A self-aligned pixel definition layer structure and processing method thereof

By adopting self-aligning pixel definition layer structure in the micro display screen and using dry etching technology to fill the pixel definition layer of the anode gap, the problems of low brightness and complex process caused by anode overlap are solved, and higher luminous brightness and Simplified process flow.

CN112750889BActive Publication Date: 2024-11-26ANHUI SEMICON INTEGRATED DISPLAY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110239350.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-04
Publication Date
2024-11-26
Estimated Expiration
2041-03-04

AI Technical Summary

Technical Problem

In the prior art, the overlap of the pixel definition layer and the anode results in optical crosstalk and electrical crosstalk, affecting luminescence efficiency and brightness, and the lithography process is complex and costly.

Method used

Using a self-aligned pixel definition layer structure, by setting an anode and a gap on the substrate and filling the pixel definition layer at the gap, using dry etching technology, a pixel definition layer with flush side walls is formed, and the anode is thinned to form a concave. Grooving structure avoids lithography processes and simplifies process flow.

Benefits of technology

It improves the luminous brightness, saves the lithography process, reduces costs, and avoids the difference between pixels caused by photolithography alignment deviation, ensuring uniformity between pixels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112750889B_ABST
    Figure CN112750889B_ABST
Patent Text Reader

Abstract

The invention discloses a self-aligned pixel definition layer structure and a processing method thereof, comprising: a substrate; an anode, a series of anodes are arranged on the substrate, and there are gaps between adjacent anodes; a pixel definition layer, filling the gaps between adjacent anodes; the side wall of the pixel definition layer is flush with the side wall of the anode; the pixel definition layer is formed by dry etching, does not occupy the anode area, does not affect the opening area, and is conducive to improving the luminous brightness; saves a photolithography process, the process is simpler, and the cost is lower.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of micro display screens, and in particular relates to a self-aligned pixel definition layer structure and a processing method thereof. Background Art

[0002] In displays, pixel definition layers (PDL) are used to define pixel areas, isolate pixels, and prevent optical and electrical crosstalk.

[0003] In the process of realizing the present invention, the inventors found that the prior art has at least the following problems: Generally, the process of photolithography plus etching is used. In order to avoid the offset caused by the photolithography alignment deviation, the PDL and the anode have a certain overlap, and the size of the overlapping area is at least 0.2-0.3um greater than the alignment accuracy. For micro-display, because the anode pixel area is very small, the overlap occupies a part of the light-emitting area, which will cause a loss of about 30% of the opening area, resulting in reduced luminous efficiency and reduced brightness. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a self-aligned pixel definition layer structure and a processing method thereof which does not occupy the anode area, does not affect the opening area, is conducive to improving the luminous brightness, saves a photolithography process, has a simpler process and lowers the cost.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a self-aligned pixel definition layer structure having:

[0006] substrate;

[0007] Anodes, wherein a series of anodes are arranged on the substrate, and gaps are provided between adjacent anodes;

[0008] The pixel definition layer fills the gap between adjacent anodes; the side wall of the pixel definition layer is flush with the side wall of the anode; and the pixel definition layer is formed by dry etching.

[0009] The material of the pixel definition layer includes silicon nitride, silicon oxide or silicon oxynitride.

[0010] A method for processing the above-mentioned self-aligned pixel definition layer structure comprises the following steps:

[0011] 1) preparing an anode on a substrate;

[0012] 2) depositing a pixel definition layer on the substrate and the anode;

[0013] 3) Dry etching the pixel definition layer. During the dry etching process, the pixel definition layer on the anode side wall will be retained;

[0014] 4) Dry etching to thin the anode to form a groove for depositing the pixel definition layer, and finally forming an anode structure defined by the pixel definition layer.

[0015] One of the above technical solutions has the following advantages or beneficial effects: it does not occupy the anode area, does not affect the opening area, and is conducive to improving the luminous brightness; it saves a photolithography process, the process is simpler, and the cost is lower. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 A schematic structural diagram of a self-aligned pixel definition layer structure provided in an embodiment of the present invention;

[0017] Figure 2 for Figure 1 A process flow chart of a self-aligned pixel definition layer structure;

[0018] The markings in the above figures are: 1, substrate, 2, anode, 3, pixel definition layer. DETAILED DESCRIPTION

[0019] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be further described in detail below with reference to the accompanying drawings.

