Method for manufacturing three-dimensional semiconductor device
Through a multi-step manufacturing method, the etching and filling technology of multi-layer strip material layers and mask material layers are used to achieve high-precision and high-density arrangement of Si pillars, solving the problem of Si pillar diameter and spacing control in the existing technology. Difficult problems have improved the high integration and high performance of circuits.
Patent Information
- Application Number
- CN201880100403.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-12-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2038-12-21
AI Technical Summary
It is difficult to achieve high density of columnar semiconductor devices with existing technology. Especially in the manufacturing process of SGT, it is difficult to control the diameter and spacing of Si columns with high precision, which affects the high integration and high performance of circuits.
A multi-step manufacturing method is used to form multi-layer strip material layers and mask material layers, and the shape and position of the Si pillars are precisely controlled through etching and filling techniques to ensure high-precision and high-density arrangement of the Si pillars, and On this basis, a gate insulating layer and a conductor layer are formed.
It achieves high-precision and high-density arrangement of Si pillars, improves the high integration and high performance of the circuit, simplifies the manufacturing process, and reduces the complexity of the steps.
Smart Images

Figure CN113228241B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a method for manufacturing a three-dimensional semiconductor device. Background Art
[0002] In recent years, three-dimensional structure transistors have been used in LSI (Large Scale Integration). Among them, SGT (Surrounding Gate Transistor), a pillar-shaped semiconductor device, has attracted attention as a semiconductor device that can provide high integration. In addition, there is a demand for further high integration and high performance of semiconductor devices with SGT.
[0003] In a general planar metal oxide semiconductor (MOS) transistor, the channel extends in a horizontal direction along the upper surface of the semiconductor substrate. In contrast, the channel of the SGT extends in a direction perpendicular to the upper surface of the semiconductor substrate (see, for example, Patent Document 1 and Non-Patent Document 1). Therefore, compared with a planar metal oxide semiconductor transistor, the SGT can achieve a higher density of semiconductor devices.
[0004] Fig.10 The schematic structure diagram of the N-channel SGT is shown. N-channel SGT is formed at the upper and lower positions of the Si column 220 (hereinafter referred to as the "Si column") having a P-type or i-type (intrinsic type) conductivity type. + The layers 221a and 221b (hereinafter, the semiconductor region containing the donor impurity at a high concentration is referred to as “N + When one side of the layer is the source, the other side becomes the drain. + The portion of the Si pillar 220 between the layers 221a and 221b becomes a channel region 222. A gate insulating layer 223 is formed to surround the channel region 222. A gate conductor layer 224 is formed to surround the gate insulating layer 223. + The layers 221a, 221b, the channel region 222, the gate insulating layer 223, and the gate conductor layer 224 are all formed in a columnar shape. Therefore, in a top view, the area occupied by the SGT is equivalent to a single source or drain N of a planar metal oxide semiconductor transistor. + Therefore, a circuit chip having SGT can achieve a smaller chip size than a circuit chip having planar metal oxide semiconductor transistors.
[0005] Therefore, there is a demand for high integration of the circuit using the SGT shown in FIG. 10 .
[0006] [Prior art literature]
[0007] [Patent Document]
[0008] (Patent Document 1) Japanese Patent Application Laid-Open No. 2-188966.
[0009] (Non-patent literature)
[0010] (Non-patent document 1) Hiroshi Takato, Kazumasa Sunouchi, Naoko Okabe, Akihiro Nitayama, Katsuhiko Hieda, Fumio Horiguchi, and Fujio Masuoka: IEEE Transaction on Electron Devices, Vol. 38, No. 3, pp. 573-578 (1991)
[0011] (Non-patent document 2) N. Loubt, et al.: “Stacked Nanosheet Gate-All-Around Transistor to Enable Scaling Beyond FinFET” 2017 Symposium on VLSI Technology of Technical Papers, pp. T230, 231 (2017). Summary of the invention
[0012] (Problems to be solved by the invention)
[0013] There is a need to realize high density of columnar semiconductor devices.
