Lithium ion battery and method for manufacturing the same

By using a three-dimensional network structure of silicon alloy phase and silicate phase in lithium-ion batteries, combined with a specific initial charging method, the problems of short storage characteristics and cycle life of lithium-ion batteries are solved, and higher battery stability is achieved. and capacity maintenance.

CN113036083BActive Publication Date: 2024-10-25TOYOTA JIDOSHA KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202011245335.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-25
Filing Date
2020-11-10
Publication Date
2024-10-25
Estimated Expiration
2040-11-10

AI Technical Summary

Technical Problem

Lithium-ion batteries containing silicon materials have room for improvement in storage characteristics and short cycle life.

Method used

The negative active material contains a silicon alloy phase and a silicate phase. The silicon alloy phase has a three-dimensional network structure. The silicate phase is arranged in the mesh to ease the volume change and hinder the electrolyte decomposition reaction. It forms a moderately dense state through a specific initial charging method. A three-dimensional network structure.

Benefits of technology

The storage characteristics and cycle life of lithium-ion batteries are improved. The three-dimensional network structure confirmed by STEM-EELS ensures the density of the Li transfer path, reduces capacity degradation, and improves battery stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113036083B_ABST
    Figure CN113036083B_ABST
Patent Text Reader

Abstract

A lithium ion battery comprises a positive electrode, a negative electrode and an electrolyte. The negative electrode comprises a negative electrode active material. The negative electrode active material comprises a silicon material. The silicon material comprises a silicon alloy phase and a silicate phase. The silicon alloy phase has a three-dimensional network structure. The silicate phase is arranged in the mesh of the three-dimensional network structure. The average mesh size of the three-dimensional network structure is 2.8nm to 3.5nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to lithium ion batteries and methods of making the same. Background Art

[0002] Japanese Patent Publication No. 2017-147247 discloses charging and discharging a negative electrode structure containing silicon oxide at a current rate of 1.1C to 3.0C. Summary of the invention

[0003] Silicon (Si) materials have been studied as negative electrode active materials for lithium-ion batteries (hereinafter referred to as "batteries"). The advantage of Si materials is that they have a large specific capacitance. The disadvantage of Si materials is that they have a short cycle life.

[0004] In the past, various studies have been conducted to improve the cycle life of Si materials. For example, in Japanese Patent Publication 2017-147247, only the negative electrode containing Si material is charged and discharged at a predetermined current rate before battery assembly. In Japanese Patent Publication 2017-147247, the Si network is developed in a three-dimensional network in the Si material through this charge and discharge. In Japanese Patent Publication 2017-147247, the cycle life is improved by the formation of the Si network. However, there is room for improvement in the storage characteristics of batteries containing Si materials.

[0005] The present disclosure provides a battery having improved storage characteristics among batteries containing Si materials.

[0006] The following is an explanation of the technical solution and effects of the present invention. However, the mechanism of action of the present invention includes presumptions. The accuracy of the mechanism of action does not limit the scope of the patent claim.

[0007] The first embodiment of the lithium ion battery disclosed herein comprises a positive electrode, a negative electrode and an electrolyte. The negative electrode comprises a negative electrode active material. The negative electrode active material comprises a silicon material. The silicon material comprises a silicon alloy phase and a silicate phase. The silicon alloy phase has a three-dimensional network structure. The silicate phase is arranged in the mesh of the three-dimensional network structure. The average mesh size of the three-dimensional network structure is 2.8nm to 3.5nm.

[0008] The Si material in the first embodiment includes a Si alloy phase and a silicate phase. The Si alloy phase contains an alloy of lithium (Li) and Si. The Si alloy phase has a three-dimensional network structure. It is believed that Li is mainly stored in the Si alloy phase. The silicate phase contains Li silicate (lithium silicate). The silicate phase is arranged in the mesh of the three-dimensional network structure. As Li is stored and released, the Si alloy phase expands and contracts. It is believed that the silicate phase can alleviate the volume change of the Si alloy phase. Moreover, it is believed that the silicate phase can hinder the decomposition reaction of the electrolyte.

[0009] The three-dimensional network structure of the Si alloy phase can be confirmed in the Si distribution image by STEM-EELS (Scninig Transmission Electron Microscopy-Electron Energy-Loss Spectroscopy).

