Modified polyphenylene ether resin, polyphenylene ether composite material and preparation method thereof, and printed circuit board
By introducing a phosphorus-containing group containing only one benzene ring or no benzene ring into polyphenylene ether resin, and combining it with specific cross-linking agents and fillers, the problem of improving flame retardancy and heat resistance of polyphenylene ether resin is solved. To solve the problem of reduced electrical properties, the polyphenylene ether composite material has high flame retardancy, heat resistance and excellent mechanical properties, making it suitable for high-speed and high-frequency signal transmission.
Patent Information
- Application Number
- CN201911022837.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-10-25
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2039-10-25
AI Technical Summary
When existing polyphenylene ether resins are improved in flame retardancy and heat resistance, their dielectric properties and mechanical properties are usually reduced, and the introduction of phosphorus-containing groups will affect their structural rigidity, making it difficult to meet the requirements of high speed, high frequency, and large capacity at the same time. signal transmission requirements.
Using a phosphorus-containing group containing only one benzene ring or no benzene ring as the end-capping group, the polyphenylene ether resin is modified, and through the substitution reaction with phosphorus-containing compounds and vinyl alcohol compounds, a high-performance Modified polyphenylene ether resin with cross-linking activity and flame retardant properties, combined with specific cross-linking agents and fillers, forms a dense polyphenylene ether composite material.
It achieves high flame retardancy, heat resistance and excellent mechanical properties of polyphenylene ether composite materials, while maintaining low dielectric constant and dielectric loss, making it suitable for high-speed and high-frequency signal transmission applications.
Smart Images

Figure CN112708128B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to polymer materials, in particular to modified polyphenylene ether resin, polyphenylene ether composite material and preparation method thereof, and printed circuit board. Background Art
[0002] With the development of the printed circuit board (PCB) industry, the application fields of PCB involve almost all electronic products, mainly including communications, aerospace, consumer electronics, automotive electronics and other industries. In the era of 5G communication, high-frequency information transmission has prompted electronic circuit design to enter the stage of high-speed information processing and high-frequency signal transmission. Ordinary circuit substrates (epoxy resin-based, cyanate resin-based copper-clad boards) have high-frequency disadvantages such as large high-frequency signal loss, severe heat generation, and unstable transmission, making it difficult to meet the requirements of high-speed information applications. For high-speed, high-frequency, and large-capacity signal transmission, it is key to develop materials with high and low dielectric constants, low dielectric loss, high reliability, high moisture and heat resistance, and high dimensional stability.
[0003] Polyphenylene ether (PPO) has a symmetrical structure, contains a large number of rigid benzene rings, has more side methyl groups, has a rigid molecular chain, and has no strong polar groups. These structural characteristics give PPO resin a high glass transition temperature and a high thermal decomposition temperature, low dielectric constant and dielectric loss. In the temperature range of -150°C to 200°C and the frequency range of 10Hz to 10GHz, the dielectric constant and dielectric loss are almost unaffected, and the water absorption rate is not more than 0.05%. These excellent properties have laid the foundation for it as an electronic material. Therefore, polyphenylene ether resin is the preferred resin material for preparing high-frequency and high-speed copper-clad laminates. However, PPO resin has poor flame retardancy and heat resistance.
[0004] In order to overcome the problem of poor flame retardancy and heat resistance, the traditional method adopts the method of adding flame retardants to polyphenylene ether to prepare composite materials. However, with the addition of flame retardants, the heat resistance and dielectric properties of the entire resin system will be reduced. Another method attempts to introduce phosphorus-containing groups into the molecular structure of polyphenylene ether in order to improve the flame retardancy of polyphenylene ether resin. At the same time, according to the general knowledge of technicians, phosphorus-containing groups are strong polar groups and have a negative effect on the properties of polyphenylene ether. Therefore, more rigid benzene rings are usually introduced at the same time as the introduction of phosphorus-containing groups, in order to reduce or avoid the adverse effects of the introduction of phosphorus-containing groups on the mechanical properties and dielectric properties of the polyphenylene ether resin itself, but the effect is not good. Summary of the invention
[0005] Based on this, it is necessary to provide a new type of modified polyphenylene ether resin using a phosphorus-containing group containing only one benzene ring or no benzene ring as a capping group, wherein the modified polyphenylene ether resin can be cross-linked to form a polyphenylene ether composite material having excellent flame retardant properties and heat resistance, as well as good mechanical properties, low dielectric constant and low dielectric loss.
