Semiconductor device and method for manufacturing semiconductor device

By using enlarged backside vias and sidewall spacers in the semiconductor device to replace the sacrificial epitaxial structure, the problem of insufficient electrical performance of the backside vias is solved, and the electrical efficiency and overall performance of the semiconductor device are improved.

CN113206062BActive Publication Date: 2024-10-18TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202110203188.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-02-23
Publication Date
2024-10-18
Estimated Expiration
2041-02-23

AI Technical Summary

Technical Problem

During the shrinking process of existing semiconductor devices, the electrical performance of the backside through-hole components is insufficient, which affects the overall circuit performance.

Method used

Using enlarged backside through-hole parts and sidewall spacers, through a combination of etching and epitaxial structures, sacrificial epitaxial plugs and sacrificial epitaxial structures are formed, and replaced with backside through-hole parts to improve the performance of the backside through-hole parts Electrical efficiency.

Benefits of technology

The electrical performance of the backside through-hole component is improved, the overall performance of the semiconductor device is enhanced, the parasitic capacitance is reduced, and the circuit performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113206062B_ABST
    Figure CN113206062B_ABST
Patent Text Reader

Abstract

A semiconductor device and a method for manufacturing the semiconductor device, the semiconductor device comprising a gate structure, a source / drain epitaxial structure, a front-side interconnection structure, a back-side via, an isolation material and a sidewall spacer. The source / drain epitaxial structure is on one side of the gate structure. The front-side interconnection structure is on the front side of the source / drain epitaxial structure. The back-side via is connected to the back side of the source / drain epitaxial structure. The isolation material is on one side of the back-side via and contacts the gate structure. The sidewall spacer is between the back-side via and the isolation material. The height of the isolation material is greater than the height of the sidewall spacer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a semiconductor device and a method for manufacturing the same. Background Art

[0002] The semiconductor integrated circuit (IC) industry has experienced exponential growth. Technological advances in IC materials and design have produced generations of ICs, each with smaller and more complex circuits than the previous generation. Over the course of IC evolution, functional density (i.e., the number of interconnected devices per chip area) has generally increased, while geometry size (i.e., the smallest component (or line) that can be produced using a manufacturing process) has decreased. This shrinking process generally provides benefits by increasing production efficiency and reducing associated costs. Summary of the invention

[0003] According to some embodiments, a semiconductor device includes a gate structure, a source / drain epitaxial structure, a front-side interconnect structure, a back-side via, an isolation material, and a sidewall spacer. The source / drain epitaxial structure is on one side of the gate structure. The front-side interconnect structure is on a front side of the source / drain epitaxial structure. The back-side via is connected to the back side of the source / drain epitaxial structure. The isolation material is on one side of the back-side via and contacts the gate structure. The sidewall spacer is between the back-side via and the isolation material. The height of the isolation material is greater than the height of the sidewall spacer.

[0004] According to some embodiments, a semiconductor device includes a plurality of channel layers, a gate structure, a first source / drain epitaxial structure, an internal spacer, a backside via, a sidewall spacer, and an isolation material. The channel layers are arranged one on top of another in a spaced-apart manner. The gate structure surrounds each channel layer. The first source / drain epitaxial structure is on one side of the gate structure and connected to the channel layer. The internal spacer is between the gate structure and the first source / drain epitaxial structure. The backside via is connected to the back side of the first source / drain epitaxial structure. The sidewall spacer contacts the gate structure and is on one side of the backside via. The isolation material is on the side of the backside via and contacts the gate structure and the sidewall spacer.

[0005] According to some embodiments, a method for manufacturing a semiconductor device includes etching a recess in a substrate. Forming a sacrificial epitaxial plug in the recess in the substrate. Forming a source / drain epitaxial structure above the sacrificial epitaxial plug. Forming a gate structure on one side of the source / drain epitaxial structure. Removing the substrate so that the sacrificial epitaxial plug protrudes from a back side of the source / drain epitaxial structure. Forming a sidewall spacer on one side of the sacrificial epitaxial plug so that a portion of the sacrificial epitaxial plug is exposed by the sidewall spacer. Forming a sacrificial epitaxial structure on the portion of the sacrificial epitaxial plug exposed by the sidewall spacer. Forming an isolation material on one side of the sacrificial epitaxial structure and on the sidewall spacer. Replacing the sacrificial epitaxial plug and the sacrificial epitaxial structure with a backside through-hole member. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] The aspects of the present disclosure will be best understood from the following detailed description when read in conjunction with the accompanying drawings. Please note that, in accordance with standard practices in the industry, various features are not drawn to scale. In fact, the dimensions of the various features may be arbitrarily increased or reduced for clarity of discussion.

[0007] Figures 1 to 20E A method of manufacturing a semiconductor device according to some embodiments of the present disclosure is described at various stages;

[0008] Fig.21A is a perspective view of a semiconductor device according to some embodiments of the present disclosure;

[0009] Fig.21B For along Fig.21A A cross-sectional view taken along line BB in FIG.

[0010] Fig. 21C For along Fig.21A A cross-sectional view taken along line CC in FIG.

[0011] Fig.21D For along Fig.21A A cross-sectional view taken along line DD in FIG.

[0012]

Explanation of symbols

[0013] 105: Hard Mask

[0014] 102: Groove

[0015] 104:Semiconductor Strip

[0016] 108: First sacrificial layer

[0017] 110:Substrate

[0018] 110a: front side

[0019] 110b: Dorsal

[0020] 112: base part

[0021] 112r: Recessed portion of source region

[0022] 120:Semiconductor stacking

[0023] 122: first semiconductor layer

[0024] 123: concave part

[0025] 124: Second semiconductor layer

[0026] 130: Isolation Structure

[0027] 140: Second sacrificial layer

[0028] 142: Groove

[0029] 150:Dummy fin structure

[0030] 152: Dielectric layer

[0031] 154: dummy fin

[0032] 158: concave part

[0033] 160: Mask layer

[0034] 170: Sacrificial gate dielectric layer

[0035] 180: dummy gate structure

[0036] 182: dummy gate layer

[0037] 184: cushion layer

[0038] 186: Mask layer

[0039] 190: Gate spacer

[0040] 205: Mask layer

[0041] 210: Internal spacer

[0042] 220: Sacrificial epitaxial plug

[0043] 230: Bottom epitaxial structure

[0044] 235: Air Gap

[0045] 240: Top epitaxial structure

[0046] 250: front side contact etch stop layer

[0047] 255: Front-side interlayer dielectric

[0048] 257: Groove

[0049] 260: Gate structure

[0050] 261: Bottom surface

[0051] 262: Gate dielectric layer

[0052] 264: Gate electrode

[0053] 266: Interface layer

[0054] 270: Front metal alloy layer

[0055] 280: Contact

[0056] 290:Front-side multi-layer interconnect

[0057] 292: via or contact

[0058] 294:Metal Wire

[0059] 310: Sidewall spacer

[0060] 310': Carpet Cover

[0061] 312: back surface

[0062] 314: Top surface

[0063] 320: Sacrificial epitaxial structure

[0064] 324: Sidewall

[0065] 326: bottom surface

[0066] 330: Isolation material

[0067] 332: Opening

[0068] 334: concave part

[0069] 340: Back contact etch stop layer

[0070] 350: Back metal alloy layer

[0071] 360: Back side through hole

[0072] 362: Part 1

[0073] 362s: Sidewall

[0074] 364: Part 2

[0075] 364s: Sidewall

[0076] 366: Part 3

[0077] 366s: Sidewall

[0078] 370: Back-side multilayer interconnect

[0079] 372:Through hole or contact

[0080] 374:Metal Wire

[0081] 375: Interface

[0082] 410: Carrier substrate

[0083] A: Area

[0084] BB:Line

[0085] CC:Line

[0086] DD:Line

[0087] D: Drain region

[0088] H1: Height

[0089] H2: Height

[0090] H3: Height

[0091] L: Channel length

[0092] S: Source region

[0093] T1: Thickness

[0094] W1: Width

[0095] W2: Width

[0096] θ1: angle

[0097] θ2: angle

[0098] θ3: Angle DETAILED DESCRIPTION

[0099] The following disclosure provides many different embodiments or examples for implementing different features of the provided subject matter. Feature examples of components and configurations will be described below to simplify the present disclosure. Of course, each of these is merely an example and is not intended to be limiting. For example, a first feature formed above or on a second feature in the subsequent description may include an embodiment in which the first feature and the second feature are formed in direct contact, and may also include an embodiment in which an additional feature may be formed between the first feature and the second feature so that the first feature and the second feature are not in direct contact. In addition, the present disclosure may repeat reference numbers and / or letters in various examples. This repetition is for the purpose of simplicity and clarity and does not itself dictate the relationship between the various embodiments and / or configurations discussed.

