Atomic layer wet etching using self-limiting and solubility-limited reactions

Through wet atomic layer etching technology, self-limiting reactions are used to form and dissolve thin layers on the surface of polycrystalline materials, which solves the problems of surface roughening and uneven rate during the etching process, achieving uniform etching and surface smoothness of the material, and is suitable for Etching of polycrystalline metals.

CN113016056BActive Publication Date: 2024-10-18TOKYO ELECTRON LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN201980074921.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-11-15
Publication Date
2024-10-18
Estimated Expiration
2039-11-15

Smart Images

  • Figure CN113016056B_ABST
    Figure CN113016056B_ABST
Patent Text Reader

Abstract

A processing system and platform for improving both microscopic and macroscopic uniformity of materials during etching is disclosed herein. These improvements can be accomplished by forming and dissolving a thin self-limiting layer on the surface of the material using atomic layer wet etching (ALE) techniques. For etching of polycrystalline materials, these self-limiting reactions can be used to prevent such roughening of the surface during etching. Thus, as disclosed herein, a wet ALE process uses sequential self-limiting reactions to first modify the surface layer of the material and then selectively remove the modified layer.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to U.S. Provisional Patent Application No. 62 / 767,808, filed on November 15, 2018, entitled “Wet Atomic Layer Etching Using Self-Limiting and Solubility-Limited Reactions,” and U.S. Patent Application No. 16 / 287,658, filed on February 27, 2019, entitled “Wet Atomic Layer Etching Using Self-Limiting and Solubility-Limited Reactions,” the disclosures of which are expressly incorporated herein by reference in their entirety. Background Art

[0003] The present disclosure relates to substrate processing. In particular, the present disclosure provides a method of etching a layer on a substrate.

[0004] During substrate processing, a variety of techniques are known for etching various layers on a substrate. Plasma etching and wet etching are two well-known techniques. Wet etching involves dispensing a chemical solution on the surface of the substrate or immersing the substrate in a chemical solution. The chemical solution typically contains a solvent, a chemical designed to react with the material on the substrate surface, and a chemical that promotes the dissolution of the reaction products. The result of exposing the substrate surface to the etchant is the removal of material from the substrate. The etchant composition and temperature can control the etching rate, specificity, and residual material on the substrate surface after etching.

[0005] Both thermodynamics and kinetics play a role in etchant formulation. For etching to be successful, the desired reaction needs to be both thermodynamically and kinetically favorable. For etching polycrystalline materials, the requirements for success become even more stringent. For these materials, it is desirable that the removal rates are substantially similar for each individual crystallite facet and grain boundary geometry, regardless of the crystallite morphology or environment. Surface roughness plays an important role in the interface quality and electrical properties of nanoscale features. When etching nanoscale polycrystalline materials, the different etching rates at the grain boundaries compared to different crystal facets produce roughening of the surface during etching. Further, it is desirable that the material removal rate should be uniform at both the macro and micro levels and occur at a rate compatible with high-volume manufacturing. Macroscopic uniformity can be addressed by careful engineering, but microscopic uniformity depends on the chemistry of the etching itself.

[0006] As the geometry of substrate structures continues to shrink and the types of structures evolve, the challenges of etching substrates increase. One technology used to address these challenges is atomic layer etching (ALE). It is generally known that the ALE process includes a process for sequentially removing thin layers through one or more self-limiting reactions. For example, ALE generally refers to a technology that can etch with atomic precision-removing one or several monolayers of material at a time. Typically, the ALE scheme relies on chemical modification of the surface to be etched and then selectively removing the modified layer. Therefore, the ALE process provides improved performance by separating the etching process into sequential steps of surface modification and modified surface removal. This process typically includes multiple cyclic series of layer modification and etching steps. The modification step can modify the exposed surface, and the etching step can selectively remove the modified layer. Therefore, in one embodiment, a series of self-limiting reactions may occur, and the cycle can be repeated. In other embodiments, the process may use only one cycle. As used herein, the ALE process may also include a quasi-ALE process. In this process, a series of modification and etching step cycles can still be used. However, the removal step may not be purely self-limiting because after removing the modified layer, the etching slows down significantly, but it may not stop completely. So far, known ALE techniques have been performed in vacuum or gas phase. This technique uses plasma or high temperature thermochemical reactions to modify the surface of the material, followed by chemical or ligand exchange reactions to volatilize the modified layer. The nature of ALE makes the surface smooth as it is etched.

