Substrate processing method and substrate processing device

By using halogen-containing gas and alkaline gas in alternating high-pressure and low-pressure cycles in the substrate processing vessel to modify and vaporize the silicon-containing film on the surface of the substrate, the problem of poor uniformity in the removal process of the silicon-containing film on the substrate surface is solved and achieved. Uniform etching and efficient removal of the substrate surface.

CN113178387BActive Publication Date: 2024-10-18TOKYO ELECTRON LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202110058361.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-01-15
Publication Date
2024-10-18
Estimated Expiration
2041-01-15

AI Technical Summary

Technical Problem

It is difficult to achieve a highly uniform removal process when removing the silicon-containing film on the surface of the substrate using the existing technology, resulting in a thickness difference between the central portion and the peripheral portion during the etching process.

Method used

By alternating high-pressure and low-pressure cycles in the processing vessel, halogen-containing gas and alkaline gas are used to modify the silicon-containing film and vaporize the reaction products, control the residue and sublimation of the reaction products, and ensure the surface stability of the substrate. Etches evenly.

Benefits of technology

It realizes the removal process with high uniformity on all parts of the substrate surface, reduces the thickness difference during the etching process, and improves the uniformity and throughput of etching.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113178387B_ABST
    Figure CN113178387B_ABST
Patent Text Reader

Abstract

The present invention provides a substrate processing method and a substrate processing device, which perform a highly uniform removal process on each part of the surface of the substrate when removing a silicon-containing film formed on the surface of the substrate. The process includes the following steps: storing the substrate with the silicon-containing film formed on the surface in a processing container; in a first step, supplying a processing gas containing a halogen-containing gas and an alkaline gas to the substrate under a first pressure in the processing container to modify the silicon-containing film and generate a reaction product; in a second step, making the processing container a second pressure lower than the first pressure to gasify the reaction product; and repeating the first step and the second step alternately, wherein the first step after the second time in the repeated process is a step of supplying the processing gas to the substrate on which the reaction product remains.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a substrate processing method and a substrate processing device. Background Art

[0002] When manufacturing semiconductor devices, a silicon-containing film such as a SiO2 film (silicon oxide film) formed on the surface of a semiconductor wafer (hereinafter referred to as a wafer) serving as a substrate is sometimes etched. Patent documents 1 and 2 describe a process called COR (Chemical Oxide Removal) as a method for etching a SiO2 film. More specifically, Patent documents 1 and 2 describe the following process as the COR process: modifying the SiO2 film with HF (hydrogen fluoride) gas and NH3 (ammonia) gas, and sublimating the reaction product generated by the modification of the SiO2 film by reducing the pressure of the environment around the wafer.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent No. 5809144

[0006] Patent Document 2: Japanese Patent No. 6568769 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] The present disclosure provides a technology that can perform a highly uniform removal process on each portion within the surface of a substrate when removing a silicon-containing film formed on the surface of a substrate.

[0009] Solutions for solving problems

[0010] The substrate processing method disclosed herein comprises the following steps: storing a substrate having a silicon-containing film formed on the surface thereof in a processing container;

[0011] In a first step, a processing gas including a halogen-containing gas and an alkaline gas is supplied to the substrate while the pressure in the processing container is at a first pressure, so as to modify the silicon-containing film and generate a reaction product.

[0012] A second step of making the pressure in the processing container lower than the first pressure to gasify the reaction product;

[0013] Repeating the process, alternately repeating the first process and the second process,

[0014] The first step after the second time in the repeated step is a step of supplying the processing gas to the substrate on which the reaction product remains.

[0015] Effects of the Invention

[0016] According to the present disclosure, when removing a silicon-containing film formed on the surface of a substrate, it is possible to perform a highly uniform removal process on each portion within the surface of the substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a longitudinal sectional side view of a substrate processing apparatus for performing substrate processing according to one embodiment.

[0018] Figure 2 1 is a timing chart showing the supply of each gas and the change in the opening degree of the valve performed in the substrate processing apparatus.

[0019] Figure 3A 1 is a schematic diagram showing a surface of a wafer processed in the substrate processing apparatus.

[0020] Figure 3B It is a longitudinal sectional side view showing the surface of the wafer.

[0021] Figure 3C It is a longitudinal sectional side view showing the surface of the wafer.

[0022] Figure 4A It is a longitudinal sectional side view showing the surface of the wafer.

[0023] Figure 4B It is a longitudinal sectional side view showing the surface of the wafer.

