Silver electrolyte for depositing a dispersion silver layer and contacting a surface having a dispersion silver layer

Through the electrolyte composed of silver potassium cyanide, grain refining agent and dispersant, combined with specific solid components, the problem of uneven dispersion of solid components during the deposition process is solved, and silver with high conductivity and wear resistance is achieved Layer deposition reduces costs and extends the service life of the contacts.

CN112368423BActive Publication Date: 2024-11-19ROSENBERGER HIGH FREQUENCY TECH GMBH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980044371.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-07-05
Filing Date
2019-06-26
Publication Date
2024-11-19
Estimated Expiration
2039-06-26

AI Technical Summary

Technical Problem

Existing silver electrolytes cannot evenly disperse solid components during deposition, resulting in increased surface inhomogeneity and cost, and require high deposition temperatures and expensive additive systems to improve conductivity and wear resistance.

Method used

The electrolyte consisting of potassium silver cyanide, grain refining agent and dispersant is combined with specific solid components such as graphite and dry lubricants to form a dispersed silver layer on the substrate through electrochemical deposition to ensure uniformity of the solid components. Dispersed and highly conductive.

Benefits of technology

The uniform deposition of the silver layer is achieved, wear resistance and conductivity are improved, the pluggable force is reduced, the service life of the contacts is extended, and the dependence on high-cost additives is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002871812070000141
    Figure BDA0002871812070000141
  • Figure BDA0002871812070000151
    Figure BDA0002871812070000151
Patent Text Reader

Abstract

The invention relates to a silver electrolyte for depositing a silver layer on a substrate, comprising silver potassium cyanide, potassium cyanide in an amount of at least 10 g / L, at least one grain refiner in an amount of 0.2 to 10 g / L, at least one dispersant in an amount of 1 to 10 g / L, at least one solid component in an amount of 1 to 150 g / L, wherein the particles of the solid component have an average particle size (d ) of 10 nm to 100 μm. 50 ). Furthermore, a contact surface and a method for depositing such a contact surface are shown, as well as the use of the electrolyte according to the invention in strip plating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a silver electrolyte for depositing a silver layer on a substrate, a method for depositing a dispersion silver layer on a substrate and a contact surface, wherein an electrochemically deposited dispersion silver layer is arranged on the substrate. The invention also relates to the use of the contact surface for electrical contacting in a plug connection and the use of a silver electrolyte for coating a substrate by means of strip plating. Background Art

[0002] Silver is a very versatile material. Due to its ductility and softness, it can be processed in a variety of ways. Silver has the best thermal and electrical conductivity of all metals. This makes silver an interesting material for the electrical and electronics industry, especially for coating surfaces, especially contact surfaces. As interfaces for transmitting high currents, plugs and plug contacts are used, which have the lowest possible contact resistance, so silver coatings are often used in contact elements that are installed in such plug connectors and provide electrical contact in the plugged state.

[0003] Silver electrolytes are used for silver coating of substrates and for producing contact surfaces. In this context, various silver-containing solutions and dispersions are referred to as silver electrolytes, which are used for electrochemically, in particular electroplating, silvering surfaces. Silver electrolyte solutions may contain various further additives, such as grain refiners, dispersants, brighteners or solid components.

[0004] For use in the electrical and electronic sector, especially in plugs and plug contacts, electrical conductivity, contact resistance and friction coefficient are particularly important. In particular, the requirements for silver layers, especially electroplated silver layers, are to be considered to be increasing, especially with regard to increasing electron mobility.

[0005] If two silver-coated surfaces are moved back and forth over each other, high forces are required for this purpose, since plugging forces and pulling forces act. This is disadvantageous for contact with silver surfaces, since silver surfaces have a relatively high coefficient of friction, which leads to high plugging forces and pulling forces, especially in the case of plugging contact. Due to the high coefficient of friction, the silver surfaces wear, which severely limits the number of possible plugging cycles. In addition, there is the problem that silver surfaces tend to cold weld. However, the contact resistance of the system of two silver-coated surfaces is advantageous.

[0006] DE 10346206 A1 describes a contact surface for electrical contact. Finely dispersed graphite particles are deposited in the illustrated silver layer (which is produced by means of an electroplating method). By incorporating graphite into the silver layer, a reduction in friction is achieved, thereby achieving lower plugging forces, improved corrosion protection, and a longer contact life due to increased wear protection. At the same time, good electrical contact is ensured.

[0007] DE 10 2008 030 988 B4 describes an electrochemical coating of a component, wherein the layer has a metallic structure and carbon nanotubes are introduced into the layer together with a dry lubricant. The introduction of the carbon nanotubes increases the electrical and thermal conductivity of the layer, and by mixing with a further dry lubricant the layer can be optimized for different purposes in terms of its wear behavior.

