A method for preparing polyamide elastomer

By removing impurity and performing condensation reaction in a horizontal high-viscosity self-cleaning reactor, the problem of the influence of residues in the polyamide prepolymer is solved, and the high-performance preparation of polyamide elastomers is achieved , exhibits excellent mechanical properties.

CN112745498BActive Publication Date: 2024-11-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911042152.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-10-30
Publication Date
2024-11-01
Estimated Expiration
2039-10-30

AI Technical Summary

Technical Problem

In the prior art, the remaining monomers and oligomers in the polyamide prepolymers affect the performance of subsequent synthetic elastomers, and the kettle reaction leads to incomplete reactions and insufficient mixing of high viscosity materials.

Method used

By removing impurity of the polyamide prepolymer, the condensation reaction is carried out using a horizontal high-viscosity self-cleaning reactor to eliminate residual monomers and oligomers, and the thoroughness of the reaction is achieved.

Benefits of technology

The resulting polyamide elastomer has excellent comprehensive mechanical properties, and has good hardness, tensile strength and elasticity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for preparing a polyamide elastomer, which comprises prepolymerizing a monomer for generating polyamide with a diacid monomer to obtain a double-terminal carboxyl polyamide prepolymer; extracting the double-terminal carboxyl polyamide prepolymer with desalted water, drying and melting the double-terminal carboxyl polyamide prepolymer in sequence to obtain a molten double-terminal carboxyl polyamide prepolymer; mixing the molten double-terminal carboxyl polyamide prepolymer with polytetrahydrofuran ether and / or polyetheramine and a catalyst, and then feeding the mixture into a horizontal high-viscosity self-cleaning reactor for reaction to obtain a polyamide elastomer. The polyamide elastomer prepared by the method has good mechanical properties and low cost, and is conducive to large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a polyamide elastomer, in particular to a method for producing a high-performance polyamide elastomer by removing impurities from a polyamide prepolymer and utilizing a high-viscosity self-cleaning reactor, belonging to the technical field of elastomers. Background Art

[0002] Thermoplastic polyamide elastomer (TPAE) is a segmented block copolymer. It is composed of multiple blocks alternating, and its repeated blocks are composed of monomer units with completely different chemical structures. One block is a hard segment, and its homopolymer has a high glass transition temperature (Tg) or melting point (Tm); the other is a soft segment, which can be either a crystalline polymer or an amorphous polymer. In thermoplastic polyamide elastomers, the soft segment and the hard segment are alternately connected to form an alternating block copolymer.

[0003] TPAE can be divided into nylon 6 series, nylon 66 series, nylon 12 series, etc. according to the type of polyamide constituting the hard segment. Among the commercialized products, nylon 12 series is the most common.

[0004] In the elastomer synthesized by the Chinese patent (CN200780022484), the polyether prepolymer uses commercial XYX triblock polyether diamine, and the typical product is HUNTSMAN's XTJ-542 (amino-terminated polytetrahydrofuran ether diol-polypropylene glycol copolymer). The synthesis process of the embodiment includes a method of adding polyamide monomer and polyether prepolymer at one time and a two-step method of synthesizing polyamide prepolymer first and then adding polyether.

[0005] The process described in the Chinese patent (CN200910200343) is as follows: first, a block copolymer of caprolactam and diisocyanate is prepared by a hydrolysis ring-opening polymerization method, and the block copolymer is composed of two polyamide 6 segments and one diisocyanate segment. Then, the polyamide 6-diisocyanate copolymer is used as a prepolymer and esterified with a polyether prepolymer to form a polyamide elastomer.

[0006] The Chinese patent (CN201110301764) introduces a solution polymerization method, which firstly prepares a polyamide prepolymer with an amino group and a polyether prepolymer with an isocyanate group, and then uses dimethyl sulfoxide or dimethylacetamide as a solvent to form a solution system for polycondensation to prepare a polyamide elastomer. The solution reaction is more complete than the bulk reaction and is also easier to implement.