[0024] Figure 4C It is a longitudinal sectional side view showing the surface of the wafer.

[0025] Figure 5A It is a longitudinal sectional side view showing the surface of the wafer.

[0026] Figure 5B It is a longitudinal sectional side view showing the surface of the wafer.

[0027] Figure 5C It is a longitudinal sectional side view showing the surface of the wafer.

[0028] Figure 6 It is a longitudinal sectional side view showing the surface of the wafer.

[0029] Fig. 7A 1 is a schematic diagram showing a surface of a wafer processed in the substrate processing apparatus.

[0030] Figure 7B It is a longitudinal sectional side view showing the surface of the wafer.

[0031] Figure 7C It is a longitudinal sectional side view showing the surface of the wafer.

[0032] Fig. 8A It is a longitudinal sectional side view showing the surface of the wafer.

[0033] Figure 8B It is a longitudinal sectional side view showing the surface of the wafer.

[0034] Figure 8C It is a longitudinal sectional side view showing the surface of the wafer.

[0035] Fig.9A It is a longitudinal sectional side view showing the surface of the wafer.

[0036] Fig. 9B It is a longitudinal sectional side view showing the surface of the wafer.

[0037] Fig. 9C It is a longitudinal sectional side view showing the surface of the wafer.

[0038] Fig.10 It is a graph which shows the evaluation test result.

[0039] Description of Reference Numerals

[0040] W: wafer; 11: process container; 43: process gas; 44: AFS layer. DETAILED DESCRIPTION

[0041] (First Embodiment)

[0042] Reference Figure 1 A substrate processing device 1 according to an embodiment of the present disclosure is illustrated in a longitudinal sectional side view. The substrate processing device 1 is a device that stores a wafer W having a SiO2 film formed on the surface in a processing container 11 that forms a vacuum environment, and etches the SiO2 film by the COR process described in the background technology item. More specifically, the substrate processing device 1 performs the following processes: HF gas and NH3 gas are supplied to the above-mentioned wafer W as processing gases to modify the SiO2 film and generate reaction products, and the supply of the processing gas is stopped and the reaction products are sublimated. The substrate processing device 1 removes the SiO2 film by the above-mentioned processes. The above-mentioned reaction product is ammonia fluorosilicate (AFS).

[0043] For the sake of convenience, the period of supplying the processing gas is defined as the first period, and the period of stopping the supply of the processing gas and allowing the AFS to sublime is defined as the second period. When processing one wafer W, the first period and the second period are repeated alternately. In order to perform the above-mentioned sublimation of the AFS, during the second period, the pressure in the processing container 11 is lower than the pressure in the first period.

[0044] Reference numeral 12 in the figure denotes a transfer port for wafers W opened in the side wall of the processing container 11, which is opened and closed by a gate valve 13. A mounting table 21 for mounting wafers W is provided in the processing container 11. The wafers W are carried in and out of the processing container 11 through the transfer port 12 by a transfer mechanism (not shown). In addition, lift pins (not shown) are provided on the mounting table 21 to transfer wafers W between the transfer mechanism entering the processing container 11 and the mounting table 21.

[0045] A heating unit 22 is embedded in the mounting table 21 to heat the wafer W mounted on the mounting table 21 to, for example, 80 degrees or more, more specifically, to, for example, 100 degrees. The heating unit 22 is configured to form a flow path that forms a part of a circulation passage for a fluid such as water for adjusting the temperature, and the wafer W is heated by heat exchange with the fluid. However, the heating unit 22 is not limited to a flow path of such a fluid, and may also be composed of, for example, a heater that is a resistance heater. In addition, for example, the wafer W is heated to the same temperature during the first period and the second period, and the sublimation of the AFS mentioned above has nothing to do with the temperature change of the wafer W, but is caused by the pressure change in the processing container 11 as described above.

[0046] In addition, one end of the exhaust pipe 23 opens in the processing container 11, and the other end of the exhaust pipe 23 is connected to an exhaust mechanism 25, such as a vacuum pump, via a valve 24 as a pressure changing mechanism. The exhaust volume in the processing container 11 is adjusted by changing the opening of the valve 24, and as a result, the pressure in the processing container 11 is adjusted. Therefore, in the second period described above, the opening of the valve 24 becomes larger than that in the first period.

