Mn-Bi-Sb based magnetic material and method for producing the same

By introducing Sb to replace Bi in Mn-Bi-based magnetic materials and optimizing the process flow, the manufacturing challenges of Mn-Bi-based magnetic materials have been solved, and the magnetic properties, especially the remanent magnetization, coercivity and maximum energy product, have been improved, making them suitable for high-temperature environments.

CN112992456BActive Publication Date: 2024-11-29HYUNDAI MOTOR CO LTD +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202010782869.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-06
Publication Date
2024-11-29
Estimated Expiration
2040-08-06

AI Technical Summary

Technical Problem

Existing Mn-Bi based magnetic materials suffer from difficulties in forming LTP-MnBi single phase, Mn oxide formation, and reduced magnetism during manufacturing. Furthermore, their maximum magnetic energy product is low, failing to meet the requirements for high-performance permanent magnets.

Method used

By partially replacing Bi with Sb in Mn-Bi-based magnetic materials, Mn-Bi-Sb-based magnetic materials are formed. Mn-Bi-Sb-based thin strips are prepared using melting, rapid solidification and heat treatment processes, and the crystal structure is optimized to improve the magnetism.

Benefits of technology

The remanent magnetization, coercivity, and maximum energy product of Mn-Bi-Sb based magnetic materials were improved, resulting in higher magnetic performance indicators and making them suitable for high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112992456B_ABST
    Figure CN112992456B_ABST
Patent Text Reader

Abstract

The present invention discloses a Mn-Bi-Sb-based magnetic material and a method for manufacturing the same. In particular, the Mn-Bi-Sb-based magnetic material includes Mn and Bi forming a hexagonal crystal structure, and a portion of the Bi element forming the crystal structure is replaced by Sb, thereby improving its magnetic properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a Mn-Bi-Sb-based magnetic material and a method for manufacturing the same, in particular, a portion of Bi element of the Mn-Bi-Sb-based magnetic material is replaced by Sb to improve magnetic properties. Background Art

[0002] Magnetic materials are materials used for bidirectional conversion of electrical energy and mechanical energy, and are core materials widely used in high-efficiency motors and generators.

[0003] Magnetic materials include soft magnetic materials and hard magnetic materials, which differ in the size of the external magnetic field that can change the direction of the magnetic poles. Hard magnetic materials can include, for example, permanent magnets, which usually generate a magnetic field at all times because the magnetic poles are aligned in a constant direction through magnetization. This magnetic field can be used to generate torque without applying additional energy.

[0004] The performance of a permanent magnet can be expressed by a BxH value, which is the product of the external magnetic field (H) applied to the magnet and the magnetic field (B) provided by the magnet at its operating point, and the maximum value is defined as the maximum magnetic energy product ((BH)max) and represents the performance index of the permanent magnet.

[0005] Recently, in the transportation and energy industries, magnetic materials have been used as primary power converters in auxiliary positions, increasing the demand for high-performance permanent magnets in the next generation industries.

[0006] In particular, the demand for electric vehicles has increased rapidly due to the increasing importance of replacing petroleum energy and developing low-carbon emission green industries in recent years. Therefore, the demand for magnetic materials used for permanent magnets is increasing in accordance with the trend of higher efficiency, lighter weight and smaller size of motors used in electric vehicles.

[0007] For example, ferrite and Nd-based magnets have been most widely used as magnetic materials. Nd-based magnets only require about 1 / 8 of the volume of ferrite magnets to obtain the same energy as ferrite magnets. Therefore, ferrite-based magnets are used for low-cost and low-performance products, while Nd-based magnets with a higher maximum magnetic energy product are used for high-efficiency and high-performance products.

[0008] In the case of Nd-based magnets, the maximum magnetic energy product of the magnet reaches a theoretical value during manufacture. On the other hand, since Nd-based magnets have low thermal stability, in order to increase the coercive force when used in electric motors, Nd-based magnets contain heavy rare earth elements such as Dy and Tb. However, in the case of heavy rare earth resources, there is a problem that heavy rare earth resources reduce the remanence (residual magnetization) of Nd-based magnets, thereby reducing the maximum magnetic energy product overall. In addition, rare earth elements have become expensive due to the uneven geographical distribution of resources and the weaponization of resources using the uneven distribution.