[0007] Other known sequential etching techniques include using oxygen plasma, ozone or hydrogen peroxide as a self-limiting oxidation step to etch III-V semiconductors and acid wet etching to selectively remove oxides. However, although the prior art provides a sequential etching process, it lacks atomic layer control due to the need for aggressive oxidants.

[0008] As the size of features being etched continues to decrease, it becomes increasingly difficult to meet micro- and macro-etch uniformity requirements to an acceptable degree using known etching techniques. It would therefore be desirable to provide an improved etching process. Summary of the invention

[0009] A processing system and platform for improving both microscopic and macroscopic uniformity of materials during etching is disclosed herein. These improvements can be accomplished by forming and dissolving a thin self-limiting layer on the surface of the material using wet ALE techniques. For etching of polycrystalline materials, these self-limiting reactions can be used to prevent such roughening of the surface during etching. Thus, as disclosed herein, the wet ALE process uses sequential self-limiting reactions to first modify the surface layer of the material and then selectively remove the modified layer.

[0010] In one embodiment, a method of etching a substrate is provided. The method may include receiving a substrate having an exposed first material, the first material including a polycrystalline material. The method further includes selectively etching the polycrystalline material, the selective etching including chemically modifying a surface of the polycrystalline material by exposing the surface to a chemical solution to provide a modified surface layer, and selectively removing the modified surface layer by exposing the modified surface layer of the polycrystalline material to a liquid chemical solution.

[0011] In one embodiment, chemical modification of the surface of the polycrystalline material comprises oxidizing the polycrystalline material using an oxidant. In one embodiment, the oxidant comprises a gaseous environment containing oxygen, a chemical solution containing dissolved oxygen or other oxidants, or a solvent (such as water) that directly participates in the surface oxidation. In another embodiment, the oxidant is an oxygen-saturated chemical solution comprising oxygen dissolved in water, ethanol, or acetone.

[0012] In another embodiment, the chemical modification further comprises passivating the modified layer of polycrystalline material using a complexing agent. In one embodiment, the complexing agent comprises citrate.

[0013] In another embodiment, the chemical modification further comprises passivating the modified layer in the polycrystalline material by exposing the substrate to citric acid. In another embodiment, the chemical modification comprises exposing the substrate to molecular oxygen and citrate.

[0014] In another embodiment, the method of etching a substrate further comprises rinsing the substrate with a solvent after the chemical modification and before the selective removal.

[0015] In another embodiment of the above method of etching a substrate, the selectively removing includes exposing the modified layer of polycrystalline material to an aqueous solution to dissolve the modified layer.

[0016] In other embodiments, the method of etching a substrate is utilized, wherein chemical modification and selective removal are performed sequentially and alternately. In some embodiments, the sequential steps of chemical modification and selective removal are (1) partially overlapped in time or (2) performed continuously. In some embodiments, the sequential steps of chemical modification and selective removal do not overlap in time.

[0017] In yet another embodiment, before performing the above-mentioned selective etching, selective dry etching of the polycrystalline material may be performed by exposing the polycrystalline material to a gas phase environment.

[0018] In one embodiment, the polycrystalline material may be a transition metal or may be a noble metal. In a preferred embodiment, the polycrystalline material is ruthenium or cobalt.

[0019] In another embodiment, a method of etching a substrate is described. The method may include receiving a substrate having a first material consisting of a polycrystalline material and a second material consisting of a different material, wherein an exposed surface of the polycrystalline material has a surface roughness characterized by a first surface roughness value. The method further includes chemically modifying the polycrystalline material by exposing the substrate to a first wet chemical solution to produce a chemically modified layer, and then exposing the substrate to a second wet chemical solution to dissolve the chemically modified layer and reduce the surface roughness to a second surface roughness value. In one embodiment, the polycrystalline material is a transition metal. In another embodiment, the chemical modification of the polycrystalline material includes oxidizing the polycrystalline material using an oxidant. In yet another embodiment, the method further includes etching the polycrystalline material on the substrate using a dry etching process, wherein the first surface roughness value is a result of the dry etching process. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] A more thorough understanding of the present invention and its advantages may be obtained by referring to the following description in conjunction with the accompanying drawings, wherein like reference numerals indicate like features. It should be noted, however, that these drawings only illustrate exemplary embodiments of the disclosed concept and are therefore not to be considered limiting of the scope, as the disclosed concept may admit to other equally effective embodiments.

