All-solid-state battery and method for manufacturing the same

By forming gaps around the surface of the Si-based negative active material in an all-solid-state battery, the problem of increased confinement pressure caused by the Si-based active material is solved, achieving the effects of reducing the confinement pressure and improving the thermal stability of the battery.

CN113036084BActive Publication Date: 2024-10-22TOYOTA JIDOSHA KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011499090.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-25
Filing Date
2020-12-17
Publication Date
2024-10-22
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

In all-solid-state batteries, the Si-based active material has a large theoretical capacity, but its volume changes greatly during charge and discharge, resulting in an increase in confinement pressure. It is difficult to effectively reduce the confinement pressure with existing technology.

Method used

A void is formed in a 0.3 μm area around the surface of the Si-based negative electrode active material. The void ratio is 10% or more and 70% or less. A pore-forming material such as polymethyl methacrylate resin (PMMA) is used and the pore-forming material is removed by heat treatment. , forming a negative active material layer and reducing the confinement pressure.

Benefits of technology

Through the formation of voids on the surface of the Si-based negative active material, the confinement pressure of the all-solid-state battery is significantly reduced, the decrease in energy density is suppressed, and the thermal stability of the battery is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113036084B_ABST
    Figure CN113036084B_ABST
Patent Text Reader

Abstract

The present invention relates to an all-solid-state battery and a method for manufacturing an all-solid-state battery. The main purpose is to provide an all-solid-state battery capable of reducing confinement pressure. In the present disclosure, the above-mentioned problems are solved by providing an all-solid-state battery, which is an all-solid-state battery having a positive electrode active material layer, a negative electrode active material layer containing a Si-based negative electrode active material, and a solid electrolyte layer formed between the positive electrode active material layer and the negative electrode active material layer, wherein the negative electrode active material layer has voids in a region (region A) of 0.3 μm around the surface of the Si-based negative electrode active material, and the void ratio in the region A is greater than 10% and less than 70%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an all-solid-state battery and a method for manufacturing the all-solid-state battery. Background Art

[0002] All-solid-state batteries are batteries having a solid electrolyte layer between a positive electrode layer and a negative electrode layer, and have an advantage in that safety devices can be easily simplified compared to liquid-based batteries having an electrolyte solution containing a flammable organic solvent.

[0003] For example, Patent Document 1 discloses a fully solid lithium secondary battery using composite active material particles formed by coating active material particles with a sulfide solid electrolyte, and discloses the use of Si as active material particles. In addition, Patent Document 2 discloses a fully solid lithium ion battery using a porous active material molded body having voids. In addition, although not a fully solid battery, Patent Document 3 discloses a negative electrode active material having a structure having voids around Si or Si alloy.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2016-207418

[0007] Patent Document 2: Japanese Patent Application Publication No. 2014-154236

[0008] Patent Document 3: International Publication No. 2019-131519 Pamphlet Summary of the invention

[0009] Problems to be solved by the invention

[0010] As shown in Patent Document 1, it is known to use Si-based active materials in all-solid batteries. Si-based active materials have a large theoretical capacity and are effective for high energy density of batteries, but their volume changes during charge and discharge are large, and the confinement pressure of all-solid batteries may increase. The present disclosure is made in view of the above actual situation, and its main purpose is to provide an all-solid battery that can reduce the confinement pressure.

[0011] Means for solving problems

[0012] In order to solve the above-mentioned problems, the present disclosure provides an all-solid-state battery, which is an all-solid-state battery having a positive electrode active material layer, a negative electrode active material layer containing a Si-based negative electrode active material, and a solid electrolyte layer formed between the positive electrode active material layer and the negative electrode active material layer, wherein the negative electrode active material layer has voids in a region (region A) of 0.3 μm around the surface of the Si-based negative electrode active material, and the porosity in the region A is greater than 10% and less than 70%.

[0013] According to the present disclosure, voids are formed around the Si-based negative electrode active material, and thus an all-solid-state battery capable of reducing the confinement pressure can be obtained.

[0014] In the above disclosure, the porosity in the region (region B) where the region of the Si-based negative electrode active material and the region A are removed from the entire region of the negative electrode active material layer may be smaller than the porosity in the region A.

[0015] In the above disclosure, the void ratio in the region B may be less than 10%.

[0016] In the above disclosure, the surface of the Si-based negative electrode active material may be covered with a covering portion including the voids and the solid electrolyte.

[0017] In the above disclosure, the above solid electrolyte may be an oxide solid electrolyte.

[0018] In addition, the present disclosure provides a method for manufacturing an all-solid-state battery, which comprises: a preparation step, in which a negative electrode composite is prepared, wherein the negative electrode composite contains a composite negative electrode active material having a pore-forming material-containing layer formed on the surface of a Si-based negative electrode active material; a negative electrode composite layer forming step, in which the negative electrode composite is used to form a negative electrode composite layer; a pressing step, in which the negative electrode composite layer is pressed; and a void forming step, in which the pore-forming material is removed from the pressed negative electrode composite layer to form a void in a region (region A) of 0.3 μm around the surface of the Si-based negative electrode active material.