[0007] The Chinese patent (CN201410667956) introduces a one-step hydrolysis and ring-opening method for preparing polyamide elastomers. The polyether prepolymer, caprolactam monomer, dicarboxylic acid and catalyst are directly mixed to initiate hydrolysis and ring-opening polymerization and polycondensation reaction between prepolymers.

[0008] The Chinese patent (CN201510085070) introduces the use of copolyamide as the hard segment of polyamide elastomer. The process adopted is a two-step method of first hydrolyzing and ring-opening to prepare a copolyamide prepolymer, and then adding a polyether prepolymer for condensation reaction.

[0009] The Chinese patent (CN201410009966) uses a heat-resistant modified polyurethane prepolymer and a polyamide prepolymer to react to prepare a polyamide elastomer. The heat-resistant modified polyurethane prepolymer is prepared by reacting a polyether with an isocyanate to generate a polyurethane prepolymer, and then adding pyromellitic anhydride to react. The isocyanate end group of the prepolymer is then reacted with a carboxyl-terminated polyamide prepolymer to generate a block copolymer.

[0010] The Chinese patent (CN200910200344) uses the reaction of amino-terminated polyether and anionic initiator to prepare active species, and then adds caprolactam to initiate anionic polymerization to generate polyamide elastomer. The anionic polymerization reaction of caprolactam is fast and easier to carry out than esterification reaction.

[0011] The above patents all involve the synthesis of polyamide prepolymers. The presence of residual monomers and oligomers in the prepolymers greatly interferes with the subsequent synthesis of elastomers and affects the properties of the elastomers. In addition, in the prior art, the condensation reaction of polyamide prepolymers and polyether prepolymers mostly adopts kettle reactors. However, due to the high viscosity of polyamide prepolymers, polyether prepolymers and their intermediates, the mixing effect is not sufficient and the reaction is not complete. Summary of the invention

[0012] In view of the shortcomings of the prior art, the purpose of the present invention is to propose a method for removing impurities from a polyamide prepolymer and condensing it in combination with a high-viscosity self-cleaning reactor to synthesize a polyamide elastomer. The method eliminates the influence of residual polyamide monomers and oligomers in the polyamide prepolymer, and utilizes a high-viscosity self-cleaning reactor for condensation reaction to make the reaction thorough, and the resulting elastomer has excellent comprehensive chemical properties.

[0013] In order to achieve the above technical objectives, the present invention provides a method for preparing a polyamide elastomer, which comprises the following steps:

[0014] 1) prepolymerizing a polyamide-generating monomer and a diacid monomer to obtain a double-terminal carboxyl polyamide prepolymer;

[0015] 2) extracting the double-terminal carboxyl polyamide prepolymer with desalted water, drying and melting the prepolymer to obtain a molten double-terminal carboxyl polyamide prepolymer;

[0016] 3) After the molten double-terminated carboxyl polyamide prepolymer is mixed with polytetrahydrofuran ether and / or polyether amine and a catalyst, the mixture is sent into a horizontal high-viscosity self-cleaning reactor for reaction to obtain a polyamide elastomer.

[0017] In a preferred embodiment, the monomers for forming polyamide include at least one of caprolactam, diamine dibasic acid salt, and aminocarboxylic acid monomers.

[0018] In a preferred embodiment, the diamine dibasic acid salt includes at least one of hexamethylenediamine adipate, decanediaminum sebacate, and hexamethylenediamine dodecanedioate.

[0019] In a preferred embodiment, the aminocarboxylic acid monomer includes at least one of undecylaminoundecanoic acid and dodecylaminododecanoic acid.

[0020] In a preferred embodiment, the prepolymerization conditions are: pressure of 0.1-2.0 MPa and temperature of 240-280°C.

[0021] In a preferred embodiment, the number average molecular weight of the polyamide prepolymer is 500 to 3000.

