wherein n is a rational number satisfying the weight average molecular weight of the compound represented by Chemical Formula 1 of 10,000 to 2,000,000.

10. The encapsulation material for an organic electronic device according to claim 1 or 2, characterized in that: The metal layer includes one or more selected from iron, bismuth, tin, indium, silver, copper, zinc, antimony, nickel, chromium, aluminum, cobalt, manganese, titanium, molybdenum, silicon, magnesium, tungsten and alloys thereof.

11. The encapsulation material for an organic electronic device according to claim 1 or 2, characterized in that: It includes 2 long-side cutting surfaces and 2 short-side cutting surfaces satisfying the following equation 2, Equation 2: The cone angle deviation of the long side cutting surface is less than the cone angle deviation of the short side cutting surface. In Equation 2, the cone angle deviation of the long-side cut surface is the difference between the cone angles of the two long-side cut surfaces located in the opposite directions, and the cone angle deviation of the short-side cut surface is the difference between the cone angles of the two short-side cut surfaces located in the opposite directions.

12. The encapsulation material for an organic electronic device according to claim 11, characterized in that: The cone angle of the long side cutting surface is 80 to 90 degrees. The taper angle is the angle formed between the bottom surface end of the bottom layer of the cut surface and the top surface end of the top layer of the cut surface, with the bottom surface of the cut surface as a reference, when viewed from the side of the tapered cut surface to be measured.

13. A method for manufacturing an encapsulation material for an organic electronic device, characterized in that: include: The first step is to prepare a composite sheet including a metal layer, a packaging resin layer and a release layer; In the second step, the two sides of the long side of the composite sheet are cut. When the cutting is performed, the release layer of the composite sheet faces the upper knife of the slitting machine, and the side pressure applied to the upper knife is 0.5 to 2.5 kgf / cm 2 , when slitting, the insertion depth of the upper knife relative to the lower knife is 0.3 to 2.0 mm; and The third step is to shear the composite sheet to be cut along the short side direction. The second step and the third step are continuous processes.

14. The method for manufacturing an encapsulation material for an organic electronic device according to claim 13, characterized in that: The slitting is performed by a slitting machine, wherein the upper knife of the slitting machine is a circular knife, and an insertion portion for inserting the upper knife is formed on the lower knife.

15. The method for manufacturing an encapsulation material for an organic electronic device according to claim 13, characterized in that: When the above-mentioned slitting is performed, the blade surface values ​​of the upper blade and the lower blade are independently 0.10 to 0.30 mm.

16. The method for manufacturing an encapsulation material for an organic electronic device according to claim 14, characterized in that: The material of the upper blade includes high speed steel, and the material of the lower blade includes super hard steel.

17. The method for manufacturing an encapsulation material for an organic electronic device according to claim 13, characterized in that: The shearing is performed by a shearing machine including an upper knife having a blade angle of 0.140 to 0.300 degrees and a lower knife having a blade angle of 0.005 degrees or less.

18. The method for manufacturing an encapsulation material for an organic electronic device according to claim 13, wherein: The face value of the upper blade used for shearing is 0.10 to 2.0 mm.

19. The method for manufacturing an encapsulation material for an organic electronic device according to claim 13, characterized in that: When shearing is performed, the interval between the upper blade and the lower blade is 0.5 μm to 50 μm.

20. The method for manufacturing an encapsulation material for an organic electronic device according to claim 13, wherein: When the above shearing is performed, the cutting speed is 150 to 300 mm / sec.

21. The method for manufacturing an encapsulation material for an organic electronic device according to claim 13, characterized in that: When the processes from the first step to the third step are continuous processes, the speed at which the composite sheet of the first step is subjected to the second step and the third step is 1.0 to 10.0 m / min. In the second step, the rotation speed of the upper knife of the slitting machine is 1.0 to 10.0 m / min, and the rotation direction of the upper knife is the positive direction of the composite sheet moving direction.

22. The method for manufacturing an encapsulation material for an organic electronic device according to claim 13, characterized in that: The long side cut surface of the composite sheet formed by the slitting in the second step and the short side cut surface of the composite sheet formed by the shearing in the third step satisfy the following equation 3: Equation 3: The average cone angle of the short-side cutting surface ≤ the average cone angle of the long-side cutting surface, In Equation 3, when viewed from the side of the tapered measurement target cut surface, the taper angle is the angle formed between the bottom surface end of the bottom layer of the cut surface and the top surface end of the top layer of the cut surface, with the bottom surface of the cut surface as a reference.

23. The method for manufacturing an encapsulation material for an organic electronic device according to claim 13, characterized in that: The short side cutting surface of the sheared composite sheet includes a first short side cutting surface and a second short side cutting surface. In the case of a composite sheet including a metal layer, an encapsulating resin layer, and a release layer, the taper angles of the first short-side cutting surface and the second short-side cutting surface are 73 to 90 degrees. In the case where the release layer is removed and the metal layer and the encapsulation resin layer are included, the taper angles of the first short-side cut surface and the second short-side cut surface are 67 to 90 degrees.

Citation Information

Patent Citations

  • Liquid crystal sealant and liquid crystal cell using the same

    JP2016024240A

  • Encapsulation, methodo for preparing the same and encapsulation method of electronic devices using the same

    KR1020150074980A

  • Method of Manufacturing Organic Electroluminescence Element and Manaufacturing Apparatus

    US20080226942A1