[0006] A modified polyphenylene ether resin having the following structural characteristics:
[0007]
[0008] Wherein, Y is -CH2-, -CH(CH3)-, -C(CH3)2-, -O- or carbonyl;
[0009] m and n are each independently a positive integer from 1 to 15;
[0010] R1 to R 23 are each independently hydrogen, methyl or halo;
[0011] R0 is
[0012]
[0013] In one embodiment, R0 is:
[0014]
[0015] In one embodiment,
[0016] Y is -CH2-, carbonyl, -CH(CH3)-, or -C(CH3)2-;
[0017] m and n are each independently a positive integer of 4 to 15.
[0018] The present invention also provides a method for preparing a modified polyphenylene ether resin, wherein a monomer 1 is used to modify the polyphenylene ether resin; the monomer 1 is prepared by a substitution reaction between a phosphorus-containing compound and a vinyl-containing alcohol compound:
[0019] Wherein, the phosphorus-containing compound is selected from at least one of phosphorus oxychloride, ethyl dichlorophosphate, phenyl dichlorophosphate, phenyl phosphoryl dichloride and pyrophosphoryl chloride;
[0020] The vinyl alcohol compound is selected from at least one of propylene alcohol, methpropylene alcohol and 2-hydroxyethyl acrylate;
[0021] The polyphenylene ether resin is hydroxyl-terminated polyphenylene ether.
[0022] In one embodiment, the phosphorus-containing compound is selected from at least one of phosphorus oxychloride, ethyl dichlorophosphate and pyrophosphoryl chloride.
[0023] In one embodiment, the number average molecular weight of the polyphenylene ether resin is 1500-2500 g / mol.
[0024] In one embodiment, the preparation method of the modified polyphenylene ether resin comprises the following steps:
[0025] Preparation of the monomer 1: dissolving the phosphorus-containing compound in an organic solvent, adding the vinyl-containing alcohol compound under alkaline conditions, and performing a substitution reaction to obtain the monomer 1;
[0026] Preparation of the modified polyphenylene ether resin: The monomer 1 and the polyphenylene ether resin are mixed and subjected to a substitution reaction under the action of a catalyst.
[0027] In one embodiment, in the preparation of the monomer 1, the molar ratio of the chlorine group in the phosphorus-containing compound to the hydroxyl group in the vinyl-containing alcohol compound is greater than 1;
[0028] In the preparation of the modified polyphenylene ether resin, the molar ratio of the chlorine groups in the phosphorus-containing compound to the hydroxyl groups in the polyphenylene ether resin is greater than 3.
[0029] The present invention also provides a polyphenylene ether composite material, which is formed by curing the modified polyphenylene ether resin or the modified polyphenylene ether resin prepared by the preparation method.
[0030] In one embodiment, the polyphenylene ether composite material is made of raw materials including the following components in parts by weight:
[0031] 100 parts of the modified polyphenylene ether resin or the modified polyphenylene ether resin prepared by the preparation method,
[0032]
[0033]
[0034] In one embodiment, the cross-linking agent includes a main cross-linking agent and an auxiliary cross-linking agent; the main cross-linking agent is styrene-butadiene copolymer and / or maleic anhydride-modified styrene-butadiene copolymer, and the auxiliary cross-linking agent is triallyl isocyanurate.
[0035] In one embodiment, the cross-linking agent includes a main cross-linking agent and an auxiliary cross-linking agent in a weight ratio of 1:0.4-0.6.
[0036] In one embodiment, the initiator is a peroxide initiator; and / or
[0037] The filler is silicon dioxide; and / or
[0038] The fibers are glass fibers.
[0039] The present invention also provides a method for preparing the polyphenylene ether composite material, comprising the following steps:
[0040] The modified polyphenylene ether resin or the modified polyphenylene ether resin prepared by the preparation method, a crosslinking agent, an initiator and a filler are mixed in a solvent, impregnated with the fiber, dried and solidified.