[0008] DE 2543082A1 discloses a silver electrolyte for producing a silver coating, which also contains graphite, a gloss additive and a wetting agent. The graphite must be kept in suspension during deposition by pumping the bath containing the electrolyte in circulation.

[0009] The prior art describes silver electrolytes which additionally contain glossing agents or other substances which improve deposition, such as xanthates, urethanes or door putty oils. The electrolyte solutions also appear to require mechanical intervention to keep the solid components in suspension. Electrolytes containing various solid components are also described in the prior art in order to obtain properties of the deposition surface which are lost due to expensive additive systems.

[0010] A disadvantage of known silver electrolytes for depositing silver on surfaces is that they do not disperse the substances to be dispersed sufficiently uniformly in the electrolyte, which leads on the one hand to an uneven distribution of the solid components in the deposited layer and on the other hand to partial complete non-deposition. Likewise, some electrolytes are not suitable for uniformly dispersing the various types of solid components, so that pumping circulation or stirring is required during deposition, which has a negative impact on the uniformity of the surface obtained. In order to overcome these disadvantages, expensive additive systems are usually used, which can have an adverse effect on the deposited surface and, moreover, lead to increased costs.

[0011] The known electrolytes are not able to disperse further particles, in particular dry lubricants, sufficiently well to obtain a surface into which other substances, such as additives, are simultaneously introduced which negatively influence the resulting dispersion layer. This results in, among other things, inhomogeneities of the known surfaces.

[0012] Furthermore, it is disadvantageous that, up to now, it has usually been necessary to use a combination of solid components, such as carbon nanotubes and dry lubricants, in order to achieve suitable surface properties and to compensate for the shortcomings of the additive system. This also results in additional substances that negatively affect the homogeneity and further increase the costs. In addition, additives that are intended to improve deposition make process control and process monitoring even more expensive and complex.

[0013] A further disadvantage of the known electrolytes is that a high deposition temperature must be selected in order to ensure adequate deposition. Summary of the invention

[0014] The object of the present invention is therefore to provide a silver electrolyte which allows good dispersion of the solid components and at the same time allows the elimination of expensive additive systems for achieving uniform deposition. Another object of the present invention is to provide surfaces, in particular contact surfaces, which have increased wear resistance and good electrical conductivity. The object of the present invention is also to provide a deposition method for producing coated surfaces, in particular contact surfaces, with improved durability.

[0015] Durability here means a reduction in the required plugging force with increasing possible plugging cycles, a reduction in cold welding (ie welding of the soft silver layer due to microvibrations) and the maintenance of the most favorable possible contact resistance over the longest possible period of time.

[0016] The object of the invention is achieved by a silver electrolyte according to claim 1. Preferred embodiments of the silver electrolyte according to the invention are given in the dependent claims, which can be selectively combined with one another.

[0017] The invention also provides a method for depositing a dispersion silver layer on a substrate according to claim 8. Preferred embodiments of the method according to the invention are given in the dependent claims, which can optionally be combined with one another.

[0018] The invention also comprises a contact surface according to the following claim 12. Preferred embodiments of the contact surface according to the invention are given in the dependent claims, which can optionally be combined with one another.

[0019] The invention furthermore relates to the use of the contact surface according to the invention for electrical contacting in plug connections and to the use of the dispersion silver electrolyte according to the invention for coating substrates by means of tape application.

[0020] The silver electrolyte for depositing a silver layer on a substrate comprises, according to the invention,

[0021] a) Potassium silver cyanide,

[0022] b) potassium cyanide with a content of at least 10 g / L,

[0023] c) at least one grain refiner having a content of 0.2 to 10 g / L;

[0024] d) at least one dispersant having a content of 1 to 10 g / L;

[0025] e) at least one solid component having a content of 1 to 150 g / L,

[0026] The particles of the solid component have an average particle size (d 50 ).

[0027] Surprisingly, it has been found that, by means of a silver electrolyte in the composition shown, various solid components can be uniformly dispersed to obtain a surface with a dispersion silver layer, which has an improved durability and good electrical conductivity. The electrolyte of the invention is characterized in that extremely different dispersion silver layers can be produced with it. These layers are characterized by their good contact resistance with improved friction values ​​or increased hardness, depending on the type and amount of the solid components introduced. The durability based on wear or friction of these layers exceeds that of a simple silver layer. In addition, the electrolyte of the invention is particularly well suited for uses in which solid components are used as the substance to be dispersed. In addition, a silver layer with good electrical conductivity is obtained by means of the electrolyte of the invention, so that the addition of further substances such as carbon nanotubes can be omitted. In addition, the electrolyte of the invention can be used both at low current densities and at high current densities. Therefore, the electrolyte can be used for various purposes and can be used, for example, for strip plating.