[0019] According to the present disclosure, since a pore-forming material is used, an all-solid-state battery can be manufactured in which voids are maintained around the surface of a Si-based negative electrode active material.

[0020] In the above disclosure, the void ratio in the above region A may be 10% or more and 70% or less.

[0021] In the above disclosure, the pore-forming material may be polymethyl methacrylate resin (PMMA).

[0022] In the above disclosure, the removal of the pore-forming material can be performed by heat treatment.

[0023] Effects of the Invention

[0024] The all-solid-state battery disclosed herein achieves the effect of being able to reduce the confinement pressure. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic cross-sectional view showing an example of an all-solid-state battery in the present disclosure.

[0026] Figure 2 This is a schematic cross-sectional view showing an example of a negative electrode active material layer in the present disclosure.

[0027] Figure 3 This is a cross-sectional SEM image of the negative electrode active material layer in Example 2.

[0028] Figure 4 These are the results of changes in the restraint pressure in the examples and comparative examples.

[0029] Description of Reference Numerals

[0030] 1…Positive electrode active material layer

[0031] 2…Negative electrode active material layer

[0032] 3…Solid electrolyte layer

[0033] 4…Positive electrode collector

[0034] 5…Negative electrode collector

[0035] 6…Si-based negative electrode active material

[0036] 7…Gap

[0037] 8…covered part

[0038] 10…All-solid-state battery DETAILED DESCRIPTION

[0039] The all-solid-state battery and the method for manufacturing the all-solid-state battery in the present disclosure are described in detail below.

[0040] A. All-solid-state battery

[0041] Figure 1 : is a schematic cross-sectional view showing an example of an all-solid-state battery in the present disclosure. Figure 2 This is a schematic cross-sectional view showing an example of a negative electrode active material layer in the present disclosure. Figure 1 The all-solid battery 10 shown in the figure has: a positive electrode active material layer 1, a negative electrode active material layer 2, and a solid electrolyte layer 3 formed between the positive electrode active material layer 1 and the negative electrode active material layer 2, and also has a positive electrode collector 4 for collecting current from the positive electrode active material layer 1 and a negative electrode collector 5 for collecting current from the negative electrode active material layer 2. These components can be housed in a general outer packaging. In addition, as Figure 2 As shown in (a), the negative electrode active material layer in the present disclosure contains Si-based negative electrode active material 6, and has voids 7 in the range of 0.3 μm around the surface of the Si-based negative electrode active material 6, and the ratio of the voids 7 (porosity) is within a predetermined range. Figure 2As shown in (b), the surface of the Si-based negative electrode active material 6 may be covered with the covering portion 8 .

[0042] According to the present disclosure, voids are formed around the surface of the Si-based negative electrode active material, so that an all-solid-state battery that can reduce the constraint pressure can be made. In addition, since the constraint pressure can be reduced, the reduction in energy density associated with the enlargement of the restraint body that constrains the all-solid-state battery can also be suppressed. In the field of all-solid-state batteries, for example, a composite active material in which active material particles are coated with a sulfide-based solid electrolyte is used as in Patent Document 1, thereby attempting to improve battery performance. On the other hand, when using a high-capacity Si-based negative electrode active material, the expansion and contraction associated with charging and discharging tends to become larger, and there is room for improvement in reducing the constraint pressure of the battery. However, as described above, in the present disclosure, since voids are formed around the Si-based negative electrode active material at a specified ratio, the constraint pressure of the all-solid-state battery can be reduced.

[0043] Among them, Patent Document 2 discloses the use of a porous active material molded body with voids for the negative electrode. However, in Patent Document 2, by making the pores of the active material molded body also contain a solid electrolyte, the contact area between the active material molded body and the solid electrolyte layer is expanded, and the high capacity of the battery is achieved. Therefore, in Patent Document 2, there are no voids in the battery state, and the use of non-expanding negative electrode active materials such as LTO is used as a premise, and the use of Si-based negative electrode active materials is not envisioned. In addition, in Patent Document 3 on liquid batteries, it is recorded that a structure with voids around Si or Si alloys is prepared in advance, and it is used to manufacture negative electrodes and lithium-ion batteries. Usually, in the manufacture of liquid batteries, high pressurization pressure is not applied. Therefore, when the technology described in Patent Document 3 is applied to an all-solid battery manufactured by applying a high pressurization pressure, the voids around Si or Si alloys collapse.

[0044] 1. Negative electrode active material layer

[0045] The negative electrode active material layer is a layer containing a Si-based negative electrode active material.

[0046] As the above-mentioned Si-based negative electrode active material, for example, Si simple substance, Si alloy, and Si oxide can be listed. The Si alloy preferably contains Si element as the main component. The proportion of Si element in the Si alloy can be, for example, 50 mol% or more, 70 mol% or more, or 90 mol% or more. As the Si alloy, for example, Si-Al alloy, Si-Sn alloy, Si-In alloy, Si-Ag alloy, Si-Pb alloy, Si-Sb alloy, Si-Bi alloy, Si-Mg alloy, Si-Ca alloy, Si-Ge alloy, Si-Pb alloy, etc. can be listed. The Si alloy can be a two-component alloy or a multi-component alloy of three or more components.

