Semiconductor element and method for manufacturing the same
By using porous dielectric structures and energy processing technology in semiconductor components, the challenges of quality, yield, and reliability as the size of semiconductor components become smaller are solved, and the effects of reducing coupling capacitance and operating current consumption are achieved.
Patent Information
- Application Number
- CN202011517348.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-12-21
AI Technical Summary
In the process of reducing the size of semiconductor devices, it is difficult to improve quality, yield and reliability, especially in terms of reducing coupling capacitance and operating current consumption.
A semiconductor element is designed that uses a porous dielectric structure. By forming a porous intermediate layer and spacers on the substrate, and setting a porous cover layer on the gate structure, combined with energy treatment of energy-removable materials, a 25% to 100% porosity structure to reduce coupling capacitance and operating current consumption.
It effectively reduces the resistance and capacitance delay and operating current consumption of semiconductor components, and improves the quality and reliability of components.
Smart Images

Figure CN113161352B_ABST
Abstract
Description
Technical Field
[0001] This application claims priority to and the benefit of U.S. Application No. 16 / 751,168, filed on January 23, 2020, the contents of which are incorporated herein by reference in their entirety.
[0002] The present disclosure relates to a semiconductor element and a method for preparing the semiconductor element, and more particularly to a semiconductor element having a porous dielectric structure and a method for preparing the semiconductor element having the porous dielectric structure. Background Art
[0003] Semiconductor components are used in various electronic applications, such as personal computers, mobile phones, digital cameras, or other electronic devices. The size of semiconductor components is gradually getting smaller to meet the increasing demand for computing power. However, during the process of decreasing size, different problems will increase. Therefore, there are still challenges in achieving improved quality, yield and reliability.
[0004] The above “prior art” description is only to provide background technology, and does not admit that the above “prior art” description reveals the subject matter of the present disclosure, does not constitute the prior art of the present disclosure, and any description of the above “prior art” should not be regarded as any part of this case. Summary of the invention
[0005] An embodiment of the present disclosure provides a semiconductor device, comprising a substrate; two conductive features, which are disposed away from each other and located on the substrate; and a porous middle layer, which is disposed between the two conductive features and adjacent to the two conductive features. A porosity of the porous middle layer is between 25% and 100%.
[0006] In some embodiments of the present disclosure, the porous intermediate layer comprises an energy-removable material, which is composed of a base material and a decomposable porogen material.
[0007] In some embodiments of the present disclosure, the base material includes silicon oxide, and the decomposable porogen material includes a plurality of compounds including a plurality of unsaturated bonds.
[0008] Another embodiment of the present disclosure provides a semiconductor device, including a substrate; a gate structure located on the substrate; two source / drain regions disposed adjacent to two sides of the gate structure; and two porous spacers disposed between the two source / drain regions and the gate structure and adjacent to the two conductive features. A porosity of the two porous spacers is between 25% and 100%.
[0009] In some embodiments of the present disclosure, the semiconductor device further includes a porous capping layer located on the gate structure and between the two porous interspacers. A porosity of the porous capping layer is between 25% and 100%.
[0010] In some embodiments of the present disclosure, the semiconductor device further includes two lower etching stop layers located under the two porous spacers.
[0011] In some embodiments of the present disclosure, the semiconductor device further includes a fin, and the fin is located between the gate structure and the substrate.
[0012] In some embodiments of the present disclosure, the fin includes a protrusion and two recessed portions, the two recessed portions are arranged adjacent to both sides of the protrusion, wherein a top surface of the protrusion is located on a vertical horizontal plane, which is higher than a vertical horizontal plane of the top surface of the recessed portion, the gate structure is located on the protrusion, and the two source / drain regions are located on the recessed portions.
[0013] In some embodiments of the present disclosure, the semiconductor device further includes a first termination layer located between the fin and the substrate.
[0014] In some embodiments of the present disclosure, the first termination layer has a thickness ranging from 1 nm to 50 nm.
[0015] In some embodiments of the present disclosure, the semiconductor device further includes a plurality of capping layers located on the two source / drain regions, and the plurality of capping layers are made of silicate metal.
[0016] In some embodiments of the present disclosure, the gate structure has a gate isolation layer, a gate conductive layer and a gate filling layer, the gate isolation layer is located on the protrusion, the gate conductive layer is located on the gate isolation layer, and the gate filling layer is located on the gate conductive layer.
[0017] In some embodiments of the present disclosure, the semiconductor device further comprises a plurality of contact points located on the plurality of cover layers, and the plurality of contact points are made of tungsten, copper, cobalt, ruthenium or molybdenum.
[0018] In some embodiments of the present disclosure, the semiconductor device further includes a plurality of contact pads located between the plurality of contact points and the plurality of cover layers, and the plurality of contact pads are made of nitride metal.
[0019] Another embodiment of the present disclosure provides a method for preparing a semiconductor device. The method includes: providing a substrate; forming two conductive features disposed away from each other on the substrate; forming a porous intermediate layer between the two conductive features and adjacent to the two conductive features; depositing an energy removable material between the two conductive features and adjacent to the two conductive features; and performing an energy treatment to convert the energy removable material into a porous intermediate layer. A porosity of the porous intermediate layer is between 25% and 100%.
[0020] In some embodiments of the present disclosure, the energy removable material includes a base material and a decomposable porogen material.
[0021] In some embodiments of the present disclosure, an energy source of the energy treatment is heat, light, or a combination thereof.
[0022] In some embodiments of the present disclosure, the base material includes methylsilsesquioxane or silicon oxide.
[0023] In some embodiments of the present disclosure, the method for preparing the semiconductor device further includes forming a first termination layer on the substrate. The first termination layer has a thickness ranging from 1 nm to 50 nm.
[0024] In some embodiments of the present disclosure, the method for preparing the semiconductor device further includes forming a plurality of fins on the first termination layer.
[0025] Due to the design of the semiconductor device disclosed in the present invention, a coupling capacitance between the gate structure and the source / drain region can be reduced; thus, the resistance capacitance delay (RC delay) of the semiconductor device can be reduced. In addition, due to the presence of the covering layer, an operating current consumption of the semiconductor device can be reduced.
[0026] The above has outlined the technical features and advantages of the present disclosure in a fairly broad manner, so that the detailed description of the present disclosure below can be better understood. Other technical features and advantages that constitute the subject matter of the claims of the present disclosure will be described below. Those with ordinary knowledge in the technical field to which the present disclosure belongs should understand that the concepts and specific embodiments disclosed below can be used to modify or design other structures or processes to achieve the same purpose as the present disclosure. Those with ordinary knowledge in the technical field to which the present disclosure belongs should also understand that such equivalent constructions cannot depart from the spirit and scope of the present disclosure as defined by the appended claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] A more comprehensive understanding of the disclosure of the present application may be obtained by referring to the embodiments and claims in conjunction with the accompanying drawings, in which the same reference numerals refer to the same elements.