[0041] The invention also provides a printed circuit board, the substrate of which is made of the polyphenylene ether composite material.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] According to the common knowledge of those skilled in the art, one of the reasons why polyphenylene ether has a high glass transition temperature and a high thermal decomposition temperature, a low dielectric constant and a dielectric loss is that its structure contains a large number of rigid benzene rings and has no structural characteristics of strong polar groups. Therefore, if the flame retardancy and heat resistance of polyphenylene ether are improved by introducing phosphorus-containing groups, since the phosphorus-containing groups are strong polar groups, more (more than 2) benzene rings are usually introduced at the same time to ensure the rigidity of the structure, thereby ensuring its mechanical properties and dielectric properties.
[0044] The present invention changes this traditional concept, and innovatively modifies polyphenylene ether with an alkenyl-containing and phosphorus-containing end-capping group containing only one benzene ring or no benzene ring, so as to prepare a novel modified polyphenylene ether resin. The modified polyphenylene ether resin has small end-group reaction hindrance and high cross-linking activity, which is conducive to cross-linking to form a densely structured polyphenylene ether composite material, thereby ensuring its mechanical properties and dielectric properties, and at the same time, the flame retardant properties of phosphorus can be brought into play, so that the prepared polyphenylene ether composite material has good flame retardancy and heat resistance. DETAILED DESCRIPTION
[0045] The modified polyphenylene ether resin, the polyphenylene ether composite material and the preparation method thereof, and the printed circuit board of the present invention are further described in detail below in conjunction with specific embodiments.
[0046] The embodiment of the present invention provides a modified polyphenylene ether resin having the following structural features:
[0047]
[0048] Wherein, Y is -CH2-, -CH(CH3)-, -C(CH3)2-, -O- or carbonyl;
[0049] m and n are each independently a positive integer from 1 to 15;
[0050] R1 to R 23 are each independently hydrogen, methyl or halo;
[0051] R0 is
[0052]
[0053] Preferably, R0 does not contain a benzene ring. Using R0 as the end group to modify the polyphenylene ether has a small reaction steric hindrance and a higher cross-linking activity, which is beneficial to improving the mechanical properties and dielectric properties of the modified polyphenylene ether resin. Specifically, R0 is:
[0054]
[0055] In one specific embodiment, Y is -CH2-, carbonyl, -CH(CH3)-, or -C(CH3)2-; m and n are independently one of positive integers from 4 to 15. Correspondingly, the number average molecular weight of the polyphenylene ether resin before modification (i.e., when R0 is hydroxyl) is 1500-2500 g / mol.
[0056] The embodiment of the present invention further provides a method for preparing a modified polyphenylene ether resin, wherein a monomer 1 is used to modify the polyphenylene ether resin; the monomer 1 is prepared by a substitution reaction between a phosphorus-containing compound and a vinyl-containing alcohol compound:
[0057] Wherein, the phosphorus-containing compound is selected from at least one of phosphorus oxychloride, ethyl dichlorophosphate, phenyl dichlorophosphate, phenyl phosphoryl dichloride and pyrophosphoryl chloride;
[0058] The vinyl alcohol compound is selected from at least one of propylene alcohol, methpropylene alcohol and 2-hydroxyethyl acrylate;
[0059] The polyphenylene ether resin is hydroxyl-terminated polyphenylene ether.
[0060] It can be understood that, in order to carry out the modification, the monomer 1 should have an active group that can react with the polyphenylene ether resin. For example, if the polyphenylene ether resin is a hydroxyl-terminated polyphenylene ether, the monomer 1 should have a group that can undergo a substitution reaction with the hydroxyl group, such as a chlorine group. That is to say, after the phosphorus-containing compound and the vinyl-containing alcohol compound undergo a substitution reaction, the prepared monomer 1 should still have a residual chlorine group for the modification.
[0061] Preferably, the monomer 1 does not contain a benzene ring. Specifically, the phosphorus-containing compound is selected from at least one of phosphorus oxychloride, ethyl dichlorophosphate and pyrophosphoryl chloride.
[0062] In one specific embodiment, the number average molecular weight of the polyphenylene ether resin is 1500 to 2500 g / mol. In one more specific embodiment, the polyphenylene ether resin is NORYL TM SA120 resin or NORYL TM SA90 resin.