[0010] According to the first embodiment, the compactness of the three-dimensional network structure can be changed according to the initial charging conditions of the battery. Since the three-dimensional network structure has a moderate compactness, it has a tendency to improve the storage characteristics. That is, when the average mesh size of the three-dimensional network structure is greater than 2.8nm and less than 3.5nm, there is a tendency to improve the storage characteristics.

[0011] The three-dimensional network structure (Si alloy phase) is also considered to function as a transfer path for Li. It is considered that the transfer path for Li has appropriate density, and capacity degradation is unlikely to occur.

[0012] In the lithium ion battery described in the above first aspect, the negative electrode active material may further include a carbon material.

[0013] The second method of manufacturing a lithium-ion battery disclosed in the present invention includes assembling a lithium-ion battery and performing an initial charge on the lithium-ion battery. The lithium-ion battery includes a positive electrode, a negative electrode, and an electrolyte. The negative electrode includes a negative electrode active material. The negative electrode active material includes a precursor of a silicon material. The composition of the precursor is represented by SiOx. In the formula, the relationship 0<x<2 is satisfied. The initial charge includes a first stage and a second stage. In the first stage, charging is performed at a first current rate until an intermediate voltage. In the second stage, charging is performed from an intermediate voltage to a maximum voltage at a second current rate. The first current rate is lower than 0.5C. The second current rate is higher than the first current rate. The intermediate voltage is above 3.75V.

[0014] In the present disclosure, "C" is used as a unit of current rate. "1C" is defined as a current rate at which the full charge capacity of a battery is charged in 1 hour. For example, 0.5C represents a current rate 0.5 times that of 1C. According to the current rate of 0.5C, the full charge capacity is charged in 2 hours.

[0015] In the present disclosure, the initial charge is divided into two stages. In the first stage, charging is performed at a relatively low current rate until the intermediate voltage. In the second stage, charging is performed from the intermediate voltage to the maximum voltage at a relatively high current rate. Although the mechanism is not clear, under the conditions described in the second mode, there is a tendency to form a three-dimensional network structure with moderate density.

[0016] In the method for producing a lithium ion battery according to the second aspect, the negative electrode active material may further include a carbon material. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Hereinafter, features, advantages, and technical and industrial significance of exemplary embodiments of the present invention will be described with reference to the accompanying drawings, wherein like numerals represent like elements.

[0018] Figure 1 This is a first schematic diagram of the lithium ion battery in this embodiment.

[0019] Figure 2 This is a second schematic diagram of the lithium ion battery in this embodiment.

[0020] Figure 3 It is a schematic cross-sectional view of the electric storage element in this embodiment.

[0021] Figure 4 This is the first example of Si distribution image using STEM-EELS.

[0022] Figure 5 This is the second example of Si distribution image using STEM-EELS.

[0023] Figure 6 This is a schematic flowchart of the method for manufacturing a lithium ion battery in this embodiment. DETAILED DESCRIPTION

[0024] Hereinafter, an embodiment of the present disclosure (hereinafter also referred to as “the present embodiment”) will be described. However, the following description does not limit the scope of the patent claims.

[0025] In the present embodiment, for example, descriptions such as "2.8 nm to 3.5 nm" indicate a range including boundary values ​​unless otherwise specified. That is, for example, "2.8 nm to 3.5 nm" indicates a range of "2.8 nm or more and 3.5 nm or less".

[0026] Lithium-ion battery

[0027] The "lithium-ion battery" in this embodiment refers to a secondary battery that uses lithium (Li) ions as charge carriers (carriers). The battery in this embodiment can have any form. The battery can be, for example, a square battery, a cylindrical battery, or a pouch-type battery. In this embodiment, a pouch-type battery is described as an example. Pouch-type batteries are also called "laminated batteries."

[0028] Figure 1 1 is a schematic diagram of a lithium-ion battery in this embodiment. Battery 100 is a pouch-type battery. Battery 100 includes an outer packaging material 90. Outer packaging material 90 is a bag made of an aluminum laminate film. Outer packaging material 90 is sealed. Outer packaging material 90 can be sealed by heat sealing, for example. Positive terminal 81 and negative terminal 82 are respectively exposed outside outer packaging material 90.

[0029] Figure 2 This is a second schematic diagram of a lithium ion battery in this embodiment. The outer packaging material 90 contains the storage element 50 and the electrolyte (not shown). That is, the battery 100 includes the storage element 50 and the electrolyte. The positive terminal 81 and the negative terminal 82 are connected to the storage element 50, respectively.