[0021] Figures 1A to 1C Kinetic analysis of polycrystalline metal etching is presented.

[0022] FIG. 2A to FIG. 2D An exemplary etch cycle for an exemplary ALE metal wet etch is shown.

[0023] Figure 3 Shown in FIG. 2A to FIG. 2D The effect of solvent rinsing during the etching cycle is shown.

[0024] Figure 4 Demonstrated peak-to-peak roughness reduction that can occur in an ALE metal wet etch process.

[0025] Figure 5 and Figure 6 Exemplary methods for processing substrates according to the techniques described herein are demonstrated. DETAILED DESCRIPTION

[0026] A processing system and platform for improving both microscopic and macroscopic uniformity of materials during etching is disclosed herein. These improvements can be accomplished by forming and dissolving a thin self-limiting layer on the surface of the material using wet ALE techniques. For etching of polycrystalline materials, these self-limiting reactions can be used to prevent roughening of the surface during etching. Thus, as disclosed herein, the wet ALE process uses sequential self-limiting reactions to first modify the surface layer of the material and then selectively remove the modified layer.

[0027] As described herein, methods for implementing sequential self-limiting reactions using wet chemical methods are provided. Using the wet ALE process of these methods, the surface reaction in the etching solution is self-limiting, so the total etching amount can be an integer multiple of the etching amount of each cycle. Therefore, the method can also be referred to as "digital etching". The technology described herein can be used for a variety of materials known in the field of substrate processing. Such materials may include polycrystalline materials. In one embodiment, the polycrystalline material may be a metal. In some embodiments, the metal may be a transition metal. In other embodiments, the metal is a noble metal. In some specific embodiments, the metal may be composed of ruthenium (Ru) or cobalt (Co).

[0028] In one embodiment, the wet etching technique described consists of sequentially exposing the substrate surface to two or more etchant solutions. The first etchant reacts with the surface of the substrate in a self-limiting manner. The second etchant dissolves the reaction products and exposes a fresh surface that is free to react with the first etchant in subsequent cycles. Compared to dry ALE, which is a dry process that relies on the volatility of the reaction products, this wet etching ALE relies on the solubility of the reaction products to remove them. For self-limitation, it is desirable that the surface reaction products are generally insoluble in the first etchant. However, the reaction products are easily soluble in the second etchant to remove material in digital etching.

[0029] Additionally, the substrate surface to be removed readily reacts with components of the first etchant in a self-limiting manner, but not with the second etchant. The difference in substrate reactivity and product solubility can be accomplished by different chemical additives in a common solvent or by using different solvents for each of the two etchants.

[0030] The described method provides atomic layer control. The method can be general to any type of material etched using wet chemistry. The method can expand the role of solvent selection in the solubility of the passivation layer. Further, complexing agents can be used as a method to control the solubility of the reaction products.

[0031] The techniques described herein provide the opportunity for multiple advantages over other etching methods. These techniques provide the benefits of ALE, such as precise control of the total etch volume, control of surface roughness, and improved wafer-level uniformity. These techniques also provide several benefits of wet etching, such as simplicity of the etching chamber, atmospheric etching conditions, and the speed at which etching can be completed.

[0032] Wet ALE is accomplished by exposing the substrate surface to multiple etchants in sequence. Each etchant typically includes a solvent that may contain one or more of the following: a chemical that reacts with the substrate surface, a chemical that reacts with a product formed on the substrate surface, a chemical that promotes dissolution of a product formed on the substrate surface, or a chemical that promotes cleaning of the substrate surface. The substrate may be rinsed with an inert solution between exposures to sequential etchants to prevent cross contamination of the etchants. The substrate may also be exposed to a gas phase reactant between etchant exposures to drive additional chemistry.