[0063] In one specific embodiment, the preparation method of the modified polyphenylene ether resin comprises the following steps:
[0064] Preparation of the monomer 1: dissolving the phosphorus-containing compound in an organic solvent, adding the vinyl-containing alcohol compound under alkaline conditions, and performing a substitution reaction to obtain the monomer 1;
[0065] Preparation of the modified polyphenylene ether resin: The monomer 1 and the polyphenylene ether resin are mixed and subjected to a substitution reaction under the action of a catalyst.
[0066] In one specific embodiment, in the preparation of the monomer 1, the molar ratio of the chlorine group in the phosphorus-containing compound to the hydroxyl group in the vinyl-containing alcohol compound is greater than 1; thereby, the chlorine group in the phosphorus-containing compound will not completely react with the hydroxyl group in the vinyl-containing alcohol compound, so that subsequent modification can be carried out;
[0067] In the preparation of the modified polyphenylene ether resin, the molar ratio of the chlorine group in the phosphorus-containing compound to the hydroxyl group in the polyphenylene ether resin is greater than 3; thus, during the modification process, a large excess of monomer 1 is beneficial to complete replacement of the terminal hydroxyl group of the polyphenylene ether resin by monomer 1.
[0068] In one specific embodiment, in the preparation of the monomer 1, the molar ratio of the chlorine group in the phosphorus-containing compound to the hydroxyl group in the vinyl-containing alcohol compound is 3:1.5-2.5; in the preparation of the modified polyphenylene ether resin, the molar ratio of the chlorine group in the phosphorus-containing compound to the hydroxyl group in the polyphenylene ether resin is 2.5:0.5-1.
[0069] In the preparation of the above monomer 1, the type of the organic solvent is not limited, as long as it is inert and does not react chemically with the phosphorus-containing compound and the vinyl-containing alcohol compound. Preferably, it is an alkaline organic solvent that can bind protons, thereby promoting the rapid progress of the substitution reaction. In one specific embodiment, the organic solvent is tetrahydrofuran.
[0070] In the preparation of the above monomer 1, the alkaline condition may be provided by any type of alkaline compound, including organic bases and inorganic bases. In a specific embodiment, the alkaline condition is provided by triethylamine.
[0071] In the preparation of the modified polyphenylene ether resin, the catalyst is preferably a copper catalyst, which has a mild reaction, making the reaction process easier to control and convenient for industrial application. In a specific embodiment, the copper catalyst is cupric chloride.
[0072] In one specific embodiment, in the preparation of the monomer 1, the substitution reaction time is 2 to 6 hours and the temperature is room temperature; and / or in the preparation of the modified polyphenylene ether resin, the substitution reaction time is 2 to 6 hours and the temperature is 65 to 70°C.
[0073] In one specific embodiment, a purification step is further included: in the preparation of the modified polyphenylene ether resin, after the substitution reaction is completed, the reaction product is first filtered, the filtrate is concentrated under reduced pressure to remove the solvent and unreacted products, and the obtained concentrate is washed with water and chloroform, extracted, and then dried over anhydrous magnesium sulfate.
[0074] An embodiment of the present invention further provides a polyphenylene ether composite material, which is formed by curing the aforementioned modified polyphenylene ether resin or the modified polyphenylene ether resin prepared by the aforementioned preparation method.
[0075] In one specific embodiment, the polyphenylene ether composite material is made of raw materials including the following components in parts by weight:
[0076] 100 parts of the modified polyphenylene ether resin or the modified polyphenylene ether resin prepared by the aforementioned preparation method,
[0077]
[0078] By mixing the aforementioned modified polyphenylene ether resin or the modified polyphenylene ether resin prepared by the aforementioned preparation method with a crosslinking agent, an initiator, a filler and fibers according to the aforementioned weight parts, a higher crosslinking reaction rate and fast curing can be obtained.