[0047] A gas shower head 26 as a processing gas supply mechanism is provided on the upper side of the processing container 11 so as to face the mounting table 21. The gas shower head 26 is connected to the downstream side of the gas supply passages 31 to 34, and the upstream side of the gas supply passages 31 to 34 is connected to the gas supply sources 36 to 39 via respective flow adjustment units 35. Each flow adjustment unit 35 includes a valve and a mass flow controller. The gas supplied from the gas supply sources 36 to 39 is cut off from the supply to the downstream side by opening and closing the valve included in the flow adjustment unit 35.

[0048] HF gas as a halogen-containing gas, NH3 gas as an alkaline gas, Ar (argon) gas, and N2 (nitrogen) gas are respectively supplied from gas supply sources 36, 37, 38, and 39. Therefore, these HF gas, NH3 gas, Ar gas, and N2 gas can be supplied from the gas shower head 26 into the processing container 11. In the first period, Ar gas and N2 gas are supplied into the processing container 11 together with HF gas and NH3 gas as carrier gas. In addition, in the second period, N2 gas is also supplied into the processing container 11 as a purge gas to purge the processing container 11.

[0049] The substrate processing apparatus 1 includes a control unit 10 as a computer, and the control unit 10 includes a program. The program is stored in a storage medium such as an optical disk, a hard disk, a magneto-optical disk, or a DVD, and is installed in the control unit 10. The control unit 10 outputs a control signal to each part of the substrate processing apparatus 1 through the program to control the operation. Specifically, the opening degree of the valve 24 of the exhaust pipe 23, the opening and closing of the valve constituting the flow adjustment unit 35, etc. are controlled by the program. A step group is assembled for the above-mentioned program so that the operation of each part can be controlled as described above to perform the processing described later.

[0050] Figure 2 1 is a timing chart showing the switching timing between the state of supplying each gas to the processing container 11 and the state of stopping the supply, and the timing of changing the opening of the valve 24 when processing the wafer W in the substrate processing apparatus 1. As described above, in the substrate processing apparatus 1, the processing is performed by alternating the first period and the second period, wherein the first period is the period of supplying the processing gas to the wafer W, and the second period is the period of reducing the pressure in the processing container 11 compared with the first period to sublime the AFS. The processing in the first period is the first process, and the processing in the second period is the second process, and the repeated process of repeating these first and second processes is performed. The valve 24 is not fully opened in each second period, so that in the second period, the processing container 11 is set to a lower exhaust volume and a higher pressure. The reason for limiting the opening of the valve 24 in this way is explained below together with a series of processes performed on the wafer W. In addition, the time t1 to t2 and t3 to t4 shown in the timing chart are the first period, and the time t2 to t3 and t4 to t5 are the second period.

[0051] Refer to the above Figure 2 and Figure 3A to Figure 6 The processing performed on the wafer W will be described. Figure 3A to Figure 6 1 and 10 are longitudinal sectional side views of the surface of the wafer W. In each of these drawings, the center portion of the wafer W is shown on the left side, and the peripheral portion of the wafer W is shown on the right side. Figure 3AThe figure shows a wafer W before being processed by a substrate processing device 1, in which a plurality of convex portions, for example, composed of a polysilicon film 41, are arranged in the horizontal direction, and a SiO2 film 42 is formed in a manner embedded between the convex portions. The substrate processing device 1 etches the SiO2 film 42 in a manner that leaves its lower end portion. In addition, the processing gas (HF gas and NH3 gas) is shown as 43 in each figure. For example, it is assumed that due to the characteristics of the device, when the processing gas 43 is supplied, the concentration of the processing gas 43 has a deviation between the center and the peripheral portion of the wafer W, and the concentration of the processing gas 43 in the center portion is high.

[0052] The above Figure 3A The wafer W shown in FIG. 1 is carried into the processing container 11, placed on the mounting table 21 and heated to the above-mentioned temperature. Furthermore, the valve 24 is set to a first opening to make the processing container 11 a vacuum environment with a first pressure, for example, 2.6Pa to 533Pa, and the processing gas 43, Ar gas and N2 gas are respectively supplied into the processing container 11. Figure 3B , Figure 2 middle time t1).

[0053] The surface of the SiO2 film 42 reacts with the processing gas 43 to generate AFS, forming an AFS layer 44 ( Figure 3C ). Next, the supply of the processing gas 43 and the Ar gas into the processing container 11 is stopped, and the opening of the valve 24 is increased to a second opening (time t2), and the pressure in the processing container 11 is reduced to a second pressure, for example, 0 Pa to 200 Pa. In addition, the second opening is a partially open opening as described above.