[0009] Therefore, research has been conducted on materials for non-rare earth permanent magnets having new compositions which, unlike conventional rare earth magnets, have a reduced amount of heavy rare earth elements or contain no rare earth elements.

[0010] Among the materials of non-rare earth permanent magnets, the maximum magnetic energy product of Mn-Bi-based magnets is greater than that of ferrite-based magnets, and has a coercive force greater than that of Nd-based magnets at high temperatures. Therefore, Mn-Bi-based magnets have been actively studied due to their advantages of improving automobile fuel efficiency through miniaturization, weight reduction, and improved motor efficiency.

[0011] The theoretical maximum magnetic energy product ((BH)max) of Mn-Bi based magnets is 17.7MGOe, which means excellent magnetic properties, and also has high uniaxial crystal magnetic anisotropy energy characteristics (2.2x10 7 erg / cm 3 (at 500K)). At high temperature (200°C), the coercivity of Mn-Bi based magnets is greater than that of Nd based magnets.

[0012] The technology of synthesizing Mn-Bi based magnets may include a thin film process and a powder process.

[0013] For example, in a thin film process, after depositing a Mn layer and a Bi layer using a sputtering method, an LTP-MnBi phase is generated by heat treatment. Therefore, the characteristics vary depending on the substrate type, and the variables of the in-situ heat treatment process are important.

[0014] In the powder process, magnetic thin ribbons are made from Mn-Bi ingots, which are then powdered and batched through heat treatment and pulverization processes. In order to increase the content of LTP-MnBi, it is important to control the melt spinning process and heat treatment conditions.

[0015] Meanwhile, when a Mn-Bi based magnet is manufactured using a thin film process, a high saturation magnetization value can be obtained, but it is impossible to manufacture the Mn-Bi based magnet in an industrially available batch form.

[0016] In addition, when manufacturing Mn-Bi based magnets using a powder process, it is difficult to manufacture LTP-MnBi single phase. In addition, there are problems such as poor magnetic properties due to the formation of Mn oxides and phase decomposition of LTP-MnBi during powder formation, and poor compatibility with Nd-based hard magnetic materials (Nd 2 Fe 14 B, theoretical (BH) max = 64MGOe), the theoretical maximum energy product is relatively low.

[0017] The contents described as background art are only for understanding the context of the present invention and should not be considered as corresponding to the prior art known to those skilled in the art. Summary of the invention

[0018] In a preferred aspect, a Mn-Bi-Sb based magnetic material and a method for manufacturing the same are provided, wherein a portion of the Bi element is substituted with Sb to improve magnetic properties.

[0019] In one aspect, a Mn-Bi-Sb-based magnetic material is provided, which may include a hexagonal crystal structure formed of a material containing manganese (Mn) and bismuth (Bi). In particular, a portion of the Bi element forming the crystal structure may be substituted with antimony (Sb).

[0020] The substitution amount of Sb may be about 3.0 atomic % or less.

[0021] Mn-Bi-Sb based magnetic materials can be x Bi 100-x-y Sb y Indicates that x is 48 to 56 and y is 3.0 or less.

[0022] Preferably, the magnetic material can be Mn 54 Bi 46-y Sb y Indicates that, and y is 3.0 or less.

[0023] The magnetic substance may include about 50% or more of a low temperature MnBi phase (LTP-MnBi).

[0024] The remaining Bi phase and the Mn oxide (Mn-oxide) phase may not be formed in the magnetic material.

[0025] The magnetic substance may suitably contain the remaining Bi phase and the Mn oxide (Mn-oxide) phase in an amount of about 10 wt % or less based on the total weight of the magnetic substance.

[0026] The magnetic substance may suitably have a saturation magnetization value (Ms) of about 38 emu / g or more.

[0027] The magnetic substance may suitably have a coercive force (Hc) of 500 Oe or more.

[0028] The hexagonal crystal structure may also be formed of a material consisting essentially of manganese (Mn) and bismuth (Bi) or a material consisting of manganese (Mn) and bismuth (Bi).