[0033] The etchant in a wet ALE process will typically react with the substrate surface in a self-limiting manner. The etchant may react with the substrate surface to form a chemically modified layer on the substrate surface, the etchant may react with the modified layer, may dissolve the modified layer, or may perform some combination of these processes. Generally, it is desirable that the etchant is selective and self-limiting. It is also desirable that the substrate surface can be affected by the etchant while the underlying layers remain unchanged. The thickness of the self-limiting reaction is typically on the atomic scale. A monolayer is ideal, but not required.

[0034] Exposure to a single etchant can be accomplished by a variety of techniques, including by immersing the substrate in a bath, exposing the substrate to an aerosol spray, or dispensing the etchant onto the substrate in a spin chamber. In each case, it is preferred that the dose of etchant is sufficient to drive the reaction to its self-limiting value over the entire substrate surface.

[0035] The substrate used with the techniques disclosed herein can be any substrate on which it is desired to etch the material. For example, in one embodiment, the substrate can be a semiconductor substrate having one or more semiconductor processing layers formed thereon (all processing layers together can include the substrate). In one embodiment, the substrate can be a substrate that has been subjected to multiple semiconductor processing steps that have produced a variety of structures and layers, all of which are known in the art of substrate processing. In one embodiment, the substrate can be a semiconductor wafer including the various structures and layers formed.

[0036] As described above, the techniques described herein can be used to etch a variety of materials. Such materials can include polycrystalline materials. Such materials can include metals, including but not limited to transition metals and noble metals. In an exemplary embodiment, the material to be etched can be a polycrystalline cobalt material. As provided below, the techniques described herein are described in conjunction with the etching of polycrystalline cobalt materials. However, those skilled in the art will recognize that such examples are merely exemplary and that other materials can be used.

[0037] Many chemistries can etch polycrystalline cobalt, but controlling surface roughness during etching is difficult. It is difficult to prevent pitting and preferential etching at grain boundaries. Since zero-valent cobalt is generally insoluble, it must first be oxidized. As used herein, oxidation of cobalt refers to increasing the formal charge of cobalt. The oxidized species can then dissolve into solution. Kinetic analysis of a general two-step etching process (oxidation followed by dissolution) shows three related reaction rates: K ox,b , the oxidation rate at the grain boundary, K ox,g , the oxidation rate at the grain surface, K d , oxide dissolution rate. The relative rates of these reactions determine the roughness after etching. These reactions are present in Figures 1A to 1C , these figures show the kinetics of polycrystalline metal etching. Figures 1A to 1C As shown, a polycrystalline metal (to be etched), such as cobalt 105, is surrounded by a dielectric 110, and oxidized metal regions 115A, 115B, and 120 are formed on top of the cobalt 105. Figure 1A As shown, an oxidized metal region 115A is formed at the grain boundary 125 of the cobalt 105. An oxidized metal region 115B is formed on the surface of the grain. Equations 1 and 2 show oxidation equations for oxidation at the grain surface and at the grain boundary, respectively.

[0038] Equation 1

[0039] Equation 2

[0040] Equation 3 shows an exemplary dissolution reaction of cobalt oxide when citric acid is utilized in the reaction.

[0041] Equation 3

[0042] If K ox,b (Oxidation rate at grain boundaries) is greater than K ox,g (the oxidation rate at the grain surface), preferential oxidation may occur at the grain boundary. ox ) is much larger than the dissolution reaction rate (K d ), then the surface roughness increase may not occur, for example Figure 1B As shown ( Figure 1BThe oxidized metal region 120 is a structure of cobalt oxide on the surface of the structure. If the oxidation reaction rate (K ox ) is less than or equal to the dissolution reaction rate (K d ), the surface roughness may increase, for example Figure 1C In the above equation, the oxidized cobalt is presented as cobalt oxide. However, the oxidized cobalt formed may consist of cobalt oxide, cobalt hydroxide, cobalt oxyhydroxide, or some combination of these species.