[0054] Due to the above-mentioned deviation in the concentration of the processing gas 43, at time t2, the center of the wafer W reacts more with the processing gas 43 than the peripheral portion, forming a thicker AFS layer 44. Furthermore, after time t2, since the valve 24 is not fully opened and the exhaust volume is suppressed as described above, the processing gas 43 is not purged out of the processing container 11 in one breath, but is purged out slowly. In addition, since the valve 24 is not fully opened and the pressure drop is suppressed, the AFS layer 44 is prevented from rapidly sublimating as a whole, and sublimates gradually from the upper side of the AFS layer 44. While sublimation is performed in this way, on the other hand, the processing gas 43 remaining in the processing container 11 acts on the upper part of the unreacted SiO2 film 42 through the AFS layer 44. Therefore, in each of the center and peripheral portions of the wafer W, the positions of the upper and lower ends of the AFS layer 44 move downward (towards the bottom surface of the wafer W) ( Figure 4A When the purging of the processing gas 43 is completed, the generation of new AFS stops, while sublimation further proceeds ( Figure 4B ).

[0055] Next, the opening of the valve 24 is lowered to return to the first opening, and the pressure in the processing container 11 rises to the first pressure, and the sublimation of the AFS layer 44 stops. While changing the opening of the valve 24, the processing gas 43 and the Ar gas are again supplied to the processing container 11 (time t3, Figure 4C ). At the time point t2, the thickness of the AFS layer 44 is larger in the center of the wafer W than in the peripheral part. Therefore, at the time point t3, the thickness of the AFS layer 44 is also larger in the center of the wafer W than in the peripheral part. Then, after the time t3, the newly supplied processing gas 43 reacts in the center and peripheral parts of the wafer W and the AFS layer 44 becomes thicker. However, when the thickness of the AFS layer 44 exceeds a certain size, the processing gas cannot penetrate the AFS layer 44 and the reaction cannot proceed. In other words, the generation of AFS is saturated. In this way, the reaction in the center of the wafer W stops and the increase in the thickness of the AFS layer 44 stops. However, on the other hand, the reaction continues in the peripheral part of the wafer W where the thickness of the AFS layer 44 is smaller, and the thickness of the AFS layer 44 increases. Therefore, the thickness of the AFS layer 44 in the center and peripheral parts of the wafer W and the height position of the lower end of the AFS layer 44 are aligned ( Figure 5A ).

[0056] After that, the supply of the processing gas 43 and the Ar gas into the processing container 11 is stopped again, and the opening of the valve 24 is increased to the second opening again (time t4), thereby reducing the pressure in the processing container 11 to the second pressure described above. Then, similarly to the period between time t2 and t3, the sublimation of AFS and the generation of AFS using the remaining processing gas 43 are performed, and the upper and lower ends of the AFS layer 44 move downward ( Figure 5B When the purge of the processing gas 43 is completed, the generation of new AFS stops and sublimation proceeds ( Figure 5C ).

[0057] Then, the opening of the valve 24 is reduced to the first opening, and the supply of the processing gas 43 and the Ar gas into the processing container 11 is restarted (time t5). During time t4-t5, sublimation proceeds at the center and the periphery of the wafer W, and the thickness of the AFS layer 44 decreases, thereby reacting with the processing gas 43 at the center and the periphery of the wafer W, and the thickness of the AFS layer 44 increases.

[0058] Afterwards, the first period of processing, i.e., the supply of processing gas, and the second period of processing, i.e., sublimation, are repeated by repeatedly switching the supply and cutoff of processing gas 43 and Ar gas and changing the opening of valve 24, so as to etch SiO2 film 42. In this process, even if the thickness of AFS layer 44 in the center of wafer W is greater than the thickness of AFS layer 44 in the peripheral portion due to the characteristics of the above-mentioned device, the reaction of the center of wafer W when processing gas 43 is supplied can be suppressed by AFS layer 44 with increased thickness. Since the reaction is suppressed in this way, SiO2 film 42 is etched while aligning the thickness and height position of AFS layer 44 between the center and the peripheral portion of wafer W. Then, when the first period of processing and the second period of processing are performed for a predetermined number of times and SiO2 film 42 reaches the desired thickness ( Figure 6 ), the wafer W is moved out of the processing container 11 and the processing is completed.