[0029] In one aspect, a method for manufacturing a Mn-Bi-Sb-based magnetic material is provided, which may include preparing an intermetallic compound by melting manganese (Mn), bismuth (Bi) and antimony (Sb), preparing a Mn-Bi-Sb-based mixed molten solution by melting the intermetallic compound, forming a Mn-Bi-Sb-based thin ribbon by cooling the Mn-Bi-Sb-based mixed molten solution, and converting the Mn-Bi-Sb-based thin ribbon into a magnetic Mn-Bi-Sb-based thin ribbon by heat treatment. Preferably, Mn, Bi and Sb are melted at least substantially simultaneously, that is, Mn, Bi and Sb are melted simultaneously or approximately simultaneously, or Mn, Bi and Sb are melted within about 60, 50, 40, 30, 20, 10, 5, 3, 2 or 1 minute or less of each other.

[0030] The preparation of the intermetallic compound may include mixing Mn, Bi and Sb to satisfy the x Bi 100-x-y Sb y , wherein x is 48 to 56 and y is 3.0 or less, followed by cooling, thereby preparing a Mn—Bi—Sb based ingot as an intermetallic compound.

[0031] The preparation of the intermetallic compound may include mixing Mn, Bi and Sb to satisfy the 54 Bi 46-y Sb y , wherein y is 3.0 or less, followed by cooling, thereby preparing a Mn—Bi—Sb based ingot as an intermetallic compound.

[0032] Forming the Mn—Bi—Sb based ribbon may include cooling the Mn—Bi—Sb based mixed molten solution using a rapid solidification process (RSP) to form the Mn—Bi—Sb rapid quenched ribbon.

[0033] The conversion into the magnetic Mn-Bi-Sb based ribbon may include heat treating the Mn-Bi-Sb quenched ribbon at a temperature in the range of about 270 to 330°C.

[0034] The conversion into the magnetic Mn-Bi-Sb based ribbon may include heat treating the Mn-Bi-Sb quenched ribbon in an inert gas atmosphere for about 12 to 48 hours.

[0035] According to various exemplary embodiments of the present invention, a Mn-Bi-Sb-based magnetic material can be manufactured in which a portion of the Bi element is simply replaced by Sb. The Mn-Bi-Sb-based magnetic material can have magnetic properties superior to those of a Mn-Bi-based magnetic material (which is a binary system).

[0036] For example, the Mn-Bi-Sb-based magnetic material may have increased residual magnetization value (Mr), coercive force (Hc) and squareness ratio (Mr / Ms) characteristics compared to the Mn-Bi-based magnetic material. For example, the Mn-Bi-Sb-based magnetic material may have an improved maximum magnetic energy product (increased by 924.05%) compared to the Mn-Bi-based magnetic material. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The above and other objects, features and advantages of the present invention will be more clearly understood from the following detailed description presented in conjunction with the accompanying drawings, in which:

[0038] Figure 1 is a Bethe-Slater plot for explaining formation of an exemplary Mn—Bi—Sb-based magnetic substance according to an exemplary embodiment of the present invention;

[0039] Figure 2 is a diagram for explaining formation of an exemplary Mn—Bi—Sb-based magnetic substance according to an exemplary embodiment of the present invention;

[0040] Figure 3 is a diagram showing an exemplary crystal structure of LTP-MnBi;

[0041] Figure 4 is a graph obtained by comparing an exemplary Mn—Bi—Sb-based magnetic substance according to an exemplary embodiment of the present invention before and after heat treatment;

[0042] Figure 5 and Figure 6 is a diagram showing an X-ray diffraction pattern of an exemplary Mn-Bi-Sb-based magnetic substance depending on a change in Sb content;

[0043] Figure 7 is a graph showing a hysteresis curve of an exemplary Mn-Bi-Sb-based magnetic substance depending on a change in Sb content; and

[0044] Figure 8 is a graph showing magnetic properties of an exemplary Mn—Bi—Sb-based magnetic substance depending on changes in Sb content. DETAILED DESCRIPTION

[0045] Embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below, but will be implemented in various forms, and this embodiment is only intended to complete the disclosure of the present invention, and this embodiment is provided to fully inform those skilled in the art of the scope of the present invention.