[0100] Additionally, to facilitate description of the relationship of one element or feature to another element or feature as illustrated in the figures, spatially relative terms, such as "below," "beneath," "lower," "above," "upper," and the like, may be used herein. The spatially relative terms are intended to encompass different orientations of the element in use or operation in addition to the orientation depicted in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations), and the spatially relative descriptors used herein should be similarly interpreted accordingly.

[0101] As used herein, "approximately," "about," "approximately," or "substantially" shall generally mean within 20% or within 10% or 5% of a given value or range. The numerical quantities given herein are approximate, meaning that the terms "approximately," "about," "approximately," or "substantially" may be inferred without explicit statement.

[0102] Gate all around (GAA) transistor structures may be patterned by any suitable method. For example, these structures may be patterned using one or more photolithography processes including double patterning or multi-patterning processes. Generally, double patterning or multi-patterning processes combine photolithography processes with self-alignment processes to produce patterns having a pitch that is, for example, smaller than that otherwise obtainable using a single direct photolithography process. For example, in one embodiment, a sacrificial layer is formed over a substrate and the sacrificial layer is patterned using a photolithography process. Spacers are formed alongside the patterned sacrificial layer using a self-alignment process. The sacrificial layer is then removed, and the remaining spacers may then be used to pattern the GAA structure.

[0103] The present disclosure relates to semiconductor devices and methods for forming the same. More particularly, some embodiments of the present disclosure relate to GAA devices including enlarged backside vias that are used to improve the electrical performance of the backside vias. The GAA devices provided herein include p-type GAA devices or n-type GAA devices. In addition, the GAA device may have one or more channel regions (e.g., nanowires) associated with a single continuous gate structure or multiple gate structures. A person of ordinary skill in the art may recognize other examples of semiconductor devices that may benefit from the aspects of the present disclosure. For example, some embodiments as described herein may also be applied to fin transistor (FinFET) devices, omega gate (Ω-gate) devices and / or pie gate (π-gate) devices.

[0104] Figures 1 to 20E A method of manufacturing a semiconductor device at various stages according to some embodiments of the present disclosure is described. In some embodiments, Figures 1 to 20EThe semiconductor device shown in the figure may be an intermediate device manufactured during the processing of an integrated circuit (IC) or a portion thereof. The IC may include static random access memory (SRAM), logic circuits, passive components (such as resistors, capacitors and inductors) and / or active components (such as p-type field effect transistors (PFET), n-type FETs (NFET), multi-gate FETs, metal-oxide semiconductor field effect transistors (MOSFET), complementary metal-oxide semiconductor (CMOS) transistors, bipolar transistors, high voltage transistors, high frequency transistors, other memory cells and combinations thereof.

[0105] refer to Figure 1 . A substrate 110 is provided, which may be a portion of a wafer. The substrate 110 has a front side 110a and a back side 110b opposite the front side 110a. In some embodiments, the substrate 110 may include silicon (Si). Alternatively, the substrate 110 may include germanium (Ge), silicon germanium (SiGe), gallium arsenide (GaAs), or other suitable semiconductor materials. In some embodiments, the substrate 110 may include a semiconductor-on-insulator (SOI) structure, such as a buried dielectric layer. Also alternatively, the substrate 110 may include a buried dielectric layer, such as a buried oxide (BOX) layer, formed by a method known as separation by implantation of oxygen (SIMOX) technology, wafer bonding, SEG, or another start-up method. In various embodiments, the substrate 110 may include any of a variety of substrate structures and materials.

[0106] A first sacrificial layer 108 is formed on the front side 110a of the substrate 110. The first sacrificial layer 108 may be epitaxially grown on the substrate 110 so that the first sacrificial layer 108 forms a crystalline layer. The first sacrificial layer 108 and the substrate 110 have different or the same materials and / or compositions. In some embodiments, the first sacrificial layer 108 is made of silicon germanium (SiGe) or silicon. In some embodiments, the first sacrificial layer 108 is omitted.

[0107] The semiconductor stack 120 is formed on the first sacrificial layer 108 by epitaxy, so that the semiconductor stack 120 forms a crystalline layer. The semiconductor stack 120 includes a first semiconductor layer 122 and a second semiconductor layer 124 that are alternately stacked. The first semiconductor layer 122 and the second semiconductor layer 124 are made of materials with different lattice constants, and may include one or more layers of Si, Ge, SiGe, GaAs, InSb, GaP, GaSb, InAlAs, InGaAs, GaSbP, GaAsSb, or InP. In some embodiments, the first semiconductor layer 122 and the second semiconductor layer 124 are made of silicon, silicon compounds, silicon germanium, germanium, or germanium compounds. Figure 1 In the embodiment, three first semiconductor layers 122 and three second semiconductor layers 124 are disposed. However, the number of these layers is not limited to three, and may be as low as 1 (per layer) and in some embodiments, 2 layers or 4 to 10 layers of each of the first semiconductor and second semiconductor layers are formed. By adjusting the number of stacked layers, the drive current of the GAA FET device can be adjusted.

[0108] In some embodiments, the first semiconductor layer 122 can be a SiGe layer having a germanium atomic percentage greater than zero. In some embodiments, the germanium percentage of the first semiconductor layer 122 is in a range between about 15 percent and about 100 percent. In some embodiments, the thickness of the first semiconductor layer 122 is in a range between about 3 nm and about 20 nm.

[0109] In some embodiments, the second semiconductor layer 124 may be a pure silicon layer without germanium. The second semiconductor layer 124 may also be a substantially pure silicon layer, for example, having a germanium atomic percentage of less than about 1 percent. In addition, the second semiconductor layer 124 may be intrinsic, which is not doped with p-type and n-type impurities. In some embodiments, the thickness of the second semiconductor layer 124 is in a range between about 3 nm and about 60 nm.

[0110] A patterned hard mask 105 is formed over the semiconductor stack 120. In some embodiments, the patterned hard mask 105 is formed of silicon nitride, silicon oxynitride, silicon carbide, silicon carbonitride, or the like. The patterned hard mask 105 covers a portion of the semiconductor stack 120 while leaving another portion of the semiconductor stack 120 uncovered.

[0111] refer to Figure 2 . Figure 1The semiconductor stack 120, the first sacrificial layer 108 and the substrate 110 are patterned using the patterned hard mask 105 as a mask to form the trenches 102. Accordingly, a plurality of semiconductor strips 104 are formed. The trenches 102 extend into the substrate 110 and have longitudinal directions that are substantially parallel to each other. The trenches 102 form base portions 112 in the substrate 110, wherein the base portions 112 protrude from the substrate 110, and the semiconductor strips 104 are formed on the base portions 112 of the substrate 110, respectively. Alternatively, the remaining portions of the semiconductor stack 120 and the sacrificial layer 108 are therefore referred to as semiconductor strips 104.

[0112] An isolation structure 130, which may be a shallow trench isolation (STI) region, is formed in the trench 102. The formation may include, for example, filling the trench 102 with a dielectric layer using flowable chemical vapor deposition (FCVD) and performing chemical mechanical polish (CMP) to make the top surface of the dielectric material flush with the top surface of the hard mask 105. The isolation structure 130 is then recessed. The top surface of the resulting isolation structure 130 may be flush with the bottom surface of the first sacrificial layer 108, or may be at an intermediate level between the top and bottom surfaces of the first sacrificial layer 108.

[0113] refer to Figure 3 The second sacrificial layers 140 are formed on the isolation structures 130 and cover the semiconductor strips 104 respectively. In some embodiments, the second sacrificial layers 140 are made of a semiconductor material such as silicon germanium or other suitable materials. In some other embodiments, the second sacrificial layers 140 may be a dielectric material. The second sacrificial layers 140 are separated from each other so that trenches 142 are formed between the second sacrificial layers.

