Electrolyte membrane for fuel cell and method for manufacturing the same
By depositing catalyst metal on the polymer electrolyte membrane to form a reinforcement layer and impregnating it with ionomer, the problem of electrolyte membrane deterioration caused by hydrogen permeation is solved, and the effect of reducing the catalyst load and improving the durability of the fuel cell is achieved.
Patent Information
- Application Number
- CN202011172667.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-30
- Filing Date
- 2020-10-28
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-10-28
AI Technical Summary
In polymer electrolyte membrane fuel cells, the permeation of hydrogen leads to deterioration of the electrolyte membrane, resulting in a decrease in durability, and the prior art tends to destroy insulation and increase metal load when adding a catalyst to the ion exchange layer.
By depositing the catalyst metal on the polymer film to form a reinforcement layer and impregnating with ionomers to obtain an electrolyte film, the catalyst metal is deposited only on the surface of the reinforcement layer, reducing the load of the catalyst and effectively removing oxygen through the porous structure.
The loading of the catalyst metal is significantly reduced, while the durability and functional performance of the electrolyte membrane are improved, the life of the electrolyte membrane is extended, and the open circuit voltage of the fuel cell is increased.
Smart Images

Figure CN112751043B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to an electrolyte membrane for a fuel cell having improved chemical durability and a method of manufacturing the same. Background Art
[0002] In a polymer electrolyte membrane fuel cell (PEMFC), an electrolyte membrane is used to transport hydrogen ions. To transport hydrogen ions, an ion exchange material is used to manufacture the electrolyte membrane. The ion exchange material contains water so as to selectively move hydrogen ions generated at the anode to the cathode.
[0003] The durability of the electrolyte membrane is reduced due to the degradation of the electrolyte membrane caused by hydrogen crossover. Due to the hydrogen crossover, hydrogen comes into contact with oxygen at the interface between the electrolyte membrane and the cathode, thereby generating hydrogen peroxide. Hydrogen peroxide decomposes into hydroxyl radicals (·OH) and hydroperoxyl radicals (·OOH), etc., thereby degrading the electrolyte membrane.
[0004] In recent years, in order to reduce costs and reduce the ionic resistance of the electrolyte membrane, the thickness of the electrolyte membrane has become thinner and thinner. The thinner the electrolyte membrane, the greater the amount of hydrogen permeation. As a result, the life of the electrolyte membrane is gradually reduced.
[0005] In order to solve the above problems, a technology has been proposed to add a small amount of catalyst to the ion exchange layer of the electrolyte membrane to prevent the generation of free radicals. However, as described above, when the catalyst is added to the ion exchange layer, the insulation of the electrolyte membrane is easily destroyed and the amount of catalyst added is increased.
[0006] The above information disclosed in this Background section is only for enhancement of understanding of the background of the present disclosure and therefore it may contain information that does not form the prior art that is already known in this country to one of ordinary skill in the art. Summary of the invention
[0007] The present disclosure has been made to solve the above-mentioned problems associated with the prior art.
[0008] An object of the present disclosure is to provide an electrolyte membrane for a fuel cell capable of preventing the transmission of hydrogen and / or oxygen, and a method for manufacturing the same.
[0009] Another object of the present disclosure is to provide an electrolyte membrane for a fuel cell, which can remove oxygen more efficiently than a conventional electrolyte membrane in which a catalyst is added to an ion exchange layer, and a method of manufacturing the same.
[0010] Another object of the present disclosure is to provide an electrolyte membrane for a fuel cell and a method for manufacturing the same, which electrolyte membrane for a fuel cell can significantly reduce the loading amount of catalyst metal while exhibiting the same or further improved functions as conventional electrolyte membranes in which a catalyst is added to an ion exchange layer.
[0011] The purpose of the present disclosure is not limited to the above-mentioned purpose. The purpose of the present disclosure will be clearly understood from the following description, and the purpose of the present disclosure can be achieved by the means defined in the claims and their combinations.