[0028] In the electrolyte according to the invention, the solid components are dispersed homogeneously. The particularly homogeneous dispersion ensures a homogeneous incorporation of the solid components into the deposited silver layer. In addition, the use of the electrolyte according to the invention reduces the concomitant incorporation of additives that usually negatively affect homogeneity.

[0029] Furthermore, the electrolyte is suitable for use with different solid components, so that the surface properties can be adapted to different applications. A further advantage of the electrolyte according to the invention is that the layer thickness can be varied and adapted to the respective application.

[0030] "Substituted" in the sense of the present invention means that a hydrogen atom on a hydrocarbon is replaced by another atom or group of atoms.

[0031] In the sense of the present invention, “solid components” are components which are not present in solution but are present as solids in the electrolyte and are also referred to in conjunction with the dispersion silver layer of the present invention as finely divided solid components.

[0032] In the sense of the present invention, the average particle size (d 50 ) means that 50% of the solid component particles have a diameter smaller than a given value.

[0033] In the context of the present invention, "grain refinement" is the process of changing the grain size of the silver deposit to a smaller grain size.

[0034] “Dry lubricants” in the sense of the present invention are substances which improve the sliding properties of a surface.

[0035] In the sense of the present invention, a “hard material” is a substance which is characterized by its particularly high hardness.

[0036] The silver electrolyte is a solution, preferably an aqueous solution. The electrolyte may also contain additional solvents.

[0037] Unless otherwise stated, all content data in g / L are below based on the total volume of the electrolyte.

[0038] In an advantageous embodiment, the content of potassium silver cyanide in the electrolyte is at least 10 g / L, preferably at least 25 g / L, more preferably at least 40 g / L, and even more preferably at least 50 g / L.

[0039] The silver content in the electrolyte is advantageously at least 15 g / L, preferably at least 20 g / L, more preferably at least 25 g / L, and still more preferably at least 27 g / L.

[0040] Preferably, the silver content in the electrolyte is between 1 and 100 g / L, preferably between 5 and 50 g / L, and even more preferably between 10 and 30 g / L.

[0041] Preferably, the content of potassium silver cyanide in the electrolyte is at most 150 g / L, preferably at most 125 g / L, more preferably at most 100 g / L, and still more preferably at most 75 g / L.

[0042] The content of potassium cyanide is preferably at least 20 g / L, preferably at least 50 g / L, more preferably at least 80 g / L, still more preferably at least 100 g / L, further still more preferably at least 120 g / L and most preferably at least 140 g / L.

[0043] In an advantageous embodiment, the at least one grain refiner is selected from naphthalenesulfonic acid, naphthalenesulfonic acid derivatives or mixtures thereof.

[0044] The content of grain refiner is advantageously between 0.2 and 8 g / L, preferably between 0.3 and 6 g / L, more preferably between 0.4 and 5 g / L and still more preferably between 0.5 and 3 g / L.

[0045] The dispersant preferably contains C1-C 25 Alkyl sulfates containing an alkyl group, and preferably containing a C1-C 20 Preferably, the dispersant comprises an alkyl sulfate having a C1-C 20 alkyl sulfates, and more preferably, having C1-C 20 Sodium alkyl sulfate of an alkyl group. The alkyl group may be linear and / or branched.

[0046] Preferably, the at least one dispersant is present in an amount between 0.2 and 9 g / L, preferably between 0.3 and 8 g / L, more preferably between 0.4 and 7 g / L and more preferably between 0.5 and 6 g / L.

[0047] Preferably, the content of at least one solid component is between 5 and 125 g / L, preferably between 10 and 100 g / L, more preferably between 15 and 90 g / L, and still more preferably between 20 and 80 g / L.

[0048] Preferably, the content of at least one solid component is at least 5 g / L, preferably at least 10 g / L, more preferably at least 15 g / L, still more preferably at least 20 g / L, further still more preferably at least 30 g / L, and most preferably at least 40 g / L.

[0049] In an advantageous embodiment, the particles of the at least one solid component have an average particle size (d ) of 50 nm to 75 μm, preferably 100 nm to 50 μm, more preferably 500 nm to 35 μm, and more preferably 1 μm to 20 μm. 50 The diameter of the solid component and thus the average particle size (d 50 ) is determined by means of laser diffraction.

[0050] Suitable solid components are all types of organic or inorganic particles.

[0051] Preferably, the at least one solid component is a dry lubricant, a hard material or a mixture thereof, preferably a dry lubricant.

