Polarizing plate with phase difference layer

By using the protective layer and phase difference layer design of thermoplastic acrylic resin in a polarizing plate with phase difference layer, the problem of reducing optical characteristics in a heating and humidification environment is solved, and a thinner and high durability polarizing plate is achieved, with good performance. Anti-reflection characteristics.

CN113227854BActive Publication Date: 2024-11-05NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980086368.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-12-27
Filing Date
2019-12-26
Publication Date
2024-11-05
Estimated Expiration
2039-12-26

AI Technical Summary

Technical Problem

The existing polarizer with phase difference layer has reduced optical characteristics and durability in a heating and humidification environment, making it difficult to maintain thinner performance.

Method used

The organic solvent solution of thermoplastic acrylic resin is used as the material for the protective layer, and a thin layer is formed by curing, and the glass transition temperature is set to 95°C or above. At the same time, a phase difference layer is arranged on the visual identification side of the polarizing plate, and a single layer or layer is used. Structural phase difference layer design.

Benefits of technology

A polarizing plate that maintains optical characteristics and durability in a heating and humidified environment is realized, ensuring thinner and high durability of the polarizing plate, while avoiding shrinkage of the protective layer and enhancing the anti-reflection characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113227854B_ABST
    Figure CN113227854B_ABST
Patent Text Reader

Abstract

A polarizing plate with a phase difference layer that is very thin and has excellent durability is provided. The polarizing plate with a phase difference layer of the present invention comprises a polarizing plate and a phase difference layer, wherein the polarizing plate comprises a polarizer and a protective layer disposed on one side of the polarizer, and the phase difference layer is disposed on the side of the polarizing plate opposite to the protective layer. The protective layer is composed of a cured product of a coating film of an organic solvent solution of a thermoplastic acrylic resin, and the glass transition temperature of the protective layer is above 95°C. In one embodiment, the thickness of the protective layer is 10 μm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polarizing plate with a phase difference layer. Background Art

[0002] In an image display device (such as a liquid crystal display device, an organic EL display device), due to its image formation method, a polarizing plate is often configured on at least one side of the display unit. Furthermore, in practice, a phase difference plate is often used in combination with a polarizing plate, and a polarizing plate with a phase difference layer formed by integrating a polarizing plate with a phase difference plate is widely used (for example, patent document 1). In recent years, image display devices have been further thinned and flexible, and as a result, there is also a strong demand for the thinning of polarizing plates with phase difference layers. However, the thinner the polarizing plate with a phase difference layer, the more significant the problem of reduced durability of optical properties in a heated and humidified environment.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent No. 3325560 Summary of the invention

[0006] Problem that the invention aims to solve

[0007] The present invention has been made to solve the above-mentioned conventional problems, and a main object of the present invention is to provide a polarizing plate with a retardation layer which is excellent in durability even though it is very thin.

[0008] Solutions for solving problems

[0009] The polarizing plate with a phase difference layer of the present invention comprises a polarizing plate and a phase difference layer, wherein the polarizing plate comprises a polarizer and a protective layer disposed on one side of the polarizer, and the phase difference layer is disposed on the side of the polarizing plate opposite to the protective layer. The protective layer is composed of a solidified product of a coating film of an organic solvent solution of a thermoplastic acrylic resin, and the glass transition temperature of the protective layer is above 95°C.

[0010] In one embodiment, the phase difference layer is a single layer, the Re (550) of the phase difference layer is 100nm to 190nm, and the angle between the slow axis of the phase difference layer and the absorption axis of the polarizer is 40° to 50°. In this case, the phase difference layer can be a resin film or an oriented solidified layer of a liquid crystal compound.

[0011] In another embodiment, the phase difference layer has a stacked structure of a first layer and a second layer; the Re (550) of the first layer is 200nm to 300nm, and the angle between its slow axis and the absorption axis of the polarizer is 10° to 20°; the Re (550) of the second layer is 100nm to 190nm, and the angle between its slow axis and the absorption axis of the polarizer is 70° to 80°. In this case, the first layer and the second layer can be a resin film or an orientation solidification layer of a liquid crystal compound.

[0012] In one embodiment, the protective layer has a thickness of 10 μm or less.

[0013] In one embodiment, the protective layer has an iodine adsorption amount of 4.0 wt % or less.

[0014] In one embodiment, the thermoplastic acrylic resin has at least one selected from the group consisting of a lactone ring unit, a glutaric anhydride unit, a glutarimide unit, a maleic anhydride unit, and a maleimide unit.

[0015] In one embodiment, the polarizing plate with a retardation layer is disposed on a viewing side of an image display device, and the protective layer is disposed on a viewing side.

[0016] Effects of the Invention

[0017] According to the present invention, a polarizing plate with a retardation layer having excellent durability even though it is very thin can be obtained by forming a protective layer in the polarizing plate with a retardation layer with a cured product of a coating film of an organic solvent solution of a thermoplastic acrylic resin and setting its glass transition temperature to a predetermined value or higher. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The figure is a schematic cross-sectional view of a polarizing plate with a phase difference layer according to one embodiment of the present invention.

[0019] Figure 2 This is a schematic cross-sectional view of a polarizing plate with a phase difference layer according to another embodiment of the present invention.

[0020] Figure 3 This is a schematic diagram showing an example of a drying shrinkage treatment using a heating roll in a method for producing a polarizing plate that can be used in a polarizing plate with a retardation layer according to an embodiment of the present invention. DETAILED DESCRIPTION

[0021] (Definition of terms and symbols)

[0022] The definitions of terms and symbols in this specification are as follows.

[0023] (1) Refractive index (nx, ny, nz)

[0024] "nx" is the refractive index in the direction where the refractive index in the plane is the maximum (ie, the slow axis direction), "ny" is the refractive index in the direction orthogonal to the slow axis in the plane (ie, the fast axis direction), and "nz" is the refractive index in the thickness direction.

[0025] (2) In-plane phase difference (Re)

[0026] "Re(λ)" is the in-plane phase difference measured at 23°C using light of wavelength λnm. For example, "Re(550)" is the in-plane phase difference measured at 23°C using light of wavelength 550nm. Re(λ) is obtained by the formula: Re(λ) = (nx-ny) × d, assuming the thickness of the layer (film) is d (nm).

[0027] (3) Retardation in the thickness direction (Rth)

[0028] "Rth(λ)" is the phase difference in the thickness direction measured at 23°C using light of wavelength λnm. For example, "Rth(550)" is the phase difference in the thickness direction measured at 23°C using light of wavelength 550nm. Rth(λ) is calculated by the formula: Rth(λ) = (nx-nz) × d, assuming that the thickness of the layer (film) is d (nm).

[0029] (4) Nz coefficient

[0030] The Nz coefficient is obtained by Nz=Rth / Re.

[0031] (5) Angle

[0032] When an angle is mentioned in this specification, the angle includes both clockwise and counterclockwise angles relative to a reference direction. Therefore, for example, "45°" means ±45°.

[0033] A. Overview of polarizing plate with phase difference layer

[0034] Figure 1Schematic cross-sectional view of a polarizing plate with a phase difference layer according to an embodiment of the present invention. The polarizing plate 100 with a phase difference layer shown in the figure has: a polarizer 10, a protective layer 20 arranged on one side of the polarizer 10, and a phase difference layer 40 arranged on the other side of the polarizer 10. The polarizer 10 and the protective layer 20 constitute a polarizing plate. Therefore, the polarizing plate with a phase difference layer has: a polarizing plate including a polarizer and a protective layer arranged on one side of the polarizer; and a phase difference layer arranged on the side of the polarizing plate opposite to the protective layer. As needed, the polarizing plate may also include another protective layer (not shown) on the side of the polarizer 10 opposite to the protective layer 20. In other words, the polarizing plate 100 with a phase difference layer may also include another protective layer (not shown) between the polarizer 10 and the phase difference layer 40. In the polarizing plate with a phase difference layer, the thickness of the polarizer 10 is preferably less than 8 μm.

[0035] Figure 1 In the embodiment shown, the phase difference layer 40 is a single layer. In this case, Re (550) of the phase difference layer 40 is, for example, 100 nm to 190 nm, and the angle between the slow axis of the phase difference layer 40 and the absorption axis of the polarizer 10 is, for example, 40° to 50°. In this case, it is preferred that another phase difference layer (not shown) is provided on the outside of the phase difference layer 40 (on the side opposite to the polarizer 10). For the other phase difference layer, typically, the refractive index characteristic shows the relationship of nz>nx=ny. Or, as Figure 2 As shown, in the polarizing plate 101 with a phase difference layer of another embodiment, the phase difference layer 40 has a stacked structure of a first layer 41 and a second layer 42. In this case, Re (550) of the first layer 41 is, for example, 200nm to 300nm, and the angle between the slow axis of the first layer 41 and the absorption axis of the polarizer 10 is, for example, 10° to 20°; Re (550) of the second layer 42 is, for example, 100nm to 190nm, and the angle between the slow axis of the second layer 42 and the absorption axis of the polarizer 10 is, for example, 70° to 80°. In any embodiment, the phase difference layer 40 can be a resin film or an oriented solidified layer of a liquid crystal compound. When the phase difference layer 40 has a stacked structure, typically, the first layer 41 and the second layer 42 are respectively oriented solidified layers of a resin film or a liquid crystal compound.

[0036] In an embodiment of the present invention, the protective layer 20 is composed of a cured product of a coating film of an organic solvent solution of a thermoplastic acrylic resin. When such a composition is used, the protective layer can be made very thin (for example, less than 10 μm). Furthermore, the protective layer can be formed directly (that is, without an adhesive layer or an adhesive layer) on the polarizer. According to an embodiment of the present invention, as described above, the polarizer and the protective layer are very thin, and the adhesive layer or the adhesive layer can be omitted, so the total thickness of the polarizing plate with a phase difference layer can be made very thin. In the case where the phase difference layer is composed of a resin film, the total thickness of the polarizing plate with a phase difference layer is, for example, less than 80 μm, preferably less than 70 μm, and more preferably less than 60 μm. The lower limit of the total thickness of the polarizing plate with a phase difference layer can be, for example, 30 μm. In the case where the phase difference layer is composed of an oriented solidified layer of a liquid crystal compound, the total thickness of the polarizing plate with a phase difference layer is, for example, less than 25 μm, preferably less than 22 μm, and more preferably less than 20 μm. The lower limit of the total thickness of the polarizing plate with a phase difference layer can be, for example, 10 μm.

[0037] Furthermore, in an embodiment of the present invention, the glass transition temperature (Tg) of the protective layer 20 is above 95°C, preferably above 100°C, more preferably above 105°C, further preferably above 110°C, and particularly preferably above 115°C. When the Tg of the protective layer is within such a range, a polarizing plate (resulting in a polarizing plate with a phase difference layer) having excellent durability even when it is very thin can be realized by utilizing the synergistic effect of the effect brought about by the cured product of the coating film of the organic solvent solution of the thermoplastic acrylic resin constituting the protective layer. Specifically, a polarizing plate (resulting in a polarizing plate with a phase difference layer) in which the reduction of optical properties is suppressed even in a heated and humidified environment can be realized. On the other hand, the Tg of the protective layer is preferably below 300°C, more preferably below 250°C, further preferably below 200°C, and particularly preferably below 160°C. When the Tg of the protective layer is within such a range, excellent formability can be used.

[0038] As described above, according to an embodiment of the present invention, a polarizing plate (a polarizing plate with a phase difference layer) can be realized in which the reduction of optical characteristics is suppressed even in a heated and humidified environment. The change ΔTs of the single transmittance Ts and the change ΔP of the polarization degree P of such a polarizing plate (a polarizing plate with a phase difference layer) after being placed in an environment of 85°C and 85% RH for 48 hours are very small. The single transmittance Ts can be measured using, for example, an ultraviolet-visible spectrophotometer (manufactured by JASCO Corporation, product name "V7100"). The polarization degree P is calculated using the following formula from the single transmittance (Ts), parallel transmittance (Tp) and orthogonal transmittance (Tc) measured using an ultraviolet-visible spectrophotometer.