[0012] In one aspect, the present disclosure provides a method for manufacturing an electrolyte membrane for a fuel cell, the method comprising the steps of: preparing a polymer membrane; depositing a catalyst metal on one surface or opposite surfaces of the polymer membrane to obtain a reinforcement layer; and impregnating the reinforcement layer with an ionomer to obtain the electrolyte membrane.
[0013] The method may further include the step of drying the electrolyte membrane.
[0014] The polymer membrane may include polytetrafluoroethylene (PTFE).
[0015] The catalyst metal may include one selected from the group consisting of platinum (Pt), gold (Au), palladium (Pd), rhodium (Rh), iridium (Ir), ruthenium (Ru), and combinations thereof.
[0016] The catalyst metal may have a particle form, and the particle diameter of the catalyst metal may be 1 nm to 50 nm.
[0017] The catalyst metal may be deposited on the polymer film by sputtering or atomic layer deposition (ALD).
[0018] Before and / or after deposition of the catalyst metal, the polymer film is stretched to obtain a reinforcement layer.
[0019] The reinforcement layer may be a porous film including a surface and pores, and the catalyst metal may be deposited only on the surface of the reinforcement layer.
[0020] The loading of the catalyst metal deposited on the reinforcement layer can be 0.001 mg / cm 2 Up to 0.1mg / cm 2 .
[0021] The thickness of the reinforcement layer may be 5 μm to 15 μm, and the porosity of the reinforcement layer may be 70% to 90%.
[0022] The maximum tensile strength of the reinforcement layer based on ASTM D882 may be 5 MPa to 110 MPa.
[0023] The step of impregnating the reinforcement layer with the ionomer to obtain the electrolyte membrane may include: coating the ionomer on a release paper; disposing the reinforcement layer on the ionomer to impregnate one surface of the reinforcement layer with the ionomer; and impregnating the other surface of the reinforcement layer with the ionomer.
[0024] In another aspect, the present disclosure provides an electrolyte membrane for a fuel cell, the electrolyte membrane including: a reinforcement layer impregnated with an ionomer and having a catalyst metal deposited on one surface or opposite surfaces of the reinforcement layer; and an ion exchange layer formed on the opposite surface of the reinforcement layer.
[0025] The catalyst metal may include one selected from the group consisting of platinum (Pt), gold (Au), palladium (Pd), rhodium (Rh), iridium (Ir), ruthenium (Ru), and combinations thereof.
[0026] The reinforcement layer may include uniaxially or biaxially stretched porous expanded polytetrafluoroethylene (e-PTFE).
[0027] The catalyst metal may have a particle form, and the particle diameter of the catalyst metal may be 1 nm to 50 nm.
[0028] The reinforcement layer may be a porous film including a surface and pores, and the catalyst metal may be deposited only on the surface of the reinforcement layer.
[0029] The loading of the catalyst metal deposited on the reinforcement layer can be 0.001 mg / cm 2 Up to 0.1mg / cm 2 .
[0030] The thickness of the reinforcement layer may be 5 μm to 15 μm, and the porosity of the reinforcement layer may be 70% to 90%.
[0031] The maximum tensile strength of the reinforcement layer based on ASTM D882 may be 5 MPa to 110 MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The above and other features of the present disclosure will now be described in detail with reference to certain exemplary embodiments shown in the accompanying drawings, which are given hereinafter by way of illustration only and thus do not limit the present disclosure, and in which:
[0033] Figure 1 is a flow chart showing a method for manufacturing an electrolyte membrane for a fuel cell according to the present disclosure;
[0034] Figure 2A is a plan view showing a polymer film on which a catalyst metal is deposited;
[0035] Figure 2B It is shown that by uniaxial stretching Figure 2AA plan view of a porous reinforcement layer on which a catalyst metal is deposited obtained by using a polymer film;
[0036] Figure 2C It is shown that by biaxial stretching Figure 2A A plan view of a porous reinforcement layer on which a catalyst metal is deposited obtained by using a polymer film;
[0037] Figure 3 is a cross-sectional view schematically showing a reinforcing layer according to the present disclosure; and
[0038] Figure 4 is a cross-sectional view schematically showing an electrolyte membrane according to the present disclosure.