[0047] The shape of the Si-based negative electrode active material can be, for example, a particle shape, a thin film shape, etc. When the Si-based negative electrode active material is in the form of particles, the average particle size (D 50 ) is, for example, 1 nm or more, 10 nm or more, or 1 μm or more. On the other hand, the average particle size (D 50 ) is, for example, 10 μm or less, 5 μm or less, or 3 μm or less. The average particle size can be determined, for example, based on image analysis using a SEM (scanning electron microscope). The number of samples is preferably large, for example, 100 or more.

[0048] In addition, the negative electrode active material layer in the present disclosure has voids in the region (region A) of 0.3 μm around the surface of the above-mentioned Si-based negative electrode active material. The so-called "region of 0.3 μm around the surface of the Si-based negative electrode active material" refers to the region from the surface of the Si-based negative electrode active material along the normal direction toward the outside of the Si-based negative electrode active material to 0.3 μm in the cross-sectional view of the Si-based negative electrode active material. Region A is generally defined as the region surrounding the entire circumference of the Si-based negative electrode active material. In addition, the "surface of the Si-based negative electrode active material" does not mean the surface of the coating portion described later.

[0049] The negative electrode active material layer in the present disclosure is characterized by the porosity in the "region of 0.3 μm around the surface of the Si-based negative electrode active material". This region A is a region very close to the surface of the Si-based negative electrode active material, and the voids in region A play an important role in suppressing the volume change of the Si-based negative electrode active material. In addition, the voids in region A are formed, for example, by removing the pore-forming material, and the influence of the pore-forming material is significantly manifested in the region close to the surface of the Si-based negative electrode active material coated with the pore-forming material-containing layer described later. From these viewpoints, the negative electrode active material layer in the present disclosure is characterized by the porosity in the "region of 0.3 μm around the surface of the Si-based negative electrode active material".

[0050] The porosity in region A is 10% or more, 20% or more, 30% or more, or 40% or more. On the other hand, the porosity in region A is 70% or less, 60% or less, or 50% or less. If the porosity in region A is too small, the volume change of the Si-based negative electrode active material may not be fully suppressed. If the porosity in region A is too large, the contact area between the Si-based negative electrode active material and the solid electrolyte is reduced, and the resistance may increase.

[0051] The porosity in region A can be determined, for example, by SEM (scanning electron microscope) observation. Specifically, first, a cross-sectional SEM image of the negative electrode active material layer is obtained. From the obtained SEM image, image analysis software is used to identify the voids and determine the area. Then, the porosity (%) is calculated as the area ratio according to the following formula. Preferably, the number of samples is large, for example, more than 20, more than 30, more than 50, or more than 100.

[0052] Void ratio (%) = 100 × (void area in region A) / (area of ​​region A)

[0053] In addition, in the negative electrode active material layer of the present disclosure, it is preferred that the porosity in the region (region B) where the region of the Si-based negative electrode active material and the region A are removed from the entire region of the negative electrode active material layer is smaller than the porosity in region A. Here, the so-called "region where the region of the Si-based negative electrode active material and the region A are removed from the entire region of the cross section of the negative electrode active material layer" refers to the region where the cross section of the Si-based negative electrode active material and the cross section of the region A are removed from the entire region of the cross section of the negative electrode active material layer.

[0054] The porosity in region B is, for example, less than 10%, may be less than 8%, may be less than 5%, may be less than 3%, or may be less than 1%. On the other hand, the porosity in region B may be 0% or greater than 0%. The smaller the porosity in region B, the higher the overall filling rate of the negative electrode active material layer, the higher the energy density, and thus it is preferred. In addition, the difference in porosity between region A and region B (porosity of region A (%) - porosity of region B (%)) is, for example, less than 70%, may be less than 60%, may be less than 50%, or may be less than 40%. On the other hand, the above difference is, for example, more than 1%, may be more than 5%, may be more than 10%, may be more than 20%, or may be more than 30%. The porosity in region B can be obtained by the same method as the porosity in region A.

[0055] The method of adjusting the porosity will be described in "B. Method for producing an all-solid-state battery".

[0056] In addition, the surface of the Si-based negative electrode active material in the present disclosure may be covered with a covering portion including voids and a solid electrolyte. The covering portion includes at least a part of the voids in the region A.

[0057] Examples of the solid electrolyte include sulfide solid electrolytes and oxide solid electrolytes described below, and oxide solid electrolytes are preferred because they can improve the thermal stability of the negative electrode.

[0058] As for the proportion of the solid electrolyte in the covered portion, when the Si-based negative electrode active material is set to 100 weight %, it is, for example, 1 weight % or more, 5 weight % or more, or 10 weight % or more. On the other hand, as for the proportion of the solid electrolyte in the covered portion, when the Si-based negative electrode active material is set to 100 weight %, it is, for example, 60 weight % or less, 40 weight % or less, or 20 weight % or less.