[0022] In a preferred solution, the extraction conditions are: a temperature of 90 to 150° C. and an extraction time of 3 to 12 hours. The double-terminated carboxyl polyamide prepolymer of the present invention can effectively remove unreacted monomers, residual acid, oligomers, etc. after being extracted with desalted water. By using the preferred extraction conditions, the weight percentage of residual monomers and oligomers in the polyamide prepolymer can be reduced to less than 0.6%.

[0023] The drying of the present invention is carried out under vacuum or nitrogen protection to make the water content lower than 0.1%.

[0024] In a preferred embodiment, the number average molecular weight of the polytetramethylene ether or polyetheramine is 500 to 3000.

[0025] In a preferred embodiment, the polyetheramine is a polyether containing double-terminal amino groups; the polyether structure in the polyether containing double-terminal amino groups is polyethylene glycol, polypropylene glycol or polytetrahydrofuran, or a copolymer structure of at least two of polyethylene glycol, polypropylene glycol and polytetrahydrofuran.

[0026] In a preferred embodiment, the double-terminal carboxyl polyamide prepolymer accounts for 20% to 50% of the weight of the polyamide elastomer.

[0027] In a preferred embodiment, the reaction conditions are: temperature of 180-280° C. and pressure of 0-60 KPa.

[0028] The present invention obtains a prepolymer by ring-opening polymerization of caprolactam monomers, or polycondensation of diamine dibasic acid monomers or aminocarboxylic acid monomers, and introduces an appropriate amount of diacid monomers during the preparation of the prepolymer to ensure that both ends of the polyamide prepolymer are carboxyl groups. The diacid monomers are common fatty diacids such as adipic acid.

[0029] The double-terminal carboxyl polyamide prepolymer of the present invention is melted by a screw extruder during the melting process.

[0030] The horizontal high-viscosity self-cleaning reactor of the present invention is such as the LIST-CRP type high-viscosity self-cleaning reactor of LIST Company of Switzerland or the STC type high-viscosity self-cleaning reactor of Yuanzheng Technology of Hangzhou. A high-viscosity self-cleaning reactor structure is cited as an example, such as a horizontal arrangement, with a barrel structure. The feed port and the discharge port are arranged at both ends of the barrel, and the shell of the barrel is provided with a vacuum suction port connected to its inner cavity. The barrel is provided with a single-axis or double-axis rotor structure inside, which drives the polyamide melt to move forward and forms a mass transfer interface at the same time, so that small molecules are discharged by vacuum suction. The design of the rotor and the inner cavity of the barrel has a self-cleaning effect and can avoid melt retention. A three-way valve is provided at the outlet of the reactor, one of which is for the discharge of the reactor, and the other is for returning the melt to the inlet of the reactor through a conveying screw or a melt pump. The reactor adopts an intermittent operation mode, and the reaction material moves from the inlet to the outlet, and then returns to the inlet for circulation. After the reaction is completed, the three-way valve is switched to the discharge direction to extrude the elastomer product. The present invention utilizes a horizontal high-viscosity self-cleaning reactor for the first time to realize polycondensation between a double-terminal carboxyl polyamide prepolymer and polytetrahydrofuran ether or polyetheramine, so that the reaction is complete and a high-performance polyamide elastomer is obtained.

[0031] The catalyst of the present invention is a conventional polycondensation catalyst, such as tetrabutyl titanate or triphenyl phosphite, and its addition amount is 0.1% to 3% of the system mass, preferably 0.4% to 2%.

[0032] Compared with the prior art, the technical solution of the present invention brings the following beneficial technical effects:

[0033] The present invention extracts the polyamide prepolymer by an extraction method, which can effectively and deeply remove residual monomers, oligomers, residual acids, etc., and reduce the influence of these small molecules on subsequent condensation reactions.

[0034] The invention adopts a high-viscosity self-cleaning reactor to carry out the condensation reaction of polyamide and polyether, has a strong stirring, dispersing and mixing effect on the high-viscosity material, the condensation reaction is carried out thoroughly, and the generated elastomer has excellent performance.