[0114] A plurality of dummy fin structures 150 are respectively formed in the trenches 142. In some embodiments, a dielectric layer is conformally formed on the second sacrificial layer 140, and a filling material is filled in the trenches 142. A planarization (e.g., CMP) process is then performed to remove excess portions of the dielectric layer and the filling material to form dummy fin structures 150 in the trenches 142, respectively. Thus, each dummy fin structure 150 includes a dielectric layer 152 and a dummy fin 154 on the dielectric layer 152. In some embodiments, the dielectric layer 152 is deposited using an ALD process or other suitable process. In some embodiments, the dielectric layer 152 and the dummy fin 154 include silicon nitride, silicon oxide, silicon oxynitride, SiCN, SiCON, SiOC, or other suitable materials. For example, the dielectric layer 152 includes silicon nitride, and the dummy fin 154 includes silicon dioxide.

[0115] Subsequently, the dummy fin structures 150 are recessed to form recesses 158 on the dummy fin structures. In some embodiments, multiple etching processes are performed to recess the dummy fin structures 150. The etching processes include dry etching processes, wet etching processes, or a combination thereof. Mask layers 160 are then formed in the recesses 158, respectively. In some embodiments, the mask layers 160 are formed of silicon nitride, silicon oxynitride, silicon carbide, silicon carbonitride, or the like. For example, a mask material is formed on the second sacrificial layer 140 and the dummy fin structures 150, and a planarization (e.g., CMP) process is performed to remove excess portions of the mask material to form the mask layer 160.

[0116] refer to Figure 4 . The second sacrificial layer 140 and the patterned hard mask 105 are removed, and a sacrificial gate dielectric layer 170 is conformally formed on the mask layer 160, the dummy fin structure 150, and the first and second semiconductor layers 122 and 124. In some embodiments, the sacrificial gate dielectric layer 170 includes silicon dioxide, silicon nitride, a high-κ dielectric material, or other suitable materials. In various examples, the sacrificial gate dielectric layer 170 is deposited by: an ALD process, a CVD process, a subatmospheric chemical vapor deposition (SACVD) process, a flowable CVD process, a PVD process, or other suitable processes. For example, the sacrificial gate dielectric layer 170 can be used to prevent subsequent processing (e.g., subsequent formation of a dummy gate structure) from damaging the first and second semiconductor layers 122 and 124.

[0117] Subsequently, dummy gate structures 180 are formed on the sacrificial gate dielectric layer 170. Each dummy gate structure 180 includes a dummy gate layer 182, a liner layer 184 formed over the dummy gate layer 182, and a mask layer 186 formed over the liner layer 184. In some embodiments, a dummy gate material (not shown) may be formed over the sacrificial gate dielectric layer 170, and the liner layer 184 and the mask layer 186 may be formed over the dummy gate material. The dummy gate material is then patterned using the liner layer 184 and the mask layer 186 as a mask to form the dummy gate layer 182. Thus, the dummy gate layer 182, the liner layer 184, and the mask layer 186 are referred to as dummy gate structures 180. In some embodiments, the dummy gate layer 182 may be made of polycrystalline silicon (poly-Si), polycrystalline silicon germanium (poly-SiGe), or other suitable materials. The liner layer 184 may be made of silicon nitride or other suitable materials, and the mask layer 186 may be made of silicon dioxide or other suitable materials.

[0118] refer to Figure 5. Gate spacers 190 are formed on the sidewalls of the dummy gate structure 180, respectively. The gate spacers 190 may include sealing spacers and main spacers (not shown). The gate spacers 190 include one or more dielectric materials, such as silicon oxide, silicon nitride, silicon oxynitride, SiCN, SiCxOyNz, or a combination thereof. The sealing spacers are formed on the sidewalls of the dummy gate structure 180 and the main spacers are formed on the sealing spacers. The gate spacers 190 can be formed using deposition methods such as plasma enhanced chemical vapor deposition (PECVD), low-pressure chemical vapor deposition (LPCVD), sub-atmospheric chemical vapor deposition, or similar deposition methods. The formation of the gate spacers 190 may include blanket forming a spacer layer, and then performing an etching operation to remove horizontal portions of these spacer layers. The remaining vertical portions of the gate spacer layer form the gate spacers 190.

[0119] Subsequently, the first and second semiconductor layers 122 and 124 and the first sacrificial layer 108 are patterned using the dummy gate structure 180 and the gate spacer 190 as a mask so that a portion of the base portion 112 of the substrate 110 is exposed. During this etching process, the mask layer 160 may be recessed at areas not covered by the dummy gate structure 180 or the gate spacer 190. In some embodiments, the patterning process is performed using an anisotropic dry etching process. In some embodiments, the dry etching process etches the first and second semiconductor layers 122 and 124 and the first sacrificial layer 108 (e.g., Si and SiGe) much faster than etching the mask layer 160 (e.g., metal oxide, SiON, and SiOCN). Due to this etching selectivity, the dry etching process vertically patterns the first and second semiconductor layers 122 and 124 and the first sacrificial layer 108 without completely etching the mask layer 160. In Figure 5 In the embodiment, a portion of the mask layer 160 covered by the dummy gate structure 180 or the gate spacer 190 has a height greater than a height of the recessed portion of the mask layer 160 .

[0120] refer to Figure 6 The first semiconductor layer 122 is horizontally recessed (etched), so that the edge of the first semiconductor layer 122 is substantially located below the gate spacer 190 and forms a recess 123. The etching of the first semiconductor layer 122 includes wet etching and / or dry etching.

[0121] refer to Figure 7The inner spacers 210 are respectively formed in the recessed portions 123 of the first semiconductor layer 122 (see Figure 6 ). For example, in Figure 6 A dielectric material layer is formed over the structure of , and one or more etching operations are performed to form these internal spacers 210. In some embodiments, the internal spacers 210 include a silicon nitride-based material (such as SiN, SiON, SiOCN, or SiCN and combinations thereof) and are different from the material of the gate spacers 190. In some embodiments, the internal spacers 210 are silicon nitride. The internal spacers 210 can completely fill the recess 123, such as Figure 7 As shown. The dielectric material layer can be formed using CVD (including LPCVD and PECVD), PVD, ALD or other suitable processes. The etching operation includes one or more wet and / or dry etching operations. In some embodiments, the etching is an isotropic etching in some embodiments.

[0122] refer to Fig. 8A and Figure 8B ,in Figure 8B For along Fig. 8A A cross-sectional view taken along line BB in FIG. Figure 7 The mask layer 205 is formed over the structure. For clarity, the mask layer 205 is illustrated with a dotted line. The mask layer 205 is formed to cover the drain region D of the substrate portion 112 but not to cover at least one source region S of the substrate portion 112, and then the source region S of the substrate portion 112 is recessed, thereby generating at least one source region recess 112r in the substrate portion 112. In some embodiments, the mask layer 205 may be a photoresist mask formed by a suitable photolithography process. For example, the photolithography process may include a process such as Figure 7 A photoresist layer is spin-coated over the structure shown in FIG. 2 , a post-exposure bake process is performed, and the photoresist layer is developed to form a mask layer 205. In some embodiments, patterning the resist to form a patterned mask element can be performed using an electron beam (e-beam) lithography process or an extreme ultraviolet (EUV) lithography process.

[0123] Once the mask layer 205 is formed, the source region recess 112r can be formed in the source region S using, for example, an anisotropic etching process. In some embodiments, the anisotropic etching can be performed by dry chemical etching using a plasma source and a reactive gas. By way of example and not limitation, the plasma source can be an inductively coupled plasma (ICR) source, a transformer coupled plasma (TCP) source, an electron cyclotron resonance (ECR) source, or the like, and the reactive gas can be a fluorine-based gas (such as SF6, CH2F2, CH3F, CHF3, or the like), other chlorine-based gases (e.g., Cl2), hydrogen bromide gas (HBr), oxygen (O2), the like, or a combination thereof.

[0124] refer to 9A to 9C ,in Fig. 9B For along Fig.9A A cross-sectional view taken along line BB in FIG. Fig. 9C For along Fig.9A . An epitaxial growth process is performed to grow epitaxial material in the source region recess 112r until the epitaxial material accumulates to fill the sacrificial epitaxial plug 220 of the source region recess 112r. The epitaxial material has a different composition than the substrate 110, thus resulting in different etching selectivities between the sacrificial epitaxial plug 220 and the substrate 110. For example, the substrate 110 is silicon and the sacrificial epitaxial plug 220 is silicon germanium. In some embodiments, the sacrificial epitaxial plug 220 is silicon germanium without p-type dopants (e.g., boron) and n-type dopants (e.g., phosphorus) because the sacrificial epitaxial plug 220 will be removed in subsequent processes and does not serve as a source terminal of a transistor of a final IC product.