[0059] In addition, the coating portion may contain a conductive material as required. As the conductive material, for example, a carbon material may be cited. As the carbon material, for example, a particulate carbon material such as acetylene black (AB), Ketjen black (KB), a fibrous carbon material such as carbon fiber, carbon nanotube (CNT), carbon nanofiber (CNF), vapor grown carbon fiber (VGCF) may be cited.

[0060] The coverage of the coating portion is, for example, 70% or more, 75% or more, or 80% or more. On the other hand, the coverage of the coating portion may be 100% or less. The coverage of the coating portion can be determined by X-ray photoelectron spectroscopy (XPS).

[0061] The thickness of the coating portion is, for example, 0.05 μm or more, 0.3 μm, or greater than 0.3 μm. On the other hand, the thickness of the coating portion is, for example, 1 μm or less. The thickness of the coating portion can be determined by observation using a transmission electron microscope (TEM) or a scanning electron microscope (SEM). Furthermore, the thickness of the coating portion may be smaller than the thickness corresponding to region A, i.e., 0.3 μm, or may be the same or greater than the thickness.

[0062] The proportion of the negative electrode active material in the negative electrode active material layer is, for example, 20% by weight or more, 30% by weight or more, or 40% by weight or more. On the other hand, the proportion of the negative electrode active material is, for example, 80% by weight or less, 70% by weight or less, or 60% by weight or less.

[0063] The negative electrode active material layer may contain only the above-mentioned Si-based negative electrode active material, or may contain other negative electrode active materials. In the latter case, the proportion of the Si-based negative electrode active material in the total negative electrode active material may be 50% by weight or more, 70% by weight or more, or 90% by weight or more.

[0064] Furthermore, the negative electrode active material layer may contain at least one of a solid electrolyte, a conductive material, and a binder as necessary.

[0065] Examples of the solid electrolyte include the same solid electrolytes as those used for the above-mentioned coating portion.

[0066] Examples of the binder include rubber-based binders such as butene rubber (BR) and styrene butadiene rubber (SBR), and fluoride-based binders such as polyvinylidene fluoride (PVDF).

[0067] The thickness of the negative electrode active material layer is, for example, 0.3 μm or more and 1000 μm or less.

[0068] 2. Positive electrode active material layer

[0069] The positive electrode active material layer contains at least a positive electrode active material, and may contain at least one of a solid electrolyte, a conductive material, and a binder as required. The solid electrolyte, conductive material, and binder are the same as those described in the above "1. Negative electrode active material layer", so the description here is omitted.

[0070] Examples of the positive electrode active material include oxide active materials. Examples of the oxide active material include LiCoO2, LiMnO2, LiNiO2, LiVO2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 and other rock salt layered active materials, LiMn2O4, Li4Ti5O 12 、Li(Ni 0.5 Mn 1.5 )O4 and other spinel active materials, LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4 and other olivine active materials. The surface of the positive electrode active material may be covered with a Li ion conductive oxide. Examples of Li ion conductive oxides include LiNbO3, Li4Ti5O 12 、Li3PO4.

[0071] The ratio of the positive electrode active material in the positive electrode active material layer is, for example, more than 20 wt %, can be more than 30 wt %, and can also be more than 40 wt %. On the other hand, the ratio of the positive electrode active material is, for example, less than 80 wt %, can be less than 70 wt %, and can also be less than 60 wt %.

[0072] The thickness of the positive electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less. The positive electrode active material layer is formed by, for example, applying a composite material containing at least a positive electrode active material and a dispersion medium and drying the composite material.

[0073] 3. Solid electrolyte layer

[0074] The solid electrolyte layer is a layer formed between the positive electrode active material layer and the negative electrode active material layer, and contains at least a solid electrolyte. Examples of the solid electrolyte include inorganic solid electrolytes such as sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and halide solid electrolytes.

[0075] Examples of the sulfide solid electrolyte include solid electrolytes containing Li element, X element (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, In), and S element. In addition, the sulfide solid electrolyte may further contain at least one of O element and halogen element. Examples of the halogen element include F element, Cl element, Br element, and I element.

[0076] The sulfide solid electrolyte preferably includes an ion conductor containing Li element, A element (A is at least one of P, As, Sb, Si, Ge, Al and B), and S element. Furthermore, the ion conductor preferably has a high Li content.

[0077] The sulfide solid electrolyte may contain a lithium halide in addition to the above-mentioned ion conductor. Examples of the lithium halide include LiF, LiCl, LiBr and LiI, among which LiCl, LiBr and LiI are preferred. The proportion of LiX (X = F, I, Cl, Br) in the sulfide solid electrolyte is, for example, 5 mol% or more, and may be 15 mol% or more. On the other hand, the proportion of the above-mentioned LiX is, for example, 30 mol% or less, and may be 25 mol% or less.