[0035] The polyamide elastomer prepared by the invention has excellent comprehensive mechanical properties such as hardness, tensile strength and elasticity. DETAILED DESCRIPTION

[0036] The following examples are intended to further illustrate the present invention, rather than to limit the scope of protection of the claims of the present invention.

[0037] Example 1

[0038] 400g of caprolactam, 87.6g of adipic acid and 6g of desalted water were added to the polymerization kettle, polymerized at 260℃ and 0.6MPa for 2 hours, slowly reduced to normal pressure, continued to react for 2 hours, evacuated to an absolute pressure of 70KPa, reacted for 2 hours, and obtained nylon 6 prepolymer. The vacuum was eliminated with high-purity nitrogen, and the nylon 6 prepolymer was pressed out of the polymerization kettle. After pelletizing, it was extracted with desalted water at an extraction temperature of 96℃. The extraction water was replaced every 2 hours, and extracted three times in total. After the extraction, the extractable content of nylon 6 prepolymer was 0.4%. The nylon 6 prepolymer was dried under nitrogen protection for 16 hours and contained 0.06% water. The number average molecular weight of nylon 6 prepolymer was 812.6.

[0039] Nylon 6 prepolymer was melted and plasticized by a single screw extruder, 600g of polytetrahydrofuran ether glycol (number average molecular weight 1000) and 7g of tetrabutyl titanate catalyst were mixed and pumped into the extruder through a metering pump. The above mixture was sent to the LIST-CRP high viscosity self-cleaning reactor of LIST Company of Switzerland, the reaction temperature was 260℃, the vacuum degree was 1KPa, and the reaction time was 6 hours. The polyamide elastomer was obtained by melt extrusion granulation. The tested melting point was 190℃, the tensile strength was 11.53MPa, and the elongation at break was 381.3%.

[0040] Example 2

[0041] 350g of caprolactam, 94.9g of adipic acid and 6g of desalted water were added to a polymerization kettle, polymerized at 260°C and 0.6MPa for 2 hours, slowly decompressed to normal pressure, continued to react for 2 hours, evacuated to an absolute pressure of 70KPa, reacted for 2 hours, and obtained a nylon 6 prepolymer. The vacuum was eliminated with high-purity nitrogen, and the nylon 6 prepolymer was pressed out of the polymerization kettle. After pelletizing, it was extracted with desalted water at an extraction temperature of 105°C. The extraction water was replaced every 2 hours, and extracted three times in total. After the extraction, the extractable content of the nylon 6 prepolymer was 0.32%. The nylon 6 prepolymer was dried under nitrogen protection for 16 hours and contained 0.06% water. The number average molecular weight of the nylon 6 prepolymer was 684.4.

[0042] Nylon 6 prepolymer was melted and plasticized by a single screw extruder, 650g of polytetrahydrofuran ether glycol (number average molecular weight 1000) and 5g of tetrabutyl titanate catalyst were mixed and pumped into the extruder through a metering pump. The above mixture was sent to the LIST-CRP high viscosity self-cleaning reactor of LIST Company of Switzerland, the reaction temperature was 260℃, the vacuum degree was 1KPa, and the reaction time was 6 hours. The polyamide elastomer was obtained by melt extrusion granulation. The tested melting point was 189℃, the tensile strength was 10.5MPa, and the elongation at break was 531.1%.

[0043] Example 3

[0044] 350g of caprolactam, 47.5g of adipic acid and 6g of desalted water were added to the polymerization kettle, polymerized at 260℃ and 0.6MPa for 2 hours, slowly reduced to normal pressure, continued to react for 2 hours, evacuated to an absolute pressure of 70KPa, reacted for 2 hours, and obtained nylon 6 prepolymer. The vacuum was eliminated with high-purity nitrogen, and the nylon 6 prepolymer was pressed out of the polymerization kettle. After pelletizing, it was extracted with desalted water at an extraction temperature of 105℃. The extraction water was replaced every 2 hours, and extracted three times in total. After the extraction, the extractable content of nylon 6 prepolymer was 0.36%. The nylon 6 prepolymer was dried under nitrogen protection for 16 hours and contained 0.06% water. The number average molecular weight of nylon 6 prepolymer was 1369.