[0028] Figure 1 FIG. 4 is a top view of a semiconductor device according to an embodiment of the present disclosure.
[0029] Figure 2 For along Figure 1 Schematic cross-sectional view along the middle section line AA'.
[0030] Figure 3 For along Figure 1 Schematic cross-sectional view along the section line BB'.
[0031] Figures 4 to 8 In some embodiments of the present disclosure, each semiconductor element is similar to Figure 2 Schematic cross-sectional view shown.
[0032] Fig. 9 FIG. 4 is a top view of a semiconductor device according to an embodiment of the present disclosure.
[0033] Fig.10 For along Fig. 9 Schematic cross-sectional view along the middle section line AA'.
[0034] Fig.11 The figure is a schematic flow chart of a method for preparing a semiconductor element according to an embodiment of the present disclosure.
[0035] Fig.12 FIG. 4 is a top view schematically showing a semiconductor device at an intermediate stage of a method for manufacturing the semiconductor device according to an embodiment of the present disclosure.
[0036] Fig.13 A part of the method for preparing the semiconductor device according to an embodiment of the present disclosure is provided. Fig.12 A schematic cross-sectional view of the section line A-A'.
[0037] Fig.14 A part of the method for preparing the semiconductor device according to an embodiment of the present disclosure is provided. Fig.12 A schematic cross-sectional view of the section line BB'.
[0038] Fig.15 FIG. 4 is a top view of a semiconductor device at an intermediate stage according to an embodiment of the present disclosure.
[0039] Fig.16 A part of the method for preparing the semiconductor device according to an embodiment of the present disclosure is provided. Fig.15 A schematic cross-sectional view of the section line A-A'.
[0040] Fig.17 A part of the method for preparing the semiconductor device according to an embodiment of the present disclosure is provided. Fig.15 A schematic cross-sectional view of the section line BB'.
[0041] Figure 18 to Figure 25 The various parts of the method for preparing the semiconductor element according to one embodiment of the present disclosure are as follows Fig.15 A schematic cross-sectional view of the section line A-A'.
[0042] Fig.26 FIG. 4 is a top view of a semiconductor device at an intermediate stage according to an embodiment of the present disclosure.
[0043] Fig. 27 A part of the method for preparing the semiconductor device according to an embodiment of the present disclosure is provided. Fig.26 A schematic cross-sectional view of the section line A-A'.
[0044] Fig.28 A part of the method for preparing the semiconductor device according to an embodiment of the present disclosure is provided. Fig.26 Schematic cross-sectional view of section line BB'.
[0045] Fig.29 FIG. 4 is a top view of a semiconductor device at an intermediate stage according to an embodiment of the present disclosure.
[0046] Figure 30 to Figure 35 The various parts of the method for preparing the semiconductor element according to one embodiment of the present disclosure are as follows Fig.29 A schematic cross-sectional view of the section line A-A'.
[0047] The reference numerals are described as follows:
[0048] 100A: Semiconductor components
[0049] 100B: Semiconductor components
[0050] 100C: Semiconductor components
[0051] 100D: Semiconductor components
[0052] 100E: Semiconductor components
[0053] 100F: Semiconductor components
[0054] 100G: Semiconductor Components
[0055] 101: Base
[0056] 103: First termination layer
[0057] 105: Insulation layer
[0058] 107: Fins
[0059] 107C: Fins
[0060] 107F: Fins
[0061] 107P: Protrusion
[0062] 107R: Depression
[0063] 201: Gate structure
[0064] 203: Gate isolation layer
[0065] 205: Gate conductive layer
[0066] 207: Gate filling layer
[0067] 209: Porous cap layer
[0068] 211: Lower etching stop layer
[0069] 213: Porous interstitial
[0070] 213B: Porous interstitial
[0071] 301: Source / drain region
[0072] 301C: Source / Drain Region
[0073] 301F: Source / Drain Region
[0074] 301G: Source / Drain Region
[0075] 303: Overlay
[0076] 303G: Covering layer
[0077] 305: Touchpoint
[0078] 307: Contact point pad
[0079] 401: First isolation layer
[0080] 403: Second isolation layer
[0081] 501: Dummy gate structure
[0082] 503: Dummy gate lower layer
[0083] 505: Virtual gate mask layer
[0084] 507: First virtual gap
[0085] 507R: Recessed
[0086] 509: Second virtual gap
[0087] 601: First virtual interstitial material
[0088] 603: Second virtual interstitial material
[0089] 605: Lower etch stop layer material
[0090] 607: Energy Removable Materials
[0091] 701: First groove
[0092] 703: Second groove
[0093] A: Etching mask
[0094] X: Direction
[0095] Y: direction
[0096] Z: Direction
[0097] 10: Preparation method
[0098] 20: Energy Processing
[0099] S11: Steps
[0100] S13: Steps
[0101] S15: Steps
[0102] S17: Steps
[0103] S19: Steps
[0104] S21: Steps
[0105] S23: Steps
[0106] S25: Steps
[0107] S27: Steps
[0108] S29: Steps
[0109] S31: Steps DETAILED DESCRIPTION
[0110] Specific examples of components and configurations are described below to simplify the embodiments of the present disclosure. Of course, these embodiments are for illustration only and are not intended to limit the scope of the present disclosure. For example, in the description, the first component is formed on the second component, which may include an embodiment in which the first and second components are in direct contact, and may also include an embodiment in which additional components are formed between the first and second components so that the first and second components are not in direct contact. In addition, the embodiments of the present disclosure may repeat reference numbers and / or letters in many examples. The purpose of these repetitions is to simplify and clarify, and unless otherwise specified in the text, they do not themselves represent a specific relationship between the various embodiments and / or the configurations discussed.
[0111] Additionally, for ease of description, spatially relative terms such as "beneath," "below," "lower," "above," "upper," etc. may be used herein to describe the relationship of one element or feature shown in the figures to another (other) element or feature. The spatially relative terms are intended to encompass different orientations of the elements in use or operation in addition to the orientation shown in the figures. The device may have other orientations (rotated 90 degrees or in other orientations) and the spatially relative descriptors used herein may be interpreted accordingly.
[0112] It should be understood that when forming a component on, connected to, and / or coupled to another component, it may include embodiments in which these components are in direct contact, and may also include embodiments in which additional components are formed between these components so that these components are not in direct contact.