[0059] For example, the flow rate of HF gas in the first period is 10 sccm to 550 sccm, the flow rate of NH3 gas is 10 sccm to 660 sccm, the flow rate of N2 gas is 0 sccm to 1000 sccm, and the flow rate of Ar gas is, for example, 0 sccm to 1000 sccm. For example, the flow rate of N2 gas in the second period is 0 sccm to 1000 sccm. In addition, for example Figure 6 As shown, in order to completely remove the AFS layer 44, the last second period among the repeated second periods may be set longer than the other second periods. That is, for example, the lengths of the second periods other than the last one may be the same, and only the length of the last second period may be different. In addition, the lengths of the first periods may be the same, for example. In addition, in order to completely remove the AFS layer 44, the opening of the valve 24 in the last second period may be greater than the opening of the valve 24 in the other second periods.

[0060] Incidentally, when the first period and the second period are repeated as described above, it is considered that the valve 24 is fully opened in the second period, the exhaust volume is increased and the pressure is reduced in the processing container 11 so as to quickly start the next first period after the first period ends. In other words, it is considered to exhaust the processing container 11 in a manner that shortens the period during which the processing gas 43 is not supplied. However, when such a process is performed, the processing gas 43 and the AFS layer 44 are quickly removed at the beginning of the second period, so the deviation of the AFS amount in the surface of the wafer W that may occur in the first period as described above cannot be eliminated. Therefore, the etching amount of the SiO2 film 42 in the surface of the wafer W after the etching is completed will be biased.

[0061] However, according to Figure 3A to Figure 6In the processing of the substrate processing apparatus 1 described in the second embodiment, the opening of the valve 24 is limited in the second period, and in the first period after the second time, the processing gas 43 is supplied to the wafer W in the state where the AFS layer 44 remains on the SiO2 film 42. At this time, the amount of newly generated AFS is adjusted according to the thickness of the AFS layer 44 remaining on the surface of the wafer W. Thus, when the processing of the wafer W is completed, as shown in FIG. Figure 6 As shown, the SiO 2 film 42 is etched uniformly at each portion in the surface of the wafer W, and the height of the remaining SiO 2 film 42 at each portion in the surface is uniform.

[0062] In addition, when explaining this process, the case where the process gas is supplied in the first period so that the amount of AFS generated in the peripheral portion is small between the center portion and the peripheral portion of the wafer W is described. However, as described above, the amount of new AFS generated is adjusted according to the thickness of the AFS layer 44 remaining on the wafer W, so when the process gas is supplied so that the amount of AFS generated in the center portion is less than the amount of AFS generated in the peripheral portion, the deviation of the etching amount of the SiO2 film 42 can be suppressed by this process. Furthermore, it is possible to achieve uniform etching amount in each portion within the surface of the wafer W, not limited to between the center portion and the peripheral portion.

[0063] In addition, if it is assumed that the valve 24 is fully opened during the second period, the exhaust volume will differ due to the performance deviation between the plurality of substrate processing apparatuses 1, and the sublimation amount of AFS between the substrate processing apparatuses 1 may be varied. However, as described above, the valve 24 is not fully opened during the second period in each substrate processing apparatus 1 so that the AFS layer 44 remains during the second period in the substrate processing apparatus 1. That is, by setting the opening of the valve 24 during the second period to an appropriate opening for each substrate processing apparatus 1, the uniformity of the processing between the apparatuses can be improved. Furthermore, according to the above-mentioned processing, during the second period when the supply of the processing gas is stopped, the processing gas 43 also remains for a long time, and AFS is also generated. Therefore, the throughput can be improved.

[0064] In addition, in the above-mentioned processing example, for the sake of convenience, the increase of the thickness of the AFS layer 44 is stopped in the first period of the second time, but the processing can also be performed in a manner that the increase of the thickness of the AFS layer 44 stops in the first period after the third time. In addition, an example in which AFS remains on the wafer W in each first period after the second time is described, but AFS does not need to remain every time like this. For example, when processing one wafer W, if the first period is set to 10 times, the opening of the valve 24 in each second period can also be controlled so that the processing is performed in a state where no AFS remains on the wafer W in the first period of the first five times, and the processing is performed in a state where AFS remains on the wafer W in the first period of the last five times.