[0043] Specifically, if oxidation is faster than dissolution, the surface presented to the etching solution will be oxidized metal. Unless self-limited, the thickness of the oxide layer will continue to grow. If self-limited, the oxide layer of finite thickness will propagate downward through the cobalt as the metal is etched. In this case, since the oxidation rate at the grain boundaries and grain surfaces is not important, a smooth etching will be produced-dissolution is the rate determining step. However, if dissolution is faster than oxidation, the metal surface will come into contact with the etching solution because the oxidized cobalt dissolves into the solution as fast as it forms. In this case, the etching rate is controlled by the oxidation kinetics, so the faster oxidation rate at the grain boundaries produces faster etching, pitting, and increased surface roughness at the grain boundaries.

[0044] As described below, the following is a method to temporarily separate the oxidation and dissolution steps of the etching process. Each reaction is performed in its own etching solution. The oxidation step is self-limiting, and the dissolution step is selective to remove only the oxidized metal. If these conditions are generally met, the total etch amount will be an integer multiple of the self-limiting oxide thickness. This process will provide a wet ALE process that will cause the surface roughness to decrease as the etching progresses.

[0045] In order to provide an oxidation rate much faster than the dissolution rate, the oxidation step can be performed with a solvent in which the oxidation product is insoluble. This allows a self-limiting oxide layer to form without losing any material to dissolution. The oxidized surface can then be exposed to an etchant that will dissolve the oxide layer without further oxidizing the surface. Complexing agents can be used to promote the solubility of the oxidized metal species. If these complexing agents are present in the oxidizing etchant, self-limiting metal complexes are formed. If the etchant used for dissolution can dissolve the complex without dissolving the oxidized metal, then the etchant can also oxidize because the dissolution is still self-limiting. It is also possible to complex and dissolve by multiple etchants. For example, etchant 1 forms complex 1 on the surface. Etchant 2 dissolves complex 1 and forms complex 2 on the surface. Etchant 1 then dissolves complex 2 and continues the cycle by forming complex 1 again. This technique can advantageously increase the etching rate per cycle.

[0046] To etch cobalt, in one embodiment, oxygen is used as an oxidant and the complexing agent includes a citrate. In one embodiment, the oxidant includes an oxygen-containing gaseous environment or an oxygen-saturated chemical solution. Exemplary oxygen-saturated chemical solutions include, but are not limited to, oxygen dissolved in water, ethanol, or acetone. In one embodiment, citric acid is used as a complexing agent. Citric acid reacts with cobalt oxide to form a substance soluble in an aqueous solution. The reaction between citric acid and cobalt oxide is also self-limiting. When the cobalt oxide surface is exposed to citric acid, a single monolayer product is formed. Citric acid does not react with metallic cobalt. Contact with air or dissolved oxygen in the solution forms a self-limiting natural oxide layer on cobalt. The natural oxide layer can be composed of cobalt oxide, cobalt hydroxide, cobalt oxyhydroxide, or some combination of these species. This completes the oxidation portion of wet ALE. Non-aqueous solvents (such as acetone or isopropanol) can be used for the complexing step. Cobalt citrate is insoluble in these solvents, so a monolayer of cobalt citrate is formed as a self-limiting passivation layer. The non-aqueous solution of citric acid can be used as an etching bath or dispensed on the substrate surface in a spin chamber. During this step, a self-limiting cobalt citrate layer is formed. This reaction is fast and self-limiting. If both dissolved oxygen and citric acid are contained in the solution, the oxidation and complexation steps can be completed in the same solution. The etchant can contain both components because both reactions are self-limiting and there is no reaction between molecular oxygen in solution and citric acid.

[0047] After the complexing step, a solvent rinse can be performed to remove excess citric acid solution without disturbing the self-limiting cobalt complex. The rinse can be done in a solvent bath or by dispensing the solvent onto the substrate in a spin chamber. The solvent used for the complexing step can be used for the rinse step, but any solvent in which the complexing agent is soluble but the metal complex is not soluble can be used. This rinse step prevents mixing of the oxidizing / complexing solution and the dissolving solution. A mixture of these solutions can spontaneously etch the cobalt. Forgoing the rinse step can allow spontaneous etching of the cobalt and prevent many of the benefits of digital etching.