[0039] Polarization degree (P) (%) = {(Tp-Tc) / (Tp+Tc)}1 / 2 ×100

[0040] It should be noted that the above Ts, Tp and Tc are Y values ​​obtained by measuring using a 2 degree field of view (C light source) of JIS Z 8701 and performing a sensitivity correction. In addition, Ts and P are substantially characteristics of the polarizer. ΔTs and ΔP are respectively obtained by the following formulas.

[0041] ΔTs(%)=Ts 48 -Ts 0

[0042] ΔP(%)=P 48 -P 0

[0043] Here, Ts 0 is the monomer transmittance before placement (initial), Ts 48 is the monomer transmittance after placement, P 0 is the polarization degree before placement (initial), P 48 is the degree of polarization after standing. ΔTs is preferably 3.0% or less, more preferably 2.7% or less, and even more preferably 2.4% or less. ΔP is preferably -0.05% to 0%, more preferably -0.03% to 0%, and even more preferably -0.01% to 0%.

[0044] The polarizing plate with a phase difference layer of the present invention may also include phase difference layers other than those mentioned above. The optical properties (such as refractive index properties, in-plane phase difference, Nz coefficient, photoelastic coefficient), thickness, configuration position, etc. of such phase difference layers can be appropriately set according to the purpose.

[0045] The polarizing plate with a phase difference layer of the present invention may also include a conductive layer or an isotropic substrate with a conductive layer (neither of which is shown in the figure). The conductive layer or the isotropic substrate with a conductive layer is typically arranged on the outside of the phase difference layer 40 (the side opposite to the polarizer 10). In the case where a conductive layer or an isotropic substrate with a conductive layer is provided, the polarizing plate with a phase difference layer can be applied to a so-called inner touch panel type input display device in which a touch panel is embedded between a display unit (e.g., a liquid crystal unit, an organic EL unit) and a polarizing plate.

[0046] The polarizing plate with a retardation layer may be in a long strip shape or in a sheet shape. When the polarizing plate with a retardation layer is in a long strip shape, it is preferably wound into a roll to form a polarizing plate roll with a retardation layer.

[0047] Typically, the polarizing plate with a phase difference layer has an adhesive layer as the outermost layer on one side (typically, the phase difference layer 40 side), which can be attached to the display unit. As needed, a surface protection film and / or a carrier film can be temporarily bonded to the polarizing plate with a phase difference layer in a removable manner to enhance and / or support the polarizing plate with a phase difference layer. In the case where the polarizing plate with a phase difference layer includes an adhesive layer, a separator is temporarily bonded to the surface of the adhesive layer in a removable manner, which can protect the adhesive layer until actual use and realize the roll-up of the polarizing plate with a phase difference layer.

[0048] The polarizing plate with phase difference layer of the present invention is very thin as described above, and therefore, it can be suitably used in a flexible image display device. More preferably, the image display device has a curved shape (substantially a curved display screen), and / or can be bent or bent. As a specific example of an image display device, a liquid crystal display device, an electroluminescent (EL) display device (e.g., an organic EL display device, an inorganic EL display device) can be cited. It goes without saying that the above description does not prevent the polarizing plate with phase difference layer of the present invention from being applied to a general image display device.

[0049] Hereinafter, the components of the polarizing plate with a retardation layer will be described in detail.

[0050] B.Polarizing plate

[0051] B-1. Polarizer

[0052] Any appropriate polarizer can be used as the polarizer. The polarizer can be typically produced using a laminate of two or more layers. The method for producing the polarizer will be described in the section D below as the method for producing a polarizing plate.

[0053] The thickness of the polarizer is preferably 1 μm to 8 μm, more preferably 1 μm to 7 μm, and even more preferably 2 μm to 5 μm.

[0054] The boric acid content of the polarizer is preferably 10% by weight or more, more preferably 13% by weight to 25% by weight. As long as the boric acid content of the polarizer is within such a range, the ease of curling adjustment during lamination can be well maintained by the synergistic effect with the iodine content described later, and the curling during heating can be well suppressed, while improving the durability of the appearance during heating. The boric acid content can be calculated, for example, by the neutralization method using the following formula as the amount of boric acid contained in the polarizer per unit weight.

[0055]

[0056] The iodine content of the polarizer is preferably 2% by weight or more, more preferably 2% to 10% by weight. As long as the iodine content of the polarizer is within this range, the synergistic effect with the boric acid content can well maintain the ease of curling adjustment during lamination, and well suppress curling during heating, while improving the durability of the appearance during heating. In this specification, "iodine content" refers to the amount of all iodine contained in the polarizer (PVA-based resin film). More specifically, iodine is present in the polarizer in the form of iodide ions (I - ), iodine molecule (I 2 ), polyiodide ions (I 3 - ,I 5 - ) and other forms, the iodine content in this specification refers to the amount of iodine including all these forms. The iodine content can be calculated, for example, by the standard curve method of fluorescent X-ray analysis. It should be noted that the polyiodide ions exist in the polarizer in the form of a PVA-iodine complex. By forming such a complex, absorption dichroism can be exhibited in the wavelength range of visible light. Specifically, the complex of PVA and triiodide ion (PVA·I 3 - ) has an absorption peak near 470nm, and the complex of PVA and pentaiodide ion (PVA·I 5 - ) has an absorption peak near 600nm. As a result, polyiodide ions can absorb light in a wide range of visible light depending on their form. On the other hand, iodide ions (I - ) has an absorption peak near 230nm and does not substantially participate in the absorption of visible light. Therefore, the polyiodide ions present in the form of a complex with PVA are mainly related to the absorption performance of the polarizer.

[0057] The polarizer preferably exhibits absorption dichroism at any wavelength between 380 nm and 780 nm. The single transmittance Ts of the polarizer is preferably 40% to 48%, more preferably 41% to 46%. The polarization degree P of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and further preferably 99.9% or more.

[0058] B-2. Protective layer

[0059] As described above, the protective layer is composed of a cured product of a coating film of an organic solvent solution of a thermoplastic acrylic resin (hereinafter referred to as an acrylic resin). Components of the protective layer are described in detail below, followed by a description of the characteristics of the protective layer.

[0060] B-2-1. Acrylic resin

[0061] The Tg of the acrylic resin (including a mixture of two or more acrylic resins and a mixture of an acrylic resin and other resins as described later) is as described in the description of the protective layer in the above section A.

[0062] As the acrylic resin, any appropriate acrylic resin can be used as long as it has the Tg as described above. The acrylic resin typically contains an alkyl (meth)acrylate as a main component as a monomer unit (repeating unit). In this specification, "(meth)acrylic acid" refers to acrylic acid and / or methacrylic acid. As the alkyl (meth)acrylate constituting the main skeleton of the acrylic resin, there can be exemplified an alkyl (meth)acrylate having a carbon number of 1 to 18 in a linear or branched alkyl group. These can be used alone or in combination. Furthermore, any appropriate comonomer can be introduced into the acrylic resin by copolymerization. The repeating unit derived from the alkyl (meth)acrylate is typically represented by the following general formula (1):

[0063]

[0064] In the general formula (1), R 4 represents a hydrogen atom or a methyl group, R 5 represents a hydrogen atom or an optionally substituted aliphatic or alicyclic hydrocarbon group having 1 to 6 carbon atoms. Examples of the substituent include halogen and hydroxyl groups. Specific examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, benzyl (meth)acrylate, dicyclopentyloxyethyl (meth)acrylate, dicyclopentyl (meth)acrylate, chloromethyl (meth)acrylate, 2-chloroethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2,3,4,5,6-pentahydroxyhexyl (meth)acrylate, 2,3,4,5-tetrahydroxypentyl (meth)acrylate, methyl 2-(hydroxymethyl)acrylate, ethyl 2-(hydroxymethyl)acrylate, and methyl 2-(hydroxyethyl)acrylate. In the general formula (1), R 5 A hydrogen atom or a methyl group is preferred. Therefore, a particularly preferred alkyl (meth)acrylate is methyl acrylate or methyl methacrylate.

[0065] The acrylic resin may contain only a single (meth)acrylic acid alkyl ester unit, or may contain R 4 and R 5 Different multiple alkyl (meth)acrylate units.

[0066] The content ratio of the (meth) alkyl acrylate unit in the acrylic resin is preferably 50 mol% to 98 mol%, more preferably 55 mol% to 98 mol%, further preferably 60 mol% to 98 mol%, particularly preferably 65 mol% to 98 mol%, and most preferably 70 mol% to 97 mol%. If the content ratio is less than 50 mol%, there is a risk that the effects (e.g., high heat resistance, high transparency) derived from the (meth) alkyl acrylate unit cannot be fully exerted. If the above-mentioned content ratio is greater than 98 mol%, the resin becomes brittle and easily cracked, and the high mechanical strength cannot be fully exerted, resulting in a risk of poor productivity.

[0067] The acrylic resin preferably has a repeating unit containing a ring structure. Examples of the repeating unit containing a ring structure include a lactone ring unit, a glutaric anhydride unit, a glutarimide unit, a maleic anhydride unit, and a maleimide (N-substituted maleimide) unit. The repeating unit containing a ring structure may contain only one type in the repeating unit of the acrylic resin, or may contain two or more types.

[0068] The lactone ring unit is preferably represented by the following general formula (2):

[0069]

[0070] In the general formula (2), R 1 , R 2 and R 3 Each independently represents a hydrogen atom or an organic residue having 1 to 20 carbon atoms. It should be noted that the organic residue may also contain an oxygen atom. The acrylic resin may contain only a single lactone ring unit, or may contain R in the above general formula (2). 1 , R 2 and R 3 A plurality of different lactone ring units. An acrylic resin having a lactone ring unit is described in, for example, Japanese Patent Application Laid-Open No. 2008-181078, the contents of which are incorporated herein by reference.

[0071] The glutarimide unit is preferably represented by the following general formula (3):

[0072]

[0073] In the general formula (3), R 11 and R 12 Each independently represents hydrogen or an alkyl group having 1 to 8 carbon atoms, and R 13 represents an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an aryl group having 6 to 10 carbon atoms. 11 and R 12 are independently hydrogen or methyl, R 13is hydrogen, methyl, butyl or cyclohexyl. 11 is methyl, R 12 is hydrogen, R 13 The acrylic resin may contain only a single glutarimide unit or may contain R in the above general formula (3). 11 , R 12 and R 13 Different multiple glutarimide units. Acrylic resins having glutarimide units are described in, for example, Japanese Patent Publication No. 2006-309033, Japanese Patent Publication No. 2006-317560, Japanese Patent Publication No. 2006-328334, Japanese Patent Publication No. 2006-337491, Japanese Patent Publication No. 2006-337492, Japanese Patent Publication No. 2006-337493, and Japanese Patent Publication No. 2006-337569, and the descriptions of these publications are cited in this specification as reference. It should be noted that the glutaric anhydride unit is excluding the glutaric anhydride unit in the general formula (3) replaced by R 13 Except that the substituted nitrogen atom is replaced by an oxygen atom, the above description on the glutarimide unit is applicable.

[0074] The structures of the maleic anhydride unit and the maleimide (N-substituted maleimide) unit can be identified by their names, and thus a specific description thereof will be omitted.

[0075] The content ratio of the repeating unit containing a ring structure in the acrylic resin is preferably 1 mol% to 50 mol%, more preferably 10 mol% to 40 mol%, and further preferably 20 mol% to 30 mol%. When the content ratio is too low, Tg may be lower than 110°C, and the heat resistance, solvent resistance and surface hardness of the obtained protective layer may become insufficient. When the content ratio is too high, the formability and transparency may be insufficient.