[0125] refer to Fig.10. A bottom epitaxial structure 230 is formed on the base portion 112 of the substrate 110 and the sacrificial epitaxial plug 220, respectively. In some embodiments, a semiconductor material is deposited on the base portion 112 and the sacrificial epitaxial plug 220 to form the bottom epitaxial structure 230. These semiconductor materials include single element semiconductor materials such as germanium (Ge) or silicon (Si), compound semiconductor materials such as gallium arsenide (GaAs) or aluminum gallium arsenide (AlGaAs), or semiconductor alloys such as silicon germanium (SiGe) or gallium arsenic phosphide (GaAsP). The bottom epitaxial structure 230 has a suitable crystal orientation (e.g., (100), (110), or (111) crystal orientation). The epitaxial process includes CVD deposition technology (e.g., vapor-phase epitaxy (VPE) and / or ultra-high vacuum CVD (UHV-CVD)), molecular beam epitaxy, and / or other suitable processes. In some embodiments, the bottom epitaxial structure 230 is intrinsic. That is, the bottom epitaxial structure 230 is undoped. The undoped bottom epitaxial structure 230 is beneficial for reducing leakage current from the top epitaxial structure 240 to the substrate 110. The top surface of the bottom epitaxial structure 230 can be at an intermediate level between the bottom surface and the top surface of the bottommost inner spacer 210.

[0126] The top epitaxial structures 240 are formed on the bottom epitaxial structures 230, respectively. In some embodiments, semiconductor materials are deposited on the bottom epitaxial structures 230 to form the top epitaxial structures 240. These semiconductor materials include single element semiconductor materials such as germanium (Ge) or silicon (Si), compound semiconductor materials such as gallium arsenide (GaAs) or aluminum gallium arsenide (AlGaAs), or semiconductor alloys such as silicon germanium (SiGe) or gallium arsenic phosphide (GaAsP). The top epitaxial structure 240 has a suitable crystal orientation (e.g., (100), (110), or (111) crystal orientation). In some embodiments, the top epitaxial structure 240 includes a source / drain epitaxial structure. In some embodiments, when an N-type device is required, the top epitaxial structure 240 may include epitaxially grown silicon phosphide (SiP) or silicon carbide (SiC). In some embodiments, when a P-type device is required, the top epitaxial structure 240 may include epitaxially grown silicon germanium (SiGe). The epitaxy process includes CVD deposition techniques (e.g., vapor-phase epitaxy (VPE) and / or ultra-high vacuum CVD (UHV-CVD)), molecular beam epitaxy, and / or other suitable processes. The desired p-type or n-type impurities may or may not be doped during the epitaxy process. Doping may be achieved by an ion implantation process, a plasma immersion ion implantation (PIII) process, and / or a solid source diffusion process, other suitable processes, or a combination thereof.

[0127] The dummy fin structure 150 is used to limit the spacer for epitaxially growing the top epitaxial structure 240. As a result, the top epitaxial structure 240 is defined between the dummy fin structures 150. This can be used to produce any desired size of the top epitaxial structure 240, and in particular to produce a small top epitaxial structure 240 for reducing parasitic capacitance. For example, the width of the top epitaxial structure 240 (i.e., the space between two adjacent dummy fin structures 150) is in the range of about 3 nm to about 100 nm. In addition, an air gap 235 can be formed under the top epitaxial structure 240. For example, the air gap 235 is defined by the top epitaxial structure 240, the bottom epitaxial structure 230, the dummy fin structure 150, and the isolation structure 130. In some embodiments, the top epitaxial structure 240 contacts the dummy fin structure 150, and the bottom epitaxial structure 230 is spaced apart from the dummy fin structure 150.

[0128] A front side contact etch stop layer (CESL) 250 is conformally formed over the dummy fin structure 150 and the top epitaxial structure 240. In some embodiments, the front side contact etch stop layer 250 may be one or more stress-bearing layers. In some embodiments, the front side contact etch stop layer 250 has a tensile stress and is formed of silicon nitride (Si3N4). In some other embodiments, the front side contact etch stop layer 250 includes a material such as an oxynitride. In still other embodiments, the front side contact etch stop layer 250 may have a composite structure including multiple layers, such as a silicon nitride layer overlying a silicon oxide layer. The front side contact etch stop layer 250 may be formed using plasma enhanced CVD (PECVD), however, other suitable methods such as low pressure CVD (LPCVD), atomic layer deposition (ALD), and the like may also be used.

[0129] A front interlayer dielectric (ILD) 255 is then formed on the front contact etch stop layer 250. The front interlayer dielectric 255 can be formed by chemical vapor deposition (CVD), high-density plasma CVD, spin coating, sputtering, or other suitable methods. In some embodiments, the front interlayer dielectric 255 includes silicon oxide. In some other embodiments, the front interlayer dielectric 255 may include silicon oxynitride, silicon nitride, a compound including silicon, oxygen, carbon, and / or hydrogen (e.g., silicon oxide, SiCOH, and SiOC), a low-k material, or an organic material (e.g., a polymer). After the front interlayer dielectric 255 is formed, a planarization operation such as CMP is performed so that the liner layer 184 and the mask layer 186 (see Fig.9A ) is removed and the dummy gate layer 182 and the mask layer 160 are exposed.

[0130] refer to FIG. 11A to FIG. 11D ,in Fig. 11B For along Fig.11A The cross-sectional view taken along line BB in FIG. Fig. 11C For along Fig.11A A cross-sectional view taken along line CC in FIG. Fig.11D For along Fig.11A The dummy gate layer 182 and the sacrificial gate dielectric layer 170 are then removed (see Fig.10), thereby exposing the second semiconductor layer 124. The front interlayer dielectric 255 protects the top epitaxial structure 240 during the removal of the dummy gate layer 182. The dummy gate layer 182 can be removed using plasma dry etching and / or wet etching. When the dummy gate layer 182 is polysilicon and the front interlayer dielectric 255 is silicon oxide, a wet etchant such as a tetramethylammonium hydroxide solution (TMAH) solution can be used to selectively remove the dummy gate layer 182. Thereafter, the dummy gate layer 182 is removed using plasma dry etching and / or wet etching. Subsequently, the sacrificial gate dielectric layer 170 is also removed. Thus, the uppermost semiconductor layer 124 is exposed.

[0131] In the dummy gate layer 182 (see Fig.10 ) is removed, the remaining first semiconductor layer 122 is removed (see Fig.9A ), thereby forming a sheet (or wire or rod or column) of the second semiconductor layer 124. The first semiconductor layer 122 may be removed or etched using an etchant capable of selectively etching the first semiconductor layer 122.

[0132] In some embodiments, the interface layer 266 is optionally formed to surround the exposed surface of the second semiconductor layer 124 and the exposed surface of the base portion 112 of the substrate 110. In various embodiments, the interface layer 266 may include a dielectric material such as silicon oxide (SiO2) or silicon oxynitride (SiON), and may be formed by chemical oxidation, thermal oxidation, atomic layer deposition (ALD), chemical vapor deposition (CVD), and / or other suitable methods.

[0133] The gate structure 260 is formed and / or filled between the gate spacers 190 or the inner spacers 210. That is, the gate structure 260 surrounds (wrapped) the semiconductor layer 124. The gate spacers 190 are disposed on opposite sides of the gate structure 260. Each gate structure 26 includes a gate dielectric layer 262 and a gate electrode 264. The gate electrode 264 includes one or more work function metal layers and a filling metal. The gate dielectric layer 262 is formed conformally. The second semiconductor layer 124 is called a channel of the semiconductor device. The gate dielectric layer 262 surrounds the second semiconductor layer 124, and the space between the second semiconductor layers 124 remains after the gate dielectric layer 262 is deposited. In some embodiments, the gate dielectric layer 262 includes a high-k material (k greater than 7), such as hafnium oxide (HfO2), zirconium oxide (ZrO2), lanthanum oxide (La2O3), hafnium aluminum oxide (HfAlO2), hafnium silicon oxide (HfSiO2), aluminum oxide (Al2O3), or other suitable materials. In some embodiments, the gate dielectric layer 262 can be formed by performing an ALD process or other suitable process.

[0134] The work function metal layer of the gate electrode 264 is conformally formed on the gate dielectric layer 262, and in some embodiments, the work function metal layer surrounds the second semiconductor layer 124. The work function metal layer may include materials such as TiN, TaN, TiAlSi, TiSiN, TiAl, TaAl, or other suitable materials. In some embodiments, the work function metal layer may be formed by performing an ALD process or other suitable process.