[0048] After complexation and solvent rinsing, the cobalt citrate layer is removed using an aqueous solution. The substrate can be immersed in a water bath, or water can be dispensed onto the substrate surface in a spin chamber. Cobalt citrate is readily soluble in aqueous solutions; however, cobalt oxide and metallic cobalt are not. This process is performed in FIG. 2A to FIG. 2D Four steps are shown, which illustrate one etching cycle.

[0049] like Figure 2A As shown, the first step of the etching cycle includes oxidizing the surface of cobalt 215. Figure 2A As shown, cobalt 215 is embedded in dielectric 220. The oxidation of the surface of cobalt 215 can be accomplished by exposing the surface of cobalt 215 to the atmosphere, an oxygen environment, or an oxygen-saturated solution of water, ethanol, acetone, or other solutions. Figure 2AAs shown, cobalt 215 is exposed to oxygen 205 in acetone / isopropanol 225. As a result, Figure 2B As shown, a self-limiting cobalt oxide layer 235 is formed on the cobalt 215. Then, by dissolving citric acid in acetone or isopropanol and then exposing the surface to a non-citric acid aqueous solution, such as Figure 2B The self-limiting layer of cobalt citrate complex 245 is formed when exposed to cobalt oxide layer 235, as indicated by citrate 210. Figure 2C As shown, a portion of the cobalt oxide layer 235 has been consumed. Eventually, one or more complexation cycles will consume the cobalt oxide layer 235. Then Figure 2D As shown in , the self-limiting layer of cobalt citrate complex 245 is removed by water 230 of the water rinse as indicated by the removal of cobalt citrate complex 245 into solution. It should be noted that the self-limiting rates of oxide consumption / cobalt citrate complex formation and removal of cobalt citrate complex need not be the same. If two etching solutions are mixed, it may be necessary to Figure 2C and Figure 2D Solvent rinses are performed between the steps to prevent spontaneous etching. Further, the individual steps can be combined by oxygenating the solutions used in those steps, however the surface usually has to be Figure 2D and Figure 2B is rinsed between steps to prevent spontaneous etching when those solutions mix.

[0050] It will be appreciated that the specific oxidizing, complexing, and dissolving solutions described above are exemplary only. Thus, a wide range of solutions may be used, such as those that may be appropriate for the particular material being etched, and the concepts described herein are not limited to the specific oxidizing, complexing, and dissolving solutions described. For example, an oxidizing agent (such as oxygen, ozone, water, nitrous oxide, or hydrogen peroxide), a complexing agent (such as a citrate, acetate, a carboxylate-containing species, or an amine-containing species), and a dissolving solution (such as acetonitrile) may be used.

[0051] Figure 3 The etching behavior of cobalt with and without solvent flushing is shown, plotting thickness versus number of etching cycles. Specifically, Figure 3 The amount of etching per cycle is shown for multiple cycles of the process. With solvent flushing, as shown by curve 310, each etching cycle removes approximately 0.28 nm of cobalt. This etching amount is close to a single monolayer of cobalt. Without the etching step, as shown by curve 305, each etching cycle removes more than twice the material (0.6 nm of cobalt), indicating that spontaneous etching occurs due to mixing of the etching solutions.

[0052] The self-limiting oxide thickness can be changed based on the solvent and oxidant used. The self-limiting thickness of the metal complex layer can be changed by using different complexing agents. For molecular oxygen and citric acid, about 0.28nm of cobalt is removed per etch cycle. Stronger oxidants do not increase the amount of cobalt removed per etch cycle, indicating that the thickness of the cobalt citrate layer determines the etch rate per cycle.

[0053] There are a number of ways to structure the sequential etchant exposures to accomplish the same etching chemistry. An etchant containing dissolved oxygen or some other oxidant and citric acid can be used to form a self-limiting cobalt citrate layer. A sequential exposure to an oxidizing etchant in solution or in the vapor phase followed by exposure to citric acid containing etchant can be used instead. In both cases, the cobalt citrate layer is removed by a subsequent water rinse. A third technique is to include an oxidant in the water rinse. The rinse removes the self-limiting cobalt citrate layer and forms a self-limiting cobalt oxide layer. A subsequent exposure to a non-aqueous citric acid solution reforms the self-limiting cobalt citrate layer for the next etching cycle.