[0076] The acrylic resin may contain repeating units other than the (meth)acrylic acid alkyl ester unit and the repeating unit containing a ring structure. Examples of such repeating units include repeating units derived from vinyl monomers copolymerizable with the monomers constituting the above units (other vinyl monomer units). Examples of other vinyl monomers include acrylic acid, methacrylic acid, crotonic acid, 2-(hydroxymethyl)acrylic acid, 2-(hydroxyethyl)acrylic acid, acrylonitrile, methacrylonitrile, ethacrylonitrile, allyl glycidyl ether, maleic anhydride, itaconic anhydride, N-methylmaleimide, N-ethylmaleimide, N-cyclohexylmaleimide, aminoethyl acrylate, propylaminoethyl acrylate, dimethylaminoethyl methacrylate, ethylaminopropyl methacrylate, cyclohexylaminoethyl methacrylate, N-vinyldiethylamine, N-acetylvinylamine, allylamine, methylallylamine, N-methylallylamine, 2-isopropenyl-oxazoline, 2-vinyl-oxazoline, 2-acryloyl-oxazoline, N-phenylmaleimide, phenylaminoethyl methacrylate, styrene, α-methylstyrene, p-glycidylstyrene, p-aminostyrene, and 2-styryl-oxazoline. These may be used alone or in combination. The type, amount, combination, content ratio, etc. of other vinyl monomer units may be appropriately set depending on the purpose.

[0077] The weight average molecular weight of the acrylic resin is preferably 1,000 to 2,000,000, more preferably 5,000 to 1,000,000, further preferably 10,000 to 500,000, particularly preferably 50,000 to 500,000, and most preferably 60,000 to 150,000. The weight average molecular weight can be obtained by gel permeation chromatography (GPC system, manufactured by Tosoh Corporation) in terms of polystyrene. In addition, tetrahydrofuran can be used as a solvent.

[0078] The acrylic resin may be prepared by appropriately combining the above-mentioned monomer units and polymerizing them by any appropriate polymerization method. Two or more acrylic resins having different monomer units may be mixed.

[0079] In the embodiment of the present invention, acrylic resins and other resins can be used in combination. That is, the monomer components constituting the acrylic resin can be copolymerized with the monomer components constituting other resins, and the copolymer can be used for the formation of the protective layer described later; the mixture of the acrylic resin and other resins can also be used for the formation of the protective layer. As other resins, thermoplastic resins such as styrene resins, polyethylene, polypropylene, polyamide, polyphenylene sulfide, polyetheretherketone, polyester, polysulfone, polyphenylene ether, polyacetal, polyimide, and polyetherimide can be cited. The type and blending amount of the resin used in combination can be appropriately set according to the purpose and the desired properties of the obtained film. For example, a styrene resin (preferably an acrylonitrile-styrene copolymer) can be used in combination as a phase difference controller.

[0080] When an acrylic resin and other resins are used in combination, the content of the acrylic resin in the mixture of the acrylic resin and other resins is preferably 50% by weight to 100% by weight, more preferably 60% by weight to 100% by weight, further preferably 70% by weight to 100% by weight, and particularly preferably 80% by weight to 100% by weight. When the content is less than 50% by weight, there is a risk that the high heat resistance and high transparency inherent in the acrylic resin may not be fully exhibited.

[0081] B-2-2. Composition and characteristics of protective layer

[0082] As described above, the protective layer is composed of a cured product of a coating film of an organic solvent solution of an acrylic resin. As long as it is a cured product of such a coating film, the thickness can be made very thin compared to the thin film of an extruded film. As described above, the thickness of the protective layer is less than 10 μm, preferably less than 7 μm, more preferably less than 5 μm, and further preferably less than 3 μm. The lower limit of the thickness of the protective layer may be, for example, 1 μm. In addition, although it is not clear in theory, the cured product of such a coating film has a smaller shrinkage during film forming than the cured product of a thermosetting (cured) resin or an active energy ray-curing resin (such as an ultraviolet curing resin) and does not contain residual monomers, etc. Therefore, it has the advantage of being able to suppress the deterioration of the film itself and suppressing the adverse effects on the polarizing plate (polarizer) caused by residual monomers, etc. Furthermore, since the hygroscopicity and moisture permeability are smaller than the cured product of an aqueous coating film such as an aqueous solution or an aqueous dispersion, it has the advantage of excellent humidification durability. As a result, a polarizing plate (a polarizing plate with a retardation layer) that can maintain optical properties even in a heated and humidified environment and has excellent durability can be realized.

[0083] The Tg of the protective layer is as described in the above item A.

[0084] The iodine adsorption of the protective layer is preferably 4.0 wt % or less, more preferably 3.0 wt % or less, further preferably 2.0 wt % or less, particularly preferably 1.0 wt % or less, and particularly preferably 0.5 wt % or less. The smaller the iodine adsorption, the more preferred, and its lower limit can be, for example, 0.1 wt %. As long as the iodine adsorption is within such a range, a polarizing plate with better durability (resulting in a polarizing plate with a phase difference layer) can be obtained. The iodine adsorption can be measured using the method described in the embodiments described below.

[0085] The protective layer is preferably substantially optically isotropic. In this specification, "substantially optically isotropic" means that the in-plane phase difference Re(550) is 0nm to 10nm, and the phase difference Rth(550) in the thickness direction is -20nm to +10nm. The in-plane phase difference Re(550) is more preferably 0nm to 5nm, further preferably 0nm to 3nm, and particularly preferably 0nm to 2nm. The phase difference Rth(550) in the thickness direction is more preferably -5nm to 5nm, further preferably -3nm to 3nm, and particularly preferably -2nm to 2nm. When the Re(550) and Rth(550) of the protective layer are within such a range, when a polarizing plate with a phase difference layer including the protective layer is applied to an image display device, adverse effects on the display characteristics can be prevented.

[0086] When the thickness of the protective layer is 3 μm, the higher the transmittance at 380 nm, the more preferred. Specifically, the transmittance is preferably 85% or more, more preferably 88% or more, and further preferably 90% or more. As long as the transmittance is within this range, the desired transparency can be ensured. The transmittance can be measured, for example, by a method according to ASTM-D-1003.

[0087] The lower the haze of the protective layer, the more preferred. Specifically, it is preferably 5% or less, more preferably 3% or less, further preferably 1.5% or less, and particularly preferably 1% or less. As long as the haze is 5% or less, the film can be given a good sense of transparency. Furthermore, even when a polarizing plate with a phase difference layer is used on the visual recognition side of the image display device, the displayed content can be visually recognized well.

[0088] When the thickness of the protective layer is 3 μm, the YI is preferably 1.27 or less, more preferably 1.25 or less, further preferably 1.23 or less, and particularly preferably 1.20 or less. When the YI is greater than 1.3, the optical transparency sometimes becomes insufficient. It should be noted that the YI can be obtained by the following formula using the tristimulus values ​​(X, Y, Z) of the color obtained by measuring using a high-speed integrating sphere spectroscopic transmittance measuring machine (trade name DOT-3C: made by Murakami Color Technology Research Institute).

[0089] YI=[(1.28X-1.06Z) / Y]×100

[0090] The b value (a measure of hue based on the Hunter color system) when the thickness of the protective layer is 3 μm is preferably less than 1.5, and more preferably less than 1.0. When the b value is 1.5 or more, an undesirable hue may sometimes appear. It should be noted that the b value can be obtained, for example, as follows: a sample of a thin film constituting the protective layer is cut into 3 cm squares, the hue is measured using a high-speed integrating sphere spectroscopic transmittance measuring machine (trade name DOT-3C: manufactured by Murakami Color Technology Research Institute), and the hue is evaluated based on the Hunter color system.

[0091] The protective layer (cured product of the coating film) may contain any appropriate additives according to the purpose. Specific examples of additives include ultraviolet absorbers; leveling agents; antioxidants such as hindered phenols, phosphorus, and sulfur; stabilizers such as light stabilizers, weather stabilizers, and heat stabilizers; reinforcing materials such as glass fiber and carbon fiber; near-infrared absorbers; flame retardants such as tris(dibromopropyl) phosphate, triallyl phosphate, and antimony oxide; antistatic agents such as anionic, cationic, and nonionic surfactants; colorants such as inorganic pigments, organic pigments, and dyes; organic fillers or inorganic fillers; resin modifiers; organic fillers or inorganic fillers; plasticizers; lubricants; antistatic agents; flame retardants, etc. Additives may be added during the polymerization of acrylic resins, or added to the solution during film formation. The type, quantity, combination, and addition amount of additives may be appropriately set according to the purpose.

[0092] An easy bonding layer can be formed on the polarizer side of the protective layer. The easy bonding layer, for example, comprises an aqueous polyurethane and an oxazoline crosslinking agent. By forming such an easy bonding layer, the adhesion between the protective layer and the polarizer can be improved. In addition, a hard coating layer can be formed on the protective layer. The hard coating layer can be formed when the protective layer is used as a protective layer on the visual recognition side of the polarizing plate on the visual recognition side. In the case of forming both the easy bonding layer and the hard coating layer, representatively, they can be formed on different sides of the protective layer, respectively.

[0093] B-3. ​​Method for manufacturing polarizing plate

[0094] B-3-1. Method for manufacturing polarizer

[0095] The method for manufacturing the polarizer described in item B-1 above comprises: forming a polyvinyl alcohol resin layer (PVA resin layer) containing a halide and a polyvinyl alcohol resin (PVA resin) on one side of a long thermoplastic resin substrate to form a laminate; and sequentially subjecting the laminate to an air auxiliary stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment, wherein the drying shrinkage treatment heats the laminate while conveying it in the long side direction, thereby shrinking it by more than 2% in the width direction. The content of the halide in the PVA resin layer is preferably 5 to 20 parts by weight relative to 100 parts by weight of the PVA resin. The drying shrinkage treatment is preferably carried out using a heating roller, and the temperature of the heating roller is preferably 60°C to 120°C. According to such a manufacturing method, a polarizer as described above can be obtained. In particular, by making a laminate including a PVA-based resin layer containing a halide, setting the stretching of the above-mentioned laminate to a multi-stage stretching including auxiliary stretching in the air and stretching in water, and heating the stretched laminate using a heating roller, a polarizer having excellent optical properties (representatively, monomer transmittance and polarization degree) and suppressed optical property unevenness can be obtained. Specifically, by using a heating roller in the drying and shrinking treatment process, the laminate can be uniformly shrunk as a whole while conveying the laminate. As a result, not only the optical properties of the obtained polarizer can be improved, but also polarizers with excellent optical properties can be stably produced, and the unevenness of the optical properties of the polarizer (especially monomer transmittance) can be suppressed. Below, halides and drying shrinkage treatment are described. For details of the manufacturing method other than these, for example, it is recorded in Japanese Patent Gazette No. 2012-73580. The entire record of the gazette is cited in this specification as a reference.

[0096] B-3-1-1. Halides

[0097] The PVA resin layer containing a halide and a PVA resin can be formed by applying a coating solution containing a halide and a PVA resin on a thermoplastic resin substrate and drying the coating film. The coating solution is typically a solution in which the halide and the PVA resin are dissolved in a solvent. As solvents, for example, water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, various glycols, polyols such as trimethylolpropane, amines such as ethylenediamine and diethylenetriamine can be cited. These can be used alone or in combination of two or more. Among these, water is preferred. The PVA resin concentration of the solution is preferably 3 to 20 parts by weight relative to 100 parts by weight of the solvent. As long as the resin concentration is such, a uniform coating film that is closely attached to the thermoplastic resin substrate can be formed.

[0098] As the halide, any appropriate halide can be used. Examples thereof include iodide and sodium chloride. As the iodide, examples thereof include potassium iodide, sodium iodide and lithium iodide. Among these, potassium iodide is preferred.

[0099] The amount of the halide in the coating solution is preferably 5 to 20 parts by weight, more preferably 10 to 15 parts by weight, based on 100 parts by weight of the PVA-based resin. If the amount of the halide is too large, the halide may bleed out and the resulting polarizer may become cloudy.