[0046] The terms used herein are only used to describe the purpose of exemplary embodiments and are not intended to limit the present invention. As used herein, the singular forms "one", "an" and "the" are intended to also include plural forms, unless the context clearly states otherwise. It will also be understood that when the terms "comprising" and / or "including" are used in this specification, it is indicated that there are the features, numerical values, steps, operations, elements, and / or components, but the presence or addition of one or more other features, numerical values, steps, operations, elements, components and / or the groups composed thereof are not excluded. As used herein, the term "and / or" includes any and all combinations of one or more related enumerated items.

[0047] Unless otherwise stated or apparent from the context, the term "about" as used herein is understood to be within the normal tolerance range in the art, such as within 2 standard deviations of the mean. "About" may be understood to be within 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, 0.1%, 0.05%, or 0.01% of the specified value. Unless otherwise apparent from the context, all numerical values ​​provided herein are modified by the term "about".

[0048] Various aspects of the Mn—Bi—Sb-based magnetic substance can be provided based on the fact that a magnetic substance having magnetic properties superior to that of the Mn—Bi-based magnetic substance is obtained when various kinds of elements are added to the Mn—Bi-based magnetic substance.

[0049] Figure 1 is a Bethe-Slater curve for explaining the formation of an exemplary Mn-Bi-Sb-based magnetic substance according to an exemplary embodiment of the present invention, and Figure 2 is a diagram for explaining formation of an exemplary Mn—Bi—Sb-based magnetic substance according to an exemplary embodiment of the present invention.

[0050] like Figure 1 As shown, magnetic materials (i.e., magnetic substances) can only exhibit ferromagnetism when the value of the exchange integral is positive.

[0051] In addition, if Figure 2 As shown, pure Mn is antiferromagnetic, but when Bi is added to form a MnBi alloy, the spacing between Mn atoms may increase due to lattice expansion.

[0052] Therefore, a / r increases, and thus J ex The value of becomes positive, which makes MnBi ferromagnetic.

[0053] For example, when different kinds of elements are added to a Mn-Bi based alloy, a magnetic substance having magnetic properties superior to those of a Mn-Bi based magnetic substance can be obtained.

[0054] Meanwhile, when adding different kinds of elements to the Mn-Bi based alloy, in order to maintain the LTP-MnBi phase, the Mn site substitution method, the Bi site substitution method and the interstitial site invasion method can be used.

[0055] Furthermore, an element suitable for addition to and substitution for another element in the composition of the Mn-Bi-based alloy should have an atomic radius and an electronic structure similar to those of the Mn-Bi-based alloy.

[0056] Preferably, a part of Bi element among elements constituting the Mn-Bi-based alloy may be substituted with Sb to form the Mn-Bi-based alloy.

[0057] In particular, in a Mn—Bi—Sb-based magnetic substance, Mn and Bi may form a hexagonal crystal structure, and a portion of the Bi element forming the crystal structure may be substituted with Sb to form the Mn—Bi—Sb-based magnetic substance.

[0058] Figure 3 : is a diagram showing the crystal structure of LTP-MnBi. In the case of a Mn-Bi-Sb-based magnetic material, Mn and Bi may form a hexagonal crystal structure, and Sb may replace certain sites of the Bi element to form a Mn-Bi-Sb-based magnetic material.

[0059] Regarding substitution of Bi with Sb, the substitution amount of Sb may preferably be about 3.0 atomic % or less.

[0060] Therefore, Mn-Bi-Sb based magnetic materials can be x Bi 100-x-y Sb y Preferably, x is 48 to 56, and y is 3.0 or less. When the content of Mn is in the range of about 48 to 56 atomic %, it can be observed that the amount of Bi phase and Mn-oxide phase that have an adverse effect on the magnetic material is about 10 weight % or less (based on the total weight of the Mn-Bi-Sb-based magnetic material). In particular, in the Mn-Bi-Sb-based magnetic material, when the content of Mn is about 54 atomic %, no Bi phase and Mn-oxide phase that have an adverse effect on the magnetic material are observed. Therefore, more preferably, the Mn-Bi-Sb-based magnetic material can be based on Mn 54 Bi 46-y Sb y y is preferably 3.0 or less.

[0061] A method for producing a Mn-Bi-Sb based magnetic material is further provided.