[0113] It should be understood that although the terms first, second, third, etc. may be used herein to describe various elements, components, regions, layers, or sections, these elements, components, regions, layers, or sections are not limited by these terms. Instead, these terms are only used to distinguish one element, component, region, layer, or section from another region, layer, or section. Therefore, without departing from the teachings of the progressive conception of the present invention, the first element, component, region, layer, or section discussed below may be referred to as a second element, component, region, layer, or section.
[0114] Unless the context indicates otherwise, as used herein, terms such as "same," "equal," "planar," or "coplanar" when referring to orientation, layout, location, shapes, sizes, amounts, or other measures do not necessarily mean an exactly identical orientation, layout, location, shape, size, amount, or other measure, but rather mean nearly identical orientation, layout, location, shape, size, amount, or other measure within acceptable variances that may occur, for example, due to manufacturing processes. The term "substantially" may be used herein to convey this meaning. For example, terms such as substantially the same, substantially equal, or substantially planar mean exactly the same, equal, or planar, or they may be the same, equal, or planar within an acceptable variance, and, for example, the acceptable variance may occur due to a manufacturing process.
[0115] In the present disclosure, a semiconductor device generally refers to a device that can operate by utilizing semiconductor characteristics, and an electro-optic device, a light-emitting display device, a semiconductor circuit, and an electronic device are all included in the category of semiconductor devices.
[0116] It should be understood that in the description of the present disclosure, above (or up) is the direction corresponding to the Z-direction arrow, and below (or down) is the relative direction corresponding to the Z-direction arrow.
[0117] Figure 1 FIG. 1 is a top view of a semiconductor device 100A according to an embodiment of the present disclosure. Figure 2 For along Figure 1 Schematic cross-sectional view along the middle section line AA'. Figure 3 For along Figure 1 For the sake of clarity, some components of the semiconductor device 100A of the present disclosure are not shown. Figure 1 middle.
[0118] Please refer to Figures 1 to 3 In the described embodiment, the semiconductor element 100A may include a substrate 101, a first stop layer 103, an insulating layer 105, a plurality of fins 107, a plurality of gate structures 201, a plurality of lower etching stop layers 211, a plurality of porous spacers 213, a plurality of source / drain regions 301, a plurality of capping layers 303, a plurality of contact points 305, a first isolation layer 401 and a second isolation layer 403.
[0119] Please refer to Figures 1 to 3 In the described embodiment, for example, the substrate 101 may be formed of the following materials: silicon, silicon carbide, germanium silicon germanium, gallium arsenic, indium arsenide, indium, or other semiconductor materials including group III, group IV, or group V. The substrate 101 may include a silicon-on-insulator structure. For example, the substrate 101 may include a buried oxide layer formed using a process such as separation by implanted oxygen.
[0120] Please refer to Figures 1 to 3 In the embodiment described, the first termination layer 103 may be disposed on the substrate 101. The first termination layer 103 may have a thickness ranging from 1 nm to 50 nm. For example, the first termination layer 103 may be made of silicon germanium, silicon oxide, silicon germanium oxide, silicon phosphide or silicophosphates.
[0121] Please refer to Figures 1 to 3In the embodiment described, a plurality of fins 107 may be disposed on the first termination layer 103. The plurality of fins 107 may provide a plurality of active regions, which are used to be located in channels formed by the semiconductor device 100A according to voltages applied to the plurality of gate structures 201. Each fin 107 may extend along a first direction X. The plurality of fins 107 may be spaced apart from each other along a second direction Y, and the second direction Y intersects the first direction X. Each fin 107 may protrude from the first termination layer 103 in a direction Z, and the direction Z is perpendicular to the first direction X and the second direction Y. Each fin 107 may include a protrusion 107P and two recesses 107R. The protrusion 107P may be disposed on the first termination layer 103 and extend along the first direction X. The two recesses 107R may be disposed corresponding to two sides of the adjacent protrusion 107P, respectively. A top surface of the protrusion 107P may be in a vertical horizontal plane, which is a vertical plane higher than the top surface of the recess 107R. For example, the plurality of fins 107 may be made of silicon, silicon carbide, silicon germanium, gallium arsenide, indium arsenide, indium, or other semiconductor materials including group III, group IV, or group V components.
[0122] It should be understood that the plurality of fins 107 include three fins, but the number of fins is not limited thereto. For example, the number of fins 107 may be less than three or greater than three.
[0123] Alternatively, in other embodiments, the semiconductor device may include a plurality of nanowires to replace the plurality of fins 107 to provide the active region.
[0124] Please refer to Figures 1 to 3 In the embodiment described, the insulating layer 105 may be disposed on the first termination layer 103 and may be located between the plurality of fins 107. The top surface of the insulating layer 105 may be located at the same vertical level as the recessed portion 107R. The insulating layer 105 may insulate the plurality of fins 107 from each other to prevent electrical leakage between adjacent semiconductor components. For example, the insulating layer 105 may be made of silicon nitride, silicon oxide, silicon oxynitride, or silicon nitride oxide.
[0125] It should be understood that in the present disclosure, silicon oxynitride refers to a substance containing silicon, nitrogen and oxygen, wherein a proportion of oxygen is greater than a proportion of nitrogen. Silicon nitride oxide refers to a substance containing silicon, nitrogen and oxygen, wherein a proportion of nitrogen is greater than a proportion of oxygen.
[0126] Please refer to Figures 1 to 3In the embodiment, the plurality of gate structures 201 may be disposed on the plurality of fins 107 and the insulating layer 105. Each gate structure 201 may extend along a direction Y. In other words, from a top view, the plurality of gate structures 201 may penetrate the plurality of fins 107. The plurality of gate structures 201 may be spaced apart from each other along a first direction X. Each gate structure 201 may include a gate isolation layer 203, a gate conductive layer 205, and a gate filling layer 207.
[0127] Please refer to Figures 1 to 3In the described embodiment, the gate isolation layer 203 may have a U-shaped cross-sectional profile. The gate isolation layer 203 may be disposed on a top surface of the protrusion 107P. The gate isolation layer 203 may have a thickness ranging from 0.5 nm to 5.0 nm. In some embodiments, the thickness of the gate isolation layer 203 may be between 0.5 nm and 2.5 nm. For example, the gate isolation layer 203 may be made of a material with a high dielectric constant, such as metal oxide, metal nitride, metal silicate, transition metal-oxide, transition metal-nitride, transition metal-silicate, oxynitride of metal, metal aluminate, zirconium silicate, zirconium aluminate, or a combination thereof. In particular, the gate isolation layer 203 may be made of hafnium oxide, hafnium silicon oxide, hafnium silicon oxynitride, hafnium tantalum oxide, hafnium titanium oxide, hafnium zirconium oxide, hafnium lanthanum oxide, lanthanum oxide, zirconium oxide, titanium oxide, tantalum oxide, yttrium oxide, strontium titanium oxide, barium titanium oxide, barium zirconium oxide, lanthanum silicon oxide, aluminum silicon oxide, aluminum oxide, silicon nitride, silicon oxynitride, silicon nitride oxide, or a combination thereof. In other embodiments, for example, the gate isolation layer 203 may be a multi-layer structure including a layer of silicon oxide and another layer of a high dielectric constant material.