[0030] Figure 3 : is a schematic cross-sectional view of the storage element in this embodiment. The storage element 50 is a stacked type. The storage element 50 is formed by stacking three or more sheet electrodes. The storage element may also be a winding type. That is, the storage element may also be formed by winding a strip electrode into a spiral shape.

[0031] The electric storage element 50 includes a positive electrode 10, a negative electrode 20, and a separator 30. That is, the battery 100 includes a positive electrode 10 and a negative electrode 20. The positive electrode 10 and the negative electrode 20 are alternately stacked. The separator 30 is disposed between the positive electrode 10 and the negative electrode 20.

[0032] negative electrode

[0033] The negative electrode 20 is in a sheet shape. The negative electrode 20 may include, for example, a negative electrode current collector 21 and a negative electrode active material layer 22. The negative electrode current collector 21 may have a thickness of, for example, 5 μm to 50 μm. The negative electrode current collector 21 may include, for example, copper (Cu) foil or the like.

[0034] The negative electrode active material layer 22 is formed on the surface of the negative electrode collector 21. The negative electrode active material layer 22 may be formed only on one side of the negative electrode collector 21. The negative electrode active material layer 22 may also be formed on both the front and back sides of the negative electrode collector 21. The negative electrode active material layer 22 may have a thickness of, for example, 10 μm to 200 μm.

[0035] The negative electrode active material layer 22 contains a negative electrode active material. That is, the negative electrode 20 contains a negative electrode active material. The negative electrode active material layer 22 may also be substantially composed of only a negative electrode active material. The negative electrode active material contains a Si material. The negative electrode active material may also be substantially composed of only a Si material.

[0036] Si Materials

[0037] The Si material may be, for example, a particle group (powder). The Si material may have, for example, a median diameter of 0.01 μm to 20 μm. The Si material may have, for example, a median diameter of 0.1 μm to 10 μm. The Si material may have, for example, a median diameter of 0.5 μm to 5 μm. The "median diameter" in this embodiment means the particle diameter at which the cumulative particle volume from the microparticle side becomes 50% of the total particle volume in the volume-based particle size distribution. The median diameter can be measured using a laser diffraction particle size distribution measuring device or the like.

[0038] In the Si material of this embodiment, it is formed by the reaction of a precursor with Li during the first charge. The precursor is an oxide of Si. The composition of the precursor is represented by the following formula (I):

[0039] SiOx (I).

[0040] In the above formula (I), the relationship of "0 < x < 2" is satisfied. For example, the relationship of "0.5 ≤ x ≤ 1.5" can be satisfied. For example, the relationship of "0.8 ≤ x ≤ 1.2" can also be satisfied.

[0041] The Si material contains a Si alloy phase and a silicate phase. The Si alloy phase contains an alloy of Li and Si. The Si alloy phase can be substantially composed only of a LiSi alloy. It is considered that Li is mainly stored in the Si alloy phase. As Li is stored and released, the Si alloy phase expands and contracts.

[0042] The silicate phase contains Li silicate. The silicate phase can be substantially composed only of Li silicate. It is considered that the silicate phase can mitigate the volume change of the Si alloy phase. Moreover, it is considered that the silicate phase can hinder the decomposition reaction of the electrolyte.

[0043] The composition of Li silicate can be represented by the following formula (II) for example:

[0044] Li y SiO z (II).

[0045] In the above formula (II), for example, the relationship of "1 ≤ y ≤ 8, 2.5 ≤ z ≤ 6" can be satisfied. In the above formula (II), for example, the relationships of "y = z = 4", "y = 2, z = 3", "y = 1, z = 2.5", "y = 3, z = 3.5", "y = 2 / 3, z = 7 / 3", "y = 8, z = 6", etc. can also be satisfied.

[0046] Average mesh size

[0047] Figure 4 is the first example of the Si distribution image by STEM-EELS. The Si alloy phase is three-dimensionally continuous. The Si alloy phase forms a network skeleton. That is, the Si alloy phase has a three-dimensional network structure. In the Si alloy phase, metallic Si is distributed at a high concentration. It is considered that the Si distribution image by STEM-EELS represents the structure of the Si alloy phase. In Figure 4 it is considered that the white part (bright part) extending three-dimensionally represents the Si alloy phase. The black part (dark part) forms the mesh of the three-dimensionally networked white part. It is considered that the black part represents the silicate phase. That is, the silicate phase is disposed in the meshes of the three-dimensional network structure.