[0045] Nylon 6 prepolymer was melted and plasticized by a single screw extruder, 650g of polytetrahydrofuran ether glycol (number average molecular weight 2000) and 10g of tetrabutyl titanate catalyst were mixed and pumped into the extruder through a metering pump. The above mixture was sent to the LIST-CRP high viscosity self-cleaning reactor of LIST Company of Switzerland, the reaction temperature was 260℃, the vacuum degree was 1KPa, and the reaction time was 6 hours. The polyamide elastomer was obtained by melt extrusion granulation. The tested melting point was 197℃, the tensile strength was 15.7MPa, and the elongation at break was 311.1%.

[0046] Example 4

[0047] 280g of caprolactam, 70g of adipic acid adipate, 94.9g of adipic acid, and 6g of desalted water were added to a polymerization kettle, polymerized at 260°C and 0.6MPa pressure for 2 hours, slowly decompressed to normal pressure, continued to react for 2 hours, evacuated to an absolute pressure of 70KPa, and reacted for 2 hours to obtain nylon 6 prepolymer. The vacuum was eliminated with high-purity nitrogen, and the nylon 6 prepolymer was pressed out of the polymerization kettle. After pelletizing, it was extracted with desalted water at an extraction temperature of 105°C. The extraction water was replaced every 2 hours, and extracted three times in total. After the extraction, the extractable content of nylon 6 / 66 prepolymer was 0.28%. The nylon 6 / 66 prepolymer was dried under nitrogen protection for 16 hours and contained 0.06% water. The number average molecular weight of nylon 6 prepolymer was 684.4.

[0048] Nylon 6 / 66 prepolymer is melted and plasticized by a single screw extruder, 650g of polytetrahydrofuran ether glycol (number average molecular weight 1000) and 5g of triphenyl phosphite catalyst are mixed and pumped into the extruder through a metering pump. The above mixture is sent to the Hangzhou Yuanzheng Technology STC type high viscosity self-cleaning reactor, the reaction temperature is 260℃, the vacuum degree is 1KPa, and the reaction time is 6 hours. The melt is extruded and granulated to obtain a polyamide elastomer. The tested melting point is 165℃, the tensile strength is 7.6MPa, and the elongation at break is 468.3%.

[0049] Example 5

[0050] 280g of caprolactam, 70g of adipic acid adipate, 94.9g of adipic acid, and 6g of desalted water were added to a polymerization kettle, polymerized at 260°C and 0.6MPa pressure for 2 hours, slowly decompressed to normal pressure, continued to react for 2 hours, evacuated to an absolute pressure of 70KPa, and reacted for 2 hours to obtain nylon 6 prepolymer. The vacuum was eliminated with high-purity nitrogen, and the nylon 6 prepolymer was pressed out of the polymerization kettle. After pelletizing, it was extracted with desalted water at an extraction temperature of 105°C. The extraction water was replaced every 2 hours, and extracted three times in total. After the extraction, the extractable content of nylon 6 / 66 prepolymer was 0.28%. The nylon 6 / 66 prepolymer was dried under nitrogen protection for 16 hours and contained 0.06% water. The number average molecular weight of nylon 6 prepolymer was 684.4.

[0051] Nylon 6 / 66 prepolymer was melted and plasticized by a single screw extruder, 650g of polyetheramine (Huntsman XTJ-542, number average molecular weight 1000) and 8g of triphenyl phosphite catalyst were mixed and pumped into the extruder through a metering pump. The above mixture was sent to the Hangzhou Yuanzheng Technology STC type high viscosity self-cleaning reactor, the reaction temperature was 260℃, the vacuum degree was 1KPa, and the reaction time was 6 hours. The melt was extruded and granulated to obtain a polyamide elastomer. The tested melting point was 158℃, the tensile strength was 6.7MPa, and the elongation at break was 502.3%.