[0079] Preferably, the cross-linking agent includes a main cross-linking agent and an auxiliary cross-linking agent; the main cross-linking agent is a styrene-butadiene copolymer and / or a maleic anhydride-modified styrene-butadiene copolymer, and the auxiliary cross-linking agent is triallyl isocyanurate. The use of a specific main cross-linking agent and an auxiliary cross-linking agent as a compound cross-linking agent can make the network structure formed by cross-linking of the aforementioned modified polyphenylene ether resin or the modified polyphenylene ether resin prepared by the aforementioned preparation method dense, while not affecting the stretching of the phosphorus-containing end group, and having better flame retardancy and heat resistance. In addition, the introduction of benzene rings through the above-mentioned main cross-linking agent can increase the rigidity of the cross-linked product, further improving the mechanical properties and dielectric properties of the polyphenylene ether composite material. In one specific embodiment, the cross-linking agent includes a main cross-linking agent and an auxiliary cross-linking agent in a weight ratio of 1:0.4 to 0.6.
[0080] More preferably, the main cross-linking agent further adopts a composite cross-linking agent, such as styrene-butadiene copolymer and maleic anhydride-modified styrene-butadiene copolymer, and introduces a cross-linking group grafted with maleic anhydride, enriching the cross-linking form of the modified polyphenylene ether resin or the modified polyphenylene ether resin prepared by the aforementioned preparation method, so that fillers of different particle sizes can be fully dispersed and filled in the system, thereby improving the mechanical properties and dielectric properties of the polyphenylene ether composite material. In one specific embodiment, the styrene-butadiene copolymer and the maleic anhydride-modified styrene-butadiene copolymer can be mixed in a weight ratio of 1:1.5 to 2.5.
[0081] In one specific embodiment, the initiator is a peroxide initiator; the filler is silicon dioxide; and the fiber is glass fiber. Specifically, it can be electronic grade low dielectric glass fiber. In addition, a solvent is also used in the preparation of the polyphenylene ether composite material to disperse the raw material components and adjust the viscosity of the system to be suitable for impregnation of the fiber. The amount used can be 100 to 200 parts. In one specific embodiment, the solvent is toluene.
[0082] The preparation method of the above-mentioned polyphenylene ether composite material comprises the following steps:
[0083] The modified polyphenylene ether resin or the modified polyphenylene ether resin prepared by the aforementioned preparation method, a crosslinking agent, an initiator and a filler are mixed in a solvent, impregnated with the fiber, dried and solidified.
[0084] The polyphenylene ether composite material can be used as a substrate for the preparation of printed circuit boards.
[0085] Specifically, an embodiment of the present invention provides a printed circuit board, the substrate of which is made of the above-mentioned polyphenylene ether composite material. The substrate has good mechanical properties, low dielectric constant, low dielectric loss, and good flame retardant properties and heat resistance, and can meet the requirements of high-speed, high-frequency, and large-capacity signal transmission.
[0086] The following are specific embodiments. Unless otherwise specified, the raw materials used are all commercially available products.
[0087] Example 1
[0088] This embodiment is a modified polyphenylene ether resin, and its raw materials and preparation method are as follows:
[0089]
[0090] 1) Phosphorus oxychloride (15.33 g, 0.1 mol) was dissolved in 100 mL of tetrahydrofuran, and stirred thoroughly under nitrogen atmosphere and ice bath conditions. A mixed solution of triethylamine (32 g) and 20 mL of tetrahydrofuran was added and reacted for 10 minutes. A mixed solution of allyl alcohol (11.62 g, 0.2 mol) and 50 mL of tetrahydrofuran was added dropwise. After the addition was completed, the reaction was continued for 4 hours.
[0091] 2) CuCl (0.03 g) was then added to the reaction solution, the temperature was raised to 68° C. and refluxed, and a solution of bis-hydroxy-terminated polyphenylene ether oligomer SA90 (average molecular weight 1600 g / mol, 72 g, 0.045 mol) and 30 mL of tetrahydrofuran was added and the reaction was continued for 4 hours.
[0092] 3) After the reaction is completed, the mixture is cooled to room temperature, and the precipitated triethylamine hydrochloride is filtered. The residual solvent and unreacted products are removed by rotary evaporation, and then the mixture is sequentially subjected to deionized water, chloroform, extraction, and anhydrous MgSO4 drying to obtain a brown transparent viscous liquid (79 g, yield 94%), which is a phosphorus-containing vinyl modified polyphenylene ether resin P1.