[0052] In an advantageous embodiment, at least one solid component is selected from silicates, sulfides, carbides, nitrides, oxides, selenides, tellurides, organic and inorganic polymers and carbon modifications. In the sense of the present invention, carbon modifications are also understood to mean, in addition to diamond, hexagonal carbon, fullerenes and graphite, graphene, carbon nanotubes, carbon black, activated carbon, graphite fluoride, graphite oxide, Al2O3-coated graphite, non-graphitic forms of carbon and other forms.

[0053] According to a preferred embodiment, the at least one solid component is selected from MoS2, WS2, SnS2, NbS2, TaS2, graphite, graphite fluoride, graphite oxide, hexagonal boron nitride, silver niobium selenide, TiN, Si3N4, TiB2, WC, TaC, B4C, Al2O3, ZrO2, cubic BN, diamond, MoSe2, WSe2, TaSe2, NbSe2, SiC, Al2O3-coated graphite, Al2O3-coated MoS2 and Al2O3-coated WS2 or a mixture thereof, preferably from MoS2, WS2, graphite, graphite oxide, hexagonal boron nitride or a mixture thereof, more preferably from graphite, graphite oxide, MoS2, WS2 or a mixture thereof, and even more preferably from graphite.

[0054] Al2O3-coated solid particles are produced by coating solid particles with the aid of controlled hydrolysis of Al(NO3)3·9H2O according to Huang & Xiong (2008) (Huang, Z.; Xiong, D. (2008): Coating of MoS2 with Al2O3 by pulse electrodeposition for Ni-MoS2 / Al2O3 composite coatings. Surfaces & Coatings & Technology 202 (2008) 3208-3214).

[0055] According to an advantageous embodiment, at least one solid component is selected from silicates, sulfides, carbides, nitrides, oxides, selenides, tellurides, organic and inorganic polymers. Preferably, the at least one solid component is selected from MoS2, WS2, SnS2, NbS2, TaS2, hexagonal boron nitride, silver niobium selenide, TiN, Si3N4, TiB2, WC, TaC, B4C, Al2O3, ZrO2, cubic BN, MoSe2, WSe2, TaSe2, NbSe2, SiC, Al2O3-coated MoS2 and Al2O3-coated WS2 or a mixture thereof, preferably consisting of MoS2, WS2, hexagonal boron nitride or a mixture thereof, more preferably consisting of MoS2, WS2 or a mixture thereof.

[0056] According to another advantageous embodiment, the at least one solid component is selected from carbon modifications. Preferably, the at least one solid component is selected from graphite, graphite fluoride, graphite oxide, diamond, Al2O3-coated graphite or a mixture thereof, preferably graphite, graphite fluoride, graphite oxide, Al2O3-coated graphite or a mixture thereof, more preferably graphite, graphite oxide or a mixture thereof, and even more preferably graphite.

[0057] Preferably, the electrolyte further comprises at least one additional solid component. The at least one additional solid component may be selected from the above-mentioned solid components.

[0058] Advantageously, the electrolyte may additionally contain a glossing agent. For this purpose, amounts of 1 to 1000 mg / L, preferably less than 50 mg / L, are generally used. Examples of glossing agents are phenylpropionic acid, phenylpropionic acid amide, triaminotriphenylmethane, 1-(p-aminophenyl)-3-methylpyrazole, stearamidopropyldimethyl-(β-hydroxyethyl)dihydrogenammonium phosphate, 1,5-diphenylcarbazide and chlorohydrate.

[0059] The silver electrolyte of the present invention may optionally contain further additives, such as stabilizers, dispersants and / or grain refiners, to further improve the properties of the electrolyte and to improve the properties of the deposited dispersion silver layer.

[0060] The above-mentioned embodiments may also be combined.

[0061] A further subject of the invention is a method for depositing a dispersion silver layer on a substrate, which according to the invention comprises the following steps:

[0062] a) providing the silver electrolyte of the present invention,

[0063] b) introducing a substrate into the silver electrolyte, and

[0064] c) performing deposition.

[0065] The method of the present invention comprises depositing a dispersion silver layer on a substrate of the silver electrolyte according to the present invention according to any of the above embodiments. The above description of the electrolyte according to the present invention also applies to the present method accordingly.

[0066] In the method according to the invention, all substrates commonly used for depositing silver layers and dispersion silver layers can be used. In the method according to the invention, the substrate preferably comprises a metal or a metal alloy. The dispersion silver layer is then deposited on the metal or metal alloy. The metal or metal alloy can, for example, contain copper and / or iron or consist of them. Likewise, further intermediate layers consisting of other metals, for example nickel or silver, can be present. These layers have various functions, for example increasing the adhesion of the dispersion silver layer on the substrate, corrosion protection, diffusion resistance, or improving other physical properties.