[0062] The method for manufacturing a Mn-Bi-Sb-based magnetic material may include: preparing an intermetallic compound by simultaneously melting Mn, Bi and Sb, preparing a Mn-Bi-Sb-based mixed molten solution by melting the intermetallic compound, forming a Mn-Bi-Sb-based thin strip by cooling the Mn-Bi-Sb-based mixed molten solution, and converting the Mn-Bi-Sb-based thin strip into a magnetic Mn-Bi-Sb-based thin strip by heat treatment.

[0063] The preparation of the intermetallic compound may include preparing Mn, Bi and Sb metal fragments having a purity of 99.99% or more. In addition, the prepared Mn, Bi and Sb may be mixed to satisfy the purity of Mn. x Bi 100-x-y Sb y , wherein x is 48 to 56 and y is 3.0 or less, followed by cooling, thereby preparing a Mn—Bi—Sb based ingot as an intermetallic compound.

[0064] In more detail, the prepared Mn, Bi and Sb may be mixed to satisfy the Mn x Bi 100-x-y Sb y The ratio of (where x is 48 to 56 and y is 3.0 or less) is then placed on a copper floor using water cooling, and then a plasma arc melting process is performed to manufacture a Mn-Bi-Sb based ingot. In order to improve the uniformity of the metal in the ingot, the remelting process may be repeated four times. In particular, the prepared Mn, Bi, and Sb may be mixed so as to satisfy the Mn 54 Bi 46-y Sb y ratio (where y is 3.0 or less).

[0065] When preparing the Mn-Bi-Sb-based mixed molten solution, the Mn-Bi-Sb-based ingot can be appropriately placed in a quartz tube and then melted by rapid induction heating in an inert Ar gas atmosphere to produce the Mn-Bi-Sb-based mixed molten solution.

[0066] The formation of the Mn-Bi-Sb based ribbon can be achieved by appropriately cooling the prepared Mn-Bi-Sb based mixed molten solution using a rapid solidification process (RSP) to form a Mn-Bi-Sb rapid quenching ribbon.

[0067] For example, the prepared Mn-Bi-Sb-based mixed molten solution can be sprayed onto the surface of a rotating metal copper wheel at a speed of about 50 m / s to quickly cool the Mn-Bi-Sb-based mixed molten solution, thereby obtaining a Mn-Bi-Sb fast-quenched thin ribbon. The melt spinning process can be carried out in an Ar gas atmosphere of sufficiently high purity.

[0068] The conversion into a magnetic Mn-Bi-Sb based ribbon may suitably comprise heat treating the Mn-Bi-Sb quenched ribbon at a temperature in the range of about 270-330°C to homogenise the Mn, Bi and Sb atoms in the ribbon.

[0069] For example, to obtain a desired hard magnetic phase, an inert gas atmosphere may be formed in a quartz tube furnace, and a Mn—Bi—Sb quenched ribbon may be loaded into the quartz tube furnace and then heat treated at a temperature in the range of about 270 to 330° C. for about 12 to 48 hours.

[0070] Example

[0071] The present invention will be described with reference to Comparative Examples and Examples.

[0072] The microstructure of the Mn-Bi-Sb quenched ribbon was observed before and after heat treatment. Figure 4 .

[0073] The Mn-Bi-Sb rapid quenching thin strip is manufactured according to the exemplary manufacturing method of the present invention, and has Mn 54 Bi 44.5 Sb 1.5 The alloy composition.

[0074] Figure 4 is a graph obtained by comparing an exemplary Mn—Bi—Sb-based magnetic substance according to an exemplary embodiment of the present invention before and after heat treatment.

[0075] like Figure 4 As shown, in the Mn-Bi-Sb quenched ribbon before heat treatment, grains with a size of less than about 1 μm are finely mixed. As a result of EDS analysis, Mn-Bi-Sb (dark gray) regions and Mn-Bi (gray) regions are identified.

[0076] The Mn-Bi-Sb region may be a quenched high temperature phase (QHTP), the formation of which is promoted by Sb.

[0077] Meanwhile, the Mn, Bi, and Sb atoms in the Mn-Bi-Sb ribbon can be homogenized after heat treatment.

[0078] Next, the X-ray diffraction patterns of the Mn-Bi-Sb based magnetic material depending on the change in Sb content were analyzed, and the mass fraction of each phase was calculated based on the results. The results are shown in Figure 5 and Figure 6 And Table 1.