[0052] Comparative Example 1

[0053] 400g of caprolactam, 87.6g of adipic acid, 600g of polytetrahydrofuran ether glycol (number average molecular weight 1000), 7g of tetrabutyl titanate catalyst, and 6g of desalted water were added to a polymerization kettle, polymerized at 260°C and 0.6MPa pressure for 2 hours, slowly reduced to normal pressure, continued to react for 2 hours, evacuated to an absolute pressure of 70KPa, reacted for 2 hours, then evacuated to 1KPa, reacted for 6 hours, and melt extruded and granulated to obtain a polyamide elastomer. The tested melting point was 188°C, the tensile strength was 10.3MPa, and the elongation at break was 221.3%.

[0054] Comparative Example 2

[0055] 350g of caprolactam, 47.5g of adipic acid and 6g of desalted water were added to a polymerization kettle, polymerized at 260℃ and 0.6MPa for 2 hours, slowly reduced to normal pressure, continued to react for 2 hours, evacuated to an absolute pressure of 70KPa, reacted for 2 hours, and obtained nylon 6 prepolymer; 650g of polytetrahydrofuran ether glycol (number average molecular weight 2000) and 5g of tetrabutyl titanate catalyst were mixed and pumped into the polymerization kettle via a metering pump. The reaction temperature was 260℃, the vacuum degree was 1KPa, and the reaction time was 6 hours. The polyamide elastomer was obtained by melt extrusion granulation. The tested melting point was 194℃, the tensile strength was 18.4MPa, and the elongation at break was 195.2%.

[0056] Comparative Example 3

[0057] 280g of caprolactam, 70g of adipic acid adipate, 94.9g of adipic acid, and 6g of desalted water were added to a polymerization kettle, polymerized at 260°C and 0.6MPa for 2 hours, slowly reduced to normal pressure, continued to react for 2 hours, evacuated to an absolute pressure of 70KPa, and reacted for 2 hours to obtain nylon 6 prepolymer. 650g of polyetheramine (Huntsman XTJ-542, number average molecular weight 1000) and 8g of triphenyl phosphite were mixed and pumped into the polymerization kettle through a metering pump, the reaction temperature was 260°C, the vacuum degree was 1KPa, and the reaction time was 6 hours. The melt was extruded and granulated to obtain a polyamide elastomer. The tested melting point was 161°C, the tensile strength was 7.7MPa, and the elongation at break was 242.3%.

[0058] Comparative Example 4

[0059] 350g of caprolactam, 47.5g of adipic acid and 6g of desalted water were added to the polymerization kettle, polymerized at 260℃ and 0.6MPa pressure for 2 hours, slowly reduced to normal pressure, continued to react for 2 hours, evacuated to an absolute pressure of 70KPa, reacted for 2 hours, and obtained nylon 6 prepolymer. It was mixed with 650g of polytetrahydrofuran ether glycol (number average molecular weight 2000) and 5g of tetrabutyl titanate catalyst, and sent to Hangzhou Yuanzheng Technology STC type high viscosity self-cleaning reactor. The reaction temperature was 260℃, the vacuum degree was 1KPa, and the reaction time was 6 hours. The melt was extruded and granulated to obtain a polyamide elastomer. The tested melting point was 191℃, the tensile strength was 14.4MPa, and the elongation at break was 295.2%.