[0093] Example 2
[0094] This embodiment is a modified polyphenylene ether resin, and its raw materials and preparation method are as follows:
[0095]
[0096] 1) Dissolve pyrophosphoryl chloride (25.17 g, 0.1 mol) in 100 mL of tetrahydrofuran, stir thoroughly under nitrogen atmosphere and ice bath conditions, add a mixed solution of triethylamine (32 g) and 20 mL of tetrahydrofuran and react for 10 minutes, add a mixed solution of allyl alcohol (17.42 g, 0.3 mol) and 50 mL of tetrahydrofuran dropwise, and continue to react for 4 hours after the addition is complete.
[0097] 2) CuCl (0.05 g) was then added to the reaction solution, the temperature was raised to 68° C. and refluxed, and a solution of bishydroxy-terminated polyphenylene ether oligomer SA90 (average molecular weight 1600 g / mol, 72 g, 0.045 mol) and 30 mL of tetrahydrofuran was added and the reaction was continued for 4 hours.
[0098] 3) After the reaction is completed, the mixture is cooled to room temperature, and the precipitated triethylamine hydrochloride is filtered. The residual solvent and unreacted products are removed by rotary evaporation, and then the mixture is successively extracted with deionized water, extracted with chloroform, and dried over anhydrous MgSO4 to obtain a brown transparent viscous liquid (89 g, yield 92%), which is a phosphorus-containing vinyl modified polyphenylene ether resin P2.
[0099] Example 3
[0100] This embodiment is a modified polyphenylene ether resin, and its raw materials and preparation method are as follows:
[0101]
[0102] 1) Dissolve ethyl dichlorophosphate (16.3 g, 0.1 mol) in 100 mL of tetrahydrofuran, stir thoroughly under nitrogen atmosphere and ice bath conditions, add a mixed solution of triethylamine (32 g) and 20 mL of tetrahydrofuran and react for 10 minutes, add a mixed solution of allyl alcohol (5.7 g, 0.1 mol) and 30 mL of tetrahydrofuran dropwise, and continue to react for 4 hours after the addition is complete.
[0103] 2) CuCl (0.05 g) was then added to the reaction solution, the temperature was raised to 68° C. and refluxed, and a solution of bishydroxy-terminated polyphenylene ether oligomer SA90 (average molecular weight 1600 g / mol, 72 g, 0.045 mol) and 30 mL of tetrahydrofuran was added and the reaction was continued for 4 hours.
[0104] 3) After the reaction is completed, the mixture is cooled to room temperature, and the precipitated triethylamine hydrochloride is filtered. The residual solvent and unreacted products are removed by rotary evaporation, and then the mixture is extracted with deionized water, extracted with chloroform, and dried over anhydrous MgSO4 to obtain a brown transparent viscous liquid (78 g, yield 93%), which is a phosphorus-containing vinyl modified polyphenylene ether resin P3.
[0105] Example 4
[0106] This embodiment is a modified polyphenylene ether resin, and its raw materials and preparation method are as follows:
[0107]
[0108] 1) Phosphorus oxychloride (15.33 g, 0.1 mol) was dissolved in 80 mL of tetrahydrofuran, and stirred thoroughly under nitrogen atmosphere and ice bath conditions. A mixed solution of triethylamine (32 g) and 20 mL of tetrahydrofuran was added and reacted for 10 minutes. A mixed solution of methyl propylene alcohol (14.42 g, 0.2 mol) and 50 mL of tetrahydrofuran was added dropwise. After the addition was completed, the reaction was continued for 4 hours.
[0109] 2) CuCl (0.03 g) was then added to the reaction solution, the temperature was raised to 68° C. and refluxed, and a solution of bis-hydroxy-terminated polyphenylene ether oligomer SA90 (average molecular weight 1600 g / mol, 72 g, 0.045 mol) and 30 mL of tetrahydrofuran was added and the reaction was continued for 4 hours.
[0110] 3) After the reaction is completed, the mixture is cooled to room temperature, and the precipitated triethylamine hydrochloride is filtered. The residual solvent and unreacted products are removed by rotary evaporation, and then the mixture is sequentially deionized water, chloroform, extracted, and dried over anhydrous MgSO4 to obtain a brown transparent viscous liquid (81 g, yield 93%), which is a phosphorus-containing vinyl modified polyphenylene ether resin P4.