[0048] In the present embodiment, the average mesh size is 2.8 nm to 3.5 nm. Within this range, improvement in storage characteristics can be expected. If the average mesh size is less than 2.8 nm, the expected storage characteristics may not be achieved. Even if the average mesh size exceeds 3.5 nm, the expected storage characteristics may not be achieved. The average mesh size may be, for example, 3.1 nm or more. For example, the average mesh size may be 3.3 nm or less.

[0049] Method for determination of average mesh size

[0050] The average mesh size in this embodiment is measured by the following procedure. The battery 100 is discharged to 2.5V at a current rate of 0.2C. After discharge, the battery 100 is disassembled to recover the negative electrode 20. The negative electrode 20 is washed with a predetermined organic solvent. After washing, the negative electrode 20 is cut to prepare a cross-sectional sample of the negative electrode active material layer 22. The surface of the cross-sectional sample is smoothed by FIB (Focused Ion Beam).

[0051] The cross-section sample is observed by STEM. The observation magnification is, for example, about 100,000 to 500,000 times. An enlarged image of the Si material is obtained as an ADF-STEM (Annular Dark Field-STEM, ambient dark field scanning transmission electron microscope) image. Furthermore, an EELS spectrum is obtained by an EELS detector.

[0052] The STEM-EELS image is formed by imaging the position where the EELS spectrum of 15 eV to 18 eV is detected. That is, a Si distribution image (e.g. Figure 4 ). In the Si distribution image, the Si alloy phase is displayed as a white portion (bright portion). The silicate phase is displayed as a black portion (dark portion). The orientation diameter of the black portion is measured at 20 locations. In this embodiment, the arithmetic mean of the orientation diameters at 20 locations is regarded as the "average mesh size".

[0053] Carbon Materials

[0054] In addition to Si material, the negative electrode active material may further include carbon material. Si material and carbon material may be composited. By further containing carbon material in the negative electrode active material, it is expected that both large capacity and long cycle life can be taken into account. The carbon material may be, for example, a particle group. The carbon material may have a median diameter of, for example, 1 μm to 20 μm. The carbon material may have a median diameter of, for example, 1 μm to 10 μm.

[0055] The carbon material may contain any optional components as long as it can function as a negative electrode active material. The carbon material may contain, for example, at least one selected from graphite, soft carbon, and hard carbon.

[0056] In the present embodiment, the mixing ratio of Si material and carbon material is arbitrary. For example, the relationship of "Si material / carbon material = 1 / 99" to "Si material / carbon material = 99 / 1" can be satisfied. For example, the relationship of "Si material / carbon material = 1 / 99" to "Si material / carbon material = 30 / 70" can be satisfied. For example, the relationship of "Si material / carbon material = 5 / 95" to "Si material / carbon material = 25 / 75" can be satisfied. For example, the relationship of "Si material / carbon material = 10 / 90" to "Si material / carbon material = 20 / 80" can also be satisfied.

[0057] Other Ingredients

[0058] In addition to the negative electrode active material, the negative electrode active material layer 22 may further include a conductive material. The conductive material has electronic conductivity. The conductive material may include optional components. The conductive material may include, for example, at least one selected from acetylene black (AB), vapor grown carbon fiber (VGCF), carbon nanotube (CNT) and graphene sheet. The amount of the conductive material may be, for example, 0.1 to 20 parts by mass relative to 100 parts by mass of the negative electrode active material.

[0059] In addition to the negative electrode active material, the negative electrode active material layer 22 may further include a binder. The binder binds the solids to each other. The binder may include optional components. The binder may include, for example, at least one selected from carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), polyacrylic acid (PAA), butyl rubber (IIR), polyimide (PI), polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF) and vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP). Relative to 100 parts by mass of the negative electrode active material, the amount of the binder may be, for example, 0.1 parts by mass to 10 parts by mass.

[0060] positive electrode

[0061] The positive electrode 10 is in a sheet shape. The positive electrode 10 may include, for example, a positive electrode current collector 11 and a positive electrode active material layer 12. The positive electrode current collector 11 may have a thickness of, for example, 5 μm to 50 μm. The positive electrode current collector 11 may include, for example, aluminum (Al) foil or the like.