[0135] The fill metal of the gate electrode 264 fills the remaining space between the gate spacers 190 and the inner spacers 210. That is, the work function metal layer contacts the gate dielectric layer 262 and the fill metal and is between the gate dielectric layer 262 and the fill metal. The fill metal may include a material such as tungsten or aluminum. After the gate dielectric layer 262 and the gate electrode 264 are deposited, a planarization process such as a CMP process may then be performed to remove excess portions of the gate dielectric layer 262 and the gate electrode 264 to form the gate structure 260.

[0136] refer to Fig.12 The front side interlayer dielectric 255 is patterned to form trenches 257 on the opposite side of the gate structure 260, and then the front side contact etch stop layer 250 is patterned to expose the top epitaxial structure 240. In some embodiments, multiple etching processes are performed to pattern the front side interlayer dielectric 255 and the front side contact etch stop layer 250. These etching processes include dry etching processes, wet etching processes, or a combination thereof.

[0137] Contacts 280 are formed in the trenches 257. Thus, the contacts 280 contact the top epitaxial structures 240, respectively. In some embodiments, some of the contacts 280 interconnect adjacent top epitaxial structures 240. In some embodiments, the contacts 280 may be made of a metal such as W, Co, Ru, Al, Cu, or other suitable materials. After the contact 280 is deposited, a planarization process such as a chemical mechanical planarization (CMP) process may then be performed. Thus, the top surface of the contact 280 and the top surface of the front-side interlayer dielectric 255 are substantially coplanar. In some embodiments, a front-side metal alloy layer (such as silicide) 270 may be formed between the contact 280 and the top epitaxial structure 240. In addition, a barrier layer may be formed in the trenches 257 before the contact 280 is formed and after the front-side metal alloy layer 270. The barrier layer may be made of TiN, TaN, or a combination thereof.

[0138] refer to Fig.13A front-side multilayer interconnection (MLI) 290 including metal layers and inter-metal dielectrics (IMDs) is formed over the substrate 110 to electrically connect various features or structures of the semiconductor device (e.g., contacts 280 and / or gate structures 260). The front-side multilayer interconnection 290 includes vertical interconnects such as vias or contacts 292, and metal lines 294 (see FIG. Fig. 20B ). The various interconnect features may be implemented with various conductive materials including copper, tungsten, and silicide. In some examples, a damascene process is used to form a copper multilayer interconnect structure.

[0139] Subsequently, a carrier substrate 410 is formed over the front-side multilayer interconnect structure 290. For example, the carrier substrate 410 is bonded to the front-side multilayer interconnect structure 290. The carrier substrate 410 may be silicon (doped or undoped), or may include other semiconductor materials such as germanium; compound semiconductors; or a combination thereof. The carrier substrate 410 may provide structural support during subsequent processing of the back side of the semiconductor device and may remain in the final product in some embodiments. In some other embodiments, the carrier substrate 410 may be removed after subsequent processing of the back side of the semiconductor device is completed. In some embodiments, the carrier substrate 410 is bonded to the uppermost dielectric layer of the multilayer interconnect structure 290 by, for example, fusion bonding.

[0140] refer to FIG. 14A to FIG. 14D ,in Fig. 14B For along Fig.14A The cross-sectional view taken along line BB in FIG. Fig. 14C For along Fig.14A A cross-sectional view taken along line CC in FIG. Fig.14D For along Fig.14A A cross-sectional view taken along line DD in FIG. Fig.13 The structure is flipped upside down, and the substrate 110 and the first sacrificial layer 108 are removed (see Fig.11D and Fig.13). Thus, the sacrificial epitaxial plug 220 and other bottom epitaxial structures 230 that do not contact the sacrificial epitaxial plug 220 are exposed. In some embodiments, the removal process includes thinning the substrate 110 from the back side of the substrate 110 until the sacrificial epitaxial plug 220 is exposed. The substrate 110 is then removed by using a selective etching process that etches the substrate 110 and the first sacrificial layer 108 (e.g., silicon) at a faster etching rate than it etches the sacrificial epitaxial plug 220 (e.g., silicon germanium) and the isolation structure 130 (e.g., dielectric material). In some embodiments, the selective etching process for selectively removing the substrate 110 may be a wet etching process that uses a wet etching solution such as tetramethylammonium hydroxide (TMAH), potassium hydroxide (KOH), NH4OH, the like, or a combination thereof.

[0141] refer to FIG. 15A to FIG. 15D ,in Fig. 15B For along Fig.15A The cross-sectional view taken along line BB in FIG. Fig. 15C For along Fig.15A A cross-sectional view taken along line CC in FIG. Fig.15D For along Fig.15A DD in FIG. 3 . The blanket layer 310 ′ of the insulating material of the sidewall spacer is conformally formed by using CVD or other suitable methods. The blanket layer 310 ′ is deposited in a conformal manner so that the blanket layer is formed to have substantially equal thickness on vertical surfaces such as the sidewalls, horizontal surfaces, and the top of the sacrificial gate structure. FIG. 15A to FIG. 15D As shown, a blanket layer 310' is formed to cover the isolation structure 130, the backside surface of the gate structure 260, the backside surface of the inner spacer 210, and the sacrificial epitaxial plug 220. In some embodiments, the blanket layer 310' is deposited to a thickness T1 in a range of about 2 nm to about 10 nm. In some embodiments, the insulating material of the blanket layer 310' is a lower-κ material. In some embodiments, the blanket layer 310' is a nitride-based material such as SiN, SiON, SiOCN, or SiCN, and combinations thereof.

[0142] refer to FIG. 16A to FIG. 16D ,in Fig. 16B For along Fig.16A The cross-sectional view taken along line BB in FIG. Fig. 16C For along Fig.16A A cross-sectional view taken along line CC in FIG. Fig.16D For along Fig.16A The blanket layer 310' is then etched using an anisotropic process (see FIG. 15A to FIG. 15D) to form a sidewall spacer 310 on an opposite side of the base portion of the sacrificial epitaxial plug 220 such that another portion of the sacrificial epitaxial plug 220 is exposed by the sidewall spacer 310. The anisotropic etching performed on the blanket layer 310' may be, for example, reactive ion etching (RIE). During the anisotropic etching process, a majority of the insulating material is removed from the horizontal surfaces, thereby leaving a dielectric spacer layer on the vertical surfaces, such as the sidewalls of the sacrificial epitaxial plug 220. In some embodiments, an etch-back process may be performed to reduce the height of the sidewall spacer 310 such that the sidewall spacer 310 directly contacts the base portion of the sacrificial epitaxial plug 220 while exposing another portion of the sacrificial epitaxial plug 220. In addition, portions of the gate structure 260 and portions of the sidewalls of the isolation structure 130 contact the sidewall spacer 310, such as Fig.16D As shown. Fig. 16C As shown, some of the bottom epitaxial structures 230 that do not contact the sacrificial epitaxial plugs 220 contact some of the sidewall spacers 310. In some embodiments, the height H1 of the sidewall spacers 310 is less than about 40 nm, for example, about 0 nm to about 40 nm.

[0143] refer to FIG. 17A to FIG. 17D ,in Fig. 17B For along Fig.17A The cross-sectional view taken along line BB in FIG. Fig. 17C For along Fig.17A A cross-sectional view taken along line CC in FIG. Fig.17D For along Fig.17A A sacrificial epitaxial structure 320 is formed on the portion of the sacrificial epitaxial plug 220 not covered by the sidewall spacer 310 by performing, for example, a selective growth process. For example, another mask layer is formed to cover Fig.16AThe structure of the sacrificial epitaxial plug 220 is formed by patterning the mask layer to expose the sacrificial epitaxial plug 220, and forming a sacrificial epitaxial structure 320 on the sacrificial epitaxial plug 220. The mask layer can be removed after the sacrificial epitaxial structure 320 is formed. In some embodiments, the sacrificial epitaxial structure 320 is free of p-type dopants (e.g., boron) and n-type dopants (e.g., phosphorus) because the sacrificial epitaxial structure 320 will be removed in a subsequent process and does not serve as a source terminal of a transistor of a final IC product. The combined structure of the sacrificial epitaxial structure 320 and the sacrificial epitaxial plug 220 can be hammer-shaped in a cross-sectional view, and is therefore referred to as a sacrificial hammer-shaped via, which will be replaced with a hammer-shaped backside via in subsequent processing. By way of example and not limitation, the atomic percentage of germanium in the sacrificial epitaxial structure 320 is in the range of about 10% to about 50%. In some embodiments, the sacrificial epitaxial structure 320 and the sacrificial epitaxial plug 220 have the same or substantially the same material. Alternatively, the sacrificial epitaxial structure 320 and the sacrificial epitaxial plug 220 have the same or similar etching selectivity.