[0065] (Second Embodiment)

[0066] Next, the second embodiment will be described with a focus on the differences between the second embodiment and the first embodiment. In the second embodiment, the processing is performed in such a way that the length of each second period described above is shorter. Assume that the SiO2 film 42 of the wafer W processed in the second embodiment is as follows: Fig. 7A As shown, the wafer W is cracked from its surface toward the lower side (bottom side of the wafer W) to form a crack 46 .

[0067] As described above, the second period is set short in the second embodiment, but in order to clearly describe the effects of the second embodiment, a comparative example in which the second period is set long will be described. In this comparative example, the opening degree of the valve 24 in the second period is set large.

[0068] In addition, Figures 7A to 9C 4 shows the surface of the wafer W processed in the second embodiment and its comparative example. In these figures, unlike the figures showing the surface of the wafer W in the first embodiment, 47 shows a solid AFS (equivalent to the AFS layer 44 in the description of the first embodiment) and a gaseous AFS with a high concentration existing around the solid AFS. That is, in Figures 7A to 9C The gas AFS not shown in the first embodiment is also shown in the figure so as not to be distinguished from the solid AFS.

[0069] Next, when the processing of the comparative example is described, Fig. 7A The wafer W shown in FIG. 1 is placed on the mounting table 21 in the processing container 11 and heated in the same manner as in the first embodiment, and a processing gas 43 (HF gas and NH 3 gas), Ar gas, and N 2 gas ( Figure 7B That is, the aforementioned first period begins, and the SiO2 film 42 is modified by the processing gas 43 to generate the AFS 47. The processing gas 43 enters the gap 46, and the surface of the peripheral wall of the gap 46 also becomes the AFS 47.

[0070] After the AFS 47 is generated, the opening of the valve 24 is changed from the first opening to the second opening, and the supply of HF gas, NH3 gas and Ar gas is stopped. That is, the second period begins, and the sublimation of the AFS 47 is performed ( Figure 7C As described above, since the second period is longer in the comparative example, the AFS 47 is removed from the wafer W by the end of the second period. Therefore, the peripheral wall of the slit 46 that becomes the AFS 47 is also removed, and the width of the slit 46 is increased.

[0071] After that, the first period is started again, and the SiO2 film 42 is modified to the AFS 47 by the processing gas 43. At this time, the processing gas 43 enters the gap 46 ( Fig. 8A ), the surface of the peripheral wall of the slit 46 becomes the AFS 47 ( Figure 8B ). Then, the second period starts again, and the AFS 47 is removed in the same manner as in the first second period. Therefore, the width of the slit 46 is further expanded in the same manner as in the first second period. Then, the first period and the second period are repeated, but the width of the slit 46 is expanded each time the first period and the second period pass. Figure 8C FIG. 4 shows the wafer W at the end of etching. Figure 8C As shown, as a result of the expansion of the gap 46, the thickness of the remaining SiO2 film 42 differs between the position where the gap 46 is formed before the process and the position where the gap 46 is not formed. That is, in the process of this comparative example, the uniformity of the process within the surface of the wafer W is reduced.

[0072] Next, refer to Figures 9A to 9C The processing of the second embodiment is described. First, the first period is started in the same manner as in the comparative example. Fig. 7A , Figure 7B As shown in FIG. 1 , various gases including the processing gas 43 are supplied to the wafer W to modify the surface of the SiO 2 film 42 into the AFS 47. Then, the second period begins. Figure 7C The sublimation of AFS 47 is performed as shown. The second period is short, and the first period is restarted quickly after the first period ends. Therefore, AFS 47 remains on the surface of the wafer W when the first period is restarted. More specifically, solid AFS 47 that was not vaporized in the second period, vaporized but not removed from the surface of the SiO2 film 42, and AFS 47 that returns to solid due to the pressure increase in the processing container 11 when the first period is restarted, remains on the surface of the SiO2 film 42. At this time, the AFS 47 that becomes solid after vaporization as described above is embedded in the gap 46.

[0073] Furthermore, the surface of the SiO2 film 42 changes to AFS47 ( Fig.9A ), but since the AFS 47 already exists in the gap 46, the processing gas 43 is inhibited from entering the gap 46 ( Fig. 9B ). Then, the first period and the second period are repeated, and in each first period, as in the second first period, the processing gas 43 is prevented from entering the gap 46. Therefore, the SiO2 film 42 is etched while the expansion of the gap 46 is suppressed. Fig. 9CFIG. 4 shows the wafer W at the end of etching. As a result of suppressing the expansion of the gap 46 as described above, as shown in FIG. Fig. 9C As shown, the difference in thickness of the remaining SiO2 film 42 is suppressed between the position where the slit 46 is formed before the process and the position where the slit 46 is not formed. That is, the process is performed with high uniformity in the surface of the wafer W.