[0100] Generally speaking, after the PVA resin layer is stretched, the orientation of the polyvinyl alcohol molecules in the PVA resin becomes higher. However, if the stretched PVA resin layer is immersed in a water-containing liquid, the orientation of the polyvinyl alcohol molecules is sometimes disordered and the orientation is reduced. In particular, when the laminate of the thermoplastic resin substrate and the PVA resin layer is stretched in boric acid water, in order to stabilize the stretching of the thermoplastic resin substrate, when the laminate is stretched in boric acid water at a relatively high temperature, the tendency for the above-mentioned orientation to decrease is significant. For example, the stretching of the PVA film itself in boric acid water is usually carried out at 60°C. In contrast, the stretching of the laminate of A-PET (thermoplastic resin substrate) and the PVA resin layer is carried out at a relatively high temperature of about 70°C. At this time, the orientation of the PVA at the initial stage of stretching will decrease in the stage before it rises by stretching in water. In this regard, by preparing a laminate of a PVA-based resin layer containing a halide and a thermoplastic resin substrate, and performing high-temperature stretching (auxiliary stretching) in air before stretching the laminate in boric acid water, the crystallization of the PVA-based resin in the PVA-based resin layer of the laminate after auxiliary stretching can be promoted. As a result, when the PVA-based resin layer is immersed in a liquid, the orientation disorder and the reduction of the orientation of the polyvinyl alcohol molecules can be suppressed more than when the PVA-based resin layer does not contain a halide. As a result, the optical properties of the polarizer obtained by the treatment process of immersing the laminate in a liquid such as dyeing treatment and underwater stretching treatment can be improved.

[0101] B-3-1-2. Drying shrinkage treatment

[0102] The drying shrinkage treatment can be carried out by heating the region as a whole, or by heating the conveying roller (using the so-called heating roller) (heating roller drying method). Preferably, both are used. By using a heating roller to dry it, the heating curling of the laminate can be effectively suppressed, and a polarizer with excellent appearance can be manufactured. Specifically, by drying the laminate along the heating roller, the crystallization of the above-mentioned thermoplastic resin substrate can be effectively promoted to increase the degree of crystallization, even at a lower drying temperature, the degree of crystallization of the thermoplastic resin substrate can be well increased. As a result, the rigidity of the thermoplastic resin substrate increases and becomes a state that can withstand the shrinkage of the PVA-based resin layer caused by drying, so that curling is suppressed. In addition, by using a heating roller, the laminate can be dried while maintaining a flat state, so that not only the generation of curling can be suppressed, but also the generation of wrinkles can be suppressed. At this time, the laminate shrinks in the width direction by the drying shrinkage treatment, so that the optical properties can be improved. This is because the orientation of PVA and PVA / iodine complex can be effectively improved. The shrinkage rate of the laminate in the width direction based on the drying shrinkage treatment is preferably 2% to 10%, more preferably 2% to 8%, and particularly preferably 4% to 6%. By using a heated roller, the laminate can be continuously shrunk in the width direction while being conveyed, and high productivity can be achieved.

[0103] Figure 3 Schematic diagram showing an example of drying shrinkage treatment. In the drying shrinkage treatment, the laminate 200 is dried while being transported by using conveying rollers R1 to R6 and guide rollers G1 to G4 heated to a predetermined temperature. In the example shown in the figure, the conveying rollers R1 to R6 are arranged so as to alternately and continuously heat the surface of the PVA resin layer and the surface of the thermoplastic resin substrate, but, for example, the conveying rollers R1 to R6 may be arranged so as to continuously heat only one surface of the laminate 200 (for example, the surface of the thermoplastic resin substrate).

[0104] The drying conditions can be controlled by adjusting the heating temperature of the conveying roller (the temperature of the heating roller), the number of heating rollers, the contact time with the heating roller, etc. The temperature of the heating roller is preferably 60°C to 120°C, more preferably 65°C to 100°C, and particularly preferably 70°C to 80°C. An optical laminate with excellent durability can be produced while the degree of crystallization of the thermoplastic resin can be increased well and curling can be suppressed well. It should be noted that the temperature of the heating roller can be measured using a contact thermometer. In the example shown in the figure, 6 conveying rollers are provided, but there is no particular limitation as long as there are multiple conveying rollers. Conveying rollers are usually provided in 2 to 40 numbers, preferably 4 to 30 numbers. The contact time (total contact time) between the laminate and the heating roller is preferably 1 second to 300 seconds, more preferably 1 to 20 seconds, and further preferably 1 to 10 seconds.

[0105] The heating roller can be set in a heating furnace (such as an oven) or in a general manufacturing line (under room temperature environment). It is preferably set in a heating furnace equipped with air supply means. By combining the drying based on the heating roller and the hot air drying, the rapid temperature change between the heating rollers can be suppressed, and the shrinkage in the width direction can be easily controlled. The temperature of the hot air drying is preferably 30°C to 100°C. In addition, the hot air drying time is preferably 1 second to 300 seconds. The wind speed of the hot air is preferably about 10m / s to 30m / s. It should be noted that the wind speed is the wind speed in the heating furnace, which can be measured using a mini fan-type digital anemometer.

[0106] It is preferred that a washing treatment be performed after the underwater stretching treatment and before the drying shrinkage treatment. The above-mentioned washing treatment can be typically performed by immersing the PVA-based resin layer in an aqueous potassium iodide solution.

[0107] Thereby, a laminate of thermoplastic resin substrate / polarizer can be obtained.

[0108] B-3-2. Method for manufacturing polarizing plate

[0109] The protective layer is formed by applying an organic solvent solution of an acrylic resin on the surface of the laminate obtained in the above section B-3-1 to form a coating film, and curing the coating film.

[0110] The acrylic resin is as described in the above section B-2-1.

[0111] As the organic solvent, any appropriate organic solvent that can dissolve or uniformly disperse the acrylic resin can be used. Specific examples of the organic solvent include ethyl acetate, toluene, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), cyclopentanone, and cyclohexanone.

[0112] The acrylic resin concentration of the solution is preferably 3 to 20 parts by weight relative to 100 parts by weight of the solvent. With such a resin concentration, a uniform coating film that is closely attached to the polarizer can be formed.

[0113] The solution can be applied to any appropriate substrate, and can also be applied to a polarizer. When the solution is applied to the substrate, the cured product of the coating film formed on the substrate is transferred to the polarizer. When the solution is applied to the polarizer, a protective layer is directly formed on the polarizer by drying (curing) the coating film. More preferably, the solution is applied to the polarizer to form a protective layer directly on the polarizer. As long as it is such a structure, the adhesive layer or adhesive layer required for transfer can be omitted, so the polarizing plate with a phase difference layer can be made thinner. As a coating method for the solution, any appropriate method can be adopted. As a specific example, roller coating, spin coating, wire rod coating, dip coating, die coating, curtain coating, spray coating, and blade coating (comma coating, etc.) can be cited.

[0114] By drying (curing) the coating film of the solution, a protective layer can be formed. The drying temperature is preferably 100 °C or lower, more preferably 50 °C to 70 °C. As long as the drying temperature is within such a range, adverse effects on the polarizing element can be prevented. The drying time can vary according to the drying temperature. The drying time can be, for example, 1 minute to 10 minutes.

[0115] By performing the above operations to form a protective layer, as a result, a laminate of a thermoplastic resin substrate / polarizing element / protective layer can be obtained. By peeling the thermoplastic resin substrate from this laminate, a polarizing plate having a polarizing element 10 and a protective layer 20 as shown in Figure 1 and Figure 2 can be obtained. By forming a retardation layer 40 on the surface of the polarizing element of such a polarizing plate, a polarizing plate with a retardation layer can be obtained. Alternatively, a resin film constituting the retardation layer can be adhered to the surface of the polarizing element of the laminate of the thermoplastic resin substrate / polarizing element, and then the thermoplastic resin substrate can be peeled off to form a protective layer on the peeled surface. In this case, a polarizing plate with a retardation layer can be obtained with high manufacturing efficiency. It should be noted that regarding the formation of the retardation layer, a method well-known in the industry is adopted, so detailed description is omitted and will be simply described in item C below.

[0116] C. Retardation layer

[0117] C-1. Retardation layer composed of a single layer

[0118] When the retardation layer is composed of a single layer, as described above, Re(550) of the retardation layer is, for example, 100 nm to 190 nm, and the angle formed by the slow axis of the retardation layer 40 and the absorption axis of the polarizing element 10 is, for example, 40° to 50°. The retardation layer is typically provided to impart antireflection characteristics to the polarizing plate. In one embodiment, it can function as a λ / 4 plate. As described above, the retardation layer can be a resin film or an orientation-cured layer of a liquid crystal compound.

[0119] For the retardation layer, it is preferable that the refractive index characteristics show the relationship of nx>ny≥nz. The in-plane retardation Re(550) of the retardation layer is, as described above, for example, 100 nm to 190 nm, preferably 110 nm to 170 nm, more preferably 130 nm to 160 nm. It should be noted that here "ny = nz" not only means that ny and nz are exactly equal, but also includes cases where they are substantially equal. Therefore, within the range that does not impair the effects of the present invention, there can be cases where ny < nz.

[0120] The Nz coefficient of the retardation layer is preferably 0.9 to 3, more preferably 0.9 to 2.5, further preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3. When such a relationship is satisfied, when the obtained polarizing plate with a retardation layer is used in an image display device, a very excellent reflection hue can be obtained.

[0121] The angle θ between the slow axis of the phase difference layer 40 and the absorption axis of the polarizer 10 is, as described above, for example, 40° to 50°, preferably 42° to 48°, and more preferably about 45°. When the angle θ is within such a range, by setting the phase difference layer to a λ / 4 plate, a polarizing plate with a phase difference layer having very excellent circular polarization characteristics (resulting in very excellent anti-reflection characteristics) can be obtained.

[0122] The phase difference layer can show an abnormal dispersion wavelength characteristic in which the phase difference value increases with the wavelength of the measured light, can show a normal wavelength dispersion characteristic in which the phase difference value decreases with the wavelength of the measured light, or can show a flat wavelength dispersion characteristic in which the phase difference value hardly changes with the wavelength of the measured light. In one embodiment, the phase difference layer shows an abnormal dispersion wavelength characteristic. In this case, the Re(450) / Re(550) of the phase difference layer is preferably greater than 0.8 and less than 1, more preferably greater than 0.8 and less than 0.95. When it is such a structure, a very excellent anti-reflection property can be achieved.

[0123] The absolute value of the photoelastic coefficient of the phase difference layer is preferably 2×10 -11 m 2 / N or less, more preferably 2.0×10 - 13 m 2 / N~1.5×10 -11 m 2 / N, more preferably 1.0×10 -12 m 2 / N~1.2×10 -11 m 2 When the absolute value of the photoelastic coefficient is within such a range, when shrinkage stress is generated during heating, the phase difference is unlikely to change. As a result, thermal unevenness of the obtained image display device can be well prevented.

[0124] C-1-1. Resin film

[0125] When the phase difference layer is a resin film, the resin film is typically a stretched film. In this case, the thickness of the phase difference layer is preferably 60 μm or less, more preferably 30 μm to 55 μm. When the thickness of the phase difference layer is within such a range, curling during heating can be well suppressed and curling during lamination can be well adjusted.

[0126] The phase difference layer can be composed of any appropriate resin film that can satisfy the above characteristics. As a representative example of such a resin, polycarbonate resins, polyester carbonate resins, polyester resins, polyvinyl acetal resins, polyarylate resins, cyclic olefin resins, cellulose resins, polyvinyl alcohol resins, polyamide resins, polyimide resins, polyether resins, polystyrene resins, acrylic resins can be listed. These resins can be used alone or in combination (for example, mixed, copolymerized). In the case where the phase difference layer is composed of a resin film showing an anomalous dispersion wavelength characteristic, a polycarbonate resin or a polyester carbonate resin (hereinafter, sometimes referred to as a polycarbonate resin) can be appropriately used.