[0128] Please refer to Figures 1 to 3In the embodiment described, the gate conductive layer 205 may have a U-shaped cross-sectional profile. The gate conductive layer 205 may be disposed on the gate isolation layer 203. The gate conductive layer 205 may have a thickness between arrive . The top surface of the gate conductive layer 205 may be located at the same vertical level as the top surface of the gate isolation layer 203. For example, the gate conductive layer 205 may be made of a conductive material, such as polysilicon, polysilicon germanium, metal nitride, metal silicide, metal oxide, metal or a combination thereof. For example, the metal nitride may be tungsten nitride, molybdenum nitride, titanium nitride or tantalum nitride. For example, the metal silicide may be tungsten silicide, titanium silicide, cobalt silicide, nickel silicide, platinum silicide or erbium silicide. For example, the metal oxide may be ruthenium oxide or indium tin oxide. For example, the metal may be tungsten, titanium, aluminum, copper, molybdenum, nickel or platinum. The gate conductive layer 205 may be used to adjust a work function of the gate structure 201.
[0129] Please refer to Figures 1 to 3 In the embodiment described, the gate filling layer 207 may be disposed on the gate conductive layer 205. A top surface of the gate filling layer 207 may be located at the same vertical level as the top surface of the gate conductive layer 205. For example, the gate filling layer 207 may be made of tungsten or aluminum. The gate filling layer 207 may be used to fill a space formed by the gate conductive layer 205.
[0130] Please refer to Figures 1 to 3 In the described embodiment, for each gate structure 201, the second lower etch stop layer 211 may be disposed on the top surface of the protrusion 107P. The second lower etch stop layer 211 may be disposed corresponding to the lower portion of both sides of the adjacent gate structure 201, respectively. In particular, the second lower etch stop layer 211 may be disposed adjacent to the lower portion of the side wall of the gate isolation layer 203. The side wall of the gate isolation layer 203 may be disposed relative to the gate conductive layer 205. The top surface of the second lower etch stop layer 211 may be located in a vertical horizontal plane, which is a vertical horizontal plane lower than the top surface of the gate isolation layer 203. It should be understood that the second lower etch stop layer 211 may extend along the second direction Y (for clarity, this embodiment is not shown). Figure 1 ). For example, the second lower etch stop layer 211 may be made of carbon-doped oxide, carbon incorporated silicon oxide, ornithine decarboxylase, or nitrogen-doped silicon carbide.
[0131] Please refer to Figures 1 to 3 In the described embodiment, a plurality of porous spacers 213 may be disposed adjacent to the sides of a plurality of gate structures 201. From a top view, the plurality of porous spacers 213 may extend along the second direction Y. For each gate structure 201, two porous spacers 213 may be disposed adjacent to both sides of the gate structure 201. The two porous spacers 213 may be disposed on two lower etching stop layers 211, respectively. The top surfaces of the two porous spacers 213 may be located at the same vertical level as the top surface of the gate isolation layer 203. The two porous spacers 213 may be made of an energy-removable material, which will be described in detail later. For each porous spacer 213, the porous spacer 213 may include a skeleton and a plurality of empty spaces, the plurality of empty spaces being disposed between the skeletons. The plurality of empty spaces may be interconnected and may be filled with air. For example, the skeleton may contain silicon oxide or methylsilsesquioxane. The two porous spacers 213 may have a porosity ranging from 25% to 100%. It should be understood that when the porosity is 100%, it means that the porous spacers 213 only include an empty space, and the porous spacers can be regarded as an air gap. In some embodiments, the porosity of the two porous spacers 213 may be between 45% and 95%. Multiple porous spacers 213 can be used to electrically insulate multiple gate structures 201 from other conductive features, such as multiple source / drain regions 301. In addition, multiple empty spaces of the porous spacers 213 can be filled with air. As a result, a dielectric constant of the porous spacers 213 can be much lower than that of a spacer, for example, the spacer can be made of silicon oxide. Therefore, the porous spacers 213 can greatly reduce the parasitic capacitance between the gate structure 201 and adjacent conductive features, such as multiple source / drain regions 301. That is, the porous spacers 213 can greatly reduce an interference effect between electronic signals generated by or applied to the gate structure.
[0132] The energy-removable material may include a material such as a thermal decomposable material, a photonic decomposable material, an e-beam decomposable material, or a combination thereof. For example, the energy-decomposable material may include a base material and a decomposable porogen material that is sacrificially removed in response to exposure to an energy source.
[0133] from Figure 1 From a top view in FIG. 1 , the plurality of source / drain regions 301 can be respectively disposed corresponding to the sides of the plurality of gate structures 201 and sandwiched between the plurality of porous spacers 213. Figure 2 From a cross-sectional view in FIG. 1 , the source / drain region 301 may be disposed on the top surface of the recessed portion 107R. The top surface of the source / drain region 301 may be located at a vertical level, which is lower than the vertical level of the top surface of the two porous spacers 213. The vertical level of the top surface of the source / drain region 301 may be higher than the vertical level of the top surface of the two lower etching stop layers 211. Figure 3 From another cross-sectional view of , the source / drain region 301 may have a pentagonal shape. The bottom of the source / drain region 301 may have a width that is the same as the top surface of the recessed portion 107R. For example, the multiple source / drain regions 301 may be made of silicon germanium or silicon carbide. Silicon germanium has a lattice constant greater than silicon. Silicon carbide has a lattice constant less than silicon. The multiple source / drain regions 301 made of silicon germanium or silicon carbide may apply a compressive or elongated stress to the multiple fins 107 to improve the mobility of multiple carriers in the channel.