[0020] See also Figure 1-2 , a self-aligned pixel definition layer structure having:

[0021] substrate;

[0022] Anode: a series of anodes are arranged on the substrate, and there are gaps between adjacent anodes;

[0023] The pixel definition layer fills the gap between adjacent anodes; the side wall of the pixel definition layer is flush with the side wall of the anode; and the pixel definition layer is formed by dry etching.

[0024] The material of the pixel definition layer includes silicon nitride, silicon oxide or silicon oxynitride.

[0025] After the pixel definition layer (silicon nitride, silicon oxide or silicon oxynitride) is deposited, the anode structure is self-aligned and the PDL layer is dry-etched. Due to the characteristics of dry etching, the PDL on the side wall of the anode will be retained, and then the anode is thinned by dry etching to form a PDL groove, and finally the anode structure defined by the PDL is formed. 1. The PDL formed by the self-alignment process does not occupy the anode area and does not affect the opening area, which is beneficial to improving the luminous brightness. 2. The self-alignment process saves a photolithography process, the process is simpler and the cost is lower. 3. The self-alignment process uses the anode structure for self-alignment and does not use photolithography, which avoids the difference between pixels caused by photolithography alignment deviation and has better uniformity between pixels. The self-aligned pixel definition layer process solves the problems that the traditional pixel definition layer occupies the pixel area, affects the opening area and causes low brightness; the process is complex and costly; and the alignment deviation causes poor uniformity between pixels.

[0026] A method for processing the above-mentioned self-aligned pixel definition layer structure comprises the following steps:

[0027] 1) preparing an anode on a substrate;

[0028] 2) depositing a pixel definition layer on the substrate and the anode;

[0029] 3) Dry etching pixel definition layer. Due to the characteristics of dry etching, the pixel definition layer on the anode side wall will be retained during the dry etching process;

[0030] 4) Dry etching to thin the anode to form a groove for depositing the pixel definition layer, and finally forming an anode structure defined by the pixel definition layer.

[0031] Step 1) includes anode deposition, photolithography, etching, and stripping, including the following steps:

[0032] a) PVD (physical vapor deposition) sequentially deposits ITO (indium tin oxide)-bottom layer, Al, and ITO-top layer, with thicknesses of 100-500A, 500-2000A, and 500-5000A, respectively, wherein the ITO deposition parameters are: ITO target, pressure 10-1000mT, power 500-5000W, Ar gas flow rate 10-100sccm, temperature 20-50°C, and time 20-200s; Al deposition parameters: Al target, pressure 10-500mT, power 500-2000W, Ar gas flow rate 10-100sccm, room temperature, and time 20-200s;

[0033] b) Photolithography machine anode lithography, coating: 1-5um photoresist, exposure: 100-1000mj energy, development: developer development 60-300s;

[0034] c) Dry etching machine etches the anode, dry etching parameters: pressure 10-100mT, power 100-2000W, Ar flow 10-100sccm, HBr flow 10-100sccm, Cl2 flow 10-100sccm, temperature 20-70℃, time 20-200s;

[0035] d) The photoresist is stripped by a stripping machine, and the stripping liquid is used for 100-1000s at a temperature of 30-80°C.

[0036] In the above step 2), CVD (chemical vapor deposition) deposits silicon nitride, silicon oxide or silicon oxynitride with a thickness of 500-5000A. The silicon nitride deposition parameters are: pressure 10-100mT, power 200-2000W, SiH4 flow rate 10-200sccm, NH3 flow rate 10-100sccm, temperature 200-400°C, and time 10-100s; silicon oxide deposition parameters are: pressure 10-100mT, power Rate 200-2000W, SiH4 flow rate 10-200sccm, N2O flow rate 10-5000sccm, temperature 200-400℃, time 10-100s; silicon oxynitride deposition parameters: pressure 10-100mT, power 200-2000W, SiH4 flow rate 10-200sccm, N2O flow rate 10-400sccm, temperature 200-400℃, time 10-100s.

[0037] In the above step 3), the dry etching machine etches silicon nitride, silicon oxide or silicon oxynitride with an etching thickness of 500-5000A; dry etching parameters: pressure 10-100mT, power 100-2000W, Ar gas flow rate 10-100sccm, CHF3 gas flow rate 10-100sccm, O2 gas flow rate 10-100sccm, temperature 20-70°C, time 100-2000s.

[0038] In the above step 4), the dry etching machine etches and thins the ITO; the top layer of ITO is etched and thinned 300-3000A, and the dry etching parameters are: pressure 10-100mT, power 100-1000W, Ar gas flow rate 10-100sccm, Cl2 gas flow rate 10-100sccm, HBr gas flow rate 10-100sccm, temperature 20-70°C, and time 20-200s.