[0062] The positive electrode active material layer 12 is formed on the surface of the positive electrode collector 11. The positive electrode active material layer 12 may be formed only on one side of the positive electrode collector 11. The positive electrode active material layer 12 may also be formed on both the front and back sides of the positive electrode collector 11. The positive electrode active material layer 12 may have a thickness of, for example, 10 μm to 200 μm.

[0063] The positive electrode active material layer 12 contains a positive electrode active material. The positive electrode active material layer 12 may be substantially composed of only the positive electrode active material. The positive electrode active material may be, for example, a particle group. The positive electrode active material may have a median diameter of, for example, 1 μm to 30 μm.

[0064] The positive electrode active material may contain an optional component. For example, the positive electrode active material may contain at least one selected from the group consisting of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and lithium iron phosphate.

[0065] The positive electrode active material layer 12 may further include a conductive material in addition to the positive electrode active material. The conductive material may include an optional component. The conductive material may include, for example, acetylene black, etc. The amount of the conductive material may be, for example, 0.1 to 10 parts by mass relative to 100 parts by mass of the positive electrode active material.

[0066] The positive electrode active material layer 12 may further include a binder in addition to the positive electrode active material. The binder may include an optional component. The binder may contain PVdF, etc. The amount of the binder may be, for example, 0.1 to 10 parts by mass relative to 100 parts by mass of the positive electrode active material.

[0067] Electrolytes

[0068] The electrolyte is a Li ion conductor. The electrolyte may be solid, gel, or liquid. That is, the battery 100 in this embodiment may be a solid-state battery, a polymer battery, or a liquid battery. In this embodiment, a liquid electrolyte is described as an example. The liquid electrolyte may contain, for example, an electrolyte solution, an ionic liquid, or the like.

[0069] The electrolyte comprises a solvent and a supporting electrolyte. The solvent is aprotic. The solvent can dissolve the supporting electrolyte. The solvent can comprise, for example, at least one selected from fluoroethylene carbonate (FEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC) and diethyl carbonate (DEC).

[0070] The supporting electrolyte includes an ionic compound. The supporting electrolyte includes Li. The supporting electrolyte may include at least one selected from LiPF6, LiBF4, and Li(FSO2)2N. For example, the concentration of the supporting electrolyte may be 0.5 mol / L to 2 mol / L.

[0071] In addition to the solvent and the supporting electrolyte, the electrolyte may further include various additives. The additives may include, for example, at least one selected from vinylene carbonate (VC), vinyl ethylene carbonate (VEC), 1,3-propane sultone (PS), cyclohexylbenzene (CHB), tert-amylbenzene (TAB) and lithium bis(oxalatoborate) (LiBOB).

[0072] Diaphragm

[0073] The separator 30 is interposed between the positive electrode 10 and the negative electrode 20. The separator 30 physically separates the positive electrode 10 and the negative electrode 20. For example, in an all-solid battery, the electrolyte may also function as a separator.

[0074] The separator 30 may be in the form of a sheet, for example. The separator 30 may have a thickness of, for example, 5 μm to 30 μm. The separator 30 is porous. A plurality of pores are formed inside the separator 30. The electrolyte can be retained in the pores. The separator 30 may have a porosity of, for example, 30% to 60%. The porosity can be measured by mercury penetration.

[0075] The diaphragm 30 may be made of, for example, polyolefin. The diaphragm 30 may be made of, for example, polyethylene (PE). The diaphragm 30 may be made of, for example, polypropylene (PP). The diaphragm 30 may have, for example, a single-layer structure. The diaphragm 30 may also be substantially composed of only a PE layer. The diaphragm 30 may have, for example, a multi-layer structure. The diaphragm 30 may be formed by sequentially stacking a PP layer, a PE layer, and a PP layer. For example, a ceramic material may be applied to the surface of the diaphragm 30. The ceramic material may impart heat resistance to the surface of the diaphragm 30.

[0076] Method for manufacturing lithium-ion battery

[0077] Figure 6 : is a schematic flow chart of the method for manufacturing a lithium ion battery in this embodiment. The method for manufacturing a lithium ion battery in this embodiment includes "(A) assembly" and "(B) initial charge".