[0134] Please refer to Figures 1 to 3 In the embodiment described, the plurality of capping layers 303 may be disposed on the plurality of source / drain regions 301 respectively. The top surfaces of the plurality of capping layers 303 may be on a vertical plane, which is located between the vertical plane of the top surfaces of the two porous spacers 213 and the vertical plane of the top surfaces of the two lower etching stop layers 211. Figure 3From a cross-sectional view in FIG. 1 , the capping layer 303 may be disposed on the outer surface of the source / drain region 301, but excludes the bottom of the source / drain region 301. For example, the plurality of capping layers 303 may be made of titanium silicide, nickel silicide, nickel platinum silicide, tantalum silicide, or cobalt silicide. The plurality of capping layers 303 may be used to reduce the contact resistance between the plurality of source / drain regions 301 and the plurality of contact points 305, which will be described later. In addition, the plurality of capping layers 303 have a lower resistance than the plurality of source / drain regions 301. Therefore, in the operation of a semiconductor element 100A, most of a current may flow through the capping layer 303 to reach the fin 107, and only a small portion of the current may flow through the source / drain region 301 to reach the fin 107. As a result, the operating current consumption of the semiconductor element 100A may be low.
[0135] Please refer to Figures 1 to 3 In the embodiment described, the first isolation layer 401 may be disposed on the plurality of capping layers 303 and the insulating layer 105. The first isolation layer 401 may be disposed around the plurality of capping layers 303 and the upper portion of the sidewalls of the plurality of porous spacers 213. For example, the first isolation layer 401 may be made of silicon oxynitride, silicon nitride oxide, silicon carbide, silicon oxide, or silicon nitride. Alternatively, in other embodiments, for example, the first isolation layer 401 may be made of a low dielectric constant dielectric material having atoms of Si, C, O, B, N, or H. For example, the dielectric constant of the low dielectric constant dielectric material may be between 2.4 and 3.5, depending on the mole fraction of the aforementioned atoms. The first isolation layer 401 may have a mechanical strength that is sufficient to support the plurality of porous spacers 213 or prevent the plurality of porous spacers 213 from collapsing.
[0136] Please refer to Figures 1 to 3 In the embodiment described above, the second isolation layer 403 may be disposed on the first isolation layer 401 and the plurality of gate structures 201. The second isolation layer 403 may be made of the same material as the first isolation layer 401, but is not limited thereto.
[0137] Please refer to Figures 1 to 3 In the embodiment, the plurality of contact points 305 can be disposed through the second isolation layer 403 and the first isolation layer 401, and respectively disposed on the plurality of cover layers 303. For example, the plurality of contact points 305 can be made of tungsten, copper, cobalt, ruthenium or molybdenum.
[0138] Figures 4 to 8 In some embodiments of the present disclosure, each semiconductor element 100B, 100C, 100D, 100E, 100F is similar to Figure 2 Schematic cross-sectional view shown. Fig. 9 FIG. 1 is a top view of a semiconductor device 100G according to an embodiment of the present disclosure. Fig.10 For along Fig. 9 Schematic cross-sectional view along the middle section line AA'.
[0139] Please refer to Figure 4 In the semiconductor device 100B, two porous spacers 213B may be disposed on a top surface of the protrusion 107P. Figure 5 In the semiconductor device 100C, each fin 107C may not have a recessed portion. The source / drain region 301C may be located at the same vertical level as a vertical level of a bottom of the gate isolation layer 203 .
[0140] Please refer to Figure 6 , the semiconductor device 100D may include a porous capping layer 209. The porous capping layer 209 may be disposed on the top surface of the gate isolation layer 203, the top surface of the gate conductive layer 205, and the top surface of the gate filling layer 207. The porous capping layer 209 may be disposed between two porous spacers 213 and below the second isolation layer 403. The porous capping layer 209 may have a porosity ranging from 25% to 100%. In some embodiments, the porosity of the porous capping layer 209 may be between 45% and 95%. The porous capping layer 209 may have the same structural features as the porous spacers 213, and may greatly reduce the parasitic capacitance between the gate structure 201 and the conductive features located above the gate structure 201.
[0141] Please refer to Figure 7 , the semiconductor device 100E may include a plurality of contact pads 307. The plurality of contact pads 307 may be respectively disposed between the plurality of contacts 305 and the plurality of cover layers 303. During the formation of the contacts 305, the contact pads 307 may serve as a protective layer for the underlying structure (e.g., the cover layer 303 and the source / drain region 301). The contact pads 307 may also serve as an adhesive layer between the contacts 305 and the cover layer 303 or between the contacts 305 and the source / drain region 301.
[0142] Please refer to Figure 8 In the semiconductor device 100F, each fin 107F may not have a recessed portion. The source / drain region 301F may be disposed in the fin 107F and respectively disposed corresponding to the two adjacent porous spacers 213. The source / drain region 301F may include silicon doped with a dopant or silicon germanium doped with a dopant. The dopant may be phosphorus, arsenic, antimony, boron or indium.
[0143] Please refer to Fig. 9 and Fig.10 In the semiconductor device 100G, the source / drain region 301G may have a square shape. The capping layer 303G may be disposed on a portion of a bottom of the source / drain region 301, a portion of a sidewall of the source / drain region 301, and a portion of a top surface of the source / drain region 301. Alternatively, in other embodiments, the source / drain region 301 may have a rectangular shape, a diamond shape, a circular shape, or a shape having more than five sides.
[0144] It should be understood that the terms "forming", "formed" and "form" may refer to and include any method of creating, building, patterning, implanting or depositing an element, a dopant or a material. Examples of preparation methods may include, but are not limited to, atomic layer deposition, chemical vapor deposition, physical vapor deposition, sputtering, co-sputtering, spin coating, diffusion, deposition, growing, implantation, lithography, dry etching and wet etching.
[0145] Fig.11 FIG. 1 is a schematic flow chart of a method 10 for manufacturing a semiconductor device 100A according to an embodiment of the present disclosure. Fig.12 FIG. 4 is a top view schematically showing a semiconductor device at an intermediate stage of a method for manufacturing the semiconductor device according to an embodiment of the present disclosure. Fig.13 A part of the method for preparing the semiconductor device 100A according to an embodiment of the present disclosure is shown in FIG. Fig.12 A schematic cross-sectional view of the section line A-A'. Fig.14 A part of the method for preparing the semiconductor device 100A according to an embodiment of the present disclosure is shown in FIG. Fig.12 Schematic cross-sectional view of section line BB'.
[0146] Please refer to Fig.11 To Fig.14, in step S11, in the described embodiment, a substrate 101 may be provided, and a first stop layer 103, an insulating layer 105, and a plurality of fins 107 may be formed on the substrate 101. The first stop layer 103 may be formed on the substrate 101. A semiconductor layer (not shown) may be formed on the first stop layer 1036 and may be etched until a top surface of the first stop layer 103 is exposed to form a plurality of fins 107. Because the etching process stops at the top surface of the first stop layer 103, a height of the plurality of fins 107 may be nearly equal to a thickness of the semiconductor layer, so that the thickness of the semiconductor layer may be effectively controlled. Therefore, the height of the plurality of fins 107 and the channel width of the semiconductor device 100A may be effectively controlled according to the requirements of the circuit design, thereby obtaining good device performance.