[0067] Electroplating or currentless methods can be used as deposition methods. Examples of electroplating methods are barrel plating, rack plating or strip plating.

[0068] The substrate is preferably cleaned, preferably degreased, before coating. Various pretreatment steps may be performed on the substrate. Here, a copper layer, a nickel layer and / or an additional silver layer may be deposited.

[0069] Preferably, the substrate is pre-silvered before step a). Preferably, the substrate is nickel-plated before pre-silvering.

[0070] According to an advantageous embodiment, the temperature when depositing in step c) is 1°C to 50°C, preferably 5°C to 40°C, more preferably 5°C to 35°C, still more preferably 10°C to 30°C, further still more preferably 15°C to 25°C, still more preferably 17°C to 22°C, and most preferably 20°C.

[0071] In an advantageous embodiment, the current density in step c) is 1.2 A / dm 2 Up to 35.0A / dm 2 , preferably 1.5A / dm 2 Up to 30.0A / dm 2 , more preferably 2.0A / dm 2 Up to 25.0A / dm 2 , more preferably 2.5A / dm 2 Up to 25.0A / dm 2 And more preferably 2.5A / dm 2 Up to 20.0A / dm 2 .

[0072] According to an advantageous embodiment, the method is strip plating.

[0073] The duration of the deposition can be selected as a function of the desired layer thickness to be achieved and the intended use, the strip coating. In principle, the duration of the deposition is not restricted.

[0074] Preferably, the duration of the deposition in step c) is from 0.1 minutes to 20 minutes, preferably from 0.15 minutes to 15 minutes and more preferably from 0.3 minutes to 10 minutes.

[0075] Preferably, step a) is performed before step b), and more preferably, step b) is performed after step c).

[0076] Another subject matter of the invention relates to a contact surface in which an electrochemically deposited dispersion silver layer is arranged on a substrate according to the invention, and

[0077] The dispersion silver layer contains particles of at least one finely divided solid component having an average particle size (d 50 ).

[0078] The above descriptions of the electrolyte according to the invention and the method according to the invention also apply accordingly to the contact surface. Thus, the finely dispersed solid component can be selected from the above-mentioned solid components. As a substrate for the contact surface according to the invention, all the above-mentioned substrates can be used.

[0079] When a dry lubricant is used as the solid component, the contact surface according to the invention allows only one of the contact partners to be provided with a dispersion silver surface. The other contact partner can consist of a conventional metal surface without solid components, in particular dry lubricant components. This makes it possible to reduce costs. However, it is also possible to provide both contact partners with a dispersion silver surface.

[0080] The contact surface according to the invention is characterized by its advantageous wear resistance. In particular, the resistance to wear due to micro-movements, so-called micro-motions, during the plugging process is significantly improved. Such micro-movements occur, for example, in plugs of automobiles due to vibrations during operation of the automobile. Wear due to micro-movements can also occur due to temperature fluctuations.

[0081] Preferably, the contact surface further comprises at least one further solid component. Preferably, the at least one further solid component is a dry lubricant or a hard material. Preferably, the at least one further solid component is selected from the solid components described above for the electrolyte according to the invention, which are also correspondingly suitable for the contact surface.

[0082] In an advantageous embodiment, the particles of the at least one finely divided solid component have an average particle size (d ) of 50 nm to 75 μm, preferably 100 nm to 50 μm, more preferably 500 nm to 35 μm, and even more preferably 1 μm to 20 μm. 50 ). The same applies to the particles of the further solid components.

[0083] The content of at least one finely divided solid component in the dispersion silver layer can be varied by changing the deposition conditions. In this way, the properties of the surface with respect to contact resistance and wear resistance can be adjusted.

[0084] Preferably, the dispersion silver layer comprises at least one finely divided solid component in an amount ranging from 0.5 wt % to 30.0 wt %, preferably from 1.0 wt % to 25 wt %, more preferably from 1.3 wt % to 20 wt %, still more preferably from 1.5 wt % to 15 wt %, still further more preferably from 2.0 wt % to 10 wt %, and still more preferably from 3.1 wt % to 10 wt %, based on the total weight of the dispersion silver layer.

[0085] Preferably, the dispersion silver layer comprises at least one finely divided solid component in an amount range of at least 3.0 wt. %, preferably at least 3.1 wt. %, more preferably at least 3.2 wt. %, still more preferably at least 3.2 wt. %, still further more preferably at least 3.3 wt. %, and still more preferably at least 3.5 wt. %, based on the total weight of the dispersion silver layer.

[0086] Preferably, the at least one finely divided solid component is selected from silicates, sulfides, carbides, nitrides, oxides, selenides, tellurides, organic and inorganic polymers and carbon modifications.