[0127] As the above-mentioned polycarbonate resin, any appropriate polycarbonate resin can be used as long as the effect of the present invention can be obtained. For example, the polycarbonate resin contains: a structural unit derived from a fluorene dihydroxy compound, a structural unit derived from an isosorbide dihydroxy compound, and a structural unit derived from at least one dihydroxy compound selected from the group consisting of alicyclic diols, alicyclic dimethanols, diethylene glycol, triethylene glycol or polyethylene glycol, and an alkylene glycol or spiro glycol. Preferably, the polycarbonate resin contains a structural unit derived from a fluorene dihydroxy compound, a structural unit derived from an isosorbide dihydroxy compound, a structural unit derived from alicyclic dimethanol and / or a structural unit derived from diethylene glycol, triethylene glycol or polyethylene glycol; more preferably, it contains a structural unit derived from a fluorene dihydroxy compound, a structural unit derived from an isosorbide dihydroxy compound, and a structural unit derived from diethylene glycol, triethylene glycol or polyethylene glycol. The polycarbonate resin may also contain a structural unit derived from other dihydroxy compounds as needed. The details of the polycarbonate resin that can be suitably used in the present invention are described in, for example, JP-A-2014-10291, JP-A-2014-26266, JP-A-2015-212816, JP-A-2015-212817, and JP-A-2015-212818, and these descriptions are incorporated herein by reference.

[0128] The glass transition temperature of the polycarbonate resin is preferably 110°C to 150°C, more preferably 120°C to 140°C. If the glass transition temperature is too low, the heat resistance tends to deteriorate, and there is a possibility of causing dimensional changes after film forming, or sometimes the image quality of the obtained organic EL panel is reduced. If the glass transition temperature is too high, sometimes the forming stability during film forming deteriorates, or sometimes the transparency of the film is impaired. It should be noted that the glass transition temperature is obtained according to JIS K 7121 (1987).

[0129] The molecular weight of the above-mentioned polycarbonate resin can be expressed by a reduced viscosity. For the reduced viscosity, dichloromethane is used as a solvent, the polycarbonate concentration is precisely adjusted to 0.6g / dL, and the temperature is 20.0°C ± 0.1°C using an Ubbelohde viscosity tube for measurement. The lower limit of the reduced viscosity is usually preferably 0.30dL / g, and more preferably 0.35dL / g or more. The upper limit of the reduced viscosity is usually preferably 1.20dL / g, more preferably 1.00dL / g, and further preferably 0.80dL / g. If the reduced viscosity is less than the aforementioned lower limit, the problem of reduced mechanical strength of the molded product sometimes occurs. On the other hand, if the reduced viscosity is greater than the aforementioned upper limit, the problem of reduced fluidity, productivity, and moldability during molding sometimes occurs.

[0130] As the polycarbonate resin film, a commercially available film can be used. Specific examples of commercial products include "Pureace WR-S", "Pureace WR-W", and "Pureace WR-M" manufactured by Teijin Co., Ltd. and "NRF" manufactured by Nitto Denko Corporation.

[0131] The phase difference layer 40 can be obtained, for example, by stretching a film formed by the above-mentioned polycarbonate resin. As a method for forming a film from a polycarbonate resin, any appropriate molding method can be used. As a specific example, compression molding, transfer molding, injection molding, extrusion molding, blow molding, powder molding, FRP molding, cast coating (such as casting), calendering, hot pressing, etc. can be listed. Extrusion molding or cast coating is preferred. This is because the smoothness of the obtained film can be improved and good optical uniformity can be obtained. The molding conditions can be appropriately set according to the composition, type, and desired properties of the phase difference layer of the resin used. It should be noted that, as mentioned above, there are many film products of polycarbonate resins on the market, so the commercially available film is provided as it is for stretching treatment.

[0132] The thickness of the resin film (unstretched film) can be set to any appropriate value depending on the desired thickness of the retardation layer, desired optical properties, stretching conditions described below, etc. It is preferably 50 μm to 300 μm.

[0133] The above-mentioned stretching can adopt any appropriate stretching method and stretching conditions (such as stretching temperature, stretching ratio, stretching direction). Specifically, various stretching methods such as free end stretching, fixed end stretching, free end shrinkage, fixed end shrinkage, etc. can be used alone, or they can be used simultaneously or successively. Regarding the stretching direction, it can also be carried out in various directions and dimensions such as the length direction, width direction, thickness direction, and inclined direction. The stretching temperature is preferably Tg-30°C to Tg+60°C relative to the glass transition temperature (Tg) of the resin film, and more preferably Tg-10°C to Tg+50°C.

[0134] By appropriately selecting the stretching method and stretching conditions, a retardation film having the desired optical properties (eg, refractive index properties, in-plane retardation, Nz coefficient) can be obtained.

[0135] In one embodiment, the phase difference film is prepared by uniaxially stretching a resin film or by fixed-end uniaxially stretching a resin film. As a specific example of fixed-end uniaxial stretching, a method of stretching a resin film in a width direction (transverse direction) while advancing the resin film in a longitudinal direction can be cited. The stretching ratio is preferably 1.1 to 3.5 times.

[0136] In another embodiment, the phase difference film can be made by continuously obliquely stretching a long strip of resin film in the direction of the above-mentioned angle θ relative to the length direction. By adopting oblique stretching, a long strip of stretched film having an orientation angle of angle θ relative to the length direction of the film (having a slow axis in the direction of angle θ) can be obtained. For example, roll-to-roll can be used when stacking with a polarizer, which can simplify the manufacturing process. It should be noted that the angle θ can be the angle between the absorption axis of the polarizer and the slow axis of the phase difference layer in the polarizing plate with a phase difference layer. The angle θ is preferably 40° to 50°, more preferably 42° to 48°, and further preferably about 45° as described above.

[0137] As a stretching machine used in the oblique stretching, for example, a tenter-type stretching machine can be cited, which can apply a conveying force or a stretching force or a pulling force at different speeds in the horizontal direction and / or the vertical direction. The tenter-type stretching machine includes a horizontal unidirectional stretching machine, a simultaneous bidirectional stretching machine, etc. As long as the long strip of resin film can be continuously stretched obliquely, any appropriate stretching machine can be used.

[0138] The stretching machine can obtain a retardation layer (substantially a long retardation film) having the desired in-plane retardation and a slow axis in the desired direction by appropriately controlling the left and right speeds.

[0139] The stretching temperature of the above-mentioned film can vary according to the desired in-plane phase difference value and thickness of the phase difference layer, the type of resin used, the thickness of the film used, the stretching ratio, etc. Specifically, the stretching temperature is preferably Tg-30°C to Tg+30°C, more preferably Tg-15°C to Tg+15°C, and most preferably Tg-10°C to Tg+10°C. By stretching at such a temperature, the present invention can obtain a phase difference layer with appropriate characteristics. It should be noted that Tg is the glass transition temperature of the constituent material of the film.

[0140] C-1-2. Orientation and solidification layer of liquid crystal compound

[0141] In the case where the phase difference layer is an oriented solidified layer of a liquid crystal compound, by using a liquid crystal compound, the difference between nx and ny of the obtained phase difference layer can be significantly increased compared to non-liquid crystal materials, so the thickness of the phase difference layer used to obtain the desired in-plane phase difference can be significantly reduced. As a result, further thinning of the polarizing plate with a phase difference layer can be achieved. In this specification, an "oriented solidified layer" refers to a layer in which a liquid crystal compound is oriented in a prescribed direction within the layer and the orientation state is fixed. It should be noted that the "oriented solidified layer" is a concept including an oriented hardened layer obtained by hardening a liquid crystal monomer as described later. In the present embodiment, representatively, the rod-shaped liquid crystal compound is oriented in a state arranged along the slow axis direction of the phase difference layer (homogeneously oriented (homogeneously oriented)).

[0142] As the liquid crystal compound, for example, a liquid crystal compound whose liquid crystal phase is a nematic phase (nematic liquid crystal) can be cited. As such a liquid crystal compound, for example, a liquid crystal polymer or a liquid crystal monomer can be used. The liquid crystal property of the liquid crystal compound can be expressed by a lyotropic or thermotropic mechanism. The liquid crystal polymer and the liquid crystal monomer can be used alone or in combination.

[0143] When the liquid crystal compound is a liquid crystal monomer, the liquid crystal monomer is preferably a polymerizable monomer and a cross-linkable monomer. This is because the orientation state of the liquid crystal monomer can be fixed by polymerizing or cross-linking (i.e., hardening) the liquid crystal monomer. After the liquid crystal monomer is oriented, for example, if the liquid crystal monomers are polymerized or cross-linked with each other, the above-mentioned orientation state can be fixed. Here, a polymer is formed by polymerization, and a three-dimensional network structure is formed by cross-linking, but these are non-liquid crystal. Therefore, the phase difference layer formed will not undergo a transition to a liquid crystal phase, a glass phase, or a crystalline phase caused by temperature changes that are unique to liquid crystal compounds. As a result, the phase difference layer is a phase difference layer with excellent stability that is not affected by temperature changes.

[0144] The temperature range in which the liquid crystal monomer exhibits liquid crystallinity varies depending on its type. Specifically, the temperature range is preferably 40°C to 120°C, more preferably 50°C to 100°C, and most preferably 60°C to 90°C.

[0145] As the above-mentioned liquid crystal monomer, any appropriate liquid crystal monomer can be used. For example, polymerizable liquid crystal primitive (mesogen) compounds described in Japanese Patent Publication No. 2002-533742 (WO00 / 37585), EP358208 (US5211877), EP66137 (US4388453), WO93 / 22397, EP0261712, DE19504224, DE4408171, and GB2280445 can be used. As a specific example of such a polymerizable liquid crystal primitive compound, for example, the trade name LC242 of BASF, the trade name E7 of Merck, and the trade name LC-Sillicon-CC3767 of Wacker-Chem can be listed. As a liquid crystal monomer, for example, a nematic liquid crystal monomer is preferred.

[0146] The oriented solidified layer of the liquid crystal compound can be formed as follows: an orientation treatment is applied to the surface of a specified substrate, a coating liquid containing a liquid crystal compound is applied to the surface so that the liquid crystal compound is oriented in a direction corresponding to the above-mentioned orientation treatment, and the orientation state is fixed, thereby forming. In one embodiment, the substrate is any appropriate resin film, and the oriented solidified layer formed on the substrate can be transferred to the surface of the polarizer 10. In another embodiment, the substrate can be another protective layer. In this case, the transfer process is omitted, and the oriented solidified layer (phase difference layer) can be continuously stacked by roller to roller after the formation of the oriented solidified layer, so the productivity is further improved.

[0147] As the above-mentioned orientation treatment, any appropriate orientation treatment can be adopted. Specifically, mechanical orientation treatment, physical orientation treatment, and chemical orientation treatment can be listed. As specific examples of mechanical orientation treatment, friction treatment and stretching treatment can be listed. As specific examples of physical orientation treatment, magnetic field orientation treatment and electric field orientation treatment can be listed. As specific examples of chemical orientation treatment, oblique evaporation method and optical orientation treatment can be listed. The processing conditions of various orientation treatments can adopt any appropriate conditions according to the purpose.

[0148] The liquid crystal compound is oriented by treating it at a temperature that exhibits a liquid crystal phase according to its type. By such temperature treatment, the liquid crystal compound becomes a liquid crystal state, and the liquid crystal compound is oriented according to the orientation treatment direction of the substrate surface.

[0149] In one embodiment, the alignment state is fixed by cooling the aligned liquid crystal compound. When the liquid crystal compound is a polymerizable monomer or a crosslinkable monomer, the alignment state is fixed by subjecting the aligned liquid crystal compound to a polymerization treatment or a crosslinking treatment.

[0150] Specific examples of the liquid crystal compound and details of the method for forming the aligned solid layer are described in Japanese Unexamined Patent Application Publication No. 2006-163343, the contents of which are incorporated herein by reference.