[0039] It should be understood that the accompanying drawings are not necessarily drawn to scale, but rather present a somewhat simplified representation of various preferred features illustrating the basic principles of the present disclosure. The specific design features of the present disclosure disclosed herein, including, for example, specific dimensions, orientations, locations, and shapes, will be determined in part by the specific intended application and use environment.
[0040] In the drawings, reference numbers refer to the same or equivalent parts of the present disclosure throughout the several figures of the drawing. DETAILED DESCRIPTION
[0041] By referring to the accompanying drawings and according to the following preferred embodiments, the above-mentioned objects and other objects, features and advantages will be clearly understood. However, the present disclosure is not limited to the embodiments and will be implemented in different forms. The embodiments introduced in this article are only to provide a thorough and complete understanding of the disclosed content and fully convey the technical concept of the present disclosure to those skilled in the art.
[0042] Throughout the description of the figures, the same reference numerals refer to the same components. In the drawings, the size of the structure is exaggerated for clarity. It will be understood that although the terms "first", "second", etc. may be used herein to describe various components, the corresponding components should not be understood to be limited by these terms, which are only used to distinguish one component from other components. For example, within the scope defined by the present disclosure, a first component may be referred to as a second component, and similarly, a second component may be referred to as a first component. Unless the context clearly indicates otherwise, the singular form also includes the plural form.
[0043] It will be further understood that the terms "comprising," "having," and the like, when used in this specification, specify the presence of the stated features, quantities, steps, operations, components, parts, or combinations thereof, but do not exclude the presence or addition of one or more other features, quantities, steps, operations, components, parts, or combinations thereof. In addition, it will be understood that when a component such as a layer, film, region, or plate is referred to as being "on" another component, it may be directly on the other component, or there may be intervening components. It will also be understood that when a component such as a layer, film, region, or plate is referred to as being "under" another component, it may be directly under the other component, or there may be intervening components.
[0044] Unless the context clearly indicates otherwise, all numerals, values and / or expressions of the amount of the expression composition, reaction conditions, polymer composition and mixture used in this specification are approximate values, reflecting the various measurement uncertainties that occur inherently when obtaining these values from other things. For this reason, it should be understood that in all cases, the term "about" should modify all numerals, values and / or expressions. In addition, when a numerical range is disclosed in the specification, unless otherwise defined, these ranges are continuous and include all values from the minimum to the maximum value within the range. In addition, when the range is an integer, unless otherwise defined, all integers from the minimum to the maximum value within the range are included.
[0045] Figure 1 is a flow chart showing a method for manufacturing an electrolyte membrane for a fuel cell according to the present disclosure. Referring to the figure, the manufacturing method includes the following steps: in S10, a polymer membrane is prepared; in S20, a catalyst metal is deposited on one surface or an opposite surface of the polymer membrane to obtain a reinforcement layer; and in S30, the reinforcement layer is impregnated with an ionomer to obtain an electrolyte membrane. The manufacturing method may further include a step of drying the electrolyte membrane.
[0046] The polymer film may include polytetrafluoroethylene (PTFE).
[0047] The shape, size and thickness of the polymer film are not particularly limited and may be appropriately adjusted according to the purpose of use.
[0048] Subsequently, in S20 , a catalyst metal is deposited on one surface or opposite surfaces of the polymer film.