[0078] Specific examples of sulfide solid electrolytes include xLi2S·(100-x)P2S5 (70≦x≦80), yLiI·zLiBr·(100-yz)(xLi2S·(1-x)P2S5) (0.7≦x≦0.8, 0≦y≦30, 0≦z≦30).

[0079] Examples of oxide solid electrolytes include Li2O-B2O3-P2O5, Li2O-SiO2, LiLaTaO (e.g., Li5La3Ta2O 12 ), LiLaZrO (e.g. Li7La3Zr2O 12 ), LiBaLaTaO (e.g. Li6BaLa2Ta2O 12 )、Li 1+x Si x P 1- x O4(0≦x<1, such as Li 3.6 Si 0.6 P 0.4 O4)、Li 1+x Al x Ge 2-x (PO4)3(0≦x≦2), Li 1+x Al x Ti 2-x (PO4)3(0≦x≦2), Li3PO (4-3 / 2x) N x (0≦x<1) etc.

[0080] The thickness of the solid electrolyte layer is, for example, 0.1 μm or more and 1000 μm or less. As a method for forming the solid electrolyte layer, for example, there is a method of applying a composite material containing at least a solid electrolyte and a dispersion medium and drying the composite material.

[0081] 4. Other components

[0082] The all-solid-state battery disclosed in the present invention has at least the above-mentioned negative electrode active material layer, positive electrode active material layer and solid electrolyte layer. Furthermore, it usually has a positive electrode collector for collecting the positive electrode active material layer and a negative electrode collector for collecting the negative electrode active material layer. As materials for the positive electrode collector, for example, SUS, aluminum, nickel, iron, titanium and carbon can be listed. On the other hand, as materials for the negative electrode collector, for example, SUS, copper and nickel can be listed. The shape and thickness of the positive electrode collector and the negative electrode collector can be appropriately adjusted according to the purpose of the battery.

[0083] 5. All-solid-state batteries

[0084] The all-solid battery in the present disclosure is preferably an all-solid lithium battery. The all-solid battery can be a primary battery or a secondary battery, and is preferably a secondary battery. This is because it can be repeatedly charged and discharged, for example, it can be used as a vehicle battery. The secondary battery also includes the primary battery use of the secondary battery (use for the purpose of initial charging only).

[0085] In addition, the all-solid battery in the present disclosure may be a single cell or a stacked battery. The stacked battery may be a monopolar stacked battery (a stacked battery of a parallel type) or a bipolar stacked battery (a stacked battery of a series type). As the shape of the all-solid battery, for example, a coin type, a laminate type, a cylindrical type, and a square type may be listed.

[0086] The all-solid-state battery in the present disclosure can be manufactured by “B. Method for manufacturing an all-solid-state battery” described later.

[0087] B. Method for manufacturing all-solid-state batteries

[0088] The manufacturing method of the all-solid-state battery disclosed in the present invention comprises: a preparation step, in which a negative electrode composite material is prepared, wherein the negative electrode composite material comprises a composite negative electrode active material having a pore-forming material-containing layer formed on the surface of a Si-based negative electrode active material; a negative electrode composite layer forming step, in which the negative electrode composite material is used to form a negative electrode composite layer; a pressing step, in which the negative electrode composite layer is pressed; and a void forming step, in which the pore-forming material is removed from the pressed negative electrode composite layer to form a void in a region (region A) of 0.3 μm around the surface of the Si-based negative electrode active material.

[0089] According to the present disclosure, since a pore-forming material is used, a fully solid battery can be manufactured in which a void is maintained around the surface of a Si-based negative electrode active material. In addition, the region B in the negative electrode active material layer can be made dense. It should be noted that in the liquid battery shown in Patent Document 3, it is not necessary to use a pore-forming material to make a void. This is because, in a liquid battery, the porosity can be controlled in the pressing process of electrode manufacturing.

[0090] 1. Preparation process

[0091] The preparation step is a step of preparing a negative electrode composite material, wherein the negative electrode composite material contains a composite negative electrode active material having a pore-forming material-containing layer containing a pore-forming material formed on the surface of a Si-based negative electrode active material. The Si-based negative electrode active material is the same as that described in the above-mentioned "1. Negative electrode active material layer", so the description here is omitted.

[0092] The pore-forming material is a material that forms the voids in the region A described above.

[0093] The pore-forming material is not particularly limited, and conventionally known materials can be used, preferably pore-forming materials that decompose due to heat. The thermal decomposition temperature of the pore-forming material is preferably below the temperature at which the solid electrolyte deteriorates, for example, preferably below 600° C. Examples of the pore-forming material include acrylic resins such as polymethyl methacrylate resin (PMMA), polystyrene, and polysiloxane-based thermosetting resins.

[0094] The average particle size of the pore-forming material is, for example, 0.05 μm or more and 100 μm or less.

[0095] In addition, the pore-forming material-containing layer may contain at least one of a solid electrolyte and a conductive material as required. When the pore-forming material-containing layer contains a solid electrolyte, the pore-forming material-containing layer becomes the above-mentioned coating portion in the all-solid-state battery. The types of solid electrolyte and conductive material are the same as those described in the above-mentioned "1. Negative electrode active material layer", so the description here is omitted.