[0111] Example 5
[0112] This embodiment is a modified polyphenylene ether resin, and its raw materials and preparation method are as follows:
[0113]
[0114] 1) Dissolve phenylphosphoryl dichloride (19.50 g, 0.1 mol) in 80 mL of tetrahydrofuran, stir thoroughly under nitrogen atmosphere and ice bath conditions, add a mixed solution of triethylamine (32 g) and 20 mL of tetrahydrofuran and react for 10 minutes, add a mixed solution of allyl alcohol (5.80 g, 0.1 mol) and 50 mL of tetrahydrofuran dropwise, and continue to react for 4 hours after the addition is complete.
[0115] 2) CuCl (0.03 g) was then added to the reaction solution, the temperature was raised to 68° C. and refluxed, and a solution of bis-hydroxy-terminated polyphenylene ether oligomer SA90 (average molecular weight 1600 g / mol, 72 g, 0.045 mol) and 30 mL of tetrahydrofuran was added and the reaction was continued for 4 hours.
[0116] 3) After the reaction is completed, the mixture is cooled to room temperature, and the precipitated triethylamine hydrochloride is filtered. The residual solvent and unreacted products are removed by rotary evaporation, and then the mixture is sequentially subjected to deionized water, chloroform, extraction, and drying with anhydrous MgSO4 to obtain a brown transparent viscous liquid (81 g, yield 94%), namely, phosphorus-containing vinyl modified polyphenylene ether resin P5.
[0117] Examples I-XI are 11 kinds of polyphenylene ether composite materials, and Comparative Examples 1-2 are two kinds of comparative polyphenylene ether composite materials, and the raw material compositions thereof are shown in Table 1 below (parts by weight):
[0118] Table 1
[0119]
[0120]
[0121] The polyphenylene ether composite materials of the above-mentioned Examples I-X1 and Comparative Examples 1-2 were prepared by the following method:
[0122] The raw materials were mixed according to the weight parts in Table 1, and the obtained mixture was adjusted to a certain viscosity, impregnated with 100 parts of glass fibers, and dried to obtain the product.
[0123] Furthermore, in order to test the performance, the product is used as a prepreg to prepare a PCB substrate. Specifically, the prepreg is cut and stacked, and cured using a vacuum press to obtain a substrate that can be used for a PCB, which is used as a test sample for performance testing.
[0124] The test method is as follows:
[0125] Tensile strength: tested according to D638 specification;
[0126] Thermal expansion effect: CTE z-axis, dimensional expansion and contraction measurement range: 50 to 260°C, TMA instrument measurement, the lower the dimensional expansion and contraction (%), the better;
[0127] Heat resistance: T288, TMA thermomechanical analysis instrument measurement: at 288°C, measure the time it takes for the copper foil board to not explode when heated;
[0128] Peel strength test: Tested in accordance with IPC-TM-650 2.4.8;
[0129] Glass transition temperature test: 40-280℃, thermomechanical analysis instrument;
[0130] Dielectric constant: Dk, measured by AET microwave dielectric analyzer. The lower the Dk value, the better the dielectric properties.
[0131] Dielectric loss: Df, measured by AET microwave dielectric analyzer. The lower the Df value, the better the dielectric properties.
[0132] Flame retardancy: UL94, where V-0 is better than V-1.
[0133] Note: Except for the dielectric constant, dielectric loss and mechanical properties (tensile strength, peel strength) tests which use substrates without copper foil, other tests require copper foil to be laid on the substrate in the conventional way.
[0134] The test results are shown in Table 2 below:
[0135] Table 2
[0136]
[0137]
[0138] It can be seen from Tables 1 and 2 that, by comparing Examples I, III and VII-IX with Comparative Examples 1-2, the polyphenylene ether composite material prepared by using the modified polyphenylene ether resin of the embodiment of the present invention has better comprehensive properties, and the flame retardant, mechanical properties, heat resistance and dielectric properties are all better. Among them, Examples I, III and VI-VIII without using benzene rings have better comprehensive performance than Example IX.