[0151] As another example of an oriented solidified layer, a discotic liquid crystal compound may be oriented in any of a vertical orientation, a mixed orientation, and an inclined orientation. A discotic liquid crystal compound is representative of a discotic liquid crystal compound in which the disc surface is oriented substantially vertically relative to the film surface of the phase difference layer. The discotic liquid crystal compound is substantially vertical in that the average value of the angle between the film surface and the disc surface of the discotic liquid crystal compound is preferably 70° to 90°, more preferably 80° to 90°, and further preferably 85° to 90°. A discotic liquid crystal compound generally refers to a liquid crystal compound having a disc-shaped molecular structure in which a cyclic mother nucleus such as benzene, 1,3,5-triazine, or calixarene is arranged at the center of the molecule, and a straight-chain alkyl, alkoxy, substituted benzoyloxy, or the like is radially substituted as its side chain. Representative examples of discotic liquid crystals include benzene derivatives, triphenylene derivatives, triindene derivatives, and phthalocyanine derivatives described in the research report of C. Destrade et al., Mol. Cryst. Liq. Cryst. Vol. 71, p. 111 (1981); cyclohexane derivatives described in the research report of B. Kohne et al., Angew. Chem. Vol. 96, p. 70 (1984); and azacrown ether-based and phenylacetylene-based macrocycles described in the research report of J. M. Lehn et al., J. Chem. Soc. Chem. Commun., p. 1794 (1985); and the research report of J. Zhang et al., J. Am. Chem. Soc. Vol. 116, p. 2655 (1994). Further specific examples of the discotic liquid crystal compound include compounds described in Japanese Patent Application Laid-Open No. 2006-133652, Japanese Patent Application Laid-Open No. 2007-108732, and Japanese Patent Application Laid-Open No. 2010-244038. The descriptions of the above documents and publications are incorporated herein by reference.

[0152] When the phase difference layer is an alignment solidified layer of a liquid crystal compound, its thickness is preferably 0.5 to 7 μm, more preferably 1 to 5 μm. By using a liquid crystal compound, an in-plane phase difference equivalent to that of a resin film can be achieved with a thickness significantly thinner than that of a resin film.

[0153] C-1-3. Another phase difference layer

[0154] As described above, when the phase difference layer 40 is composed of a single layer, it is preferred to provide another phase difference layer. The other phase difference layer can be a so-called positive C plate whose refractive index characteristics show the relationship of nz>nx=ny as described above. By using a positive C plate as another phase difference layer, it is possible to prevent reflection in the inclined direction well, and a wide viewing angle of the anti-reflection function can be achieved. In this case, the phase difference Rth(550) in the thickness direction of the other phase difference layer is preferably -50nm to -300nm, more preferably -70nm to -250nm, further preferably -90nm to -200nm, and particularly preferably -100nm to -180nm. Here, "nx=ny" not only includes the case where nx and ny are strictly the same, but also includes the case where nx and ny are substantially equal. That is, the in-plane phase difference Re(550) of the other phase difference layer may be less than 10nm.

[0155] Another phase difference layer having a refractive index characteristic of nz>nx=ny can be formed by any appropriate material. Another phase difference layer is preferably formed by a thin film containing a liquid crystal material fixed in a vertical orientation. The liquid crystal material (liquid crystal compound) capable of vertical orientation can be a liquid crystal monomer or a liquid crystal polymer. As a specific example of the liquid crystal compound and the method for forming the phase difference layer, the liquid crystal compound and the method for forming the phase difference layer described in

[0020] to

[0028] of Japanese Patent Gazette No. 2002-333642 can be listed. In this case, the thickness of the other phase difference layer is preferably 0.5μm to 10μm, more preferably 0.5μm to 8μm, and further preferably 0.5μm to 5μm.

[0156] C-2.2 Phase difference layer structure

[0157] In the case where the phase difference layer 40 has a stacked structure of a first layer 41 and a second layer 42, either the first layer 41 or the second layer 42 may function as a λ / 4 plate and the other may function as a λ / 2 plate. For example, when the first layer 41 functions as a λ / 2 plate and the second layer 42 functions as a λ / 4 plate, the in-plane phase difference Re(550) of the first layer is, as described above, for example, 200nm to 300nm, preferably 230nm to 290nm, and more preferably 250nm to 280nm. The in-plane phase difference Re(550) of the second layer is, as described above, for example, 100nm to 190nm, preferably 110nm to 170nm, and more preferably 130nm to 160nm. The angle between the slow axis of the first layer and the absorption axis of the polarizer is, as described above, for example, 10° to 20°, preferably 12° to 18°, and more preferably about 15°. As described above, the angle between the slow axis of the second layer and the absorption axis of the polarizer is, for example, 70° to 80°, preferably 72° to 78°, and more preferably about 75°. With such a configuration, characteristics close to the ideal abnormal wavelength dispersion characteristics can be obtained, resulting in very excellent anti-reflection characteristics.

[0158] For the first layer 41 and the second layer 42, one may be a resin film and the other may be an orientation solidified layer of a liquid crystal compound, both may be resin films, or both may be orientation solidified layers of liquid crystal compounds. Preferably, the first layer 41 and the second layer 42 are both resin films or orientation solidified layers of liquid crystal compounds.

[0159] The thickness of the first layer 41 and the second layer 42 can be adjusted in such a manner as to obtain the desired in-plane phase difference of the λ / 4 plate or the λ / 2 plate. For example, when the first layer 41 functions as a λ / 2 plate and the second layer 42 functions as a λ / 4 plate, and when the first layer 41 and the second layer 42 are resin films, the thickness of the first layer 41 is, for example, 40 μm to 75 μm, and the thickness of the second layer 42 is, for example, 30 μm to 55 μm. When the first layer 41 and the second layer 42 are alignment solidification layers of liquid crystal compounds, the thickness of the first layer 41 is, for example, 2.0 μm to 3.0 μm, and the thickness of the second layer 42 is, for example, 1.0 μm to 2.0 μm.

[0160] The resin films constituting the first layer and the second layer, the liquid crystal compound, the formation methods of the first layer and the second layer, the optical properties, etc. are as described above with respect to the single layer.

[0161] D. Conductive layer or isotropic substrate with conductive layer

[0162] The conductive layer can be formed by forming a metal oxide film on any appropriate substrate by any appropriate film forming method (for example, vacuum evaporation, sputtering, CVD, ion plating, spraying, etc.). As the metal oxide, for example, indium oxide, tin oxide, zinc oxide, indium-tin composite oxide, tin-antimony composite oxide, zinc-aluminum composite oxide, indium-zinc composite oxide can be listed. Among them, indium-tin composite oxide (ITO) is preferred.

[0163] When the conductive layer contains a metal oxide, the thickness of the conductive layer is preferably 50 nm or less, more preferably 35 nm or less. The lower limit of the thickness of the conductive layer is preferably 10 nm.

[0164] The conductive layer can be transferred from the substrate to the phase difference layer and the conductive layer itself can be used as a constituent layer of the polarizing plate with the phase difference layer, or it can be laminated on the phase difference layer in the form of a laminate with the substrate (substrate with the conductive layer). Preferably, the substrate is optically isotropic, so the conductive layer can be used as an isotropic substrate with a conductive layer for the polarizing plate with the phase difference layer.

[0165] As an optically isotropic substrate (isotropic substrate), any appropriate isotropic substrate can be used. As a material constituting an isotropic substrate, for example, a material having a resin without a conjugated system such as a norbornene resin and an olefin resin as the main skeleton, a material having a cyclic structure such as a lactone ring and a glutarimide ring in the main chain of an acrylic resin, etc. can be cited. If such a material is used, when forming an isotropic substrate, the phase difference caused by the orientation of the molecular chain can be suppressed to be smaller. The thickness of the isotropic substrate is preferably less than 50 μm, more preferably less than 35 μm. The lower limit of the thickness of the isotropic substrate is, for example, 20 μm.

[0166] The conductive layer and / or the conductive layer of the isotropic substrate with a conductive layer can be patterned as needed. By patterning, a conductive portion and an insulating portion can be formed. As a result, an electrode can be formed. The electrode can function as a touch sensor electrode that senses contact with the touch panel. As a patterning method, any appropriate method can be used. As specific examples of the patterning method, a wet etching method and a screen printing method can be listed.

[0167] Example

[0168] The present invention is specifically described below with reference to examples, but the present invention is not limited to these examples. The measuring methods of various properties are as follows. It should be noted that, unless otherwise specified, the "parts" and "%" in the examples are based on weight.

[0169] (1) Glass transition temperature Tg

[0170] The solution obtained by dissolving the material constituting the protective layer used in the examples and comparative examples in a prescribed solvent was applied to the substrate (PET film) using an applicator and dried at 60°C to form a coating film (thickness 40 μm). The obtained coating film was peeled off from the substrate and cut into strips as a measurement sample. The measurement sample was subjected to DMA measurement to measure Tg. The measurement device and measurement conditions are as follows.

[0171] (Measurement device)

[0172] Made by SII NanoTechnology Inc., "DMS6100"

[0173] (Measurement conditions)

[0174] ·Measurement temperature range: -80℃~150℃

[0175] Heating and cooling speed: 2℃ / min

[0176] ·Test sample width: 10mm

[0177] Distance between fixtures: 20mm

[0178] ·Measurement frequency: 1Hz

[0179] Strain amplitude: 10μm

[0180] ·Measurement atmosphere: N 2 (250mL / min)

[0181] (2) Iodine adsorption

[0182] A solution obtained by dissolving the material constituting the protective layer used in the examples and comparative examples in a predetermined solvent was applied to a substrate (PET film) using an applicator and dried at 60°C to form a coating film (thickness 40 μm). The obtained coating film was peeled off from the substrate and cut into 1 cm×1 cm (1 cm 2 ) as the test sample. The test sample is provided to the combustion IC method, and the iodine content in the sample is quantitatively analyzed. The details are as follows. Take the test sample and weigh it and put it into a headspace vial (20mL capacity). Then, a vial (2mL capacity) containing 1mL of iodine solution (iodine concentration 1 weight%, potassium iodide concentration 7 weight%) is placed in the headspace vial and covered tightly. Afterwards, the headspace vial is heated at 65°C in a dryer for 6 hours, the heated sample is taken and placed in a ceramic dish and burned using an automatic combustion device, so that the absorption liquid captures the generated gas, and then a quantitative analysis is performed to obtain the weight % of the adsorbed iodine. It should be noted that the device used is as follows.

[0183] ·Automatic sample combustion device: Mitsubishi Chemical Analytech, "AQF-2100H"

[0184] IC (anion): manufactured by Thermo Fisher Scientific, “ICS-3000”

[0185] (3) Decolorization

[0186] A test piece (50 mm × 50 mm) was cut out from the polarizing plate with a phase difference layer obtained in the embodiment and the comparative example, and the test piece formed two sides opposite to the direction perpendicular to the absorption axis direction of the polarizer and the absorption axis direction, respectively. The test piece was bonded to an alkali-free glass plate with an adhesive in such a way that the protective layer became the outer side to prepare a test sample, and the test sample was placed in an oven at 85°C and 85% RH for 48 hours for heating and humidification, and the discoloration state of the polarizing plate with a phase difference layer after humidification when it was configured to form a cross prism with the standard polarizing plate was visually observed, and evaluated according to the following criteria.

[0187] No problem: no discoloration observed

[0188] Partial discoloration: Discoloration is observed at the end

[0189] Total discoloration: The polarizing plate is obviously discolored as a whole

[0190] (4) Single-body transmittance and polarization

[0191] A test piece (50 mm × 50 mm) was cut out from the polarizing plate with a phase difference layer obtained from the embodiment and the comparative example, and the test piece formed two sides opposite to the direction perpendicular to the absorption axis direction of the polarizer and the absorption axis direction. The test piece was bonded to an alkali-free glass plate with an adhesive with the protective layer as the outer side to prepare a test sample. The single transmittance (Ts), parallel transmittance (Tp) and orthogonal transmittance (Tc) of the test sample were measured using an ultraviolet visible spectrophotometer (manufactured by JASCO Corporation, product name "V7100"), and the polarization degree (P) was calculated using the following formula. At this time, the measuring light was incident from the protective layer side.