[0060] Comparative Example 5

[0061] 280g of caprolactam, 70g of adipic acid adipate, 94.9g of adipic acid, and 6g of desalted water were added to a polymerization kettle, polymerized at 260°C and 0.6MPa pressure for 2 hours, slowly decompressed to normal pressure, continued to react for 2 hours, evacuated to an absolute pressure of 70KPa, and reacted for 2 hours to obtain nylon 6 prepolymer. The vacuum was eliminated with high-purity nitrogen, and the nylon 6 prepolymer was pressed out of the polymerization kettle. After pelletizing, it was extracted with desalted water at an extraction temperature of 105°C. The extraction water was replaced every 2 hours, and extracted three times in total. After the extraction, the extractable content of nylon 6 / 66 prepolymer was 0.28%. The nylon 6 / 66 prepolymer was dried under nitrogen protection for 16 hours and contained 0.06% water. The number average molecular weight of nylon 6 prepolymer was 684.4.

[0062] Nylon 6 / 66 prepolymer was melt-plasticized by a single screw extruder, 650g of polytetrahydrofuran ether glycol (number average molecular weight 1000) and 5g of triphenyl phosphite catalyst were mixed and pumped into the extruder through a metering pump. The above mixture was sent to a 3L stirring polymerization reactor with a reaction temperature of 260°C, a vacuum degree of 1KPa, and a reaction time of 6 hours. The melt was extruded and granulated to obtain a polyamide elastomer. The tested melting point was 169°C, the tensile strength was 9.6MPa, and the elongation at break was 262.5%.

[0063] Through the above comparison, the performance of the polyamide elastomer produced by the process of the present invention is significantly better than that produced by directly reacting the polyamide prepolymer with the polyether in a polymerization reactor.

Claims

1. A method for preparing a polyamide elastomer, characterized in that: The following steps are involved: 1) Prepolymerizing the monomers for generating polyamide with the diacid monomers to obtain a double-terminal carboxyl polyamide prepolymer; 2) extracting the double-terminal carboxyl polyamide prepolymer with desalted water, drying and melting it in sequence to obtain a molten double-terminal carboxyl polyamide prepolymer; the extraction conditions are: a temperature of 90-150° C. and an extraction time of 3-12 hours; 3) After the molten double-terminated carboxyl polyamide prepolymer is mixed with polytetramethylene ether and / or polyether amine and a catalyst, it is sent into a horizontal high-viscosity self-cleaning reactor for reaction to obtain a polyamide elastomer.

2. The method for preparing a polyamide elastomer according to claim 1, characterized in that: The monomers for generating polyamide include at least one of caprolactam, diamine dibasic acid salt and aminocarboxylic acid monomers.

3. The method for preparing a polyamide elastomer according to claim 2, characterized in that: The diamine dibasic acid salt comprises at least one of hexamethylenediamine adipate, decanediamin sebacate, and hexamethylenediamine dodecanediacid; The aminocarboxylic acid monomer includes at least one of undecylaminoundecanoic acid and dodecylaminododecanoic acid.

4. The method for preparing a polyamide elastomer according to any one of claims 1 to 3, characterized in that: The prepolymerization conditions are: pressure of 0.1-2.0 MPa and temperature of 240-280°C.

5. The method for preparing a polyamide elastomer according to claim 1, characterized in that: The number average molecular weight of the polyamide prepolymer is 500-3000.

6. The method for preparing a polyamide elastomer according to claim 1, characterized in that: The number average molecular weight of the polytetramethylene ether or polyetheramine is 500-3000.

7. The method for preparing a polyamide elastomer according to claim 1, characterized in that: The polyetheramine is a polyether containing double-terminal amino groups; the polyether structure in the polyether containing double-terminal amino groups is polyethylene glycol, polypropylene glycol or polytetrahydrofuran, or a copolymer structure of at least two of polyethylene glycol, polypropylene glycol and polytetrahydrofuran.

8. The method for preparing a polyamide elastomer according to claim 1, characterized in that: The double-terminal carboxyl polyamide prepolymer accounts for 20% to 50% of the weight of the polyamide elastomer.

9. The method for preparing a polyamide elastomer according to claim 1, characterized in that: The reaction conditions are: temperature of 180-280° C. and pressure of 0-60 KPa.