[0014] (Methods to solve the problem)
[0015] A method for manufacturing a three-dimensional semiconductor device according to a first aspect of the present invention comprises:
[0016] A step of forming a first material layer on a second substrate located on the first substrate and at least a portion of the second substrate or the entire second substrate is formed of a semiconductor layer;
[0017] A step of forming a second strip-shaped material layer on the first material layer, the second strip-shaped material layer having a first strip-shaped material layer on the top thereof extending in one direction in a top view, wherein the first strip-shaped material layer has the same top view shape;
[0018] A step of forming a second material layer and a third material layer from the bottom to cover the entirety;
[0019] The step of smoothing the entire covering so that the upper surface positions of the second material layer and the third material layer become the upper surface position of the first strip-shaped material layer;
[0020] forming a third strip material layer on top of the smoothed second material layer and sandwiched between the smoothed third material layer and the side surfaces of the first strip material layer;
[0021] a step of removing the smoothed third material layer;
[0022] The step of etching the second material layer using the first strip material layer and the third strip material layer as masks to form a fourth strip material layer connected to both sides of the second strip material layer;
[0023] A step of forming a fourth material layer and a fifth material layer from the bottom to cover the entirety;
[0024] The step of smoothing the entire covering so that the upper surface positions of the fourth material layer and the fifth material layer become the upper surface position of the first strip-shaped material layer;
[0025] forming a fifth strip-shaped material layer on top of the smoothed fourth material layer and sandwiched between the smoothed fifth material layer and the side surfaces of the third strip-shaped material layer;
[0026] a step of removing the fifth material layer;
[0027] Using the first strip material layer, the third strip material layer and the fifth strip material layer as masks, etching the fourth material layer to form a sixth strip material layer connected to a side surface of the fourth strip material layer;
[0028] The step of removing the third strip material layer and the fourth strip material layer;
[0029] A step of forming a seventh strip-shaped material layer composed of a single layer or multiple layers above or below the first strip-shaped material layer and perpendicular to the first strip-shaped material layer in a plan view;
[0030] A step of forming a first mask material layer which is rectangular or circular in a plan view and is located in a first overlapping region of the seventh strip material layer, the second strip material layer, and the sixth strip material layer in a plan view by at least the first strip material layer and the fifth strip material layer, or the second strip material layer and the sixth strip material layer; and
[0031] Using the first mask material layer as a mask, etching the second substrate to form a three-dimensional semiconductor layer composed of the semiconductor layer on the first substrate;
[0032] And the aforementioned three-dimensional semiconductor layer is used as a channel.
[0033] More preferably, in the aforementioned production method,
[0034] The step of forming the third strip material layer comprises:
[0035] Using the first strip material layer and the smoothed third material layer as masks, etching the top of the second material layer to form a first concave portion; and
[0036] The step of filling the first recess to form the third strip-shaped material layer having an upper surface position identical to that of the first strip-shaped material layer.
[0037] More preferably, in the aforementioned production method,
[0038] The step of forming the fifth strip material layer comprises:
[0039] Using the first strip material layer, the third strip material layer and the fifth material layer as masks, etching the top of the fourth material layer to form a second recess; and
[0040] The step of filling the second recess to form the fifth strip-shaped material layer having an upper surface position identical to that of the first strip-shaped material layer.
[0041] More preferably, in the aforementioned production method,
[0042] In the vertical direction, above or below the first strip material layer, a ninth strip material layer is formed, which has an eighth strip material layer extending in one direction when viewed from above and has the same shape as the seventh strip material layer when viewed from above.