[0074] In the second embodiment, the valve 24 in the second period may be fully opened or not fully opened as in the first embodiment, as long as the AFS 47 remains on the surface of the wafer W in the first period after the second time. In addition, instead of extending the second period, the valve 24 may be opened at a smaller opening so that the AFS 47 remains on the surface of the wafer W in the first period after the second time. In addition, it is described that the AFS 47 remains in each first period after the second time. That is, it is described that the AFS 47 remains in multiple first periods, but the length of the second period or the opening of the valve 24 may be controlled so that the AFS 47 remains only in the first first period of the first period after the second time. However, in order to prevent the gap 46 from expanding, it is preferred that the AFS 47 remains in each first period after the second time.

[0075] In addition, in the first embodiment described above, the opening of the control valve 24 is described so that the AFS remains on the wafer W in the first period after the second time, but the AFS can also be left by making the second period shorter as in the second embodiment. In addition, in the first and second embodiments, the silicon-containing film to be etched is not limited to the SiO2 film, and it can also be a SiON film (silicon oxynitride film). In the case of etching the SiON film in this way, it is also possible to generate AFS as a reaction product from the SiON film by using the aforementioned processing gas, so that it is possible to perform high uniformity etching in the surface of the wafer W in the same way as in the case of etching the SiO2 film. In addition, as the silicon-containing film, it is also possible to perform SiN film (silicon nitride film). In the case of etching the SiN film, AFS is generated from the SiN film by supplying NF3 gas, NH3 gas, and O2 gas as processing gases. Accordingly, it is possible to perform high uniformity etching in the surface of the wafer W in the same way as in the case of etching the SiO2 film described above.

[0076] In addition, all points of the embodiments disclosed this time should be understood as illustrative rather than restrictive. The above-mentioned embodiments can be implemented by various omissions, substitutions, changes and combinations without departing from the scope and spirit of the appended claims.

[0077] (Evaluation Test)

[0078] The evaluation test related to the technology disclosed in the present invention is described. The etching process described in the first embodiment is performed on a plurality of wafers W having SiO2 films formed on their surfaces. The etching process is performed by changing the opening of the valve 24 in the second period for each wafer W, that is, changing the pressure in the processing container 11 in the second period. Then, the average value (unit: 100) of the etching amount of the SiO2 film in each part of the surface is measured for each wafer W after the processing. ) and uniformity (Uniformity, unit: %). Uniformity refers to (maximum etching amount - minimum etching amount) / (average etching amount). Therefore, the lower the uniformity value, the higher the uniformity of the etching amount within the surface of the wafer W. In this evaluation test, the time of the second period is set to 15 seconds.

[0079] Fig.10 : is a graph showing the results of the evaluation test. The vertical axis of the graph represents the average value of the etching amount (unit: ) and uniformity (unit: %), the horizontal axis of the graph represents the relative pressure (unit: mTorr) in the processing container 11 during the second period. The relative pressure refers to the relative pressure when the pressure measured when the valve 24 is fully open is 0 mTorr, and is therefore the pressure difference relative to the 0 mTorr. The relative pressure during the first period was 3000 mTorr (400 Pa). In the graph, square dots are used to represent the average value of the etching amount, and circles are used to represent the uniformity. When the relative pressures are 500 mTorr (66.7 Pa), 1500 mTorr (200 Pa), 2000 mTorr (267 Pa), 2500 mTorr (333 Pa), and 3000 mTorr, the average values ​​of the etching amounts are respectively In addition, when the relative pressure is 500mTorr, 1500mTorr, 2000mTorr, and 2500mTorr, the uniformity is 2.59%, 1.23%, 0.98%, 0.76%, and 0.66%, respectively. Thus, the higher the relative pressure in the second period, the higher the uniformity of the etching amount in the surface of the wafer W (the lower the uniformity). In addition, the higher the relative pressure in the second period, the greater the average etching amount.

[0080] Therefore, according to the above test results, it is estimated that by controlling the pressure in the processing container 11 during the second period, as shown in FIG. Figure 3A to Figure 6 As described in the second embodiment, the processing gas is supplied in a state where the AFS layer remains, and the etching uniformity is improved. In addition, it is estimated that the higher the relative pressure in the second period, the more etching is performed by the processing gas remaining in the second period. In this way, according to the evaluation test, it is confirmed that by using this technology, etching can be performed with high uniformity in the surface of the wafer W, and the etching rate can be increased to improve the throughput.