[0079] The mass fraction (wt %) of each phase was calculated using the Rietveld refinement method, Jade 9.5 program and the obtained X-ray diffraction pattern.

[0080] Figure 5 and Figure 6 : is a graph showing an X-ray diffraction pattern of a Mn-Bi-Sb-based magnetic substance depending on a change in the Sb content. Table 1 shows the mass fraction of each phase depending on a change in the Sb content.

[0081] Table 1

[0082] Sb substitution amount (y) LTP-MnBi (wt%) <![CDATA[Bi 9 Mn 10 Sb (wt%)]]> 0.0 100 - 0.5 100 - 1.0 88.2 11.8 1.5 83.7 16.3 2.0 80.7 19.3 2.5 61.9 38.1 3.0 55.3 44.7 5.0 - 100

[0083] like Figure 5 As shown in Table 1, the sample is composed of Mn 54 Bi 46-y Sb y Magnetic thin ribbons in which the substitution amount y of Sb is changed to 0, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0 and 5.0, and an X-ray diffraction pattern obtained by heat treating the sample in an Ar gas atmosphere at 300°C for 24 hours is shown.

[0084] For example, when y is 0, a LTP-MnBi single phase is formed, and when the content of Sb is increased, a Bi 9 Mn 10 Sb phase.

[0085] In addition, as the amount of Sb substitution increases, the weight fraction of the LTP-MnBi phase decreases, and its weight fraction is 0 weight % under the condition that y is 5.0.

[0086] At the same time, in Mn 54 Bi 46-y Sb y No Bi phase or Mn-oxide phase is observed in the diffraction pattern of because, for example, the composition and heat treatment conditions of Mn-Bi-Sb are optimized.

[0087] The Bi phase or Mn-oxide phase that negatively affects the magnetic material is a phase generated during heat treatment and does not exhibit hard magnetism. The Bi phase or Mn-oxide phase reduces the magnetic properties of the magnetic material relative to its total volume or total weight (emu / cm 3 or emu / g).

[0088] Furthermore, by observing the formation of Mn-oxide phase during the heat treatment, the oxide appeared due to insufficient optimization of the heat treatment process, which was the reason for the rapid decrease in the magnetic properties of the magnetic material.

[0089] Figure 6 The change in the position of the 101 peak, which is a main peak of the LTP-MnBi phase in the X-ray diffraction pattern of the Mn-Bi-Sb magnetic ribbon, depending on the amount of Sb substitution is shown.

[0090] The main peak of LTP-MnBi shifts to a larger angle (high-angle shift) as the Sb content increases until y becomes 3. This indicates that the lattice of the crystal structure shrinks and the substitution of Sb atoms affects the lattice constant of LTP-MnBi.

[0091] In addition, the radii of Bi and Sb atoms are 156 pm and 140 pm (empirical sizes), respectively, and as Bi atoms are replaced by Sb atoms, the LTP-MnBi crystal structure undergoes lattice contraction, which is consistent with the change in the position of the main peak of LTP-MnBi.

[0092] The magnetic properties of the Mn-Bi-Sb based magnetic material depending on the change in Sb content were examined, and the results are shown in Tables 2 and 3. Figure 7 and Figure 8 The saturation magnetization is the value measured when the maximum externally applied magnetic field is 25kOe.

[0093] Table 2

[0094]

[0095]

[0096] Figure 7 and Figure 8 Graphs showing the change in magnetic properties of a Mn-Bi-Sb-based magnetic material depending on the Sb content. Figure 7 shows the hysteresis curve, Figure 8 The maximum magnetic energy product ((BH)max), squareness ratio (Mr / Ms), coercive force (Hc) and residual magnetization value (Mr) are shown.

[0097] As shown in Table 2 and Figure 7 As shown in Figure 2, as the amount of Sb substitution increases, the saturation magnetization value (Ms) decreases, and begins to decrease rapidly when y is 2.0. This is consistent with the results of X-ray diffraction (XRD) analysis, because, for example, as the Sb content increases, Bi as a non-magnetic phase 9 Mn 10 The phase fraction of Sb increases.