[0192] Polarization degree (P) (%) = {(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100

[0193] It should be noted that the above Ts, Tp and Tc are Y values ​​obtained by measuring with a 2-degree field of view (light source C) according to JIS Z 8701 and correcting the visual sensitivity. In addition, Ts and P are substantially characteristics of the polarizer.

[0194] Then, the polarizing plate with a retardation layer was placed in an oven at 85°C and 85% RH for 48 hours for heating and humidification (heating test). 0 And the single transmittance Ts after heating test48 , the single transmittance change ΔTs is calculated using the following formula.

[0195] ΔTs(%)=Ts 48 -Ts 0

[0196] Similarly, the polarization degree P before the heating test 0 And the polarization degree P after heating test 48 , use the following formula to calculate the change in polarization degree ΔP.

[0197] ΔP(%)=P 48 -P 0

[0198] In addition, the heating test was carried out by preparing a test sample in the same manner as in the above-mentioned decolorization.

[0199] (5) Front reflectivity

[0200] A test piece (50 mm × 50 mm) was cut out from the polarizing plate with a phase difference layer obtained from the embodiment and the comparative example, and the test piece formed two sides opposite to the direction perpendicular to the absorption axis direction of the polarizer and the absorption axis direction. The test piece was bonded to an alkali-free glass plate using an adhesive in a manner that the protective layer was on the outside to prepare a test sample. The test sample was subjected to a humidification test at 85°C and 85% RH for 48 hours. The test sample after the above-mentioned humidification test was arranged on a reflective plate (manufactured by Toray Film Co., Ltd., trade name "DMS-X42"; reflectivity 86%) in a manner that the glass and the reflective plate were opposite to each other (i.e., the protective layer was on the outside). Next, the front reflectance was measured using a spectrophotometer (CM-2600d manufactured by Konica Minolta) using the SCI method.

[0201] <Example 1>

[0202] 1. Preparation of polarizer / resin substrate laminate

[0203] As the resin substrate, a long amorphous polyethylene terephthalate copolymer film (thickness: 100 μm) having a water absorption rate of 0.75% and a Tg of about 75° C. was used. One surface of the resin substrate was subjected to a corona treatment.

[0204] To 100 parts by weight of a PVA-based resin prepared by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "GOHSEFIMER Z410") in a ratio of 9:1, 13 parts by weight of potassium iodide was added to prepare a PVA aqueous solution (coating solution).

[0205] The PVA aqueous solution was applied to the corona-treated surface of the resin substrate and dried at 60° C., thereby forming a PVA-based resin layer having a thickness of 13 μm, thereby producing a laminate.

[0206] The obtained laminate was subjected to free-end uniaxial stretching to 2.4 times in the longitudinal direction (longitudinal direction) between rolls having different peripheral speeds in an oven at 130° C. (in-air auxiliary stretching treatment).

[0207] Next, the laminate was immersed in an insolubilization bath (boric acid aqueous solution prepared by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilization treatment).

[0208] Next, the polarizer was immersed in a dyeing bath (an iodine aqueous solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 relative to 100 parts by weight of water) at a temperature of 30° C. for 60 seconds while adjusting the concentration so that the single body transmittance (Ts) of the final polarizer became 41.5%±0.1% (dyeing treatment).

[0209] Next, the film was immersed in a crosslinking bath (boric acid aqueous solution prepared by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment).

[0210] Then, while the laminate was immersed in a boric acid aqueous solution (boric acid concentration: 4.0 wt%) at a liquid temperature of 70°C, it was uniaxially stretched in the longitudinal direction (long side direction) between rolls of different peripheral speeds to a total stretching ratio of 5.5 times (underwater stretching treatment).

[0211] Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution prepared by mixing 4 parts by weight of potassium iodide with respect to 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment).

[0212] Thereafter, the laminate was dried in an oven maintained at 90° C. while being brought into contact with a SUS heating roll having a surface temperature maintained at 75° C. for about 2 seconds (drying shrinkage treatment). The shrinkage rate in the width direction of the laminate due to the drying shrinkage treatment was 5.2%.

[0213] As described above, a polarizer with a thickness of 5 μm was formed on the resin substrate to produce a laminate of polarizer / resin substrate. Single-unit transmittance of polarizer (initial single-unit transmittance) Ts 0 is 41.5, polarization degree (initial polarization degree) P 0 It is 99.996%.

[0214] 2. Preparation of phase difference film constituting phase difference layer

[0215] 2-1. Polymerization of polyester carbonate resin

[0216] The polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and a reflux condenser controlled at 100° C. 29.60 parts by mass (0.046 mol) of bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane, 29.21 parts by mass (0.200 mol) of isosorbide (ISB), 42.28 parts by mass (0.139 mol) of spiroglycol (SPG), 63.77 parts by mass (0.298 mol) of diphenyl carbonate (DPC) and 1.19×10 calcium acetate monohydrate as a catalyst were added. -2 Mass parts (6.78×10 -5 mol). After the reactor is replaced with nitrogen under reduced pressure, it is heated with a heat medium and stirring is started when the internal temperature reaches 100°C. 40 minutes after the start of heating, the internal temperature reaches 220°C, and the pressure is reduced while controlling to maintain the temperature, and it becomes 13.3kPa 90 minutes after reaching 220°C. The phenol vapor produced as a by-product of the polymerization reaction is introduced into a reflux condenser at 100°C, so that a certain amount of monomer components contained in the phenol vapor are returned to the reactor, and the uncondensed phenol vapor is introduced into a condenser at 45°C for recovery. After nitrogen is introduced into the first reactor to temporarily restore the pressure to atmospheric pressure, the oligomerized reaction liquid in the first reactor is moved to the second reactor. Next, the temperature and pressure reduction in the second reactor are started, and the internal temperature reaches 240°C and the pressure reaches 0.2kPa in 50 minutes. Thereafter, polymerization is carried out until the specified stirring power is reached. When a predetermined power was reached, nitrogen gas was introduced into the reactor to restore the gas pressure, and the produced polyester carbonate resin was extruded into water, and the strands were cut to obtain pellets.

[0217] 2-2. Preparation of phase difference film

[0218] The obtained polyester carbonate resin (pellets) was vacuum dried at 80°C for 5 hours, and then a thin film forming device equipped with a single screw extruder (manufactured by Toshiba Machine Co., Ltd., barrel setting temperature: 250°C), a T-die (width 200mm, setting temperature: 250°C), a cooling roller (setting temperature: 120-130°C) and a winder was used to prepare a long strip of resin film with a thickness of 135μm. The obtained long strip of resin film was stretched in the width direction at a stretching temperature of 133°C and a stretching ratio of 2.8 times to obtain a retardation film with a thickness of 48μm. The Re(550) of the obtained retardation film was 141nm, Re(450) / Re(550) was 0.82, and the Nz coefficient was 1.12.

[0219] 3. Preparation of polarizing plate with phase difference layer

[0220] The phase difference film obtained in 3. is bonded to the surface of the polarizer of the laminate obtained in 1. by means of an acrylic adhesive (thickness 5 μm). At this time, the bonding is performed in such a way that the absorption axis of the polarizer and the slow axis of the phase difference film form an angle of 45°. The resin substrate is peeled off to obtain a polarizing plate with a phase difference layer having a phase difference layer / polarizer structure.

[0221] 20 parts of an acrylic resin (lactone ring unit 30 mol%) of polymethyl methacrylate having a lactone ring unit are dissolved in 80 parts of methyl ethyl ketone to obtain an acrylic resin solution (20%). The acrylic resin solution is applied to the surface of the polarizer of the polarizing plate obtained above using a wire rod, and the coated film is dried at 60°C for 5 minutes to form a protective layer in the form of a cured product of the coating film. The thickness of the protective layer is 3 μm, the Tg is 119°C, and the iodine adsorption amount is 0.25 wt%. As described above, a polarizing plate with a phase difference layer having a structure of a protective layer (cured product of the coating film) / polarizer / phase difference layer is obtained. The obtained polarizing plate with a phase difference layer is provided for the evaluation of (3) to (5) above. Furthermore, the protective layer is visually observed for shrinkage after formation. The results are shown in Table 1.

[0222] <Example 2>

[0223] The same operation as in Example 1 was performed to form a protective layer, except that an acrylic resin of polymethyl methacrylate having a maleic anhydride unit (maleic anhydride unit 7 mol%) was used instead of an acrylic resin of polymethyl methacrylate having a lactone ring unit. The thickness of the protective layer was 3 μm and Tg was 115° C. A polarizing plate with a phase difference layer was prepared in the same manner as in Example 1, except that the protective layer was used. The obtained polarizing plate with a phase difference layer was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0224] <Example 3>

[0225] The same operation as in Example 1 was performed except that an acrylic resin of 100% polymethyl methacrylate (manufactured by Kusumoto Chemicals Co., Ltd., product name "B-728") was used instead of an acrylic resin of polymethyl methacrylate having a lactone ring unit. A protective layer was formed. The thickness of the protective layer was 3 μm, Tg was 116° C., and the iodine adsorption was 0.34% by weight. A polarizing plate with a phase difference layer was prepared in the same manner as in Example 1 except that the protective layer was used. The obtained polarizing plate with a phase difference layer was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0226] <Example 4>

[0227] The same operation as in Example 1 was performed except that an acrylic resin of polymethyl methacrylate having a glutarimide ring unit (glutarimide ring unit 4 mol%) was used instead of an acrylic resin of polymethyl methacrylate having a lactone ring unit. The protective layer was formed in the same manner as in Example 1. The thickness of the protective layer was 3 μm, Tg was 103° C., and the iodine adsorption was 2.3 wt %. A polarizing plate with a phase difference layer was prepared in the same manner as in Example 1 except that the protective layer was used. The obtained polarizing plate with a phase difference layer was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0228] <Example 5>

[0229] The same operation as in Example 1 was performed except that an acrylic resin of a different polymethyl methacrylate having a lactone ring unit (lactone ring unit 20 mol%) was used to form a protective layer. The thickness of the protective layer was 3 μm, Tg was 104° C., and the iodine adsorption was 2.8 wt %. A polarizing plate with a phase difference layer was prepared in the same manner as in Example 1 except that the protective layer was used. The obtained polarizing plate with a phase difference layer was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0230] <Example 6>

[0231] The same operation as in Example 1 was performed except that an acrylic resin of a copolymer of methyl methacrylate / butyl methacrylate (molar ratio 80 / 20) was used instead of an acrylic resin of polymethyl methacrylate having a lactone ring unit. The protective layer was formed in the same manner as in Example 1. The thickness of the protective layer was 3 μm, Tg was 95° C., and the iodine adsorption was 3.8% by weight. A polarizing plate with a phase difference layer was prepared in the same manner as in Example 1 except that the protective layer was used. The obtained polarizing plate with a phase difference layer was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0232] <Example 7>

[0233] 1. Preparation of polarizer / resin substrate laminate

[0234] In the same manner as in Example 1, a laminate of a polarizer / resin substrate was produced.

[0235] 2. Preparation of the First and Second Oriented Solidified Layers Constituting the Phase Difference Layer

[0236] 10 g of polymerizable liquid crystal showing a nematic liquid crystal phase (manufactured by BASF: trade name "Paliocolor LC242", represented by the following formula) and 3 g of a photopolymerization initiator for the polymerizable liquid crystal compound (manufactured by BASF: trade name "IRGACURE907") were dissolved in 40 g of toluene to prepare a liquid crystal composition (coating liquid).