[0087] According to an advantageous embodiment of the contact surface, the at least one finely dispersed solid component is selected from silicates, sulfides, carbides, nitrides, oxides, selenides, tellurides, organic and inorganic polymers. Preferably, the at least one finely dispersed solid component is selected from MoS2, WS2, SnS2, NbS2, TaS2, hexagonal boron nitride, silver niobium-selenide, TiN, Si3N4, TiB2, WC, TaC, B4C, Al2O3, ZrO2, cubic BN, MoSe2, WSe2, TaSe2, NbSe2, SiC, Al2O3-coated MoS2 and Al2O3-coated WS2 or mixtures thereof, preferably consists of MoS2, WS2, hexagonal boron nitride or mixtures thereof, more preferably consists of MoS2, WS2 or mixtures thereof.

[0088] According to another advantageous embodiment of the contact surface, the at least one finely divided solid component is selected from carbon modifications. Preferably, the at least one finely divided solid component is selected from graphite, fluorinated graphite, graphite oxide, diamond, Al2O3-coated graphite or mixtures thereof, preferably graphite, fluorinated graphite, graphite oxide, Al2O3-coated graphite or mixtures thereof, more preferably graphite, graphite oxide or mixtures thereof, and even more preferably graphite.

[0089] According to another advantageous embodiment, the at least one finely dispersed solid component is selected from MoS2, WS2, SnS2, graphite, graphite oxide, graphite fluoride, hexagonal boron nitride, silver niobium-selenide, SiC, Al2O3-coated graphite, Al2O3-coated MoS2 and Al2O3-coated WS2 or a mixture thereof, preferably consisting of MoS2, WS2, graphite and hexagonal boron nitride or a mixture thereof.

[0090] In another advantageous embodiment of the contact surface, the at least one finely divided solid component is selected from graphite, MoS2, WS2 or mixtures thereof, preferably consists of graphite, and the dispersion silver layer contains the at least one finely divided solid component in an amount of at least 3.0 wt.-%, preferably at least 3.1 wt.-%, more preferably at least 3.2 wt.-%, and even more preferably at least 3.3 wt.-% and even more preferably at least 3.5 wt.-%, based on the total weight of the dispersion silver layer.

[0091] Preferably, the dispersion silver layer has a coefficient of friction μ at 0.3 N after 100 cycles of less than 1.4, preferably less than 1.2, more preferably less than 1.0, still more preferably less than 0.8, still further more preferably less than 0.6 and still more preferably 0.4.

[0092] Preferably, the contact resistance is less than 1.0 mΩ, preferably less than 0.8 mΩ, more preferably less than 0.75 mΩ, still more preferably less than 0.7 mΩ, still more preferably less than 0.65 mΩ after 100 cycles at 1.0 N.

[0093] Preferably, the dispersion silver layer has a coefficient of friction μ at 1.0 N after 100 cycles of less than 1.0, preferably less than 0.8, more preferably less than 0.6, still more preferably less than 0.5 and still further more preferably less than 0.45.

[0094] The layer thickness of the deposited dispersion silver layer is preferably between 0.5 μm and 200 μm, preferably between 1 μm and 100 μm, particularly preferably between 1.1 μm and 25 μm.

[0095] Advantageously, the contact surface is a micro-rough surface. The microstructure has a favorable effect on the tribological and electrical properties.

[0096] Preferably, the contact surface has a micro-roughness as described below by the average roughness value Ra of at least 0.05 μm, preferably at least 0.1 μm, more preferably at least 0.2 μm and still more preferably at least 0.3 μm.

[0097] Preferably, the touch surface has a micro-roughness as described below by the average roughness value Ra in the range of 0.05 μm to 20 μm, preferably 0.1 μm to 10 μm, more preferably 0.2 μm to 6 μm and still more preferably at least 0.3 μm to 5 μm.

[0098] Preferably, the contact surface has a fretting life at 1.0 N according to Song of greater than 7500 cycles, preferably greater than 10000 cycles, more preferably greater than 15000 cycles, still more preferably greater than 20000 cycles, and still more preferably greater than 25000 cycles.

[0099] The above-mentioned contact surface can be produced by means of the method according to the invention described above. Therefore, the present invention also includes a contact surface obtainable by the method according to the invention, wherein an electrochemically deposited dispersion silver layer is arranged on a substrate, and wherein the dispersion silver layer comprises at least one having an average particle size (d 50 ) of finely dispersed solid components.

[0100] The above statements about the electrolyte according to the invention, the method according to the invention and the contact surface according to the invention also apply accordingly to the contact surface obtainable by means of the method according to the invention. Thus, the finely divided solid component can be selected from the solid components mentioned above. As substrates for the contact surface according to the invention, all the aforementioned substrates can be used.