[0054] The use of the disclosed etching chemistry reduces the surface roughness of the cobalt film during etching. In one embodiment, the root mean square (RMS) roughness of the cobalt film as received is ~1.5 nm RMS roughness. After etching 10 nm of cobalt, the roughness is reduced to ~0.6 nm. This roughness level is maintained for additional etching. After removing 30 nm of cobalt, the RMS roughness remains at ~0.6 nm. Figure 4 The peak-to-peak roughness is also reduced as shown in FIG, which plots curve height versus substrate position. More specifically, Figure 4 Peak-to-peak roughness of cobalt films after varying amounts of wet ALE is shown. The initial roughness of the unetched reference is shown as curve 405. This initial roughness of >5 nm is reduced to ~1.5 nm after only 10 nm of cobalt is removed, as shown by curve 415. This improvement is maintained for additional etching, as shown by curve 410, which shows 30 nm of cobalt etching.

[0055] Cobalt wet ALE can be performed in a spin chamber where the substrate is rotated while the etching solution is dispensed onto the substrate surface. The motion of the substrate distributes the etchant evenly over the substrate surface. The dispensing time for each etchant must be long enough so that a self-limiting reaction thickness is achieved across the substrate surface. The chemistry being dispensed can be switched between etching components to accomplish digital etching. The rinse solution can be dispensed between the complexing solution and the dissolving solution to prevent spontaneous etching of cobalt during transient mixing of the solutions when transitioning between solutions. A single etching cycle defined by oxidation / complexation followed by dissolution of the complex can be repeated until the appropriate amount of material is removed.

[0056] It will be appreciated that the use of a spin chamber is only one embodiment, and a variety of different process tools can be used to perform the techniques described herein. As an alternative, for example, the substrate can be immersed in a chemical bath containing an etchant. The substrate can be sequentially immersed in a bath of each etchant to prevent cross contamination of chemicals together with an intermediate rinse bath. This process can be repeated until an appropriate amount of material is removed. In yet another embodiment, the process can be used with an aerosol spray, mist or mist of each reactant. Further, it will be appreciated that even within a cycle of the process, a combination of the various tools described for applying reactants can be used.

[0057] Thus, as described herein, a technique for etching a layer is provided in which a self-limiting process is utilized to provide a smooth layer. One application of this technique may be etching a metal surface to perform a recess etch to obtain a fully self-aligned via. In this application, it is necessary to selectively etch a metal-filled trench in a dielectric material without increasing the surface roughness of the metal. It will be appreciated that this application is exemplary only, and the techniques described herein may be used in many other applications.

[0058] In one embodiment, the wet etching techniques described herein may also be combined with dry etching techniques (such as plasma etching). For example, in one embodiment, before performing the selective wet etching, the selective dry etching of the polycrystalline material may be first performed by exposing the polycrystalline material to a gas phase environment. Then, the wet etching techniques described herein may be performed. In this way, a combination of dry processing and wet processing may be achieved, wherein the wet processing provides the wet ALE benefits described herein. Thus, for example, wet etching may be utilized to reduce the surface roughness present after the dry etching process.

[0059] Figures 5 and 6 Exemplary methods for using the processing techniques described herein are presented. It will be appreciated that Figures 5 and 6 The embodiments are merely exemplary, and other methods may also use the techniques described herein. Further, additional processing steps may be added to Figures 5 and 6 In the method shown, the steps described are not intended to be exclusive. In addition, the order of the steps is not limited to the order shown in the figures, because different orders may occur and / or various steps may be performed in combination or simultaneously.

[0060] Figure 5A method for etching a substrate is presented. The method includes step 505: receiving a substrate having an exposed first material, the first material including a polycrystalline material. Then, the method includes step 510: selectively etching the polycrystalline material, the selective etching including chemically modifying a surface of the polycrystalline material by exposing the surface to a chemical solution to provide a modified surface layer, and selectively removing the modified surface layer by exposing the modified surface layer of the polycrystalline material to a liquid chemical solution.