[0147] For example, the semiconductor layer may be a silicon layer and may be epitaxially grown on the first termination layer 103. In some embodiments, a layer of photoresist material (not shown) may be deposited on the semiconductor layer and may be patterned and developed to remove a portion of the photoresist material. The remaining photoresist material may protect the underlying material during a subsequent semiconductor process, such as an etching process. It should be understood that other masks, such as a silicon oxide mask or a silicon nitride mask, may also be used in the etching process.
[0148] Please refer to Fig.14 , an isolation material such as silicon nitride, silicon oxide, silicon oxynitride or silicon nitride oxide may be deposited to fill the trenches between the plurality of fins 107 and form the insulating layer 105. The upper portion of the insulating layer 105 may be recessed to expose the upper portions of the plurality of fins 107. A recess process may include a selective etching process.
[0149] Fig.15 FIG. 4 is a top view of a semiconductor device at an intermediate stage according to an embodiment of the present disclosure. Fig.16 A part of the method for preparing the semiconductor device 100A according to an embodiment of the present disclosure is shown in FIG. Fig.15 A schematic cross-sectional view of the section line A-A'. Fig.17 A part of the method for preparing the semiconductor device 100A according to an embodiment of the present disclosure is shown in FIG. Fig.15 A schematic cross-sectional view of the section line BB'. Figure 18 to Figure 25 The following is a diagram of the various parts of the method for preparing the semiconductor device 100A according to an embodiment of the present disclosure. Fig.15 A schematic cross-sectional view of the section line A-A'.
[0150] Please refer to Fig.11 as well as Figure 15 to Figure 17In step S13, in the embodiment described, a plurality of dummy gate structures 501 may be formed on the insulating layer 105 and the plurality of fins 107. Each dummy gate structure 501 may include a dummy gate lower layer 503 and a dummy gate mask layer 505. The dummy gate lower layer 503 may be formed on the insulating layer 105 and the plurality of fins 107. For example, the dummy gate lower layer 503 may be made of polysilicon. The dummy gate mask layer 505 may be formed on the dummy gate lower layer 503. For example, the dummy gate mask layer 505 may be made of silicon nitride, silicon oxynitride, silicon nitride oxide, aluminum oxide, or zirconium oxide.
[0151] Please refer to Fig.11 , Fig.18 and Fig.19 In step S15, in the embodiment described above, a plurality of first dummy spacers 507 and a plurality of second dummy spacers 509 may be disposed adjacent to the dummy gate structure 501. Fig.18 , a layer of a first dummy spacer material 601 may be formed to cover the fin 107, the sidewalls of the dummy gate lower layer 503, the sidewalls of the dummy gate mask layer 505, and a top surface of the dummy gate mask layer 505. For example, the first dummy spacer material 601 may be silicon oxide, silicon nitride, silicon oxynitride, silicon nitride oxide, aluminum oxide, or zirconium oxide. A layer of a second dummy spacer material 603 may be formed to cover the layer of the first dummy spacer material 601. For example, the second dummy spacer material 603 may be silicon oxide, silicon nitride, silicon oxynitride, silicon nitride oxide, aluminum oxide, or zirconium oxide. The first dummy spacer material 601 may be different from the second dummy spacer material 603.
[0152] Please refer to Fig.19 , a first etching process may be performed to remove portions of the second dummy spacer material 603 and form two second dummy spacers 509 disposed adjacent to the dummy gate structure 501. The first etching process may have a first etching selectivity for the second dummy spacer material 603. The selectivity of an etching process may generally be expressed as a ratio of etching rates. For example, if one material is etched 25 times faster than the other material, the etching process may be described as having an etching rate of 25:1 or simply 25. In this regard, a higher ratio or value indicates a more selective etching process. In the first etching process, an etching rate for the second dummy spacer material 603 may be greater than an etching rate of the first dummy spacer material 601, an etching rate of the dummy gate mask layer 505, and an etching rate of the fin 107. The selectivity of the first etching process may be greater than or equal to 10, greater than or equal to 20, or greater than or equal to 25.
[0153] Please refer to Fig.19, a second etching process may be performed to remove portions of the first dummy spacer material 601 and form two first dummy spacers 507 disposed adjacent to the dummy gate structure 501. The second etching process may have an etching selectivity for the first dummy spacer material 601. In the second etching process, an etching rate of the first dummy spacer material 601 may be greater than an etching rate of the second dummy spacer material 603, an etching rate of the dummy gate mask layer 505, and an etching rate of the fin 107. The selectivity of the second etching process may be greater than or equal to 10, greater than or equal to 12, greater than or equal to 15, greater than or equal to 20, or greater than or equal to 25.
[0154] Please refer to Fig.11 as well as Figure 20 to Figure 22 In step S17, in the embodiment described above, two lower etching stop layers 211 may be formed under the two first dummy spacers 507, respectively. Fig. 20 , the second dummy spacer 509 can be used as an etching mask A. A lateral recess process can be performed to remove a portion of the two first dummy spacers 507 and simultaneously form a plurality of recessed portions 507R of the first dummy spacers. For example, the lateral recess process can be an isotropic wet etching process.
[0155] Please refer to Fig.21 , a layer of a lower etch stop layer material 605 may be deposited in the recess 507R of the first dummy spacer 507 and located on the two first dummy spacers 507, the two second dummy spacers 509 and the dummy gate mask layer 505. For example, the lower etch stop layer material 605 may be carbon-doped oxide, carbon incorporated silicon oxide, ornithine decarboxylase or nitrogen-doped silicon carbide. For example, chemical vapor deposition, plasma enhanced chemical vapor deposition, atomic layer deposition, physical vapor deposition or spin-on deposition may be used to perform the deposition of the layer of the lower etch stop layer material 605. Please refer to Fig. 22, an etch-back process may be performed to remove a portion of the layer of lower etch stop material 605 and simultaneously form the second lower etch stop layer 211. The etch-back process may be an anisotropic etching process, such as reactive ion etching or wet etching. Etch-back processes are generally difficult to control with precision. However, during the etch-back process, the second dummy spacers 509 may protect the first dummy spacers 507 so that the lengths of the features may be precisely controlled and consistently produced.