[0081] In addition, sufficient uniformity and a sufficient average value of etching amount can be obtained even when the relative pressure is set to 500mTorr, which is the lowest in the evaluation test. That is, a sufficient effect can be obtained when the pressure in the second period is 500mTorr / 3000mTorr×100=16.7% relative to the pressure in the first period. Considering that the average values ​​of uniformity and etching amount will not change much when the relative pressure is set to a slightly lower level than 500mTorr, it is considered preferable to set the pressure in the second period to more than 15% of the pressure in the first period.

Claims

1. A substrate processing method, comprising the following steps: The substrate having the silicon-containing film formed on the surface is stored in a processing container, wherein The substrate has a first recess and a second recess, and the silicon-containing film is formed in the first recess and the second recess; In a first step, a processing gas including a halogen-containing gas and an alkaline gas is supplied to the substrate while the pressure in the processing container is at a first pressure, so as to modify the silicon-containing film and generate a reaction product. A second step of making the pressure in the processing container lower than the first pressure to gasify the reaction product; as well as Repeating the process, alternately repeating the first process and the second process, wherein, in the first step after the second time of the repeated step of alternately repeating the first step and the second step, the processing gas is supplied to the substrate on which the reaction product remains, The pressure in the processing container is adjusted by changing the opening of the exhaust valve. In the first process, the opening of the exhaust valve is set to a first opening. In the second process, the opening of the exhaust valve is set to a second opening that is larger than the first opening, and the second opening is not a fully opened opening. By performing the first step for the first time, the thickness of the reaction product generated in the first recess is greater than the thickness of the reaction product generated in the second recess. By performing the second step for the first time, the thickness of the reaction product remaining in the first recess is greater than the thickness of the reaction product remaining in the second recess. Furthermore, by repeating the step, the height of the silicon-containing film remaining in the first recess is aligned with the height of the silicon-containing film remaining in the second recess.

2. The substrate processing method according to claim 1, characterized in that: The silicon-containing film is a silicon oxide film or a silicon nitride film.

3. The substrate processing method according to claim 2, characterized in that: The silicon-containing film is a silicon oxide film.

4. The substrate processing method according to any one of claims 1 to 3, characterized in that: The halogen-containing gas is hydrogen fluoride gas, and the alkaline gas is ammonia gas.

5. The substrate processing method according to any one of claims 1 to 3, characterized in that: The second pressure is greater than 15% of the first pressure.

6. A substrate processing device comprising: A processing container storing a substrate having a silicon-containing film formed on its surface, wherein: The substrate has a first recess and a second recess, and the silicon-containing film is formed in the first recess and the second recess; a pressure changing mechanism that changes the pressure in the processing container; and a processing gas supply mechanism for supplying a processing gas containing a halogen-containing gas and an alkaline gas into the processing container; The substrate processing device outputs a control signal to perform the following steps: In a first step, the processing gas is supplied to the substrate while the pressure in the processing container is at a first pressure, so as to modify the silicon-containing film and generate a reaction product. The second step is to make the pressure in the processing container lower than the first pressure so as to gasify the reaction product; as well as Repeat the steps, alternately repeating the first step and the second step, wherein, in the first step after the second time of the repeating step of alternately repeating the first step and the second step, the processing gas is supplied to the substrate on which the reaction product remains, The pressure in the processing container is adjusted by changing the opening of the exhaust valve. In the first step, the opening of the exhaust valve is set to a first opening. In the second step, the opening of the exhaust valve is set to a second opening that is larger than the first opening, and the second opening is not a fully opened opening. By performing the first step for the first time, the thickness of the reaction product generated in the first recess is greater than the thickness of the reaction product generated in the second recess. By performing the second step for the first time, the thickness of the reaction product remaining in the first recess is greater than the thickness of the reaction product remaining in the second recess. Furthermore, by repeating the steps, the height of the silicon-containing film remaining in the first recess is aligned with the height of the silicon-containing film remaining in the second recess.

Citation Information

Patent Citations

  • Manganese - - aluminum [tansokeigoukinjishiyakunoseizouhou[tansokeigoukinjishiyakunoseizouhou]

    JP1983009144B2

  • Substrate processing method and substrate processing apparatus

    US20160236244A1