[0144] Due to the different growth rates on different crystal planes on different surfaces of the sacrificial epitaxial plug 220, the growth of the sacrificial epitaxial structure 320 includes lateral growth and vertical growth. Facets are thus formed on the surface of the sacrificial epitaxial structure 320. By way of example and not limitation, Fig. 17B In the cross-sectional view of , the sacrificial epitaxial structure 320 has a suitable crystal orientation (e.g., (110) and (111) crystal orientation) so that the sacrificial epitaxial structure 320 has a hexagonal cross-section. For example, the bottom surface 326 of the sacrificial epitaxial structure 320 is a (111) facet (i.e., the bottom surface 326 is a facet facing downward facing the gate structure 260), and the sidewall 324 of the sacrificial epitaxial structure 320 is a (110) facet (sidewall facet). The epitaxial process includes CVD deposition technology (e.g., vapor-phase epitaxy (VPE) and / or ultra-high vacuum CVD (UHV-CVD)), molecular beam epitaxy and / or other suitable processes. In some embodiments, angle θ1 is formed between the bottom surface 326 and the sidewall 324 of the sacrificial epitaxial structure 320, and angle θ1 is in a range of about 140 degrees to about 180 degrees (e.g., about 144.7 degrees to about 180 degrees), which is determined by the material and / or crystal orientation of the sacrificial epitaxial structure 320.

[0145] In some embodiments, the sacrificial epitaxial structure 320 can be grown by an epitaxial deposition / partial etching process, and the growth repeats the epitaxial deposition / partial etching process at least once to expand the lateral width of the sacrificial epitaxial structure. This repeated deposition / partial etching process is also called a cyclic deposition-etch (CDE) process. In some embodiments, the sacrificial epitaxial structure 320 is grown by selective epitaxial growth (SEG). For example, the sacrificial epitaxial structure 320 is grown epitaxially using a reactive gas (such as HCl as an etching gas, GeH4 as a Ge precursor gas, dichlorosilane (DCS) and / or SiH4 as a Si precursor gas, H2 and / or N2 as a carrier gas). In some embodiments, the etching gas can be other chlorine-containing gases or bromine-containing gases, such as Cl2, BCl3, BiCl3, BiBr3 or the like. The CDE process as discussed above is only one example for explaining how to form the sacrificial epitaxial structure 320 on the sacrificial epitaxial plug 220 , and other suitable techniques may also be used to form the sacrificial epitaxial structure 320 .

[0146] refer to 18A to 18D ,in Fig.18B For along Fig.18A The cross-sectional view taken along line BB in FIG. Fig.18C For along Fig.18A A cross-sectional view taken along line CC in FIG. Fig.18D For along Fig.18A DD in FIG. 1 is a cross-sectional view taken along line DD in FIG. An isolation material 330 is formed to fill the remaining space between the isolation structures 130. Since the sacrificial epitaxial plug 220 is covered by the sacrificial epitaxial structure 320 and the sidewall spacer 310, the isolation material 330 is spaced apart from the sacrificial epitaxial plug 220. In some embodiments, the isolation material 330 can be formed by a suitable method (such as spin-on, chemical vapor deposition (CVD)) and plasma-enhanced CVD (PECVD)) of, for example, a low-κ dielectric material (a material having a lower dielectric constant than silicon dioxide), such as silicon oxynitride, phosphosilicate glass (PSG), borophosphosilicate glass (BPSG), fluorinated silicate glass (FSG), SiO x C y 、SiO x C yH z , Spin-On-Glass, Spin-On-Polymer, silicon carbide materials, compounds thereof, composites thereof, combinations thereof, or the like. Other materials, such as ultra-low κ materials (e.g., having a dielectric constant of less than about 2.9), such as κ=2.5 to 2.6, may also be used. Alternatively, isolation material 330 and isolation structure 130 have substantially the same material, such as an oxide material. These materials and processes are provided as examples and other materials and processes may be used.

[0147] Subsequently, the sacrificial epitaxial structure 320 and the sacrificial epitaxial plug 220 are replaced with the backside via 360 (see 19A to 19D Specifically, the sacrificial epitaxial structure 320 and the sacrificial epitaxial plug 220 are removed so that the opening 332 is formed between the isolation material 330 and the isolation structure 130. The removal of the sacrificial epitaxial structure 320 and the sacrificial epitaxial plug 220 is performed using, for example, CMP, hydrofluoric acid / nitric acid / acetic acid (HF / Nitric / Acetic, HNA) and / or TMAH etching. The removal of the sacrificial epitaxial structure 320 and the sacrificial epitaxial plug 220 is a selective etching process, which removes the sacrificial epitaxial structure 320 and the sacrificial epitaxial plug 220 at an etching rate much higher than the etching rate used to etch the isolation structure 130 and the isolation material 330. However, portions of the isolation structure 130 may be unintentionally removed, such as Fig.18C shown.

[0148] In some embodiments, the bottom epitaxial structure 230 is partially removed just below the sacrificial epitaxial plug 220. In other embodiments, a portion of the top epitaxial structure 240 is also removed just below the removed bottom epitaxial structure 230. In addition, the inner spacer 210 is partially removed so that the recess 334 can be formed adjacent to the inner spacer 210.

[0149] refer to 19A to 19D ,in Fig.19B For along Fig.19A The cross-sectional view taken along line BB in FIG. Fig.19C For along Fig.19A A cross-sectional view taken along line CC in FIG. Fig.19D For along Fig.19A The back contact etch stop layer 340 is formed in the opening 332 and the recess 334 (see Fig.18B) is conformally formed in a silicon nitride film. In some embodiments, the back contact etch stop layer 340 is formed of Si3N4. In some other embodiments, the back contact etch stop layer 340 includes a material such as an oxynitride. In still other embodiments, the back contact etch stop layer 340 may have a composite structure including a plurality of layers, such as a silicon nitride layer overlying a silicon oxide layer. The back contact etch stop layer 340 may be formed using plasma enhanced CVD (PECVD), however, other suitable methods may also be used, such as low pressure CVD (LPCVD), atomic layer deposition (ALD), and the like.

[0150] Subsequently, the horizontal portion of the backside contact etch stop layer 340 is removed to expose the etched top epitaxial structure 240, which serves as the source of the semiconductor device. Meanwhile, the other epitaxial structure 240 serving as the drain of the semiconductor device is covered by the isolation material 330.

[0151] At least one backside metal alloy layer 350 is formed on the etched top epitaxial structure 240. The backside metal alloy layer 350, which may be a silicide layer, is formed in the opening 332 by a self-aligned silicide (salicide) process (see Fig.18B ) and formed over the exposed top epitaxial structure 240. In some embodiments, the backside metal alloy layer 350 may include a material selected from the group consisting of titanium silicide, cobalt silicide, nickel silicide, platinum silicide, nickel platinum silicide, erbium silicide, palladium silicide, combinations thereof, or other suitable materials. In some embodiments, the backside metal alloy layer 350 may include germanium.

[0152] Next, in the opening 332 (see Fig.18B ) and a backside via 360 is formed on the backside metal alloy layer 350. Thus, the backside via 360 is electrically connected to the etched top epitaxial structure 240. In some embodiments, the backside via 360 can be made of a metal such as W, Co, Ru, Al, Cu, or other suitable materials. After the backside via 360 is deposited, a planarization process such as a chemical mechanical planarization (CMP) process can then be performed. In some embodiments, a barrier layer can be formed in the opening 322 before the backside via 360 is formed. The barrier layer can be made of TiN, TaN, or a combination thereof.

[0153] refer to FIG. 20A to FIG. 20D ,in Fig. 20B For along Fig. 20A The cross-sectional view taken along line BB in FIG. Fig. 20C For along Fig. 20A A cross-sectional view taken along line CC in FIG. Fig.20D For along Fig. 20A DD in FIG. A backside multilayer interconnection (multilayer interconnection structure) 370 including a metal layer and an inter-metal dielectric (IMD) is formed over the isolation structure 130 and the isolation material 330 to electrically connect various features or structures (e.g., one or more backside vias 360) of the semiconductor device. The backside multilayer interconnection structure 370 includes vertical connections such as vias or contacts 372 and horizontal connections such as metal lines 374. Various interconnect features may be implemented with various conductive materials including copper, tungsten, and silicide. In some examples, a damascene process is used to form the copper multilayer interconnection structure.