[0043] The seventh strip material layer is formed by the following steps:
[0044] A step of forming a sixth material layer and a seventh material layer from the bottom to cover the entirety;
[0045] The step of smoothing the entire covering so that the upper surface positions of the sixth material layer and the seventh material layer become the upper surface position of the eighth strip-shaped material layer;
[0046] Using the eighth strip material layer and the smoothed seventh material layer as masks, etching the top of the smoothed sixth material layer to form a third recess;
[0047] The step of filling the third recess to form a tenth strip material layer having an upper surface position identical to that of the eighth strip material layer;
[0048] a step of removing the sixth material layer;
[0049] Using the eighth strip material layer and the tenth strip material layer as masks, etching the sixth material layer to form an eleventh strip material layer connected to both sides of the ninth strip material layer; and
[0050] The eighth strip material layer and the ninth strip material layer are removed or the tenth strip material layer and the eleventh strip material layer are removed, and the lower layer or the upper and lower layers of the remaining strip material layer are used as the seventh strip material layer.
[0051] More preferably, in the aforementioned production method,
[0052] In a plan view, the width of one of the second strip-shaped material layer and the fourth strip-shaped material layer is formed to be larger than the width of the other.
[0053] More preferably, in the aforementioned production method,
[0054] In a plan view, the width of one of the second strip-shaped material layer and the sixth strip-shaped material layer is formed to be larger than the width of the other.
[0055] More preferably, in the aforementioned production method,
[0056] The three-dimensional semiconductor layer is a semiconductor column vertically erected on the first substrate.
[0057] More preferably, in the aforementioned production method,
[0058] The semiconductor column is composed of at least a first semiconductor column, a second semiconductor column and a third semiconductor column arranged adjacently along the one direction or a direction perpendicular to the one direction.
[0059] The method for manufacturing the three-dimensional semiconductor device includes:
[0060] A step of forming a first gate insulating layer surrounding the side surfaces of the first semiconductor column, the second semiconductor column and the third semiconductor column; and
[0061] A step of forming a first gate conductor layer surrounding the first gate insulating layer;
[0062] The first gate conductor layer is formed by filling a space between at least two of the first semiconductor pillar, the second semiconductor pillar, and the third semiconductor pillar.
[0063] More preferably, in the aforementioned production method,
[0064] The method includes removing any one of the plurality of semiconductor pillars formed on the substrate.
[0065] More preferably, in the aforementioned production method,
[0066] The method comprises the step of not forming a part of the seventh strip material layer in a plan view before forming the plurality of semiconductor pillars.
[0067] Furthermore, in a plan view, none of the plurality of semiconductor pillars is formed under the portion of the seventh strip material layer.
[0068] More preferably, in the aforementioned production method,
[0069] Include:
[0070] In parallel with the step of forming the second strip material layer having the first strip material layer on top, a step of extending a thirteenth strip material layer having a twelfth strip material layer on top along the same one direction on the first material layer, wherein the twelfth strip material layer has the same top view shape;
[0071] In parallel with the step of forming a fourth strip material layer having the third strip material layer on top, a step of extending a fifteenth strip material layer having a fourteenth strip material layer on top along the same one direction on the first material layer, wherein the fourteenth strip material layer has the same top view shape;
[0072] forming a sixteenth strip of material layer located between the fourth strip of material layer and the fifteenth strip of material layer and connected to the sides of the fourth strip of material layer and the fifteenth strip of material layer, and having the same shape as the sixth strip of material layer; and
[0073] The step of removing the third strip-shaped material layer, the fourth strip-shaped material layer, the fourteenth strip-shaped material layer and the fifteenth strip-shaped material layer.
[0074] More preferably, in the aforementioned production method,
[0075] The top of the smoothed second material layer is oxidized to form the third strip-shaped material layer.
[0076] More preferably, in the aforementioned production method,
[0077] Atomic ions are implanted into the top of the smoothed second material layer to form the third strip-shaped material layer.