[0156] Please refer to Fig.11 , Fig.23 as well as Fig.24 In step S19, in the embodiment described above, the two second dummy spacers 509 may be removed, and the plurality of fins 107 may be recessed. Fig.23 , the two second dummy spacers 509 can be removed by the first etching process. In the first etching process, an etching rate for the two second dummy spacers 509 can be greater than an etching rate for the two first dummy spacers 507, an etching rate for the dummy gate mask layer 505, an etching rate for the two lower etching stop layers 211, and an etching rate for the fin 107. Please refer to Fig.24 , a second etching process may be performed to recess a portion of the fin 107 adjacent to the side of the gate structure 201. After the second etching process, the fin 107 may include a protrusion 107P and a plurality of recesses 107R, and the recesses 107R are disposed adjacent to the protrusion 107P. In the second etching process, an etching rate for the fin 107 may be greater than an etching rate of the two first dummy spacers 507, an etching rate of the dummy gate mask layer 505, and an etching rate of the two lower etching stop layers 211.
[0157] Please refer to Fig.11 as well as Fig.25In step S21, in the embodiment, a plurality of source / drain regions 301 may be formed on the recessed portions 107R respectively and disposed adjacent to the plurality of dummy gate structures 501. The plurality of source / drain regions 301 may be formed by an epitaxial growth process. During the epitaxial growth process, the plurality of source / drain regions 301 may be doped in-situ, or after the epitaxial growth, the plurality of source / drain regions 301 may be doped by an implantation process. The plurality of source / drain regions 301 may include silicon and dopants, such as phosphorus, arsenic, antimony, boron, or indium. The plurality of source / drain regions 301 may have a doping concentration ranging from 1E19 atoms / cm3 to 5E21 atoms / cm3. An annealing process may be performed to activate the plurality of source / drain regions 301. The annealing process may have a process temperature ranging from 800°C to 1250°C. The annealing process may have a process duration between 1 millisecond and 500 milliseconds. For example, the annealing process may be a rapid thermal anneal, a laser spike anneal, or a flash lamp anneal.
[0158] Fig.26 FIG. 4 is a top view of a semiconductor device at an intermediate stage according to an embodiment of the present disclosure. Fig. 27 A part of the method for preparing the semiconductor device 100A according to an embodiment of the present disclosure is shown in FIG. Fig.26 A schematic cross-sectional view of the section line A-A'. Fig.28 A part of the method for preparing the semiconductor device 100A according to an embodiment of the present disclosure is shown in FIG. Fig.26 A schematic cross-sectional view of the section line BB'.
[0159] Please refer to Fig.11 , Fig. 27 and Fig.28In step S23, in the embodiment described, a plurality of capping layers 303 may be formed on the plurality of source / drain regions 301 respectively, and a first isolation layer 401 may be formed on the plurality of capping layers 303 and the insulating layer 105. For the formation of the plurality of capping layers 303, a metal layer may be deposited on the plurality of source / drain regions 301, and a heat treatment may be performed. For example, the metal layer may include titanium, nickel, platinum, tantalum, or cobalt. During the heat treatment, metal atoms of the metal layer may chemically react with silicon atoms of the plurality of source / drain regions 301 to form the plurality of capping layers 303. The plurality of capping layers 303 may include titanium silicide, nickel silicide, nickel platinum silicide, tantalum silicide, or cobalt silicide. The heat treatment may be a dynamic surface annealing process, and may cause a shallow-depth region of the source / drain region 301 to reach a silicidation temperature. After the heat treatment, a cleaning process may be performed to remove the unreacted metal layer. The cleaning process may use an etchant, such as hydrogen peroxide and a standard cleaning solution 1 (SC-1 solution).
[0160] Please refer to Fig. 27 and Fig.28 , an isolation material may be deposited on the plurality of capping layers 303, the insulating layer 305, the plurality of dummy gate structures 501, and the first dummy spacer 507. The deposition process may be chemical vapor deposition, plasma enhanced chemical vapor deposition, or sputtering deposition. The isolation material has a dielectric constant between 2.4 and 3.5. In order to remove excess material, provide a substantially flat surface for subsequent processing steps, and simultaneously form the first isolation layer 401, a planarization process, such as chemical mechanical polishing, may be performed until a top surface of the dummy gate mask layer 505 is exposed.
[0161] Fig.29 FIG. 4 is a top view of a semiconductor device at an intermediate stage according to an embodiment of the present disclosure. Figure 30 to Figure 35 The following is a diagram of the various parts of the method for preparing the semiconductor device 100A according to an embodiment of the present disclosure. Fig.29 A schematic cross-sectional view of the section line A-A'.
[0162] Please refer to Fig.11 as well as Figure 29 to Figure 31 In step S25, in the embodiment described above, the plurality of dummy gate structures 501 may be removed, and the plurality of gate structures 201 may be formed in situ. Fig.29 and Fig.30, the dummy gate mask layer 505 and the dummy gate lower layer 503 can be removed by a multi-step etching process. After removing the dummy gate structure 501, a first trench 701 can be formed in situ; in other words, the first trench 701 can be formed at the location previously occupied by the dummy gate structure 501. Please refer to Fig.31 , the gate structure 201 may be formed in the first trench 701. The gate structure 201 may include a gate isolation layer 203, a gate conductive layer 205, and a gate filling layer 207. The gate isolation layer 203 may be formed in the first trench 701 by a deposition process, such as chemical vapor deposition, physical vapor deposition, atomic layer deposition, thermal treatment, ozone oxidation, or a combination thereof.
[0163] Please refer to Fig.31 The gate conductive layer 205 may be formed on the gate isolation layer 203 by other deposition processes suitable for depositing conductive materials, such as chemical vapor deposition or sputtering deposition. The gate filling layer 207 may be formed on the gate conductive layer 205 by other deposition processes similar to the deposition of the gate conductive layer 205. A planarization process, such as chemical mechanical polishing, may be performed to provide a substantially planar surface for subsequent processing steps.
[0164] Please refer to Fig.11 as well as Fig.23 In step S27, in the embodiment described, the two first dummy spacers 507 may be removed, and the plurality of second trenches 703 may be formed in-situ. The two first dummy spacers 507 may be removed by an etching process. Before the etching process, a gate mask layer (not shown) may be formed on the gate structure 201 to protect the gate structure 201. In the etching process, an etching rate of the two first dummy spacers 507 may be greater than an etching rate of the first isolation layer 401, an etching rate of the gate mask layer, and an etching rate of the two lower etching stop layers 211.
[0165] Please refer to Fig.11 , Fig.33 as well as Fig.34 In step S29, in the embodiment described above, an energy removable material 607 may be deposited in the second trench 703, and an energy treatment 20 may be performed to form two porous interstitials 213 in the second trench 703. Please refer to Fig.33, an energy removable material 607 may be deposited in the second groove 703. The energy removable material 703 may include a material, such as a thermal decomposable material, a photonic decomposable material, an e-beam decomposable material, or a combination thereof. For example, the energy removable material may include a base material and a decomposable porogen material, and the decomposable porogen material is sacrificially removable based on an energy source to which it is exposed. The base material may include a methylsilsesquioxane based material. The decomposable porogen material may include a porogen organic mixture, which is a base material that provides porosity to the energy removable material. An energy source may be provided to Fig.33 The energy treatment 20 may be performed to remove the semiconductor device at an intermediate stage in the process. The energy source may include heat, light, or a combination thereof. When heat is used as the energy source, a temperature of the energy treatment may be between 800° C. and 900° C. When light is used as the energy source, an ultraviolet light may be provided. The energy treatment 20 may remove the decomposable porogen material from the energy removable material to create empty spaces (porous) where the base material remains.