[0096] In the preparation process of the present disclosure, the composite negative electrode active material can be purchased from others for preparation, or it can be prepared by making it yourself. In the latter case, it is preferred to form a pore-forming material-containing layer on the surface of the Si-based negative electrode active material by compressing and shearing the mixture containing the Si-based negative electrode active material and the pore-forming material. The above-mentioned composite negative electrode active material can be obtained. In addition, the above-mentioned mixture may contain the above-mentioned solid electrolyte and conductive material. The conditions of the compression and shearing treatment can be appropriately set.

[0097] The proportion of the pore-forming material in the mixture is, for example, 5% by weight or more, or 10% by weight or more, when the Si-based negative electrode active material is 100% by weight. On the other hand, the proportion of the pore-forming material is, for example, 40% by weight or less, 30% by weight or less, or 20% by weight or less. By adjusting the proportion of the pore-forming material, the porosity in the region A and the difference in porosity between the region B and the region A can be adjusted.

[0098] The thickness of the pore-forming material-containing layer is equal to the particle size of the pore-forming material when no solid electrolyte is present. The thickness of the pore-forming material layer when a solid electrolyte is present is the same as the thickness of the coating portion described in the above “1. Negative electrode active material layer”.

[0099] The negative electrode composite material contains at least the above-mentioned composite negative electrode active material, and may contain at least one of a solid electrolyte, a conductive material, and a binder as required. The solid electrolyte, conductive material, and binder are the same as those described in the above-mentioned "1. Negative electrode active material layer", so the description here is omitted.

[0100] As a method for preparing the negative electrode composite material, there is exemplified a method of dispersing the above-mentioned materials in a dispersion medium such as heptane.

[0101] 2. Negative electrode composite layer formation process

[0102] The negative electrode mixed material layer forming step is a step of forming a negative electrode mixed material layer using a negative electrode mixed material.

[0103] As a method for forming the negative electrode composite material layer, for example, a method of applying the negative electrode composite material to a substrate and drying it can be cited. As a coating method, for example, screen printing, gravure printing, die coating, doctor blade method, inkjet method, metal mask printing method, electrostatic coating method, dip coating method, spray coating method, roller coating method can be cited. There is no particular limitation on the substrate on which the negative electrode composite material is coated, and for example, a negative electrode collector and a transfer sheet can be cited.

[0104] 3. Pressing process

[0105] The pressing step is a step of pressing the negative electrode mixed material layer.

[0106] The pressing method is not particularly limited as long as it is a method that can apply pressure to the negative electrode mixed material layer, and an example thereof may be roll pressing. The linear pressure applied during pressing is, for example, 15 kN / cm to 50 kN / cm.

[0107] 4. Gap Formation Process

[0108] The void forming step is a step of removing the pore-forming material from the negative electrode composite material layer after the pressing, and forming voids in a region (region A) of 0.3 μm around the surface of the Si-based negative electrode active material. The "region A" is the same as that described in the above "1. Negative electrode active material layer", so the description here is omitted.

[0109] In the void forming step, the pore forming material may be removed so that the void ratio in the region A becomes 10% or more and 70% or less.

[0110] As for the method of removing the pore-forming material, as long as the pore-forming material can be removed from the negative electrode composite layer, there is no particular limitation, and it can be appropriately selected according to the type of the pore-forming material. For example, in the case where the pore-forming material is decomposed by heat, the method of removing the pore-forming material can be heat treatment. Heat treatment can be a treatment in which a temperature above the thermal decomposition temperature of the pore-forming material is applied for a predetermined time.

[0111] In the void forming step, the pore-forming material contained in the negative electrode composite layer may be completely removed or a portion of the pore-forming material may be removed, but the former is preferred because the porosity can be easily adjusted by adjusting the thickness of the pore-forming material-containing layer and the coating portion and the amount of pore-forming material added.

[0112] 5. Other processes

[0113] In the manufacturing method of the all-solid-state battery disclosed in the present invention, the negative electrode can be formed by the above-mentioned process. In addition, generally, the manufacturing method of the all-solid-state battery has: a positive electrode forming process for forming a positive electrode, and a solid electrolyte layer forming process for forming a solid electrolyte layer. Furthermore, there is generally an assembly process for assembling a stacked body, which sequentially has the positive electrode, solid electrolyte layer and negative electrode manufactured as described above. Furthermore, in the manufacturing method of the all-solid-state battery disclosed in the present invention, a negative electrode precursor can be formed by the above-mentioned preparation process, negative electrode composite layer forming process and pressing process, and a stacked body sequentially having a positive electrode, a solid electrolyte layer and a negative electrode precursor is assembled, and then the above-mentioned gap forming process is performed.

[0114] 6. All-solid-state batteries

[0115] The all-solid-state battery manufactured by the above method is the same as that described in the above-mentioned "A. All-solid-state battery", so the description here is omitted.

[0116] The present disclosure is not limited to the above-mentioned embodiments. The above-mentioned embodiments are illustrative, and embodiments having substantially the same configuration and achieving the same effects as the technical concept described in the patent claims of the present disclosure are all included in the technical scope of the present disclosure.

[0117] Example

[0118] [Example 1]

[0119] (Preparation of composite negative electrode active material)

[0120] Si particles (average particle size 5 μm) and PMMA (specific gravity 1.2 g / cm2) as negative electrode active materials were added to a particle composite device (NOB-MINI, manufactured by Hosokawa Micron Co., Ltd.) in the amounts shown in Table 1 below. 3 , average particle size 0.3 μm). The interval between the rotating blade (paddle) of the compression shear rotor and the inner wall of the processing container was set to 1 mm, the paddle circumferential speed was set to 25 m / s, and the processing time was set to 20 minutes, and the compression shearing treatment was performed to obtain a composite negative electrode active material.

[0121] (Production of negative electrode)

[0122] The above-mentioned composite negative electrode active material is added in an amount of 50wt%, the sulfide solid electrolyte (10LiI-15LiBr-75 (0.75Li2S-0.25P2S5)) is added in an amount of 37wt%, the conductive material (VGCF) is added in an amount of 10wt%, and the binder (PVdF) is added in an amount of 3wt% into a dispersion medium (heptane). The dispersion medium is ultrasonically treated for 5 minutes using an ultrasonic homogenizer to obtain a negative electrode composite. The negative electrode composite is applied to a collector foil (SUS, 25μm thick) and dried, and then rolled at a linear pressure of 50kN / cm. The collector foil with the negative electrode composite layer is punched into pieces of φ13.29mm (1.4cm 2 Then, PMMA was removed by heat treatment at 430° C. for 5 minutes, thereby obtaining a negative electrode (current collector foil with a negative electrode active material layer).

[0123] (Production of Evaluation Batteries)

[0124] The positive electrode active material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2) in an amount of 84.7wt%, sulfide solid electrolyte (10LiI-15LiBr-75(0.75Li2S-0.25P2S5)) in an amount of 13.4wt%, conductive material (VGCF) in an amount of 1.3wt%, and binder (PVdF) in an amount of 0.6wt% are put into a dispersion medium (heptane). The dispersion medium is ultrasonically treated for 5 minutes using an ultrasonic homogenizer to obtain a positive electrode composite. The positive electrode composite is applied to a collector foil (Al foil, 20μm thick) and dried, and then rolled at a linear pressure of 50kN / cm. The collector foil with the positive electrode composite layer is punched into pieces of φ11.3mm (1cm 2 ), and the positive electrode was obtained.

[0125] Sulfide solid electrolyte (10LiI-15LiBr-75 (0.75Li2S-0.25P2S5)) was added in an amount of 99.5wt% and binder (PVdF) was added in an amount of 0.5wt% into a dispersion medium (heptane). The dispersion medium was ultrasonically treated for 5 minutes using an ultrasonic homogenizer to obtain a composite material. The obtained composite material was coated on a substrate (Al foil, 20μm thick) to a thickness of 15μm, dried, and then punched into φ13.3mm (1.4cm 2 ), a solid electrolyte layer (separator layer) was obtained.

[0126] The positive electrode, separator layer, and negative electrode were stacked with their centers aligned and pressed at a surface pressure of 5 tons / cm 2Each layer was closely bonded together. Then, the laminate was sealed with an electrode sheet and restrained at 5 MPa to produce an evaluation battery (all-solid lithium battery). The evaluation battery was produced so that the capacity was 2 mAh.

[0127] [Example 2 to Example 4]

[0128] An evaluation battery was prepared in the same manner as in Example 1 except that the amount of PMMA was changed as shown in Table 1 in the preparation of the composite negative electrode active material.

[0129] [Examples 5 and 6]

[0130] A composite negative electrode active material (coated composite negative electrode active material) was prepared in the same manner as in Example 1, except that an oxide solid electrolyte (Li2O-B2O3-P2O5, average particle size 0.1 μm) was used in the preparation of the composite negative electrode active material and the amount of PMMA was changed as shown in Table 1. The coated composite negative electrode active material was added in an amount of 55 wt%, the sulfide solid electrolyte (10LiI-15LiBr-75 (0.75Li2S-0.25P2S5)) was added in an amount of 32 wt%, the conductive material (VGCF) was added in an amount of 10 wt%, and the binder (PVdF) was added in an amount of 3 wt%, and they were added in a dispersion medium (heptane). The dispersion medium was subjected to ultrasonic treatment for 5 minutes using an ultrasonic homogenizer to obtain a negative electrode composite. An evaluation battery was prepared in the same manner as in Example 1, except that the negative electrode was prepared using the negative electrode composite.

[0131] [Comparative Example 1]

[0132] An evaluation battery was prepared in the same manner as in Example 1 except that the amount of PMMA was changed as shown in Table 1 in the preparation of the composite negative electrode active material.