[0078] (A) Assembly

[0079] The manufacturing method of the lithium ion battery in this embodiment includes assembling a battery 100. The battery 100 includes a positive electrode 10, a negative electrode 20 and an electrolyte. The details of the battery 100 are as described above. The battery 100 is assembled by any method. Before the initial charge, the negative electrode active material includes a precursor of a Si material. The composition of the precursor is represented by the above formula (I).

[0080] (B) Initial charging

[0081] The method for manufacturing a lithium-ion battery in this embodiment includes performing an initial charge on the battery 100. During the initial charge, the precursor (SiOx) reacts with Li. As a result, it is believed that the precursor is disproportionated into a Si alloy phase and a silicate phase. Furthermore, it is believed that the Si alloy phase grows in a three-dimensional network to form a three-dimensional network structure. In this embodiment, the initial charge is performed so that the three-dimensional network structure has an average mesh size of 2.8nm to 3.5nm.

[0082] The initial charge is performed by a charging device. The charging device may also be a charging and discharging device. The initial charge may be performed at room temperature. For example, the initial charge may be performed in a thermostatic chamber set at 15°C to 30°C.

[0083] In this embodiment, the initial charge is divided into two stages. That is, the initial charge includes a first stage and a second stage.

[0084] Phase 1

[0085] The first stage is charging from the voltage of the uncharged state to the intermediate voltage. The charging in the first stage may be a constant current (CC) method. In the first stage, charging is performed at a first current rate until the intermediate voltage.

[0086] The intermediate voltage is 3.75 V or higher. If the intermediate voltage is less than 3.75 V, the average mesh size may exceed 3.5 nm. The intermediate voltage may be, for example, 3.75 V to 3.9 V.

[0087] The first current rate is lower than 0.5 C. If the first current rate is higher than 0.5 C, the average mesh size may exceed 3.5 nm. For example, the first current rate may be 0.1 C to 0.3 C.

[0088] Phase 2

[0089] After reaching the intermediate voltage, the initial charging moves from the first stage to the second stage. The second stage is charging from the intermediate voltage to the maximum voltage. The charging in the second stage can be CC mode. In the second stage, charging is performed from the intermediate voltage to the maximum voltage at the second current rate.

[0090] The second current rate is higher than the first current rate. If the second current rate is lower than the first current rate, the average mesh size may be less than 2.8 nm. The second current rate may be, for example, 0.3C to 1C.

[0091] The maximum voltage is a voltage higher than the intermediate voltage. The maximum voltage is the maximum value of the voltage in the initial charge. The maximum voltage in the initial charge may be equal to the maximum voltage in the operating voltage range of the battery 100. The maximum voltage may be, for example, 4.1V to 4.3V. The maximum voltage may be, for example, 4.2V to 4.3V. The initial charge is completed when the voltage of the battery 100 reaches the maximum voltage.

[0092] Other operations

[0093] After the initial charge, for example, the battery 100 may be discharged. After the initial charge, for example, heat aging may be performed on the battery 100. For example, the battery 100 may be left at a temperature of 50° C. to 70° C. for about 24 to 48 hours.

[0094] The lithium ion battery is manufactured by the above-mentioned treatment. In the lithium ion battery (finished product) of this embodiment, the storage characteristics can be expected to be improved. This is considered to be because the three-dimensional network structure of the Si alloy phase has appropriate density.

[0095] Hereinafter, an embodiment of the present disclosure (hereinafter also referred to as "this embodiment") will be described. However, the following description does not limit the scope of protection claimed.

[0096] Lithium-ion battery manufacturing

[0097] Various lithium-ion batteries were manufactured through the following steps.

[0098] Example 1

[0099] (A) Assembly

[0100] 1. Preparation of positive electrode

[0101] The following materials were prepared.

[0102] Positive electrode active material: LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (median diameter 10μm)

[0103] Conductive material: Acetylene black

[0104] Adhesive: PVdF

[0105] Dispersion medium: N-methyl-2-pyrrolidone

[0106] Positive electrode collector: Al foil

[0107] The slurry is prepared by mixing the positive electrode active material, the conductive material, the binder and the dispersion medium. The slurry is applied to the surface (front and back sides) of the positive electrode collector and dried to form a positive electrode active material layer on the surface of the positive electrode collector. The composition of the positive electrode active material layer is "positive electrode active material / conductive material / binder = 87 / 10 / 3 (mass ratio)".

[0108] Through the above process, a positive electrode original plate is manufactured. By cutting the positive electrode original plate, a plurality of positive electrodes are manufactured.