[0049] The catalyst metal may include one selected from the group consisting of platinum (Pt), gold (Au), palladium (Pd), rhodium (Rh), iridium (Ir), ruthenium (Ru) and combinations thereof. The catalyst metal refers to the catalyst metal itself, rather than the catalyst metal supported on a carrier such as a carbon nanotube. When the catalyst metal is supported on a carrier and then disposed on a polymer membrane, the particle size of the catalyst metal becomes too large, so that the catalyst metal may become an obstacle to the movement of ions in the electrolyte membrane. Therefore, in the present disclosure, the catalyst metal itself is disposed on the polymer membrane to solve the above problems. Specifically, the catalyst metal may have a particle form, and its particle size may be 1nm to 50nm.
[0050] The catalyst metal may be deposited on one surface or opposite surfaces of the polymer film by sputtering or atomic layer deposition (ALD). However, the present disclosure is not limited thereto. Other methods may be used without limitation as long as the method can place the catalyst metal on the polymer film in the form of particles.
[0051] Figure 2A is a plan view showing a polymer film 11 having a catalyst metal 13 deposited on one surface. Figure 2A The case where the catalyst metal 13 is deposited only on one surface of the polymer film 11 is shown. However, the present disclosure is not limited thereto. The catalyst metal 13 may be deposited on each of the opposite surfaces of the polymer film 11 as needed.
[0052] The polymer film may be stretched before and / or after the catalyst metal is deposited on the polymer film. Figure 2B is a plan view showing a porous reinforcement layer 10 on which a catalyst metal 13 is deposited, which is obtained by uniaxially stretching a polymer film after depositing the catalyst metal on the polymer film, Figure 2C is a plan view showing a porous reinforcement layer 10 on which a catalyst metal 13 is deposited, obtained by biaxially stretching a polymer film.
[0053] As described above, the porous reinforcement layer 10 may be obtained by uniaxially or biaxially stretching the polymer film 11. The reinforcement layer 10 may include expanded-polytetrafluoroethylene (e-PTFE).
[0054] Figure 3is a cross-sectional view showing the reinforcement layer 10. Referring to the figure, the reinforcement layer 10 includes a surface 20 and pores 30 formed by stretching. The catalyst metal 13 is deposited only on the surface 20. If the catalyst metal 13 is also provided in the pores 30, the loading amount of the catalyst metal may be unnecessarily increased. In addition, since the ions move within the electrolyte membrane due to the ionomer that is then impregnated in the pores, the conductivity of the ions may be reduced.
[0055] The loading amount of the catalyst metal 13 deposited on the reinforcement layer 10 may be 0.001 mg / cm 2 Up to 0.1mg / cm 2 In this specification, the supported amount of the catalyst metal 13 is calculated not based on the polymer film 11 but based on the reinforcement layer 10 obtained by stretching the polymer film 11 .
[0056] The thickness, porosity and maximum tensile strength of the reinforcing layer 10 are not particularly limited and can be appropriately adjusted according to the purpose of use. For example, the thickness of the reinforcing layer 10 can be 5 μm to 15 μm, the porosity of the reinforcing layer 10 can be 70% to 90%, and the maximum tensile strength of the reinforcing layer 10 based on ASTM D882 can be 5 MPa to 110 MPa.
[0057] In S30 , the reinforcement layer may be impregnated with the ionomer to obtain an electrolyte membrane.
[0058] General ionomers known in the art to which the present disclosure pertains may be used as the ionomer without limitation. In an example, a perfluorosulfonic acid (PFSA) polymer such as Nafion may be used.
[0059] There is no particular limitation on the impregnation method of the ionomer. A method including the steps of coating the ionomer on a release paper, providing the reinforcement layer 10 on the coated ionomer to impregnate one surface of the reinforcement layer 10 with the ionomer, and impregnating the other surface of the reinforcement layer with the ionomer may be performed.
[0060] Subsequently, the electrolyte membrane obtained by impregnating the reinforcement layer 10 with the ionomer may be dried and heat-treated.
[0061] The drying conditions and heat treatment conditions of the electrolyte membrane are not particularly limited, and the electrolyte membrane can be dried and heat treated under conditions generally set in the field to which the present disclosure belongs. For example, the drying can be performed at 25°C to 100°C, and the heat treatment can be performed at 140°C to 200°C.