[0237]

[0238] The surface of a polyethylene terephthalate (PET) film (38 μm thick) was rubbed with a rubbing cloth to perform an orientation treatment. The orientation treatment direction was set to be 15° relative to the absorption axis of the polarizer when viewed from the visual recognition side when attached to the polarizing plate. The above-mentioned liquid crystal coating liquid was applied to the orientation treatment surface using a rod coater and heated and dried at 90°C for 2 minutes to orient the liquid crystal compound. The liquid crystal layer thus formed was irradiated with 1 mJ / cm 2 The liquid crystal layer was cured by applying light to the PET film, thereby forming a liquid crystal alignment solidified layer A on the PET film. The liquid crystal alignment solidified layer A had a thickness of 2.5 μm and an in-plane phase difference Re (550) of 270 nm. Furthermore, the liquid crystal alignment solidified layer A exhibited a refractive index characteristic of nx>ny=nz.

[0239] The coating thickness was changed, and the orientation treatment direction was set to be 75° relative to the absorption axis of the polarizer when viewed from the visual recognition side. In the same manner as above, a liquid crystal orientation solidified layer B was formed on the PET film. The thickness of the liquid crystal orientation solidified layer B was 1.5 μm, and the in-plane phase difference Re (550) was 140 nm. Furthermore, the liquid crystal orientation solidified layer B showed a refractive index characteristic of nx>ny=nz.

[0240] 3. Preparation of polarizing plate with phase difference layer

[0241] The liquid crystal orientation solidification layer A and the liquid crystal orientation solidification layer B obtained in the above 2. are sequentially transferred to the polarizer surface of the laminate of the polarizer / resin substrate obtained in the above 1. At this time, the transfer (lamination) is performed in a manner that the angle formed by the absorption axis of the polarizer and the slow axis of the orientation solidification layer A is 15°, and the angle formed by the absorption axis of the polarizer and the slow axis of the orientation solidification layer B is 75°. It should be noted that each transfer (lamination) is carried out with the aid of an ultraviolet curing adhesive (thickness 1.0μm). Then, in order to strengthen, a substrate with an adhesive is bonded to the surface of the orientation solidification layer B. Then, the resin substrate is peeled off to obtain a polarizing plate with a phase difference layer having a structure of a polarizer / adhesive layer / phase difference layer (first orientation solidification layer / adhesive layer / second orientation solidification layer) / a substrate with an adhesive.

[0242] Next, a protective layer is formed on the surface of the polarizer of the polarizing plate with a phase difference layer in the same manner as in Example 3. Finally, the substrate with the adhesive layer is peeled off to obtain a polarizing plate with a phase difference layer having a structure of a protective layer (cured product of the coating film) / polarizer / phase difference layer. The obtained polarizing plate with a phase difference layer is subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0243] <Comparative Example 1>

[0244] The same operation as in Example 1 was performed to form a protective layer, except that an acrylic resin (manufactured by Kusumoto Chemicals Co., Ltd., product name "B-722") of a copolymer of methyl methacrylate / ethyl acrylate (molar ratio 55 / 45) was used instead of an acrylic resin of polymethyl methacrylate having a lactone ring unit. The thickness of the protective layer was 3 μm, Tg was 39°C, and the iodine adsorption was 1.7% by weight. In addition to using this protective layer, a polarizing plate with a phase difference layer was prepared in the same manner as in Example 1. The obtained polarizing plate with a phase difference layer was subjected to a decolorization evaluation, and the result was poor ("complete decolorization"), so the monomer transmittance and polarization degree were not evaluated. The results are shown in Table 1.

[0245] <Comparative Example 2>

[0246] Except for using an acrylic resin (manufactured by Kusumoto Chemical Industry Co., Ltd., product name "B-734") which is a copolymer of methyl methacrylate / butyl methacrylate (molar ratio 35 / 65) instead of an acrylic resin of polymethyl methacrylate having a lactone ring unit, the same operation as in Example 1 is performed to form a protective layer. The thickness of the protective layer is 3 μm, Tg is 71°C, and the iodine adsorption is 12% by weight. Except for using this protective layer, the same operation as in Example 1 is performed to prepare a polarizing plate with a phase difference layer. The obtained polarizing plate with a phase difference layer was subjected to a decolorization evaluation, and the result was poor ("complete decolorization"), so the monomer transmittance and polarization degree were not evaluated. The results are shown in Table 1.

[0247] <Comparative Example 3>

[0248] The protective layer (cured product) was formed in the same manner as in Example 1 except that an ultraviolet curable acrylic resin (manufactured by Kyoeisha Chemical, product name "LIGHT ACRYLATE HPP-A", neopentyl glycol hydroxypivalate acrylic acid adduct) was used. Specifically, a composition prepared by mixing 97 wt % of the acrylic resin and 3 wt % of a photopolymerization initiator (IRGACURE 907, manufactured by BASF) was applied to a polarizer and illuminated with a high pressure mercury lamp in a nitrogen atmosphere at a cumulative light intensity of 300 mJ / cm 2 Irradiate with ultraviolet light to form a hardened layer (protective layer). The thickness of the protective layer is 3 μm, Tg is 83° C., and the iodine adsorption is 6.6% by weight. Except for using this protective layer, the same operation as in Example 1 was performed to prepare a polarizing plate with a phase difference layer. The obtained polarizing plate with a phase difference layer was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0249] <Comparative Example 4>

[0250] A protective layer (hardened material) was formed in the same manner as in Example 1, except that an ultraviolet curable acrylic resin (manufactured by Toagosei Co., Ltd., product name "ARONIX M-402") and dipentaerythritol penta- and hexa-acrylates (penta-acrylate is 30% to 40%) were used. The method for forming the protective layer was the same as in Comparative Example 3. The thickness of the protective layer was 3 μm. A polarizing plate with a phase difference layer was prepared in the same manner as in Example 1, except that the protective layer was used. The obtained polarizing plate with a phase difference layer was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0251] <Comparative Example 5>

[0252] The protective layer (cured product) was formed in the same manner as in Example 1 except that an ultraviolet curable epoxy resin (manufactured by DAICEL, product name "CELLOXIDE 2021P") was used. Specifically, a composition prepared by mixing 95 wt% of the epoxy resin and 5 wt% of a photopolymerization initiator (CPI-100P, manufactured by San-Apro) was applied to the polarizer and illuminated with a high pressure mercury lamp in an air atmosphere at a cumulative light intensity of 500 mJ / cm 2 Irradiate with ultraviolet light to form a hardened layer (protective layer). The thickness of the protective layer is 3 μm, Tg is 95° C., and the iodine adsorption is 9% by weight. Except for using this protective layer, the same operation as in Example 1 is performed to prepare a polarizing plate with a phase difference layer. The obtained polarizing plate with a phase difference layer is subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0253] <Comparative Example 6>

[0254] Except for using a water-based polyester resin (manufactured by Nippon Synthetic Chemical Co., Ltd., product name "POLYESTER WR905"), the same operation as in Example 1 was performed to form a protective layer (cured product of the coating film). The thickness of the protective layer was 3 μm, and the iodine adsorption amount was 12% by weight. Except for using this protective layer, the same operation as in Example 1 was performed to prepare a polarizing plate with a phase difference layer. The obtained polarizing plate with a phase difference layer was evaluated for decolorization, and the result was poor ("complete dehydration"), so the monomer transmittance and polarization degree were not evaluated. The results are shown in Table 1.

[0255] <Comparative Example 7>

[0256] Except for using a water-based polyurethane resin (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name "SUPERFLEX SF210"), the same operation as in Example 1 was performed to form a protective layer (cured product of the coating film). The thickness of the protective layer was 3 μm, Tg was 107°C, and the iodine adsorption was 19% by weight. Except for using this protective layer, the same operation as in Example 1 was performed to prepare a polarizing plate with a phase difference layer. The obtained polarizing plate with a phase difference layer was subjected to a decolorization evaluation, and the result was poor ("complete decolorization"), so the monomer transmittance and polarization degree were not evaluated. The results are shown in Table 1.

[0257] <Comparative Example 8>

[0258] Except for using a water-based polyurethane resin (Unitika company, product name "ARROW BASE SE1200"), the same operation as in Example 1 was performed to form a protective layer (cured product of the coating film). The thickness of the protective layer was 3 μm and the iodine adsorption amount was 15% by weight. Except for using this protective layer, the same operation as in Example 1 was performed to prepare a polarizing plate with a phase difference layer. The obtained polarizing plate with a phase difference layer was evaluated for decolorization, and the result was poor ("complete decolorization"), so the monomer transmittance and polarization degree were not evaluated. The results are shown in Table 1.

[0259] [Table 1]

[0260]

[0261] <Evaluation>

[0262] It is clear from Table 1 that the polarizing plate with a phase difference layer in the embodiment of the present invention is a polarizing plate as follows: although it is very thin, it can also suppress the reduction of optical properties in a heated and humidified environment, has excellent durability, and does not shrink after the protective layer is formed, and can withstand practical applications. Furthermore, the front reflectivity of the polarizing plate with a phase difference layer in the embodiment of the present invention after the humidification test is very small, showing good anti-reflection properties. This means that when applied to an image display device having a metal layer such as an organic EL display device, it has the effect of preventing the reflected glare of external light caused by the metal layer.

[0263] Industrial Applicability

[0264] The polarizing plate with a phase difference layer of the present invention is suitable for use in an image display device. As the image display device, for example, portable devices such as a portable information terminal (PDA), a smart phone, a mobile phone, a clock, a digital camera, and a portable game console; OA equipment such as a computer display, a notebook computer, and a copier; household electrical appliances such as a camera, a television, and a microwave oven; vehicle-mounted equipment such as a rear monitor, a monitor for a car navigation system, and a car audio system; display equipment such as a digital signage and an information display for commercial stores; security equipment such as a monitoring monitor; and nursing and medical equipment such as a nursing monitor and a medical monitor.

[0265] Description of Reference Numerals

[0266] 10 polarizers

[0267] 20 protective layer

[0268] 40 Phase difference layer

[0269] 41 Layer 1

[0270] 42 Layer 2

[0271] 100 polarizing plate

Claims

1. A polarizing plate with a phase difference layer, comprising a polarizing plate and a phase difference layer, wherein the polarizing plate comprises a polarizer and a protective layer disposed on one side of the polarizer, the phase difference layer is disposed on the side of the polarizing plate opposite to the protective layer, and the protective layer is directly formed on the polarizer, The protective layer is composed of a cured product of a coating film of an organic solvent solution of a thermoplastic acrylic resin, and the glass transition temperature of the protective layer is 95° C. or higher. The thickness of the protective layer is less than 3 μm. The protective layer has an iodine adsorption amount of 4.0 wt % or less.

2. The polarizing plate with a phase difference layer according to claim 1, wherein: The phase difference layer is a single layer. The Re (550) of the phase difference layer is 100nm to 190nm. The angle formed between the slow axis of the phase difference layer and the absorption axis of the polarizer is 40° to 50°.

3. The polarizing plate with a phase difference layer according to claim 2, wherein: The phase difference layer is a resin film.

4. The polarizing plate with a phase difference layer according to claim 2, wherein: The phase difference layer is an alignment solidified layer of liquid crystal compounds.

5. The polarizing plate with a phase difference layer according to claim 1, wherein: The phase difference layer has a stacked structure of a first layer and a second layer. The Re (550) of the first layer is 200 nm to 300 nm, and the angle between the slow axis and the absorption axis of the polarizer is 10° to 20°. The Re (550) of the second layer is 100 nm to 190 nm, and the angle between the slow axis and the absorption axis of the polarizer is 70° to 80°.

6. The polarizing plate with a phase difference layer according to claim 5, wherein: The first layer and the second layer are respectively resin films.

7. The polarizing plate with a phase difference layer according to claim 5, wherein: The first layer and the second layer are alignment solidification layers of liquid crystal compounds, respectively.

8. The polarizing plate with a retardation layer according to any one of claims 1 to 7, wherein The thermoplastic acrylic resin has at least one selected from the group consisting of a lactone ring unit, a glutaric anhydride unit, a glutarimide unit, a maleic anhydride unit, and a maleimide unit. 9 . The polarizing plate with a retardation layer according to claim 1 , which is disposed on a viewing side of an image display device, and the protective layer is disposed on the viewing side.