[0109] 2. Preparation of negative electrode

[0110] SiO2 powder (commercially available) and metal Si powder (commercially available) are mixed. A mixed powder is prepared. A reaction container is prepared. The reaction container has a closed structure. The previously prepared mixed powder is filled into the reaction container. In the reaction container, the mixed powder is heated to a temperature of 1300 to 1400°C under an argon (Ar) atmosphere. A sublimation gas is generated. The composition of the sublimation gas is considered to be SiOx (x=1). The sublimation gas is cooled to form SiO powder. The SiO powder is captured. The SiO powder is crushed.

[0111] The following materials were prepared.

[0112] Negative electrode active material: Si material precursor (SiO prepared as described above), carbon material (commercially available artificial graphite)

[0113] Adhesive: "SBR / CMC=1 / 1 (mass ratio)"

[0114] Dispersion medium: water

[0115] Negative electrode collector: Cu foil

[0116] The negative electrode active material was prepared by mixing 76 parts by mass of the carbon material and 20 parts by mass of the precursor (SiO). The slurry was prepared by mixing the negative electrode active material, the binder and the dispersion medium. The negative electrode active material layer was formed on the surface of the negative electrode collector by applying the slurry to the surface (front and back sides) of the negative electrode collector and drying it. The composition of the negative electrode active material layer was "negative electrode active material / binder = 96 / 4 (mass ratio)".

[0117] Through the above process, a negative electrode original plate is manufactured. By cutting the negative electrode original plate, a plurality of negative electrodes are manufactured.

[0118] 3. Formation of storage elements

[0119] A separator is prepared. The separator is sandwiched between the positive electrode and the negative electrode, and the positive electrode and the negative electrode are alternately overlapped. Thus, a stacked storage element is formed. The storage element includes 7 positive electrodes and 8 negative electrodes. The positive terminal and the negative terminal are connected to the storage element.

[0120] 4.Inject liquid

[0121] As the outer packaging material, a bag made of aluminum laminated film is prepared. The storage element is housed in the outer packaging material. The electrolyte is injected into the outer packaging material. The electrolyte contains the following components.

[0122] Solvent: "FEC / EC / DMC / EMC=1 / 2 / 4 / 3 (volume ratio)"

[0123] Supporting electrolyte: LiPF6 (concentration 1.0 mol / L)

[0124] After the electrolyte was injected, the outer packaging material was sealed by heat sealing. Through the above treatment, the test battery was assembled.

[0125] (B) Initial charging

[0126] Two metal plates are prepared. The test battery is sandwiched between the two metal plates. The two metal plates are fixed so that a predetermined pressure is applied to the power storage element.

[0127] Phase 1

[0128] Under a temperature environment of 25° C., charging was performed at a first current rate of 0.1 C to an intermediate voltage of 3.75 V. Charging was performed in a CC manner.

[0129] Phase 2

[0130] Under a temperature environment of 25° C., charging was performed at a second current rate of 1 C to a maximum voltage of 4.3 V. Charging was performed in a CC manner.

[0131] After the initial charge, the test cell was discharged at a current rate of 0.2 C until it reached 2.5 V. The discharge capacity at this time was the initial capacity. Through the above treatment, a test cell was manufactured.

[0132] In this example, two test cells were manufactured for each specification. One test cell was used for the measurement of the average mesh size, and the other test cell was used for the evaluation of the storage characteristics.

[0133] Example 2

[0134] As shown in Table 1 below, a test cell was produced in the same manner as in Example 1 except that the first current rate in the initial charge was changed.

[0135] Example 3

[0136] As shown in Table 1 below, a test cell was produced in the same manner as in Example 1 except that the second current rate in the initial charge was changed.

[0137] Example 4

[0138] As shown in Table 1 below, a test cell was produced in the same manner as in Example 1 except that the intermediate voltage during the initial charge was changed.

[0139] Comparative Example 1

[0140] As shown in Table 1 below, the initial charge was not divided into the first and second stages, but was performed continuously. The current rate was 1 C. A test cell was manufactured in the same manner as in Example 1 except for this.

[0141] Comparative Example 2, Comparative Example 3

[0142] As shown in Table 1 below, a test cell was produced in the same manner as in Example 1 except that the first current rate in the initial charge was changed.