[0139] From the comparison between Examples I and II, it can be seen that when a flame retardant is added to Example I, its mechanical properties, heat resistance and dielectric properties are all reduced, which confirms that the addition of the flame retardant has an adverse effect on the properties of the modified polyphenylene ether resin, and the addition of the flame retardant also increases additional costs. Considering all factors, it is preferred not to add the flame retardant.
[0140] From the comparison between Examples I and IV-V, it can be seen that as the amount of modified polyphenylene ether resin P1 added decreases, its flame retardancy, mechanical properties and dielectric properties all decrease, and additional flame retardants need to be added to maintain the flame retardant effect of V-0. At the same time, due to the addition of flame retardants, its mechanical properties, heat resistance and dielectric properties decrease more significantly.
[0141] From the comparison between Examples III and VI, it can be seen that when only one main cross-linking agent is used, its flame retardant performance is equivalent to that of using two compounded main cross-linking agents, but the mechanical properties and dielectric properties are reduced. At the same time, from the comparison between Examples I and X, it can be seen that when only the main cross-linking agent is used without using an auxiliary cross-linking agent, its flame retardant performance, mechanical properties and dielectric properties are reduced.
[0142] From the comparison between Example I and X1, it can be seen that by properly matching the weight portions of the raw materials, better flame retardant properties, mechanical properties and dielectric properties can be obtained.
[0143] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0144] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A polyphenylene ether composite material, characterized in that: The composition is prepared by curing the following raw materials in parts by weight: The cross-linking agent includes a main cross-linking agent and an auxiliary cross-linking agent, wherein the main cross-linking agent is a styrene-butadiene copolymer and / or a styrene-butadiene copolymer modified with maleic anhydride, and the auxiliary cross-linking agent is triallyl isocyanurate; The modified polyphenylene ether resin has the following structural features: Wherein, Y is -CH2-, -CH(CH3)-, -C(CH3)2-, -O- or carbonyl; m and n are each independently a positive integer from 1 to 15; R1 to R 16 are each independently hydrogen, methyl or halo; R0 is 2. The polyphenylene ether composite material according to claim 1, characterized in that: R0 is:
3. The polyphenylene ether composite material according to claim 1, characterized in that: The preparation steps of the modified polyphenylene ether resin include: using monomer 1 to modify the polyphenylene ether resin; the monomer 1 is prepared by a substitution reaction between a phosphorus-containing compound and a vinyl-containing alcohol compound: Wherein, the phosphorus-containing compound is selected from at least one of phosphorus oxychloride, ethyl dichlorophosphate and pyrophosphoryl chloride; The vinyl alcohol compound is selected from at least one of propylene alcohol, methpropylene alcohol and 2-hydroxyethyl acrylate; The polyphenylene ether resin is hydroxyl-terminated polyphenylene ether.
4. The polyphenylene ether composite material according to claim 3, characterized in that: Preparation of the monomer 1: dissolving the phosphorus-containing compound in an organic solvent, adding the vinyl-containing alcohol compound under alkaline conditions, and performing a substitution reaction to obtain the monomer 1; Preparation of the modified polyphenylene ether resin: The monomer 1 and the polyphenylene ether resin are mixed and subjected to a substitution reaction under the action of a catalyst.
5. The polyphenylene ether composite material according to claim 4, characterized in that: In the preparation of the monomer 1, the molar ratio of the chlorine group in the phosphorus-containing compound to the hydroxyl group in the vinyl-containing alcohol compound is greater than 1; In the preparation of the modified polyphenylene ether resin, the molar ratio of the chlorine groups in the phosphorus-containing compound to the hydroxyl groups in the polyphenylene ether resin is greater than 3.
6. The polyphenylene ether composite material according to any one of claims 1 to 5, characterized in that: The initiator is a peroxide initiator, the filler is silicon dioxide, and the fiber is glass fiber.
7. A printed circuit board, characterized in that: The substrate is made of the polyphenylene ether composite material described in any one of claims 1-6.
Citation Information
Patent Citations
Modified polyphenylene ether polymer, polymer film, and preparation methods of modified polyphenylene ether polymer and polymer film
CN109265674A
Polyphenylene ether resin composition, resin varnish, prepreg, metal-clad laminate, and printed wiring board
JP2013023517A
Modified polyphenylene ether and halogenated organic phosphorus compound, and production method of them
JP2013023519A