[0166] Alternatively, in other embodiments, the base material may be silicon oxide. The decomposable porogen material may include a plurality of compounds including unsaturated dangling bonds, such as double dangling bonds or triple dangling bonds. During the energy treatment 20, the unsaturated dangling bonds of the decomposable porogen material may cross-link the silicon oxide of the base material. As a result, the decomposable porogen material may shrink and create a plurality of empty spaces where the base material remains. The empty spaces may be filled with air so that a dielectric constant of the empty spaces may be very low.
[0167] In some embodiments, the energy removable material may include a relatively high concentration of decomposable porous material and a relatively low concentration of base material, but is not limited thereto. For example, the energy removable material 607 may include 75% or more of the decomposable porous material and 25% or less of the base material. In other embodiments, the energy removable material 607 may include 95% or more of the decomposable porous material and 5% or less of the base material. In another embodiment, the energy removable material 607 may include 100% of the decomposable porous material and no base material. In another embodiment, the energy removable material 607 may include 45% or more of the decomposable porous material and 55% or less of the base material.
[0168] Please refer to Fig.34 After the energy treatment 20, the energy removable material 607 in the second trench 703 may be transformed into two porous intersperses 213. The base material may be transformed into a skeleton of the two porous intersperses 213, and the empty spaces may be dispersed between the skeletons of the two porous intersperses 213. Depending on the composition structure of the energy removable material 607, the two porous intersperses 213 may have a porosity of 45%, 75%, 95% or 100%. After the energy treatment 20, a planarization process, such as chemical mechanical polishing, may be performed to provide a substantially flat surface for subsequent processing steps.
[0169] Please refer to Fig.11 as well as Fig.35 , in step S31, in the described embodiment, a second isolation layer 403 may be formed on the first isolation layer 401, and a plurality of contact points 305 may be formed on the plurality of capping layers 303 respectively. The second isolation layer 403 may be formed by a process similar to that of forming the first isolation layer 401. A lithography process may be performed to define the positions of the plurality of contact points 305. After the lithography process, an etching process, such as an anisotropic dry etching process, may be performed to form a plurality of contact point openings penetrating the second isolation layer 403 and the first isolation layer 401. A deposition material may be deposited in the plurality of contact point openings by a deposition process, the deposition material being, for example, tungsten, copper, cobalt, ruthenium or molybdenum. After the deposition process, a planarization process, such as chemical mechanical polishing, may be performed to remove excess material, provide a substantially flat surface for subsequent processing steps, and simultaneously form a plurality of contact points 305.
[0170] Due to the design of the semiconductor device disclosed in the present invention, a coupling capacitance between the gate structure 201 and the source / drain region 301 can be reduced; thus, the resistance-capacitance delay (RC delay) of the semiconductor device 100A can be reduced.
[0171] Although the present disclosure and its advantages have been described in detail, it should be understood that various changes, substitutions and replacements may be made without departing from the spirit and scope of the present disclosure as defined in the claims. For example, many of the above processes may be implemented in different ways, and other processes or combinations thereof may be used to replace many of the above processes.
[0172] Furthermore, the scope of the present application is not limited to the specific embodiments of the processes, machines, manufactures, compositions of matter, means, methods, and steps described in the specification. A person skilled in the art can understand from the disclosure of the present disclosure that existing or future developed processes, machines, manufactures, compositions of matter, means, methods, or steps that have the same functions or achieve substantially the same results as the corresponding embodiments described herein can be used according to the present disclosure. Accordingly, such processes, machines, manufactures, compositions of matter, means, methods, or steps are included in the claims of the present application.
Claims
1. A semiconductor element, comprising: a base; a first stop layer located on the substrate, wherein the first stop layer has a thickness ranging from 1 nm to 50 nm; A plurality of fins are located on the first termination layer; an isolation layer located on the first termination layer and between the plurality of fins; A plurality of gate structures are disposed on the plurality of fins and the isolation layer, wherein two porous spacers are disposed adjacent to two sides of each gate structure, and wherein a porosity of the porous spacers is between 25% and 100%; A plurality of source / drain regions are disposed adjacent to the sides of the plurality of gate structures; A plurality of cover layers, correspondingly positioned on the plurality of source / drain regions; a first insulating layer, located on the plurality of cover layers and the isolation layer, wherein the first insulating layer is made of a low dielectric constant dielectric material, the dielectric material having a dielectric constant between 2.4 and 3.5; a second insulating layer, located on the first insulating layer, wherein the second insulating layer is made of a dielectric material with the same low dielectric constant as the first insulating layer; A plurality of contact points are disposed through the second insulating layer and the first insulating layer and are respectively and correspondingly located on the plurality of covering layers; and A porous capping layer is located on the plurality of grid structures, wherein a porosity of the porous capping layer is between 25% and 100%.
2. The semiconductor device according to claim 1, wherein The porous spacer comprises an energy removable material composed of a base material and a decomposable porogen material.
3. The semiconductor device according to claim 2, wherein: The base material includes silicon oxide, and the decomposable porogen material includes a plurality of compounds including a plurality of unsaturated dangling bonds.
4. The semiconductor device according to claim 1, wherein The plurality of fins are located between the gate structure and the substrate.
5. The semiconductor device according to claim 4, wherein: The fin includes a protrusion and two recessed portions, wherein the two recessed portions are arranged adjacent to both sides of the protrusion, wherein a top surface of the protrusion is located on a vertical horizontal plane, which is higher than a vertical horizontal plane of the top surface of the recessed portion, and one of the multiple gate structures is located on the protrusion, and two of the multiple source / drain regions are paired and respectively located on the recessed portions.
6. The semiconductor device according to claim 1, wherein The plurality of cover layers are made of metal silicate.
Citation Information
Patent Citations
Semiconductor device with porous dielectric structure and method for fabricating the same
US20210234033A1
Porogens, Porogenated Precursors and Methods for Using the Same to Provide Porous Organosilica Glass Films with Low Dielectric Constants
US20130095255A1
Semiconductor device and manufacturing method thereof
US20180190653A1
Contact Plugs and Methods Forming Same
US20180197970A1