[0078] More preferably, in the aforementioned production method,
[0079] Include:
[0080] In a top view, the steps of forming the second substrate by connecting two ends of one direction to the holding material layer and stacking a plurality of structures upwards with the first semiconductor layer and the eighth material layer as a group in a vertical direction;
[0081] After forming the aforementioned three-dimensional semiconductor layer, removing the aforementioned eighth material layer;
[0082] A step of forming a second gate insulating layer surrounding the first semiconductor layer of the three-dimensional semiconductor layer;
[0083] The step of forming a second gate conductor layer surrounding the second gate insulating layer;
[0084] a step of removing the aforementioned retaining material layer; and
[0085] The step of forming an impurity layer which is connected to both ends of the first semiconductor layer in the one direction in a plan view and contains donor or acceptor impurities.
[0086] A method for manufacturing a three-dimensional semiconductor device according to a second aspect of the present invention comprises:
[0087] A step of forming a first material layer on a second substrate located on the first substrate and at least a portion of the second substrate or the entire second substrate is formed of a semiconductor layer;
[0088] A step of forming a second strip-shaped material layer on the first material layer, the second strip-shaped material layer having the first strip-shaped material layer on the top thereof extending in one direction in a top view, wherein the first strip-shaped material layer has the same top view shape;
[0089] A step of forming a second material layer and a third material layer from the bottom to cover the entirety;
[0090] The step of smoothing the entire covering so that the upper surface positions of the second material layer and the third material layer become the upper surface position of the first strip-shaped material layer;
[0091] forming a third strip material layer on top of the smoothed second material layer and sandwiched between the smoothed third material layer and the side surfaces of the first strip material layer;
[0092] a step of removing the smoothed third material layer;
[0093] Using the first strip material layer and the third strip material layer as masks, etching the second material layer to form a fourth strip material layer having the third strip material layer on top;
[0094] The step of removing the first strip material layer and the second strip material layer;
[0095] A step of forming a fifth strip-shaped material layer composed of a single layer or multiple layers above or below the third strip-shaped material layer and perpendicular to the fourth strip-shaped material layer in a plan view;
[0096] A step of forming a first mask material layer which is rectangular or circular in a plan view and located in a first overlapping region of the fourth strip material layer and the fifth strip material layer in a plan view by at least the first strip material layer and the fifth strip material layer, or the second strip material layer and the sixth strip material layer; and
[0097] Using the first strip material layer as a mask, etching the second substrate to form a three-dimensional semiconductor layer composed of the semiconductor layer on the substrate;
[0098] And the aforementioned three-dimensional semiconductor layer is used as a channel.
[0099] More preferably, in the aforementioned production method,
[0100] The step of forming the third strip material layer comprises:
[0101] Using the first strip material layer and the third material layer as masks, etching the top of the second material layer to form a first concave portion; and
[0102] The step of forming the third strip-shaped material layer which fills the first recess and has an upper surface position which is the same as that of the first strip-shaped material layer.
[0103] More preferably, in the aforementioned production method,
[0104] In a plan view, the width of one of the second strip-shaped material layer and the fourth strip-shaped material layer is formed to be larger than the width of the other.
[0105] More preferably, in the aforementioned production method,
[0106] The three-dimensional semiconductor layer is a semiconductor column vertically erected on the first substrate.
[0107] More preferably, in the aforementioned production method,
[0108] The semiconductor column is composed of at least a first semiconductor column and a second semiconductor column arranged adjacent to each other along the one direction or a direction perpendicular to the one direction.
[0109] The method for manufacturing the three-dimensional semiconductor device includes:
[0110] A step of forming a first gate insulating layer surrounding the side surfaces of the first semiconductor column and the second semiconductor column; and
[0111] A step of forming a first gate conductor layer surrounding the first gate insulating layer;
[0112] The first gate conductor layer is formed by filling a space between the first semiconductor pillar and the second semiconductor pillar.
[0113] More preferably, in the aforementioned production method,
[0114] The method includes removing any one of the plurality of semiconductor pillars formed on the substrate.
[0115] More preferably, in the aforementioned production method,
[0116] The method comprises the step of not forming a part of the seventh strip material layer in a plan view before forming the plurality of semiconductor pillars.