[0062] Figure 41 is a cross-sectional view schematically showing an electrolyte membrane 1 manufactured using the above method. Referring to the figure, the electrolyte membrane 1 may include: a reinforcement layer 10 impregnated with an ionomer and having a catalyst metal 13 deposited on one surface or an opposite surface thereof; and an ion exchange layer 40 formed on the opposite surface of the reinforcement layer 10.
[0063] The ion exchange layer 40 is a layer formed of the ionomer impregnated with the reinforcement layer 10 using the above-described manufacturing method, and the thickness of the ion exchange layer 40 is not particularly limited.
[0064] In the electrolyte membrane 1, the porous reinforcement layer 10 is impregnated with ionomer between its pores. When the fuel cell is operating, oxygen can be transferred from the cathode to the anode, or hydrogen can be transferred from the anode to the cathode. In this case, the gas must pass through the pores of the reinforcement layer 10. In the present disclosure, the catalyst metal 13 is added to the surface of the reinforcement layer 10, which is a bottleneck for the gas, instead of the ion exchange layer 40, so that the movement of the gas can be effectively prevented.
[0065] Furthermore, if the catalyst metal 13 is added to the ion exchange layer 40, the oxygen element of the ionomer contained in the ion exchange layer 40 interacts with the catalyst metal 13, thereby possibly reducing the activity of the catalyst metal 13. On the other hand, since the reinforcement layer 10 is composed of a combination of carbon (C)-fluorine (F), the reinforcement layer 10 does not react with the catalyst metal 13. Therefore, according to the present disclosure, oxygen can be removed more effectively than in the case where the catalyst metal 13 is added to the ion exchange layer 40.
[0066] Example
[0067] Platinum (Pt) as a catalyst metal is deposited on polytetrafluoroethylene (PTFE) as a polymer film by sputtering. The polymer film deposited with platinum is biaxially stretched to produce a reinforcement layer. At this time, the loading amount of platinum is about 0.01 mg / cm 2 .
[0068] A predetermined amount of PFSA ionomer is applied to the release paper, and a reinforcement layer is disposed on the applied ionomer to impregnate one surface of the reinforcement layer with the ionomer. The same ionomer is applied to the other surface of the reinforcement layer to impregnate the other surface of the reinforcement layer with the ionomer.
[0069] The electrolyte membrane obtained by the above method is dried at about 80°C and then heat-treated at about 160°C.
[0070] Comparative Example
[0071] An electrolyte membrane was manufactured using the same materials and method as in Example, except that platinum (Pt) as a catalyst metal was not deposited.
[0072] Experimental example
[0073] A pair of electrodes was formed on each of the electrolyte membranes according to the examples and comparative examples to manufacture a membrane-electrode assembly, and the open circuit voltage (OCV) of each membrane-electrode assembly was measured. The results are shown in Table 1 below.
[0074] Table 1
[0075] Classification OCV[V] Comparative Example 0.990 Example 1.022
[0076] Referring to Table 1, it can be seen that in the case of using the electrolyte membrane according to the embodiment, the OCV of the membrane-electrode assembly is further improved by about 5% or more.
[0077] As is apparent from the foregoing, according to the present disclosure, the gas transmitted through the electrolyte membrane can be effectively removed, so that the open circuit voltage (OCV) of the fuel cell can be increased.
[0078] According to the present disclosure, the generation of radicals in an electrolyte membrane can be suppressed, so that a fuel cell having improved chemical durability and extended life can be obtained.
[0079] According to the present disclosure, the loading amount of catalyst metal added to the electrolyte membrane can be significantly reduced compared with the conventional technology.
[0080] The effects of the present disclosure are not limited to those described above. It should be understood that the effects of the present disclosure include all effects that can be inferred from the foregoing description of the present disclosure.