[0154] The carrier substrate 410 is then removed from the front multilayer interconnect structure 290 (see 19A to 19D ), and the structure is "turned upside down" again. Thus, a semiconductor device is formed. Specifically, the semiconductor device includes a second semiconductor layer 124 as a channel layer of the semiconductor device. The second semiconductor layers 124 are arranged one above the other in a spaced-apart manner. The gate structure 260 surrounds or wraps each of the second semiconductor layers 124. In some embodiments, the channel length L of the second semiconductor layer 124 is in the range of about 5nm to about 150nm. The semiconductor device also includes an S / D epitaxial structure (e.g., a top epitaxial structure 240 and / or a bottom epitaxial structure 230) as a source and / or drain of the semiconductor device. The S / D epitaxial structure is electrically connected to the second semiconductor layer 124 and on the opposite side of the gate structure 260. The S / D epitaxial structure can be connected to an external circuit from the front side of the semiconductor device via a contact 280. Some of the S / D epitaxial structures (e.g., the top epitaxial structure 240 connected to the backside through-hole member 360) can be further connected to an external circuit from the back side of the semiconductor device via the backside through-hole member 360. Each of the gate structure 260 and the S / D epitaxial structure has a front side facing upward and a back side facing downward. The front multilayer interconnect structure 290 is above the front side of the gate structure 260 and the S / D epitaxial structure, and the back side via 360 is connected to the back side of one of the S / D epitaxial structures.

[0155] Fig.20E for Fig. 20B Magnified view of area A in . Fig. 20B and Fig.20E, the backside through-hole member 360 includes a first portion 362, a second portion 364, and a third portion 366 between the first portion 362 and the second portion 364. The first portion 362 is closer to the top epitaxial structure 240 than the second portion 364. The first portion 362 has a substantially constant width, the second portion 364 has a substantially constant width, and the third portion 366 has a tapered sidewall 366s. That is, the third portion 366 has a width variation greater than the width variation of the first portion 362 and the width variation of the second portion 364. The width W1 of the first portion 362 is less than the width W2 of the second portion 364, so that the third portion 366 tapers from the second portion 364 toward the first portion 362. In some embodiments, the width W1 of the first portion 362 is in a range of about 5 nm to about 25 nm. In some embodiments, the width W2 of the second portion 364 is in a range of about 10 nm to about 45 nm. In addition, a height H2 of the backside via 360 is in the range of about 15 nm to about 50 nm.

[0156] In some embodiments, the angle θ1 is formed between the sidewall 366s of the third portion 366 and the sidewall 362s of the first portion 362, and the angle θ2 is greater than about 140 degrees and less than about 180 degrees, for example, about 144.7 degrees to about 179 degrees. Fig. 17B ). In some embodiments, the angle θ2 is formed between the sidewall 366s of the third portion 366 and the sidewall 364s of the second portion 364, and the angle θ1 is greater than about 140 degrees and less than about 180 degrees, for example, about 144.7 degrees to about 179 degrees. The angle θ2 is determined by the shape of the sacrificial epitaxial structure 320 (see Fig. 17B In some embodiments, the angle θ3 is formed between the sidewall 364s of the second portion 364 and the interface 375 between the back-side multilayer interconnect structure 370 and the back-side through-hole member 360, and the angle θ3 is in the range of about 54.7 degrees to about 90 degrees, for example, about 90 degrees.

[0157] In some embodiments, the semiconductor device further includes sidewall spacers 310 on opposite sides of the first portion 362 of the backside via 360. The sidewall spacers 310 are offset from the second portion 364 of the backside via 360 and aligned with the first portion 362 of the backside via 360. Fig. 20A As shown, the sidewall spacer 310 further contacts the bottom epitaxial structure 230. The height H1 of the sidewall spacer 310 is less than about 40 nm. If the height is greater than about 40 nm, the sacrificial epitaxial plug 220 (see Fig. 17B ) may not have sufficient surface area for growing sacrificial epitaxial structure 320 (see Fig. 17B). The height H2 of the backside via 360 is greater than the height H1 of the sidewall spacer 310, so that the width W2 of the second portion 364 is greater than the width W1 of the first portion 362. In some embodiments, each of the sidewall spacers 310 has a thickness T1 that is less than about 15 nm. If the thickness T1 is greater than about 15 nm, the sidewall spacers 310 cannot be conformally formed and merge between the isolation structures 130. In addition, the sidewall spacers 310 are spaced apart from the dummy fin structure 150. The uppermost surface 314 of the sidewall spacer 310 is higher than the bottommost surface 261 of the gate structure 260. In addition, the sidewall spacers 310 are spaced apart from the dummy fin structure 150.

[0158] In some embodiments, the semiconductor device further includes isolation material 330 on opposite sides of the backside via 360. Fig. 20B and Fig.20E As shown, the isolation material 330 includes a portion of the backside surface 312 that contacts the sidewall spacer 310. In addition, as shown in FIG. Fig. 20B and Fig.20D As shown, the isolation material 330 contacts the gate dielectric layer 262 of the gate structure 260, some of the inner spacers 210, some of the bottom epitaxial structure 230, the sidewall spacers 310, and the isolation structure 130. In addition, in some embodiments, the sidewall spacers 310 are sandwiched between the isolation material 330 and the isolation structure 130 and between the isolation material and the backside via 360. The sidewall spacers 310 have a different material than the isolation material 330 and / or the isolation structure 130. For example, the sidewall spacers 310 are a nitride layer and the isolation material 330 and / or the isolation structure 130 are an oxide layer. The height H3 of the isolation material 330 is greater than the height H1 of the sidewall spacers 310.

[0159] In some embodiments, the semiconductor device further includes a backside contact etch stop layer 340 that laterally surrounds the backside via 360. The backside contact etch stop layer 340 is conformal to the sidewalls of the backside via 360. The backside contact etch stop layer 340 contacts the isolation material 330 and the sidewall spacer 310. In some embodiments, due to the recess 334 (see Fig.18B ), the backside contact etch stop layer 340 includes a portion having a larger width that contacts the inner spacer 210.

[0160] like Fig. 20B and Fig.20E As shown, the size of the back side through hole member 340 is due to the sacrifice of the epitaxial structure 320 (see Fig. 17B) is formed. Thus, the contact area between the back-side via 340 and the via 372 of the back-side multilayer interconnect structure 370 is increased. This configuration reduces the total (parasitic) resistance of the interface including the back-side via 340 itself and the back-side via 340 and the via 372 of the back-side multilayer interconnect structure 370 and further improves device performance. In addition, the height H1 of the sidewall spacer 310 can tune the shape of the sacrificial epitaxial structure 320 (see Fig. 17B ), and the desired shape of the back side through-hole member 340 can be obtained.

[0161] Fig.21A is a perspective view of a semiconductor device according to some embodiments of the present disclosure, Fig.21B For along Fig.21A The cross-sectional view taken along line BB in FIG. Fig. 21C For along Fig.21A A cross-sectional view taken along line CC in FIG. Fig.21D For along Fig.21A A cross-sectional view taken along line DD in FIG. FIG. 21A to FIG. 21D Semiconductor devices and FIG. 20A to FIG. 20E The difference between the semiconductor devices in FIG. 1 and FIG. 2 is the presence of the sidewall spacer 310. FIG. 21A to FIG. 21D In the embodiment, these sidewall spacers 310 are omitted (see FIG. 20A to FIG. 20E ). FIG. 21A to FIG. 21D Other relevant structural details of the semiconductor device in FIG. 20A to FIG. 20E The semiconductor devices in are similar or substantially the same, and therefore, the description in this regard will not be repeated below.

[0162] According to some embodiments, a semiconductor device includes a gate structure, a source / drain epitaxial structure, a front-side interconnect structure, a back-side via, an isolation material, and a sidewall spacer. The source / drain epitaxial structure is on one side of the gate structure. The front-side interconnect structure is on a front side of the source / drain epitaxial structure. The back-side via is connected to the back side of the source / drain epitaxial structure. The isolation material is on one side of the back-side via and contacts the gate structure. The sidewall spacer is between the back-side via and the isolation material. The height of the isolation material is greater than the height of the sidewall spacer.