[0039] After adopting the above scheme, the anode area is not occupied, the opening area is not affected, and it is beneficial to improve the luminous brightness; a photolithography process is saved, the process is simpler and the cost is lower; the anode structure is self-aligned, and photolithography is not used, which avoids the difference between pixels caused by photolithography alignment deviation, and the uniformity between pixels is better. It solves the problem that the traditional pixel definition layer occupies the pixel area, affects the opening area and causes low brightness; the process is complex and costly; and the alignment deviation causes poor uniformity between pixels. It belongs to the display industry, especially the high-resolution micro display industry.

[0040] The present invention is described above by way of example in conjunction with the accompanying drawings. It is obvious that the specific implementation of the present invention is not limited to the above-mentioned method. As long as various non-substantial improvements are made using the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.

Claims

1. A method for processing a self-aligned pixel definition layer structure, characterized in that: have: substrate; Anodes, wherein a series of anodes are arranged on the substrate, and gaps are provided between adjacent anodes; A pixel definition layer fills the gap between adjacent anodes; the sidewall of the pixel definition layer is flush with the sidewall of the anode; the pixel definition layer is formed by dry etching; The steps include: 1) preparing an anode on a substrate; 2) depositing a pixel definition layer on the substrate and the anode; 3) Dry etching of the pixel definition layer. During the dry etching process, the pixel definition layer on the anode side wall will be retained; 4) Dry etching to thin the anode to form a groove for depositing the pixel definition layer, and finally forming an anode structure defined by the pixel definition layer; The above step 1) includes anode deposition, photolithography, etching, and stripping, including the following steps: a) PVD sequentially deposits ITO-bottom layer, Al, and ITO-top layer with thicknesses of 100-500Å, 500-2000Å, and 500-5000Å, respectively, wherein the ITO deposition parameters are: ITO target, pressure 10-1000mT, power 500-5000W, Ar gas flow rate 10-100sccm, temperature 20-50°C, and time 20-200s; Al deposition parameters are: Al target, pressure 10-500mT, power 500-2000W, Ar gas flow rate 10-100sccm, room temperature, and time 20-200s; b) Photolithography machine anode photolithography, coating: 1-5um photoresist, exposure: 100-1000mj energy, development: developer development 60-300s; c) Dry etching machine etches the anode, dry etching parameters: pressure 10-100mT, power 100-2000W, Ar flow 10-100sccm, HBr flow 10-100sccm, Cl2 flow 10-100sccm, temperature 20-70℃, time 20-200s; d) The photoresist is stripped by a stripping machine, and the stripping liquid is used for 100-1000s at a temperature of 30-80°C; In the above step 2), CVD deposits silicon nitride, silicon oxide or silicon oxynitride with a thickness of 500-5000Å. The deposition parameters for silicon nitride are: pressure 10-100mT, power 200-2000W, SiH4 flow rate 10-200sccm, NH3 flow rate 10-100sccm, temperature 200-400℃, time 10-100s; the deposition parameters for silicon oxide are: pressure 10-100mT, power 200 -2000W, SiH4 flow rate 10-200sccm, N2O flow rate 10-5000sccm, temperature 200-400℃, time 10-100s; silicon oxynitride deposition parameters: pressure 10-100mT, power 200-2000W, SiH4 flow rate 10-200sccm, N2O flow rate 10-400sccm, temperature 200-400℃, time 10-100s.

2. The method for processing a self-aligned pixel definition layer structure according to claim 1, characterized in that: The material of the pixel definition layer includes silicon nitride, silicon oxide or silicon oxynitride.

3. The method for processing a self-aligned pixel definition layer structure according to claim 2, wherein: In the above step 3), the dry etching machine etches silicon nitride, silicon oxide or silicon oxynitride with an etching thickness of 500-5000Å; dry etching parameters: pressure 10-100mT, power 100-2000W, Ar gas flow rate 10-100sccm, CHF3 gas flow rate 10-100sccm, O2 gas flow rate 10-100sccm, temperature 20-70°C, time 100-2000s.

4. The method for processing a self-aligned pixel definition layer structure according to claim 3, characterized in that: In the above step 4), the dry etching machine etches and thins the ITO; the top layer of ITO is etched and thinned to 300-3000Å, and the dry etching parameters are: pressure 10-100mT, power 100-1000W, Ar gas flow rate 10-100sccm, Cl2 gas flow rate 10-100sccm, HBr gas flow rate 10-100sccm, temperature 20-70°C, and time 20-200s.