[0101] A further subject matter of the invention relates to the use of the contact surface according to the invention for electrical contacting in a plug connection.

[0102] A further subject matter of the present invention relates to the use of the dispersion silver electrolyte according to the invention for coating substrates by means of tape application.

[0103] Further advantages of the invention are apparent from the following description of preferred exemplary embodiments, which, however, are not to be understood as limiting in any way. All embodiments of the invention can be combined with one another within the scope of the invention. DETAILED DESCRIPTION

[0104] Material

[0105] Copper plates from Wieland-Werke AG (material: CuFe2P) were used for the tests. The uncoated plates had an average roughness Ra of 0.47 μm.

[0106] KCN was purchased from Bücherl and K[Ag(CN)2] from Umicore.

[0107] SLOTOSIL SG 1911 and SLOTOSIL SG 1912 are Dr.Ing.Max Additives for KCN / silver potassium cyanide based silver electrolytes for dispersion deposition from the company SLOTOSIL GmbH & Co. KG. SLOTOSIL SG 1911 contains a naphthalenesulfonic acid derivative as a grain refiner additive. SLOTOSIL SG 1912 contains an alkyl sulfate as a dispersion stabilizer additive.

[0108] CUPRUM 11, whitening agent, CUPRUM 12, wetting agent, and antioxidant concentrate AG 111 are composed of &Co KG purchased.

[0109] The graphite used was graphite from Kropfmühl AG. The UF2-type graphite particles used had an average particle size of d50=4.5 μm.

[0110] Measurement method

[0111] Determine the solid content

[0112] The solid content (in % by weight) was determined by energy dispersive X-ray spectroscopy (EDX). For this purpose, the measurements were carried out on the deposited thin films with an X-Flash Detector 410-M (Bruker AXS Microanalysis GmbH), which was installed in an electron microscope JSM-6610LV (manufacturer: JEOL) with an excitation voltage of 25 kV. The measurement results were evaluated using the Esprit (Bruker) program.

[0113] Determine the diameter of the solid component (d 50 )

[0114] The average particle size d 50 The particle diameter of the solid component is measured in the form of

[0115] Measurement of micro-roughness (as average roughness value Ra)

[0116] By means of an optical measurement method, the microscopic roughness (as the average roughness Ra) was determined using a confocal 3D laser scanning microscope VK-X100 (manufacturer: Keyence Corporation) and subsequently evaluated using the Multi fite analyzer program (Keyence Corporation).

[0117] Coated copper plate

[0118] plating

[0119] The sample body was coated with a dispersion silver layer to obtain the contact surface. The copper plate was first copper plated, then pre-silver plated, and then coated with a dispersion silver layer.

[0120] Rinse thoroughly with water between steps.

[0121] The electroplating of copper plate includes the following steps:

[0122] Steps 1 and 2: Degreasing of the substrate according to known methods; first alkaline degreasing step, at 60°C with ultrasound assistance for 1 minute. Second alkaline electrolytic degreasing step, at room temperature (25°C) for a treatment time of 2 to 3 minutes.

[0123] Step 3: Etch the copper using a sulfuric acid-based, non-complexing agent copper activation bath. The activation was performed at room temperature (25°C) for 0.5 minutes.

[0124] Step 4: Treat with a glossy copper bath to deposit a glossy surface. The glossy copper bath is a cyanide electrolyte. The electrolyte consists of 10 g / l KOH, 115 g / l KCN, 64 g / l CuCN and 1.5 ml / l of glossy additive CUPRUM 11; 2.5 ml / l of base additive CUPRUM 12 operated at 60°C. The electrolyte has a 2A / dm 2 .

[0125] Step 5: Pre-silvering is carried out in a pre-silvering bath with a cyanide electrolyte with a low silver content (120 g / l KCN, 3.7 g / l K[Ag(CN)2]). The pre-silvering is carried out at room temperature (25°C). 2 A / dm 2 as the cathode current density.

[0126] Step 6: Deposition of dispersion silver layer.

[0127] The sheet material pretreated as described above is mounted on a rotary unit for coating.

[0128] The electrolyte has the following composition:

[0129]

[0130] The sheets were coated at different rotation speeds to simulate belt speeds of 30 m / min, 60 m / min and 100 m / min. 2 , 5A / dm 2 、10A / dm 2 、15A / dm 2 or 20A / dm 2 The deposition occurred at a current density of 1.5 Å / min. The detailed description of each test is listed in Table 1.

[0131] Step 7: Antioxidant post-treatment; Antioxidant protector 160 mL / L of antioxidant concentrate AG 111 was used at 50°C and pH 5.3. The coated sample body was immersed in the antioxidant protector for 2 minutes. Then rinsed with deionized water and dried.