[0081] The present disclosure has been described in detail with reference to the preferred embodiments of the present disclosure. However, it will be appreciated by those skilled in the art that these embodiments may be changed without departing from the principles and spirit of the present disclosure, and the scope of the present disclosure is defined by the appended claims and their equivalents.
Claims
1. A method for producing an electrolyte membrane for a fuel cell, The following steps are involved: preparing a polymer film; depositing a catalyst metal on one surface or on opposing surfaces of the polymer film to obtain a reinforcement layer; as well as impregnating the reinforcement layer with an ionomer to obtain an electrolyte membrane, The catalyst metal mentioned herein refers to the catalyst metal itself.
2. The method according to claim 1, further comprising: The following steps are involved: The electrolyte membrane is dried.
3. The method according to claim 1, in, The polymer membrane includes polytetrafluoroethylene, or PTFE.
4. The method according to claim 1, in, The catalyst metal includes one selected from the group consisting of platinum (Pt), gold (Au), palladium (Pd), rhodium (Rh), iridium (Ir), ruthenium (Ru), and combinations thereof.
5. The method according to claim 1, in, The catalyst metal is in particulate form; and The particle size of the catalyst metal is 1 nm to 50 nm.
6. The method according to claim 1, in, The catalyst metal is deposited on the polymer film by sputtering or atomic layer deposition, or ALD.
7. The method according to claim 1, in, Before and after depositing the catalyst metal, the polymer film is stretched to obtain the reinforcement layer.
8. The method according to claim 1, in, Before or after depositing the catalyst metal, the polymer film is stretched to obtain the reinforcement layer.
9. The method according to claim 1, in, The reinforcement layer is a porous membrane including a surface and pores; and The catalyst metal is deposited only on the surface of the reinforcement layer.
10. The method according to claim 1, in, The loading amount of the catalyst metal deposited on the reinforcement layer is 0.001 mg / cm 2 Up to 0.1mg / cm 2 .
11. The method according to claim 1, in, The thickness of the reinforcement layer is 5 μm to 15 μm, and the porosity of the reinforcement layer is 70% to 90%.
12. The method according to claim 1, in, The maximum tensile strength of the reinforcing layer based on ASTM D882 is 5 MPa to 110 MPa.
13. The method according to claim 1, in, The step of impregnating the reinforcement layer with an ionomer to obtain an electrolyte membrane comprises: coating the ionomer onto a release paper; disposing the reinforcement layer on the ionomer to impregnate one surface of the reinforcement layer with the ionomer; and The other surface of the reinforcement layer is impregnated with the ionomer.
14. An electrolyte membrane for a fuel cell, the electrolyte membrane being manufactured by the method of claim 1, and include: a reinforcement layer impregnated with an ionomer and having a catalyst metal deposited on one surface or opposing surfaces of the reinforcement layer; as well as An ion exchange layer is formed on an opposite surface of the reinforcement layer.
15. The electrolyte membrane according to claim 14, in, The reinforcement layer includes uniaxially or biaxially stretched porous expanded polytetrafluoroethylene, i.e., e-PTFE.
16. The electrolyte membrane according to claim 14, in, The catalyst metal is in particulate form; and The particle size of the catalyst metal is 1 nm to 50 nm.
17. The electrolyte membrane according to claim 14, in, The reinforcement layer is a porous membrane including a surface and pores; and The catalyst metal is deposited only on the surface of the reinforcement layer.
18. The electrolyte membrane according to claim 14, in, The loading amount of the catalyst metal deposited on the reinforcement layer is 0.001 mg / cm 2 Up to 0.1mg / cm 2 .
19. The electrolyte membrane according to claim 14, in, The thickness of the reinforcement layer is 5 μm to 15 μm; and The porosity of the reinforcement layer is 70% to 90%.
20. The electrolyte membrane according to claim 14, in, The maximum tensile strength of the reinforcing layer based on ASTM D882 is 5 MPa to 110 MPa.