[0117] Furthermore, in a plan view, none of the plurality of semiconductor pillars is formed under the portion of the seventh strip material layer.
[0118] More preferably, in the aforementioned production method,
[0119] Include:
[0120] Simultaneously with the formation of the first and second strip material layers, a step of forming a seventh strip material layer which is parallel to the first and second strip material layers in plan view and has a sixth strip material layer on top;
[0121] Simultaneously with the formation of the third and fourth strip material layers, a ninth strip material layer is formed which is connected to both sides of the sixth and seventh strip material layers and has the eighth strip material layer on the top; and
[0122] In parallel with the step of removing the first strip-shaped material layer and the second strip-shaped material layer, the step of removing the sixth strip-shaped material layer and the seventh strip-shaped material layer is performed.
[0123] More preferably, in the aforementioned production method,
[0124] The interval between the ninth strip-shaped material layer and the fourth strip-shaped material layer in a plan view is formed to be the same as that of one of the second strip-shaped material layer and the seventh strip-shaped material layer, or both of them.
[0125] More preferably, in the aforementioned production method,
[0126] The smoothed top of the second material layer is oxidized to form the third strip-shaped material layer.
[0127] More preferably, in the aforementioned production method,
[0128] Atomic ions are implanted into the top of the smoothed second material layer to form the third strip-shaped material layer.
[0129] More preferably, in the aforementioned production method,
[0130] Include:
[0131] In a top view, the step of forming the second substrate by connecting two ends of one direction to the holding material layer and stacking a plurality of structures upwards with the semiconductor layer and the fourth material layer as a group in a vertical direction;
[0132] After forming the three-dimensional semiconductor layer, removing the fourth material layer;
[0133] A step of forming a second gate insulating layer surrounding the semiconductor layer of the three-dimensional shape semiconductor layer;
[0134] The step of forming a second gate conductor layer surrounding the second gate insulating layer;
[0135] a step of removing the aforementioned retaining material layer; and
[0136] The step of forming an impurity layer which is connected to both ends of the semiconductor layer in the one direction in the plan view and contains donor or acceptor impurities.
[0137] [Effects of the invention]
[0138] According to the present invention, a high-density pillar-shaped semiconductor device can be realized. BRIEF DESCRIPTION OF THE DRAWINGS
[0139] Figure 1A It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0140] Figure 1B It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0141] Figure 1C It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0142] Figure 1D It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0143] Figure 1E It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0144] Figure 1F It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0145] Figure 1GIt is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0146] Figure 1H It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0147] Fig. 1I It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0148] Figure 1J It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0149] Figure 1K It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0150] Figure 1L It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0151] Figure 1M It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0152] Figure 1N It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0153] Fig.1O It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0154] Figure 1P It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0155] Figure 1Q It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0156] Figure 1R It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0157] Figure 1S It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0158] Figure 1T It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0159] Figure 1U It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0160] Figure 1V It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0161] Figure 1W It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0162] Figure 1X It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0163] Figure 1Y It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0164] Figure 1Z It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0165] Figure 1XX It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0166] Figure 1YY It is a plan view and a cross-sectional structure view for explaining the manufacturing method of the pillar-shaped semiconductor device having SGT according to the first embodiment.
[0167] Figure 2A It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a second embodiment of the present invention.
[0168] Figure 2B It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a second embodiment of the present invention.
[0169] Figure 2C It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a second embodiment of the present invention.
[0170] Figure 2D It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a second embodiment of the present invention.
[0171] Figure 3A It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a third embodiment of the present invention.
[0172] Figure 3B It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a third embodiment of the present invention.
[0173] Figure 3C It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a third embodiment of the present invention.
[0174] Figure 3D It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a third embodiment of the present invention.
[0175] Figure 3E It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a third embodiment of the present invention.
[0176] Figure 3F It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a third embodiment of the present invention.
[0177] Figure 4A It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a fourth embodiment of the present invention.
[0178] