Method for preparing quantum dots, and optical component and device including quantum dots
By using quantum dots with III-V compound cores and gradient shell structures, the problems of light emission wavelength broadening and cadmium-based quantum dot toxicity in quantum dot-enhanced films are solved, and eco-friendly quantum dots with high color purity and high luminous efficiency are realized. points, suitable for display improvements.
Patent Information
- Application Number
- CN202110021584.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-01-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-01-08
AI Technical Summary
The existing quantum dot enhancement film (QDEF) in the resin may cause the aggregation of quantum dots, broaden the light emission wavelength, and degrade the emission intensity. Moreover, cadmium-based quantum dots contain the toxic element cadmium, and their use is restricted by the Restriction of Hazardous Substances Directive (RoHS).
It uses a quantum dot structure of III-V compound core, ZnSe shell, ZnSe1-xSx middle shell, and ZnS outer shell layer. Through specific deposition steps and temperature control, a concentration gradient is formed to reduce lattice mismatch and improve luminous efficiency. and structural stability, and use non-cadmium-based materials to achieve eco-friendly quantum dot preparation.
Quantum dots with high color purity and high luminous efficiency are achieved, reducing the broadening of the emission wavelength, avoiding the use of cadmium, and meeting the needs for environmentally friendly and efficient displays.
Smart Images

Figure CN113105896B_ABST
Abstract
Description
[0001] This application claims priority to and the benefit of Korean Patent Application No. 10-2020-0003801 filed on January 10, 2020, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein in its entirety by reference. Technical Field
[0002] One or more embodiments relate to a method of preparing quantum dots, an optical member including quantum dots, and a device including quantum dots. Background Art
[0003] Quantum dots are nanocrystals of semiconductor materials and can exhibit quantum confinement effects. Quantum dots receive light from an excitation source, and when an energy excitation state is reached, the quantum dots emit energy (e.g., light) according to the corresponding energy band gap. Here, even for quantum dots formed of the same material, the wavelength (of emitted light) varies according to the particle size. Therefore, by adjusting the size of the quantum dots, (emission) light in a desired wavelength range can be obtained, and characteristics such as suitable (e.g., excellent) color purity and / or high luminous efficiency can be achieved. Therefore, quantum dots can be applied to various suitable devices or equipment.
[0004] The lighting device system can be applied to various suitable purposes. For example, the lighting device can be used for indoor or outdoor lighting, stage lighting, decorative lighting and / or a backlight unit (BLU) in a liquid crystal display (LCD) used in portable electronic products (mobile phones, video cameras, digital cameras and / or personal digital assistants (PDAs), etc.).
[0005] A typical use of the lighting device is, for example, as a BLU in an LCD. LCD is a type of flat panel display device that is currently widely used. The LCD includes two panels on which field generating electrodes such as pixel electrodes and / or common electrodes are formed, and a liquid crystal layer located between the two panels. The LCD displays an image by applying a voltage to the field generating electrodes to generate an electric field on the liquid crystal layer, changing the orientation along which the liquid crystal molecules of the liquid crystal layer are oriented by using the electric field, and controlling the polarization of incident light.
[0006] LCDs use color conversion members for color formation. When light emitted from a backlight source passes through a red color conversion member, a green color conversion member, and / or a blue color conversion member, each color conversion member reduces the amount of light to about 1 / 3, resulting in poor light efficiency.
[0007] In order to supplement (compensate for) such a decrease in light efficiency and achieve suitable (e.g., excellent) color reproducibility, blue light-emitting devices (LEDs) are recently used as light sources, and research and development is being conducted on applying quantum dot enhancement films (QDEFs) containing quantum dots to LCD backlights to improve color purity and display efficiency.
[0008] QDEF is a form in which green quantum dots and red quantum dots are dispersed in a resin and flaked, and then coated with two barrier films. The barrier film is used to protect the quantum dots from external moisture and oxygen. Typically, polyethylene terephthalate (PET) material is used as a barrier film, and cadmium-based quantum dots with suitable (e.g., excellent) performance and high color reproducibility are mainly used as quantum dots. However, QDEF has the following problems: quantum dot aggregation may occur in the resin, the emission wavelength of light may become wider, and the emission intensity may deteriorate. In addition, cadmium-based quantum dots contain the toxic element cadmium and are restricted for use according to the Restriction of Hazardous Substances Directive (RoHS). Summary of the invention
[0009] Aspects according to one or more embodiments relate to a method of preparing eco-friendly quantum dots having suitable (eg, excellent) color reproducibility, an optical member including the quantum dots, and a device including the quantum dots.
[0010] Additional aspects will be set forth in part in the description which follows and, in part, will be apparent from the description, or may be learned by practice of the presented disclosed embodiments.
[0011] According to one or more embodiments, a quantum dot may include:
[0012] Core, including III-V compounds;
[0013] a first shell surrounding the core and comprising ZnSe;
[0014] A second shell surrounding the first shell and including ZnSe 1-x S x , where x can be a real number greater than 0 and less than 1; and
[0015] A third shell surrounds the second shell and includes ZnS. A method for preparing quantum dots may include:
[0016] forming a first shell from a first solution including a first material and a second material, the first material including zinc and the second material including selenium;
[0017] forming a second shell by adding a third material including zinc and a fourth material including selenium and sulfur to the first solution to form a second solution; and
[0018] The third shell is formed by adding a fifth material including zinc to the second solution, wherein
[0019] The step of forming the first shell may include an act (a) of adding a first material and an act (b) of adding a second material, and
[0020] The step of forming the second shell may include an act (c) of adding the third material and an act (d) of adding the fourth material.
[0021] According to one or more embodiments, a quantum dot prepared according to the method may be provided.
[0022] According to one or more embodiments, an optical member including the quantum dots may be provided.
[0023] According to one or more embodiments, a device including the quantum dots may be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The above and other aspects, features and improvements of certain disclosed embodiments will become more apparent through the following description in conjunction with the accompanying drawings, in which:
[0025] Figure 1 is a schematic diagram of a quantum dot according to an embodiment;
[0026] Figure 2 is a schematic diagram of an apparatus according to an embodiment;
[0027] Figure 3 is a view showing a synthesis process and temperature of green quantum dots according to one or more embodiments;
[0028] Figure 4 is a view showing a synthesis process and temperature of red quantum dots according to one or more embodiments;
[0029] FIG. 5A to FIG. 5D are graphs showing optical characteristics of a display device manufactured according to one or more embodiments; and
[0030] Figure 6 is an image of a color gamut of a display device manufactured according to one or more embodiments. DETAILED DESCRIPTION
[0031] Now will refer to embodiment in more detail, the example of embodiment is shown in the accompanying drawings, wherein the same reference numerals refer to the same elements from time to time. In this respect, the present embodiment can have different forms, and should not be construed as being limited to the description set forth herein. Therefore, the embodiment is described below only by reference to the accompanying drawings to explain the aspects of this specification. As used herein, the term "and / or" includes any combination and all combinations of one or more related listed items. Throughout disclosure, the statement "at least one (kind / person) of a, b and c" represents only a, only b, only c, both a and b, both a and c, both b and c, all of a, b and c or its variant.
[0032] It will be understood that, although the terms “first”, “second”, etc. may be used herein to describe various elements, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element.
[0033] In the embodiments described in the present specification, an expression used in the singular encompasses an expression in the plural unless the expression used in the singular has a clearly different meaning in the context.
[0034] In this specification, it will be understood that terms such as "include", "have" and "include" are intended to indicate the presence of features or components disclosed in the specification, and are not intended to exclude the possibility that one or more other features or components may be present or may be added. For example, unless otherwise limited, terms such as "include" or "have" may mean that it is composed of only the features or components described in the specification, or may also include other components.
[0035] In the present specification, "Group III" may include Group IIIA elements and Group IIIB elements of the IUPAC periodic table. Non-limiting examples of Group III metals include aluminum (Al), indium (In), gallium (Ga), and thallium (Tl).
[0036] In the present specification, the term "quantum yield" and the term "luminous efficiency" may be used with substantially the same meaning (eg, interchangeably).
[0037] In this specification, the term "color gamut" has the same meaning as "color reproducibility" and is a numerical representation of how much of the original color can be expressed on the screen. The term "color gamut" refers to the range of colors that can be expressed in a display.
[0038] In the following, reference will be made to Figure 1 A quantum dot 100 and a method of manufacturing the quantum dot 100 according to an embodiment are described.
[0039] In some embodiments, the quantum dot 100 may include: a core 110 including a III-V compound; a first shell 120 surrounding the core 110 and including ZnSe; and a second shell 130 surrounding the first shell 120 and including ZnSe. 1-x S x , where x may be a real number greater than 0 and less than 1; and a third shell 140 surrounding the second shell 130 and including ZnS.
[0040] The method of preparing a quantum dot may include: forming a first shell 120 from a first material including zinc and a second material including selenium in a solution (ie, forming the first shell 120 from a first solution including the first material and the second material);
[0041] forming the second shell 130 by adding a third material including zinc and a fourth material including selenium and sulfur to the (first) solution (ie, adding the third material including zinc and the fourth material including selenium and sulfur to the first solution to form a second solution); and
[0042] The third shell 140 is formed by adding a fifth material including zinc to the (second) solution, wherein
[0043] The step of forming the first shell 120 may include a process (eg, action) (a) of adding a first material and a process (eg, action) (b) of adding a second material, and
[0044] The step of forming the second case 130 may include a process (eg, action) (c) of adding the third material and a process (eg, action) (d) of adding the fourth material.
[0045] In some embodiments, the step of forming the first shell 120 may include (eg, alternately) performing each of the process (eg, action) (a) and the process (eg, action) (b) at least twice.
[0046] In some embodiments, the steps of forming the first shell 120 may include sequentially performing: a process of adding a first material (e.g., action) (a1); a process of adding a second material (e.g., action) (b1); a process of adding the first material (e.g., action) (a2); and a process of adding the second material (e.g., action) (b2).
[0047] In some embodiments, in the method for preparing quantum dots, as the process (e.g., action) (a1), process (e.g., action) (b1), process (e.g., action) (a2), and process (e.g., action) (b2) are sequentially performed, the reaction temperature may gradually increase. In some embodiments, the temperature at which the process (e.g., action) (b1) is performed may be higher than the temperature at which the process (e.g., action) (a1) is performed. In some embodiments, the temperature at which the process (e.g., action) (a2) is performed may be higher than the temperature at which the process (e.g., action) (b1) is performed. In some embodiments, the temperature at which the process (e.g., action) (b2) is performed may be higher than the temperature at which the process (e.g., action) (a2) is performed.
[0048] In some embodiments, the step of forming the first shell 120 may further include sequentially performing: a process of adding the first material (eg, action) (a3); and / or a process of adding the second material (eg, action) (b3), etc.
[0049] In some embodiments, the step of forming the first shell 120 may be performed at a temperature ranging from about 180° C. to about 320° C. (eg, about 200° C. to about 300° C.).
[0050] In some embodiments, the step of forming the second shell 130 may include repeatedly performing each of the process (c) and the process (d) at least twice (eg, alternately).
[0051] In some embodiments, the steps of forming the second shell 130 may include sequentially performing: a process of adding a third material (e.g., action) (c1); a process of adding a fourth material (e.g., action) (d1); a process of adding the third material (e.g., action) (c2); and a process of adding the fourth material (e.g., action) (d2).
[0052] In some embodiments, in the method for preparing quantum dots, as the process (e.g., action) (c1), process (e.g., action) (d1), process (e.g., action) (c2), and process (e.g., action) (d2) are sequentially performed, the reaction temperature may gradually increase. In some embodiments, the temperature at which the process (e.g., action) (d1) is performed may be higher than the temperature at which the process (e.g., action) (c1) is performed. In some embodiments, the temperature at which the process (e.g., action) (c2) is performed may be higher than the temperature at which the process (e.g., action) (d1) is performed. In some embodiments, the temperature at which the process (e.g., action) (d2) is performed may be higher than the temperature at which the process (e.g., action) (c2) is performed.
[0053] In some embodiments, the step of forming the second shell 130 may further include sequentially performing: a process of adding a third material (eg, action) (c3); and / or a process of adding a fourth material (eg, action) (d3), etc.
[0054] In some embodiments, the step of forming the second shell 130 may be performed at a temperature ranging from about 240° C. to about 340° C. (eg, about 260° C. to about 320° C.).
[0055] In some embodiments, the first material and the third material may both include a zinc precursor, and the zinc precursor may be at least one selected from dimethyl zinc, diethyl zinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oxide, zinc peroxide, zinc perchlorate and zinc sulfate.
[0056] In some embodiments, the first material may include zinc stearate.
[0057] In some embodiments, the third material may include zinc stearate.
[0058] In some embodiments, the first material and the third material may be the same as each other. In some embodiments, the first material and the third material may be different from each other.
[0059] In some embodiments, the second material may include selenium powder.
[0060] In some embodiments, the second material may include selenium powder and an organic ligand. In some embodiments, the second material may include selenium powder and trioctylphosphine.
[0061] In some embodiments, the fourth material may include selenium powder and sulfur powder.
[0062] In some embodiments, the molar ratio between the selenium powder and the sulfur powder in the fourth material may be in the range of about 0.0005: 1 to about 0.1: 1. In some embodiments, when the step of forming the second shell 130 includes a process (e.g., action) (c1), a process (e.g., action) (d1), a process (e.g., action) (c2), and a process (e.g., action) (d2), the fourth material used in the process (e.g., action) (d1) and the fourth material used in the process (e.g., action) (d2) may have different molar ratios between the selenium powder and the sulfur powder.
[0063] In some embodiments, the fourth material used in process (e.g., action) (d1) can have a molar ratio between selenium powder and sulfur powder in a range of about 0.02:1 to about 0.04:1 (e.g., about 0.025:1 to about 0.035:1, or for example, about 0.03:1).
[0064] In some embodiments, the fourth material used in the process (e.g., action) (d2) can have a molar ratio between selenium powder and sulfur powder in a range of about 0.001:1 to about 0.02:1 (e.g., about 0.002:1 to about 0.01:1, or for example, about 0.005:1).
[0065] In the composition of the first shell, the composition of the second shell, and the composition of the third shell, the first shell close to the core may include Se (e.g., excluding S), the second shell may include Se and S, and the third shell may include S (e.g., excluding Se). In general, the ratio of S to Se may be higher as the distance is farther away from the core. Thus, the quantum dot may have a structure in which the lattice mismatch is reduced at the interface between the core and the first shell and between the shells. Thus, the quantum dot may have a reduced full width at half maximum (FWHM) and improved luminous efficiency and structural stability.
[0066] In some embodiments, the ZnSe 1-x S x The content of selenium in the first shell may be higher toward the first shell and lower toward the third shell, thus forming a concentration gradient. In some embodiments, the x value at the interface between the second shell and the first shell may be smaller, and the x value at the interface between the second shell and the third shell may be larger. In addition, for example, the x value may increase from the interface between the second shell and the first shell to the interface between the second shell and the third shell.
[0067] In some embodiments, the III-V compound included in the core may be GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InGaP, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, InAlPSb, or combinations thereof.
[0068] In some embodiments, the radius of the core can be in a range from about 0.5 nanometers (nm) to about 2.5 nm (eg, about 0.6 nm to about 2.4 nm, eg, about 0.75 nm to about 2.25 nm, or, eg, about 1 nm to about 2 nm).
[0069] In some embodiments, the method of preparing quantum dots may further include the step of forming a core 110. The method of forming the core 110 may include forming a group III-V compound from a group III precursor and a group V precursor.
[0070] In some embodiments, the step of forming the core 110 may be performed at a temperature ranging from about 240° C. to about 340° C. (eg, about 260° C. to about 320° C.).
[0071] In some embodiments, the step of forming the third shell 140 may be performed at a temperature lower than the temperature in the step of forming the second shell. In some embodiments, the fifth material may include at least one selected from zinc precursors. In some embodiments, the fifth material may include zinc acetate.
[0072] In addition, in some embodiments, the fifth material may include a zinc precursor and an organic ligand. In some embodiments, the organic ligand may be trioctylphosphine, trioctylphosphine oxide, oleic acid, oleylamine, octylamine, trioctylamine, hexadecylamine, octylmercaptan, dodecanethiol, hexylphosphonic acid, tetradecylphosphonic acid, octylphosphonic acid, or a combination thereof.
[0073] In some embodiments, a molar ratio between the zinc precursor and the organic ligand in the fifth material may be in a range from about 0.5:1 to about 0.7:1 (eg, about 0.55:1 to about 0.65:1, or for example, about 0.6:1).
[0074] In some embodiments, in addition to the above materials, the solution used in the method for preparing quantum dots may further include a zinc precursor and an organic ligand.
[0075] In some embodiments, the solvent included in the solution may be an organic solvent. For example, the solvent may be oleylamine and / or 1-octadecene, etc.
[0076] By referring to the examples provided herein, one of ordinary skill in the art can understand methods of preparing quantum dots.
[0077] The first shell, the second shell, and the third shell of the quantum dot may each serve as a protective layer for reducing or preventing chemical denaturation of the core to maintain semiconductor properties and / or as a charging layer for imparting electrophoretic properties to the quantum dot.
[0078] In some embodiments, the thickness of each of the first shell, the second shell, and the third shell may be in a range of about 0.5 nm to about 2 nm (e.g., about 0.6 nm to about 1.9 nm, for example, about 0.7 nm to about 1.8 nm, for example, about 1.0 nm to about 1.7 nm, or for example, about 1.2 nm to about 1.5 nm).
[0079] The quantum dots may emit visible light other than blue light. For example, the quantum dots may emit light having a maximum emission wavelength in the range of about 500 nm to about 750 nm (or, for example, about 500 nm to about 650 nm). Therefore, when the quantum dots are applied to the color conversion member, blue light may be absorbed to emit light of wavelengths in various suitable color ranges.
[0080] In some embodiments, the quantum dots may emit green light having a maximum emission wavelength in the range of about 500 nm to about 600 nm. In some embodiments, the quantum dots may emit red light having a maximum emission wavelength in the range of about 600 nm to about 750 nm. Therefore, when the quantum dots are applied to the color conversion member, green light or red light having high brightness and suitable (e.g., excellent) color purity may be obtained.
[0081] In some embodiments, the diameter of the quantum dot can be in the range of about 3 nm to about 13 nm. For example, the diameter of the quantum dot can be in the range of about 4 nm to about 12 nm (e.g., about 4 nm to about 8 nm, for example, about 5 nm to about 11 nm, for example, about 6 nm to about 10 nm, or for example, about 7 nm to about 9 nm). In some embodiments, the diameter of the quantum dot can be in the range of about 4 nm to about 6 nm, and the quantum dot can emit green light.
[0082] In some embodiments, the diameter of the quantum dots can be in a range from about 7 nm to about 9 nm, and the quantum dots can emit red light.
[0083] In some embodiments, the quantum dots may have an optical absorptivity of 80 percent (%) or more for blue light (e.g., blue light having a wavelength of 461 nm). Therefore, when the quantum dots are applied to the color conversion member, the absorption of blue light from the light source may be suitable (e.g., excellent), thereby achieving efficient optical conversion and emitting green light with high color purity.
[0084] In some embodiments, the FWHM of the emission wavelength spectrum of the quantum dots can be 60 nm or less (e.g., 55 nm or less). When the FWHM of the quantum dots is within these ranges, high color purity, suitable (e.g., excellent) color reproducibility, and / or improved wide viewing angle can be achieved.
[0085] As described above, the composition of each of the first shell, the second shell, and the third shell forms a concentration gradient, and thus has a structure with reduced lattice mismatch. Therefore, the quantum dots according to the embodiment can have a suitable (e.g., excellent) absorptivity for blue light, and reduce the generation of defects at the interface between the core and the shell, thereby protecting the core of the quantum dot with a shell of sufficient thickness, while (or in parallel) achieving high light efficiency and high color purity.
[0086] In some embodiments, the form of quantum dots can be a form commonly used in the art, and is not specifically limited. In some embodiments, quantum dots can be in a spherical form, a pyramidal form, a multi-arm form, and / or can be cubic nanoparticles, nanotubes, nanowires, nanofibers and / or nanosheet particles, etc.
[0087] In some embodiments, the quantum dots may include additional compounds in addition to the aforementioned components.
[0088] In some embodiments, the quantum dots may also include II-VI compounds, III-VI compounds, III-V compounds, IV-VI compounds, Group IV elements or compounds, I-III-VI compounds, or combinations thereof in the core, first shell, second shell, and / or third shell.
[0089] The II-VI compounds may be selected from: binary compounds selected from the group consisting of CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, MgSe, MgS and mixtures thereof; binary compounds selected from the group consisting of CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe , CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, MgZnSe, MgZnS and mixtures thereof; and a quaternary compound selected from the group consisting of CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe, HgZnSTe and mixtures thereof.
[0090] III-VI compounds may include: binary compounds (such as In 2 S 3 and / or In 2 Se 3 ); ternary compounds (such as InGaS 3 and / or InGaSe 3 ); or any combination thereof.
[0091] The III-V compound may be selected from: a binary compound selected from the group consisting of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb and mixtures thereof; a ternary compound selected from the group consisting of GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InGaP, InAlP, InNP, InNAs, InNSb, InPAs, InPSb and mixtures thereof; and a quaternary compound selected from the group consisting of GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, InAlPSb and mixtures thereof. The III-V compound may also include a Group II metal (e.g., InZnP).
[0092] The IV-VI group compound may be selected from: a binary compound selected from the group consisting of SnS, SnSe, SnTe, PbS, PbSe, PbTe and mixtures thereof; a ternary compound selected from the group consisting of SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe and mixtures thereof; and a quaternary compound selected from the group consisting of SnPbSSe, SnPbSeTe, SnPbSTe and mixtures thereof. The IV group element may be selected from the group consisting of Si, Ge and mixtures thereof. The IV group compound may be a binary compound selected from the group consisting of SiC, SiGe and mixtures thereof.
[0093] Group I-III-VI compounds may include ternary compounds such as AgInS, AgInS 2 、CuInS、CuInS 2 、CuGaO 2 、AgGaO 2 、AgAlO 2 or any combination thereof.
[0094] In this case, the binary compound, ternary compound and / or quaternary compound may be present in the particle at a uniform concentration, or may be present in the particle at a non-uniform concentration, for example, by being partially divided into different concentrations in the same particle.
[0095] In some embodiments, the first shell, the second shell, and / or the third shell may further include a metal oxide or a non-metal oxide, a semiconductor compound, or a combination thereof.
[0096] In some embodiments, the metal oxide or non-metal oxide may be a binary compound (such as SiO 2 、Al 2 O 3 、TiO 2 、ZnO、MnO、Mn 2 O 3 , Mn 3 O 4 , CuO, FeO, Fe 2 O 3 , Fe 3 O 4 , CoO, Co 3 O 4 and / or NiO) or ternary compounds (such as MgAl 2 O 4 、CoFe 2 O 4 、NiFe 2 O 4 and / or CoMn 2 O 4 ).
[0097] In some embodiments, the semiconductor compound can be CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnSeS, ZnTeS, GaAs, GaP, GaSb, HgS, HgSe, HgTe, InAs, InP, InGaP, InSb, AlAs, AlP and / or AlSb.
[0098] In some embodiments, a color conversion component comprising quantum dots may be provided.
[0099] In some embodiments, at least a portion of the color conversion member may include quantum dots (e.g., a plurality of quantum dots), and the quantum dots may absorb blue light and emit visible light other than blue light, for example, visible light having a maximum emission wavelength in the range of about 500 nm to about 750 nm (or, for example, about 500 nm to about 650 nm). Thus, the color conversion member including quantum dots may be designed to absorb blue light and emit light of wavelengths in various suitable color ranges.
[0100] In some embodiments, at least a portion of the color conversion member may include quantum dots (e.g., a plurality of quantum dots), and the quantum dots may absorb blue light and emit green light having a maximum emission wavelength in the range of about 500 nm to about 600 nm. Therefore, the color conversion member including quantum dots may emit green light having high brightness and high color purity.
[0101] equipment
[0102] According to one or more embodiments, a device including quantum dots may be provided.
[0103] In some embodiments, a color conversion component including quantum dots and an apparatus including a light source may be provided.
[0104] In some embodiments, reference Figure 2 , the device 200 may include: a substrate 210 ; a light source 220 located on the substrate 210 ; and a color conversion member 230 located on the light source 220 .
[0105] Figure 2 The device 200 shown in FIG. 2 is an example of the devices described herein. The device 200 may have various suitable forms (eg, forms known in the art), and may also include various suitable (eg, known) features.
[0106] In some embodiments, light source 220 may emit blue light having a maximum emission wavelength in a range of about 400 nm to about 490 nm.
[0107] In some embodiments, the light source 220 may be a backlight unit (BLU) used in a liquid crystal display (LCD), a fluorescent lamp, a light emitting device, an organic light emitting device, a quantum dot light emitting device (QLED), or any combination thereof, but the embodiment is not limited thereto. The color conversion member 230 may be disposed in at least one traveling direction of light emitted from the light source 220.
[0108] Here, the feature that the color conversion member 230 is disposed in at least one traveling direction of light emitted from the light source 220 may not exclude further including other elements between the color conversion member 230 and the light source 220 .
[0109] In some embodiments, a polarizer, a liquid crystal layer, a light guide plate, a diffuser plate, a prism sheet, a microlens sheet, a brightness enhancement sheet, a reflective film, a color filter, or any combination thereof may be placed between the light source 220 and the color conversion member 230 .
[0110] In some embodiments, a polarizer, a liquid crystal layer, a light guide plate, a diffusion plate, a prism sheet, a microlens sheet, a brightness enhancement sheet, a reflective film, a color filter, or any combination thereof may be disposed on the color conversion member 230 .
[0111] In some embodiments, the device 200 may include a structure in which a light source, a light guide plate, a color conversion member, a first polarizer, a liquid crystal layer, a color filter, and a second polarizer are sequentially arranged.
[0112] In some embodiments, device 200 may include a structure in which a light source, a light guide plate, a first polarizer, a liquid crystal layer, a second polarizer, and a color filter are sequentially arranged.
[0113] In an embodiment of the device 200, the color filter may include a pigment or a dye.In an embodiment of the device 200, one of the first polarizer and the second polarizer may be a vertical polarizer, and the other may be a horizontal polarizer.
[0114] In some embodiments, at least a portion of the color conversion member 230 in the device 200 may include quantum dots (e.g., a plurality of quantum dots), and the at least a portion may absorb blue light emitted from the light source 220 and emit visible light other than blue light, for example, visible light having a maximum emission wavelength in the range of about 500 nm to about 750 nm. Thus, the color conversion member including quantum dots may be designed to absorb blue light emitted from the light source and emit light of wavelengths in various suitable color ranges.
[0115] In some embodiments, at least a portion of the color conversion member 230 in the device 200 may include quantum dots (e.g., a plurality of quantum dots), and the at least a portion may absorb blue light emitted from the light source 220 and emit green light having a maximum emission wavelength in the range of about 500 nm to about 600 nm. In some embodiments, the quantum dots may emit red light having a maximum emission wavelength in the range of about 600 nm to about 750 nm. Thus, the color conversion member including the quantum dots may absorb blue light emitted from the light source and emit green light or red light having high brightness and suitable (e.g., excellent) color purity. In some embodiments, the device 200 may exhibit a National Television System Committee (NTSC) color gamut of 105% or more, for example, an NTSC color gamut of 108% or more.
[0116] The device 200 may be, for example, a transmitting device, an authentication device, and / or an electronic device, but the embodiments are not limited thereto.
[0117] The emitting device may be used in a variety of suitable displays and / or light sources, etc.
[0118] The authentication device may be, for example, a biometric authentication device that identifies an individual based on biometric information (eg, fingertips and / or pupils, etc.).
[0119] The authentication device may also include a biometric information collection unit.
[0120] The electronic device can be applied to personal computers (e.g., mobile personal computers), cellular phones, digital cameras, electronic notepads, electronic dictionaries, electronic game consoles, medical devices (e.g., electronic thermometers, sphygmomanometers, blood glucose meters, pulse measuring devices, pulse wave measuring devices, electrocardiogram recorders, ultrasonic diagnostic devices, endoscopic display devices, etc.), fish finders, various suitable measuring devices, measuring instruments (e.g., measuring instruments for automobiles, airplanes, ships, etc.), projectors, etc., but the embodiments are not limited thereto.
[0121] In an embodiment, the device 200 may include an LCD, an organic light emitting display device, or an inorganic light emitting display device.
[0122] The device 200 may also include a thin film transistor.
[0123] Hereinafter, quantum dots and methods of preparing quantum dots according to embodiments will be described in more detail with reference to examples.
[0124] Example
[0125] [Preparation Example 1] Preparation of stock solution
[0126] 1) SeTOP stock solution
[0127] 1.78 mmol of Se powder was dissolved in 1 milliliter (mL) of trioctylphosphine (TOP, 97%) to prepare a selenium and trioctylphosphine (SeTOP) stock solution.
[0128] 2) SeSTOP-1 stock solution
[0129] 0.06 mmol of Se powder and 2 mmol of sulfur powder were dissolved in 2 mL of TOP to prepare a selenium, sulfur, and trioctylphosphine (SeSTOP-1) stock solution.
[0130] 3) SeSTOP-2 stock solution
[0131] 0.02 mmol of Se powder and 4 mmol of sulfur powder were dissolved in 2 mL of TOP to prepare a selenium, sulfur, and trioctylphosphine (SeSTOP-2) stock solution.
[0132] 4) ZnSt 2 Stock solution
[0133] 4.74 mmol of zinc stearate (ZnSt 2 ) and 15 mL of octadecene were mixed in a 150 mL three-necked flask, and the mixture was heated to 120°C and then degassed. Then, the mixture was vacuum dried at 120°C for 1 hour. The temperature was raised to 250°C under a nitrogen atmosphere to prepare ZnSt 2Prepare ZnSt 2 The stock solution was stored in a three-necked flask at 250 °C under nitrogen atmosphere.
[0134] [Synthesis Example 1] Green InP / ZnSe / ZnSe x S 1-x Preparation of ZnS quantum dots (green QDs)
[0135] 0.111 g (0.225 mmol) of indium (III) iodide, 0.15 g (1.1 mmol) of zinc (II) chloride and 0.351 g (1.1 mmol) of zinc (II) iodide were mixed with 6.0 mL of industrial oleylamine. The mixture was then stirred at 120°C for 1 hour and degassed, then heated to 180°C in an inert atmosphere. When the desired temperature was reached, 0.4 mL (1.47 mmol) of tris(diethylamino)phosphine ((DEA)) as a phosphorus precursor was added. 3 P) (phosphorus:indium ratio = 6.5:1) was quickly added to the mixture.
[0136] After the injection of the phosphorus precursor, the InP nuclei were grown at the desired temperature for 14 minutes (see Figure 3 ). The ZnSeS intermediate shell was grown by sequentially and alternately injecting anion shell precursors and cation shell precursors. First, 0.09 mL of SeTOP stock solution was injected into the mixture and the temperature was maintained at 200 °C for 10 min. Then, 0.5 mL of ZnSt 2 The stock solution was slowly injected into the mixture, and the temperature was maintained at 220°C for 10 minutes. Then, 0.09 mL of SeTOP stock solution was injected into the mixture, and the temperature was maintained at 240°C for 10 minutes. Then, 0.5 mL of ZnSt 2 The stock solution was slowly injected into the mixture, and the temperature was maintained at 260°C for 10 minutes. Then, 0.09 mL of SeTOP stock solution was injected into the mixture, and the temperature was maintained at 280°C for 10 minutes. Then, 0.5 mL of ZnSt 2 The stock solution was slowly injected into the mixture and the temperature was maintained at 300°C for 10 minutes (to complete the formation of the first shell). The mixture was then cooled to 260°C and 2 mL of SeSTOP-1 stock solution was then injected and the temperature was maintained at 260°C for 10 minutes. Then, 6 mL of ZnSt 2 The stock solution was slowly injected into the mixture, and the temperature was maintained at 300°C for 20 minutes. Then, 2 mL of SeSTOP-2 stock solution was slowly injected into the mixture, and the temperature was maintained at 320°C for 20 minutes. Then, 7 mL of ZnSt 2The stock solution was slowly injected into the mixture and the temperature was maintained at 320°C for 40 minutes (to complete the formation of the second shell). Subsequently, in order to passivate the ZnS shell, the reaction flask was cooled at room temperature and 0.22 g (1.2 mmol) of zinc acetate (Zn(OAc)) was added at room temperature. 2 ) and 0.48mL (2mmol) of 1-dodecanethiol were added to the reaction flask, followed by heating to 230°C for 1 hour (thereby completing the formation of the third shell). Once the reaction is complete, the mixture is cooled to room temperature. In order to purify the crude product, 2mL of chloroform, 1mL of ethanol and excess acetone are added to the mixture solution until the solution is turbid, and then centrifuged at 10,000 revolutions per minute (rpm). After centrifugation, the supernatant is removed and the precipitate is redispersed in an organic solvent such as chloroform, toluene and / or hexane to obtain a green QD composition.
[0137] [Synthesis Example 2] Red InP / ZnSe / ZnSe x S 1-x Preparation of ZnS quantum dots (red QDs)
[0138] 0.111 g (0.225 mmol) of indium (III) iodide, 0.15 g (1.1 mmol) of zinc (II) chloride, and 0.351 g (1.1 mmol) of zinc (II) iodide were mixed with 6.0 mL of industrial oleylamine. The mixture was then stirred at 120° C. for 1 hour and degassed, and then heated to 200° C. in an inert atmosphere. The phosphorus precursor was injected and the following process was performed in substantially the same manner as in Synthesis Example 1 (see Figure 4 ) to obtain a red QD composition.
[0139] [Comparative synthesis example 1]
[0140] 0.2 mmol of indium acetate, 0.125 mmol of zinc acetate, 0.6 mmol of palmitic acid and 10 mL of 1-octadecene were added to the reactor, and the reactor was heated at 120° C. under vacuum. After 1 hour, the reactor was purged with nitrogen. After heating at 250° C., 0.15 mmol of tris(trimethylsilyl)phosphine (TMS) was rapidly injected thereinto. 3 In the embodiment of the present invention, the invention discloses a method for preparing a semiconductor nanocrystal of InP semiconductor nanocrystal. The method comprises the steps of: adding 1 mL of 1% pyrrolidone (P) and 1 mL of trioctylphosphine to a mixed solution of 1 mL of trioctylphosphine, and reacting for 20 minutes. Acetone is added to the reaction solution, which is quickly cooled to room temperature, and then centrifuged to obtain a precipitate. The precipitate is dispersed in toluene, thereby preparing a toluene dispersion of InP semiconductor nanocrystals.
[0141] 1.2 mmol (0.224 g) of zinc acetate, 2.4 mmol (0.757 g) of oleic acid and 10 mL of trioctylamine were added to the reaction flask and vacuum treated at 120° C. for 10 minutes.2 The flask was purged and the temperature was raised to 280° C. A toluene dispersion of the prepared InP semiconductor nanocrystals (OD=optical density of first exciton absorption, OD: 0.15 or 1 mL of 1 wt% toluene solution) was quickly injected therein within 10 seconds. Subsequently, 2.4 mmol of S / TOP was added thereto, and then reacted for 120 minutes.
[0142] Once the reaction was complete, ethanol was added to the reaction solution which was rapidly cooled to room temperature for precipitation. The precipitate was centrifuged and redispersed in toluene to prepare quantum dots.
[0143] [Evaluation Example 1] Evaluation of quantum dot photoluminescence
[0144] Based on the photoluminescence (PL) spectrum, the emission centroid wavelength (e.g., maximum emission wavelength), FWHM, quantum yield, and blue light absorptivity of the quantum dots prepared in Synthesis Example 1 and Synthesis Example 2 and Comparative Synthesis Example 1 were each evaluated using a quantum efficiency measurement system QE-2100 (purchased from Otsuka). The results are shown in Table 1 (excitation wavelength: 365 nm, 458 nm).
[0145] Table 1
[0146]
[0147] [Comparative Example 1]
[0148] DCR-TR711R, DCR-TR711G and DCR-TR711B (purchased from Dongjin Semichem Co., Ltd.) were used as red color filter (CF) compounds, green color filter (CF) compounds and blue color filter (CF) compounds, respectively. First, 1 cm 2 was impregnated with a mixed solution of isopropyl alcohol and acetone (volume ratio of 1:1). 2 The quartz substrate was then ultrasonicated for 10 minutes. Then, a drying process was performed under nitrogen. The dried quartz substrate was attached to a guide ring (1 cm×1 cm), and a blue CF compound, a green CF compound, and a red CF compound were uniformly coated on the corresponding quartz substrate to prepare a color filter.
[0149] A white light emitting device (LED) was used as a backlight unit (BLU), and the LCD device of Comparative Example 1 was prepared to have a structure of BLU / light guide film (LGF) / vertical polarizer / nematic liquid crystal / horizontal polarizer.
[0150] [Example 1]
[0151] The green QD stock solution of Synthesis Example 1 and the red QD stock solution of Synthesis Example 2 were dispersed in hexane at a weight ratio of 20 wt%. The resulting solution was mixed with a silicone resin to prepare a composite resin. A guide ring (1 cm × 1 cm) was attached to a dry quartz substrate, and the composite resin was uniformly coated on the substrate. Then, the substrate was dried and cured at room temperature to prepare a quantum dot enhancement film (QDEF).
[0152] A blue LED was used as a BLU to prepare an LCD device of Example 1 having a structure of BLU / LGF / QDEF / vertical polarizer / nematic liquid crystal / horizontal polarizer.
[0153] [Example 2]
[0154] A green CF compound and a red CF compound (the same as the green CF compound and the red CF compound in Comparative Example 1) were mixed with 0.3 mL of the green QD solution of Synthesis Example 1 and 0.3 mL of the red QD solution of Synthesis Example 2, respectively. Then, the two mixtures were mixed with a specific blue CF compound to obtain a new mixture. The new mixture was evenly coated on a 1 cm thick guide ring (1 cm × 1 cm) attached to it. 2 The resulting film was deposited on a quartz substrate and dried and cured at room temperature to prepare a QDCF (quantum dot color filter).
[0155] A blue LED was used as a BLU to prepare the LCD device of Example 2 having a structure of BLU / LGF / vertical polarizer / nematic liquid crystal / horizontal polarizer / QDCF.
[0156] [Evaluation Example 2] Analysis of Optical Characteristics of Display
[0157] The LCD device exhibits the best color gamut when the emission wavelengths are separated from each other within the wavelength range transmitted through the blue CF, green CF, and red CF. The crosstalk of the emission wavelengths after CF transmission has a significant impact on the efficiency of the device. Therefore, in order to analyze the optical characteristics of the display, a polarization microscope (purchased from Nikon Inc.) was used to measure and compare the photoluminescence (PL) emission spectra and FWHM after polarization.
[0158] First, blue CF, green CF, and red CF were coated on corresponding quartz slides as standard samples to measure the emission spectra. max =451nm), green CF (478nm to 595nm, λ max =527nm) and red CF (>570nm, λ max =631nm) wavelength spectrum is shown in Figure 5AIn addition, in the LCD device of the present disclosure, since blue light is emitted from the blue LED as the BLU, the emission spectrum is measured by placing the blue LED as the BLU as a standard sample (blue LED) in the PL spectrometer. As a result, the BLU emits light of the maximum emission wavelength at a wavelength of 452 nm ( Figure 5A ).
[0159] The LCD device of Comparative Example 1 emits polarized light of blue (B-CF) having a FWHM of 20.6 nm at 456 nm, polarized light of green (G-CF) having a FWHM of 49.1 nm at 541 nm, and polarized light of red (R-CF) having a FWHM of 58.7 nm at 612 nm. Significant crosstalk is exhibited between the emission spectra ( Figure 5B ).
[0160] The QDEF-LCD device of Example 1 emits blue (B-QDEF) polarized light having a FWHM of 20.4 nm at 452 nm, green (G-QDEF) polarized light having a FWHM of 31.3 nm at 528 nm, and red (R-QDEF) polarized light having a FWHM of 36.4 nm at 638 nm. There is little (e.g., no or insignificant amount) crosstalk between emission peaks ( Figure 5C ).
[0161] The QDCF-LCD device of Example 2 emits polarized light of blue (B-QDCF) having a FWHM of 20.4 nm at 452 nm, polarized light of green (G-QDCF) having a FWHM of 26.1 nm at 530 nm, and polarized light of red (R-QDCF) having a FWHM of 36.7 nm at 638 nm. As in Example 1, little (e.g., no or insignificant amount) crosstalk is exhibited between emission peaks ( Figure 5D ).
[0162] In Table 2, the LCD device of Comparative Example 1, the QDEF-LCD device of Example 1, and the QDCF-LCD device of Example 2 are compared.
[0163] Table 2
[0164]
[0165] Reference FIG. 5A to FIG. 5D As shown in Table 2, the blue emission spectrum of the QDEF-LCD device of Example 1 and the blue emission spectrum of the QDCF-LCD device of Example 2 both show a narrow FWHM of about 20 nm, and the FWHMs of the green emission spectrum and the red emission spectrum are significantly reduced compared to the LCD device of Comparative Example 1.
[0166] [Evaluation Example 3] Analysis of Display Color Reproducibility
[0167] In order to analyze the color reproducibility for evaluating the possibility (e.g., suitability) as an ultra-high-resolution LCD display, the performances of the LCD device of Comparative Example 1, the QDEF-LCD device of Example 1, and the QDCF-LCD device of Example 2 were compared with each other by estimating the coordinates in the CIE 1931 color space according to the two standards of NTSC 1953 and Rec. 2020. FIG. 5B to FIG. 5D The CIE coordinates were calculated using the PL spectrum and the CIE coordinate calculator based on MATLAB. The results are shown in Table 2. In addition, the two standard color spaces are represented in a triangular shape within the CIE color space and are shown in Figure 6 middle.
[0168] Refer to Table 2 and Figure 6 , the RGB color reproducibility of the LCD device of Comparative Example 1 is 73.7% according to the NTSC standard and 55.1% according to the Rec.2020 standard, and it is found that it is more suitable for standard resolution displays rather than ultra-high definition (UHD) displays. The color reproducibility of the QDEF-LCD device (QDCF+CF) of Example 1 is 95.2% according to the NTSC standard and 71.2% according to the Rec.2020 standard, and the color reproducibility of the QDCF-LCD device of Example 2 is 108.8% according to the NTSC standard and 81.4% according to the Rec.2020 standard. Therefore, it is found that the QDEF-LCD device of Example 1 and the QDCF-LCD device of Example 2 show improved color reproducibility. Therefore, it is found that the QDEF-LCD device of Example 1 and the QDCF-LCD device of Example 2 are suitable for UHD displays compared with the LCD device of Comparative Example 1.
[0169] As is apparent from the foregoing description, the method of preparing quantum dots is eco-friendly and can provide non-cadmium-based quantum dots with high luminous efficiency and high stability. Therefore, when the quantum dots are applied to color conversion members, crosstalk between emission wavelengths is reduced, thereby improving color reproducibility.
[0170] When describing embodiments of the inventive concept, the use of “may” refers to “one or more embodiments of the inventive concept.” Furthermore, the term “exemplary” is intended to indicate an example or illustration.
[0171] The terms used herein are only used for the purpose of describing specific example embodiments and are not intended to limit the invention. As used herein, unless the context clearly indicates otherwise, the singular forms "a", "an", and "the" are also intended to include the plural forms.
[0172] As used herein, the terms "substantially (substantially)", "approximately (about)" and similar terms are used as approximate terms rather than degree terms, and are intended to explain the inherent deviations of measured values or calculated values that will be recognized by those of ordinary skill in the art. In addition, any numerical range stated here is intended to include all sub-ranges of the same numerical precision contained in the range of the statement. For example, the range of "1.0 to 10.0" is intended to include all sub-ranges between the minimum value 1.0 of the statement and the maximum value 10.0 of the statement (and including the minimum value 1.0 of the statement and the maximum value 10.0 of the statement), that is, with a minimum value equal to or greater than 1.0 and a maximum value equal to or less than 10.0, such as 2.4 to 7.6 as an example. Any maximum numerical limit stated here is intended to include all lower numerical limits contained therein, and any minimum numerical limit stated in this specification is intended to include all higher numerical limits contained therein. Therefore, the applicant reserves the right to modify this specification (including claims) to explicitly state any sub-range contained in the range explicitly stated here. All such ranges are intended to be inherently described in this specification so that modification to explicitly state any such sub-range will meet the requirements.
[0173] It should be understood that the embodiments described herein should be considered in a descriptive sense only and not for purposes of limitation. The description of features or aspects within each embodiment should generally be considered applicable to other similar features or aspects in other embodiments. Although one or more embodiments have been described with reference to the accompanying drawings, it will be understood by those of ordinary skill in the art that various changes in form and details may be made therein without departing from the spirit and scope as defined by the claims and their equivalents.
Claims
1. A method for preparing quantum dots, in, The quantum dot includes: a core including a III-V compound; a first shell surrounding the core and including ZnSe; and a second shell surrounding the first shell and including ZnSe. 1-x S x , wherein x is a real number greater than 0 and less than 1; and a third shell surrounding the second shell and comprising ZnS, the method comprising the following steps: forming the first shell from a first solution including a first material and a second material, the first material including zinc and the second material including selenium; forming the second shell by adding a third material and a fourth material to the first solution to form a second solution, the third material including zinc and the fourth material including selenium and sulfur; and The third shell is formed by adding a fifth material to the second solution, the fifth material comprising zinc, wherein, The step of forming the first shell includes an action a of adding the first material and an action b of adding the second material, and The step of forming the second shell includes an action c of adding the third material and an action d of adding the fourth material, The step of forming the first shell includes alternately performing each of action a and action b at least twice, and the reaction temperature is gradually increased, and The step of forming the second shell includes alternately performing each of action c and action d at least twice, and the reaction temperature is gradually increased.
2. The method according to claim 1, in, The step of forming the first shell comprises sequentially performing the following actions: action b1 of adding the second material; action a1 of adding the first material; action b2 of adding the second material; and action a2 of adding the first material, Here, as action b1, action a1, action b2, and action a2 are sequentially performed, the reaction temperature gradually increases.
3. The method according to claim 1, in, The step of forming the second shell comprises sequentially performing the following actions: an action d1 of adding said fourth material; Action c1 of adding said third material; an action d2 of adding said fourth material; and action c2 of adding said third material, Here, as action d1 , action c1 , action d2 , and action c2 are sequentially performed, the reaction temperature gradually increases.
4. The method according to claim 1, in, The first material and the third material both include zinc stearate.
5. The method according to claim 1, in, The second material includes selenium powder, and The fourth material includes selenium powder and sulfur powder.
6. The method according to claim 1, in, ZnSe included in the second shell 1-x S x The selenium content in the nanostructured carbon nanotubes is higher toward the first shell and lower toward the third shell, thereby forming a concentration gradient.
7. The method according to claim 1, in, The III-V group compound is selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InGaP, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, InAlPSb and combinations thereof.
8. The method according to claim 1, in, The method also includes forming the core including the Group III-V compound from a Group III precursor and a Group V precursor.
9. The method according to claim 1, in, The step of forming the third shell is performed at a temperature lower than a temperature in the step of forming the second shell.
10. The method according to claim 1, in, The fifth material includes zinc acetate.
11. The method according to claim 1, in, The first solution also includes a zinc precursor and an organic ligand.
12. A quantum dot, the quantum dot being prepared according to the method according to any one of claims 1 to 11. 13 . An optical member comprising the quantum dots according to claim 12 .
14. The optical component according to claim 13, in, The optical component is a color conversion component.
15. A device comprising the quantum dots according to claim 12.
16. The device according to claim 15, wherein the device include: Light source, emitting light; as well as a color conversion member located on a path of the light emitted from the light source, Wherein, the color conversion component includes the quantum dots.
17. The device according to claim 16, in, The light source is an organic light emitting device or a light emitting diode, and The light source emits blue light having a maximum emission wavelength in the range of 400 nm to 490 nm.
18. The device according to claim 17, in, At least a portion of the color conversion member includes the quantum dots, and the at least a portion absorbs the blue light emitted from the light source and emits visible light other than the blue light.
Citation Information
Patent Citations
Channel formats with flexible durations in wireless communications