[0163] According to some embodiments, the semiconductor device further includes a backside contact etch stop layer conforming to the sidewall of the backside via. According to some embodiments, the backside contact etch stop layer contacts the isolation material and the sidewall spacer. According to some embodiments, the backside via includes a first portion and a second portion. The second portion is wider than the first portion. The first portion is between the second portion and the source / drain epitaxial structure. According to some embodiments, the semiconductor device further includes a metal alloy layer contacting the first portion of the backside via and the source / drain epitaxial structure. According to some embodiments, the sidewall spacer offsets the second portion of the backside via and is aligned with the first portion of the backside via. According to some embodiments, the semiconductor device further includes an internal spacer between the gate structure and the backside via. According to some embodiments, the sidewall spacer contacts the internal spacer. According to some embodiments, the isolation material contacts the internal spacer.

[0164] According to some embodiments, a semiconductor device includes a plurality of channel layers, a gate structure, a first source / drain epitaxial structure, an internal spacer, a backside via, a sidewall spacer, and an isolation material. The channel layers are arranged one on top of another in a spaced-apart manner. The gate structure surrounds each channel layer. The first source / drain epitaxial structure is on one side of the gate structure and connected to the channel layer. The internal spacer is between the gate structure and the first source / drain epitaxial structure. The backside via is connected to the back side of the first source / drain epitaxial structure. The sidewall spacer contacts the gate structure and is on one side of the backside via. The isolation material is on the side of the backside via and contacts the gate structure and the sidewall spacer.

[0165] According to some embodiments, the sidewall spacer further contacts the internal spacer. According to some embodiments, the semiconductor device further includes a second source / drain epitaxial structure on the other side of the gate structure and connected to the channel layer, and the sidewall spacer further contacts the second source / drain epitaxial structure. According to some embodiments, the semiconductor device further includes a second source / drain epitaxial structure on the other side of the gate structure and connected to the channel layer, and the isolation material further contacts the second source / drain epitaxial structure. According to some embodiments, the topmost surface of the sidewall spacer is higher than the bottommost surface of the gate structure. According to some embodiments, the semiconductor device further includes a dummy fin structure adjacent to the gate structure and the first source / drain epitaxial structure and separated from the sidewall spacer.

[0166] According to some embodiments, a method for manufacturing a semiconductor device includes etching a recess in a substrate. Forming a sacrificial epitaxial plug in the recess in the substrate. Forming a source / drain epitaxial structure above the sacrificial epitaxial plug. Forming a gate structure on one side of the source / drain epitaxial structure. Removing the substrate so that the sacrificial epitaxial plug protrudes from a back side of the source / drain epitaxial structure. Forming a sidewall spacer on one side of the sacrificial epitaxial plug so that a portion of the sacrificial epitaxial plug is exposed by the sidewall spacer. Forming a sacrificial epitaxial structure on the portion of the sacrificial epitaxial plug exposed by the sidewall spacer. Forming an isolation material on one side of the sacrificial epitaxial structure and on the sidewall spacer. Replacing the sacrificial epitaxial plug and the sacrificial epitaxial structure with a backside through-hole member.

[0167] According to some embodiments, the above method further includes forming an isolation structure in the substrate before etching the recess in the substrate. According to some embodiments, forming a sidewall spacer such that the sidewall spacer contacts the isolation structure. According to some embodiments, forming the sidewall spacer includes forming a blanket dielectric layer over the sidewall of the sacrificial epitaxial plug and conforming to the sidewall of the sacrificial epitaxial plug. Etching back the blanket dielectric layer to form the sidewall spacer. According to some embodiments, forming the isolation material such that the isolation material is spaced apart from the sacrificial epitaxial plug.

[0168] The foregoing summarizes the features of several embodiments so that those skilled in the art can better understand the aspects of the present disclosure. Those skilled in the art will appreciate that they can easily use the present disclosure as a basis for designing or modifying other processes and structures for achieving the same purposes and / or achieving the same advantages as the embodiments described herein. Those skilled in the art will also recognize that these equivalent constructions do not depart from the spirit and scope of the present disclosure, and that they can make various changes, substitutions, and modifications herein without departing from the spirit and scope of the present disclosure.

Claims

1. A semiconductor device, characterized in that: Include: a gate structure; a source / drain epitaxial structure on one side of the gate structure; a front-side interconnect structure on a front side of the source / drain epitaxial structure; a backside through-hole connected to a backside of the source / drain epitaxial structure; an isolation material on one side of the backside via and contacting the gate structure; and A sidewall spacer is between the backside through-hole component and the isolation material, wherein a height of the isolation material is greater than a height of the sidewall spacer.

2. The semiconductor device according to claim 1, wherein: A backside contact etch stop layer is also included, which is conformal to a side wall of the backside through-hole component.

3. The semiconductor device according to claim 2, wherein: The backside contact etch stop layer contacts the isolation material and the sidewall spacer.

4. The semiconductor device according to claim 1, wherein: The back side through hole component comprises: - Part I; and A second portion is wider than the first portion, wherein the first portion is between the second portion and the source / drain epitaxial structure.

5. The semiconductor device according to claim 4, wherein: A metal alloy layer is also included, contacting the first portion of the back-side through-hole component and the source / drain epitaxial structure.

6. The semiconductor device according to claim 4, wherein: The sidewall spacer is offset from the second portion of the backside via and aligned with the first portion of the backside via.

7. The semiconductor device according to claim 1, wherein: An inner spacer is also included between the gate structure and the backside through-hole component.

8. The semiconductor device according to claim 7, wherein: The sidewall spacer contacts the inner spacer.

9. The semiconductor device according to claim 8, wherein: The isolation material contacts the inner spacer.

10. A semiconductor device, characterized in that: Include: A plurality of channel layers are arranged one above the other in a spaced-apart manner; a gate structure surrounding each of the channel layers; a first source / drain epitaxial structure on one side of the gate structure and connected to the plurality of channel layers; an inner spacer between the gate structure and the first source / drain epitaxial structure; a backside through-hole member connected to a backside of the first source / drain epitaxial structure; a sidewall spacer contacting the gate structure and on one side of the backside via; and An isolation material is on the side of the backside via and contacts the gate structure and the sidewall spacer.

11. The semiconductor device according to claim 10, wherein: The sidewall spacer also contacts the inner spacer.

12. The semiconductor device according to claim 10, wherein: A second source / drain epitaxial structure is also included, which is on the other side of the gate structure and connected to the channel layers, and the sidewall spacer also contacts the second source / drain epitaxial structure.

13. The semiconductor device according to claim 10, wherein: A second source / drain epitaxial structure is also included, which is on the other side of the gate structure and connected to the channel layers, and the isolation material also contacts the second source / drain epitaxial structure.

14. The semiconductor device according to claim 10, wherein: An uppermost surface of the sidewall spacer is higher than a bottommost surface of the gate structure.

15. The semiconductor device according to claim 10, wherein: A dummy fin structure is also included, which is adjacent to the gate structure and the first source / drain epitaxial structure and is spaced apart from the sidewall spacer.

16. A method for manufacturing a semiconductor device, characterized in that: Include: etching a recess in a substrate; forming a sacrificial epitaxial plug in the recess in the substrate; forming a source / drain epitaxial structure above the sacrificial epitaxial plug; forming a gate structure on one side of the source / drain epitaxial structure; removing the substrate so that the sacrificial epitaxial plug protrudes from a back side of the source / drain epitaxial structure; forming a sidewall spacer on one side of the sacrificial epitaxial plug so that a portion of the sacrificial epitaxial plug is exposed by the sidewall spacer; forming a sacrificial epitaxial structure on the portion of the sacrificial epitaxial plug exposed by the sidewall spacer; forming an isolation material on one side of the sacrificial epitaxial structure and the sidewall spacer; and The sacrificial epitaxial plug and the sacrificial epitaxial structure are replaced with a backside via.

17. The method according to claim 16, characterized in that The method also includes forming an isolation structure in the substrate before etching the recess in the substrate.

18. The method according to claim 17, characterized in that The sidewall spacer is formed such that the sidewall spacer contacts the isolation structure.

19. The method according to claim 16, characterized in that Forming the sidewall spacer includes: forming a blanket dielectric layer over and conforming to the sidewalls of the sacrificial epitaxial plug; and The blanket dielectric layer is etched back to form the sidewall spacers.

20. The method according to claim 16, characterized in that The isolation material is formed such that the isolation material is spaced apart from the sacrificial epitaxial plug.

Citation Information

Patent Citations

  • semiconductor component WITH AIR SPACER

    DE102017113681A1

  • Backside contacts for semiconductor devices

    TW202101705A