[0061] Figure 6 A method for etching a substrate is presented. The method includes step 605 of receiving a substrate having a first material consisting of a polycrystalline material and a second material consisting of a different material, wherein an exposed surface of the polycrystalline material has a surface roughness characterized by a first surface roughness value. The method then includes step 610 of chemically modifying the polycrystalline material by exposing the substrate to a first wet chemical solution to produce a chemically modified layer, and then exposing the substrate to a second wet chemical solution to dissolve the chemically modified layer to reduce the surface roughness to a second surface roughness value.

[0062] In view of this description, further modifications and alternative embodiments of the present invention will be apparent to those skilled in the art. Therefore, this description will be construed as being illustrative only and is intended to teach those skilled in the art how to implement the present invention. It should be understood that the forms and methods of the present invention shown and described herein will be considered as currently preferred embodiments. Equivalent technologies may replace the technologies shown and described herein, and certain features of the present invention may be utilized independently of the use of other features, all of which will be apparent to those skilled in the art who benefit from the description of the present invention.

Claims

1. A method for etching a substrate, comprising: receiving the substrate, the substrate having an exposed first material, the first material comprising a polycrystalline material; as well as Selectively etching the polycrystalline material, the selective etching comprising: chemically modifying the surface of the polycrystalline material by exposing the surface to a chemical solution to provide a modified surface layer, and selectively removing the modified surface layer of the polycrystalline material by exposing the modified surface layer to a liquid chemical solution; in: The polycrystalline material has a first portion and a second portion, the first portion of the polycrystalline material corresponds to a top portion of the substrate, The modified surface layer corresponds to the first portion of the polycrystalline material, and The selective removal of the modified surface layer corresponds to removing the top portion of the substrate; and wherein the substrate further comprises a second material composed of a material different from the first material, wherein the polycrystalline material has a surface roughness characterized by a first surface roughness value; and The selective etching includes reducing the surface roughness to a second surface roughness value by exposing the substrate to a chemical solution as a first wet chemical solution that chemically modifies the polycrystalline material to form the modified surface layer, and then exposing the substrate to the liquid chemical solution as a second wet chemical solution to dissolve the modified surface layer.

2. The method of claim 1, wherein: The polycrystalline material is a transition metal.

3. The method of claim 1, wherein: The polycrystalline material includes ruthenium or cobalt.

4. The method of claim 1, wherein: The chemical modification of the surface of the polycrystalline material includes oxidation of the polycrystalline material using an oxidizing agent.

5. The method of claim 4, wherein: The oxidant includes a gaseous environment containing oxygen or a chemical solution saturated with oxygen.

6. The method of claim 4, wherein: The oxidant is an oxygen-saturated chemical solution comprising oxygen dissolved in water, ethanol or acetone.

7. The method of claim 4, wherein: The chemical modification further includes passivation of the modified surface layer in the polycrystalline material by exposing the substrate to citric acid.

8. The method of claim 4, wherein: The chemical modification includes exposing the substrate to molecular oxygen and citrate.

9. The method of claim 4, further comprising rinsing the substrate with a solvent after the chemical modification and before the selective removal.

10. The method of claim 4, wherein: The selectively removing includes exposing the modified surface layer of the polycrystalline material to an aqueous solution to dissolve the modified surface layer.

11. The method of claim 4, wherein: The chemical modification further comprises passivation of the modified surface layer of the polycrystalline material using a complexing agent.

12. The method of claim 11, wherein: The complexing agent includes citrate.

13. The method of claim 1, further comprising selectively dry etching the polycrystalline material by exposing the polycrystalline material to a vapor phase environment before performing the selective etching.

14. The method of claim 1, wherein: The chemical modification and the selective removal are performed sequentially and alternately.

15. The method of claim 14, wherein: The sequential steps of the chemical modification and the selective removal are performed partially overlapping in time or continuously.

16. The method of claim 14, wherein: The sequential steps of the chemical modification and the selective removal do not overlap in time.

17. The method of claim 1, further comprising etching the polycrystalline material on the substrate using a dry etching process, wherein: The first surface roughness value is a result of the dry etching process.

Citation Information

Patent Citations

  • Wet atomic layer etching using self-limiting and solubility-limited reactions

    US10982335B2

  • Fabrication of semiconductor interconnect structure

    US20070105377A1