[0132] The results of the characterization of the deposited dispersion silver layers are shown in Table 1. The graphite content of the graphite-containing dispersion silver layers was determined by means of EDX.

[0133] Table 1: Strip plating results

[0134]

[0135] The results presented in Table 1 show that the electrolyte according to the invention is suitable for the deposition of dispersion silver layers. Compared to electrolytes known from the prior art for producing dispersion silver layers, the particle contents achieved are significantly higher, which represents a clear improvement.

[0136] In contrast to known electrolytes for producing dispersion silver layers, the electrolyte according to the invention is particularly suitable for the deposition of dispersion silver layers by means of a tape process (roll-to-roll process).

[0137] By introducing solid components, in particular dry lubricants, into the dispersion silver layer, significantly better sliding properties are achieved, especially at high concentrations of solid components, compared to pure silver layers. A high solid particle concentration in the layer is particularly advantageous for wear caused by microvibrations (fretting). For small contact points, the probability that a sufficient amount of solid particles is present in the contact area to avoid wear is higher in the case of a high solid particle concentration. This property is of particular significance for the contact surfaces of plug connections and, as shown in the exemplary embodiments, is achieved by the method according to the invention.

Claims

1. A silver electrolyte for depositing a silver layer on a substrate, comprising a) potassium silver cyanide with a content of at least 50 g / L, b) potassium cyanide with a content of at least 100 g / L, c) at least one grain refiner having a content of 0.2 to 10 g / L; d) at least one dispersant having a content of 1 to 10 g / L; e) at least one solid component having a content of 1 to 150 g / L, The particles of the solid component have an average particle size of 10 nm to 100 μm. 50 ; wherein the grain refiner is SLOTOSIL SG 1911; and wherein the at least one dispersant comprises an unsubstituted or selectively substituted C1-C 20 Alkyl sulfates of alkyl.

2. The silver electrolyte according to claim 1, wherein the particles of the at least one solid component have an average particle size d of 1 μm to 20 μm. 50 .

3. The silver electrolyte according to claim 1 or 2, wherein at least one solid component is selected from a. graphite, graphite fluoride, graphite oxide, diamond, Al2O3 coated graphite or mixtures thereof; or b. MoS2, WS2, SnS2, NbS2, TaS2, hexagonal boron nitride, silver niobium selenide, TiN, Si3N4, TiB2, WC, TaC, B4C, Al2O3, ZrO2, cubic BN, MoSe2, WSe2, TaSe2, NbSe2, SiC, Al2O3-coated MoS2 and Al2O3-coated WS2 or their mixtures.

4. A method for depositing a dispersion silver layer on a substrate, comprising the following steps, a) providing a silver electrolyte as claimed in any one of claims 1 to 3, b) introducing a substrate into the silver electrolyte, and c) performing deposition.

5. The method according to claim 4, wherein the temperature in step c) is 15°C to 30°C.

6. The method according to claim 4, wherein the current density in step c) is 2.0 A / dm 2 Up to 25.0A / dm 2 .

7. The method according to any one of claims 4 to 6, wherein the method is strip plating.

8. A contact surface produced according to the method according to any one of claims 4 to 7, wherein an electrochemically deposited dispersion silver layer is arranged on the substrate, The dispersion silver layer comprises particles of at least one finely divided solid component having an average particle size d of 10 nm to 100 μm. 50 ; wherein the dispersion silver layer comprises the at least one finely divided solid component in an amount of 3.1 to 10 wt %, based on the total weight of the dispersion silver layer; and The contact surface has a micro-roughness in the range of 0.05 μm to 20 μm, as described by an average roughness value Ra.

9. The contact surface according to claim 8, wherein at least one finely divided solid component is selected from a. MoS2, WS2, SnS2, NbS2, TaS2, hexagonal boron nitride, silver niobium-selenide, TiN, Si3N4, TiB2, WC, TaC, B4C, Al2O3, ZrO2, cubic BN, MoSe2, WSe2, TaSe2, NbSe2, SiC, Al2O3-coated MoS2 and Al2O3-coated WS2 or mixtures thereof; or b. graphite, graphite fluoride, graphite oxide, diamond, Al2O3 coated graphite or mixtures thereof; or c. MoS2, WS2, SnS2, graphite, graphite oxide, graphite fluoride, hexagonal boron nitride, silver niobium-selenide, SiC, Al2O3-coated graphite, Al2O3-coated MoS2 and Al2O3-coated WS2 or mixtures thereof.

10. Use of a contact surface according to any one of claims 8 to 9 for electrical contacting in a plug connection.

11. Use of a dispersion silver electrolyte according to any one of claims 1 to 3 for coating substrates by means of tape application.