[0143] Comparative Example 4

[0144] As shown in Table 1 below, a test cell was produced in the same manner as in Example 1 except that the second current rate in the initial charge was changed.

[0145] Comparative Example 5

[0146] As shown in Table 1 below, a test cell was produced in the same manner as in Example 2 except that the second current rate in the initial charge was changed.

[0147] Comparative Example 6

[0148] As shown in Table 1 below, a test cell was produced in the same manner as in Example 2 except that the intermediate voltage during the initial charge was changed.

[0149] evaluate

[0150] Average mesh size

[0151] By the above method, the test cells were disassembled in each specification and the average mesh size was measured. In this example, EMC was used as the organic solvent for washing the negative electrode.

[0152] Save Features

[0153] The test battery was charged to 4.2 V at a current rate of 0.2 C. The charged test battery was stored in a thermostatic chamber set at 60° C. for 28 days.

[0154] After 28 days, the test battery was discharged to 2.5V at a current rate of 0.2C at room temperature. Then, the test battery was charged to 4.1V at a current rate of 0.2C. After charging, the test battery was discharged to 2.5V at a current rate of 0.2C. The discharge capacity at this time is the capacity after storage. The capacity retention rate is calculated by dividing the capacity after storage by the initial capacity. The capacity retention rate is shown in Table 1 below. It is believed that the higher the capacity retention rate, the better the storage characteristics.

[0155] Table 1

[0156]

[0157] result

[0158] As shown in Table 1, when the average mesh size is 2.8 nm to 3.5 nm, the storage characteristics tend to be improved.

[0159] Figure 4 This is the first example of Si distribution image using STEM-EELS. Figure 5 This is the second example of Si distribution image using STEM-EELS. Figure 4 The Si distribution image (Si alloy phase) in Comparative Example 1 is shown. Figure 5 The Si distribution image in Example 1 is shown. Figure 4 The observation magnification and Figure 5 The observation magnification is the same. Figure 5 In (Example 1), Figure 4 Compared with (Comparative Example 1), the three-dimensional network structure of the Si alloy phase is dense.

[0160] The present embodiment and the present example are examples in all aspects. The present embodiment and the present example are not restrictive. The technical scope determined by the description of the scope of the patent claim includes all changes in the sense of being equal to the description of the scope of the patent claim. The technical scope determined by the description of the scope of the patent claim includes all changes in the scope of being equal to the description of the scope of the patent claim.

Claims

1. A lithium ion battery, characterized in that: It contains positive electrode, negative electrode and electrolyte. The negative electrode comprises a negative electrode active material, The negative electrode active material comprises silicon material and carbon material, The silicon material comprises a silicon alloy phase and a silicate phase, The silicon alloy phase has a three-dimensional network structure, The silicate phase is arranged in the meshes of the three-dimensional network structure, The average mesh size of the three-dimensional network structure is 2.8nm~3.5nm.

2. A method for manufacturing a lithium ion battery, characterized in that: include: Assembling lithium-ion batteries; as well as performing initial charging on the lithium-ion battery, The lithium-ion battery comprises a positive electrode, a negative electrode and an electrolyte. The negative electrode comprises a negative electrode active material, The negative electrode active material includes a precursor of a silicon material, The composition of the precursor is represented by SiOx and satisfies 0<x<2, The initial charging includes the first stage and the second stage. In the first stage, charging is performed at a first current rate until an intermediate voltage is reached. In the second stage, charging is performed from the intermediate voltage to a maximum voltage at a second current rate, The first current rate is lower than 0.5C, The second current rate is higher than the first current rate, The intermediate voltage is greater than 3.75V.

3. The method for manufacturing a lithium ion battery according to claim 2, characterized in that: The negative electrode active material further includes a carbon material.

Citation Information

Patent Citations

  • Negative electrode for nonaqueous electrolyte secondary batteries, and nonaqueous electrolyte secondary battery using the same

    JP2017147247A

  • Non-aqueous electrolyte secondary battery negative electrode active material and non-aqueous electrolyte secondary battery

    CN104620426A

  • Negative electrode material comprising silicon flakes and method for preparing silicon flakes

    CN109478642A

  • Lithium ion secondary battery and method for manufacturing same

    CN109690859A

  • Negative electrode active material for nonaqueous electrolyte secondary battery, negative electrode for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, and method for manufacturing negative electrode material for nonaqueous electrolyte secondary battery

    JP2016164870A