[0098] In addition, if Figure 7 As shown in FIG. 1 , when y is 5, no ferromagnetism is shown in the hysteresis curve. This is because, for example, when y is 5, Bi with non-magnetic 9 Mn 10 Sb single phase.

[0099] When y is 3.0 or less, the Mn-Bi-Sb magnetic ribbon can have hard magnetism. In particular, when y is 3.0 or less, the saturation magnetization value (Ms) of the Mn-Bi-Sb magnetic material can be 38emu / g or more, and the coercive force (Hc) can be 500Oe or more.

[0100] In addition, if Figure 8 As shown, as the amount of Sb substitution increases, the coercive force (Hc), squareness ratio (Mr / Ms) and residual magnetization value (Mr) of the ribbon shape increase, because, for example, the substitution of the Sb element affects the anisotropy of the Mn-Bi-Sb magnetic ribbon.

[0101] Furthermore, the improvement of anisotropic characteristics due to the substitution of Sb may have a significant influence on the residual magnetization, coercive force, and squareness ratio, which leads to an improvement in the maximum magnetic energy product.

[0102] For example, compared with the conventional condition where y is 0, the coercive force is increased by 837.65% and the maximum magnetic energy product is increased by 924.05% in the composition where y is 1.5.

[0103] Although the present invention has been described with reference to the accompanying drawings and the preferred embodiments described above, the present invention is not limited thereto but is defined by the appended claims. Therefore, those skilled in the art can make various changes and modifications to the present invention without departing from the technical spirit of the appended claims.

Claims

1. A Mn-Bi-Sb based magnetic material, include: A hexagonal crystal structure formed by a material containing Mn and Bi, Among them, part of the Bi element that forms the crystal structure is replaced by Sb. Wherein, the magnetic material is Mn 54 Bi 46-y Sb y It means that y is 0.5 to 3.0, wherein the magnetic substance includes 50 wt % or more of a low temperature MnBi phase, and Wherein, no residual Bi oxide phase and Mn oxide phase are formed in the magnetic material.

2. A Mn-Bi-Sb based magnetic material, which is based on Mn 54 Bi 46-y Sb y where y is 0.5 to 3.0, in, The magnetic substance includes a low-temperature MnBi phase in an amount of 50 wt % or more, and Wherein, no residual Bi oxide phase and Mn oxide phase are formed in the magnetic material.

3. A method for producing the Mn-Bi-Sb based magnetic material as claimed in claim 1, the method include: preparing an intermetallic compound by a step comprising melting a material comprising Mn, Bi and Sb; preparing a Mn-Bi-Sb based mixed molten solution by a step including melting an intermetallic compound; forming a Mn-Bi-Sb-based thin strip by a step including cooling a Mn-Bi-Sb-based mixed molten solution; and The Mn-Bi-Sb based thin ribbon is transformed into a magnetic Mn-Bi-Sb based thin ribbon by heat treatment.

4. The method for producing a Mn-Bi-Sb based magnetic material according to claim 3, in, The preparation of the intermetallic compound includes: mixing Mn, Bi and Sb to meet the Mn 54 Bi 46-y Sb y wherein y is 0.5 to 3.0, followed by cooling, thereby preparing a Mn—Bi—Sb based ingot as an intermetallic compound.

5. The method for producing a Mn-Bi-Sb based magnetic material according to claim 3, in, The method for forming the Mn-Bi-Sb-based thin strip includes: cooling the Mn-Bi-Sb-based mixed molten solution by a rapid solidification process to form a Mn-Bi-Sb rapid quenching thin strip.

6. The method for producing a Mn-Bi-Sb based magnetic material according to claim 5, in, The conversion into a magnetic Mn-Bi-Sb based ribbon comprises heat treating the Mn-Bi-Sb quenched ribbon at a temperature in the range of 270 to 330°C.

7. The method for producing a Mn-Bi-Sb based magnetic material according to claim 6, in, The conversion into a magnetic Mn-Bi-Sb based ribbon comprises heat treating the Mn-Bi-Sb quenched ribbon in an inert gas atmosphere for 12 to 48 hours.

Citation Information

Patent Citations

  • MNBI-based magnetic substance, preparation method thereof, mnbi-based sintered magnet and preparation method thereof