[0133] [Comparative Example 2]

[0134] An evaluation battery was prepared in the same manner as in Example 1 except that Si particles (average particle size: 5 μm) were used instead of the composite negative electrode active material.

[0135] [Comparative Example 3]

[0136] An evaluation cell was prepared in the same manner as in Example 6, except that an oxide solid electrolyte (Li2O-B2O3-P2O5, average particle size 0.1 μm) was used in the preparation of the composite negative electrode active material instead of PMMA.

[0137]

Table 1

[0138]

[0139] [evaluate]

[0140] (Porosity)

[0141] Cross-sectional SEM images were obtained for the negative electrode active material layers obtained in Examples 1 to 6 and Comparative Examples 1 to 3. The cross-sectional SEM images were processed and the porosity in the region (region A) of 0.3 μm around the surface of the Si-based negative electrode active material was calculated by the following formula.

[0142] Void ratio (%) = 100 × (void area in region A) / (area of ​​region A)

[0143] The results are shown in Table 2. Table 2 also shows the values ​​of the amount of PMMA added in each example and comparative example expressed as a volume ratio relative to Si particles. Figure 3 middle.

[0144]

Table 2

[0145]

[0146] Figure 3 (b) Figure 3 (a) is a magnified view of a part of the image. Figure 3 As shown in (b), it was confirmed that voids were formed around the active material. In addition, as shown in Table 2, in Comparative Example 1 and Examples 1 to 6, the void ratio in Region A was correlated with the amount of PMMA added, and it was confirmed that the voids in Region A came from the pore-forming material (PMMA). It was further confirmed that since the pore-forming material was removed after the negative electrode composite layer was pressed, the void ratio in Region B was smaller than that in Region A, and the filling rate of the negative electrode active material layer as a whole was high.

[0147] (Constraint Pressure Change)

[0148] The evaluation batteries obtained in Examples 1 to 6 and Comparative Examples 1 to 3 were subjected to a charge and discharge test. The conditions of the charge and discharge test were set to a restraining pressure (fixed dimension) of 5 MPa, a charge of 0.1C, a discharge of 1C, and a cutoff voltage of 3.0V to 4.55V, and the initial charge capacity and the initial discharge capacity were obtained. The results are shown in Figure 4 In addition, during the initial charge, the restraint pressure of the evaluation battery was monitored, the restraint pressure at 4.55 V was measured, and the amount of increase in the restraint pressure relative to the state before charge and discharge was determined.

[0149] like Figure 4 As shown in , in Examples 1 to 6, the change in the confinement pressure was significantly suppressed compared to Comparative Examples 1 to 3. This confirmed that the confinement pressure can be reduced in the all-solid-state battery of the present disclosure.

[0150] (Thermal stability)

[0151] The evaluation batteries obtained in Examples 1, 2, 5, and 6 were charged, and then the negative electrodes in the charged state were taken out. The temperatures of the exothermic peaks up to 400° C. were compared by differential scanning calorimetry (DSC). The results are shown in Table 3.

[0152]

Table 3

[0153]

[0154] As shown in Table 3, it was confirmed that the thermal stability was improved in Examples 5 and 6 in which the surface of the Si-based negative electrode active material was covered with the covering portion containing the oxide solid electrolyte.

Claims

1. An all-solid-state battery comprising a positive electrode active material layer, a negative electrode active material layer containing a Si-based negative electrode active material, and a solid electrolyte layer formed between the positive electrode active material layer and the negative electrode active material layer, wherein: The negative electrode active material layer has voids in a region A of 0.3 μm around the surface of the Si-based negative electrode active material, the porosity in the region A is greater than 10% and less than 70%, and the surface of the Si-based negative electrode active material is covered by a covering portion containing the voids and a solid electrolyte.

2. The all-solid-state battery according to claim 1, wherein: The porosity in the region B where the region of the Si-based negative electrode active material and the region A are removed from the entire region of the negative electrode active material layer is smaller than the porosity in the region A.

3. The all-solid-state battery according to claim 2, wherein: The void ratio in the region B is less than 10%.

4. The all-solid-state battery according to claim 1 or claim 2, wherein: The solid electrolyte of the coating portion is an oxide solid electrolyte.

5. The method for manufacturing an all-solid-state battery according to claim 1, comprising: A preparation step, wherein a negative electrode composite material is prepared, wherein the negative electrode composite material comprises a composite negative electrode active material having a pore-forming material-containing layer formed on the surface of a Si-based negative electrode active material; a negative electrode composite material layer forming step, wherein the negative electrode composite material is used to form a negative electrode composite material layer; A pressing step, wherein the negative electrode composite material layer is pressed; and The pore forming step includes removing the pore forming material from the negative electrode mixed material layer after the pressing, and forming pores in a region A of 0.3 μm around the surface of the Si-based negative electrode active material.

6. The method for manufacturing an all-solid-state battery according to claim 5, wherein: The pore-forming material is polymethyl methacrylate resin (PMMA).

7. The method for manufacturing an all-solid-state battery according to claim 5, wherein: The pore-forming material is removed by heat treatment.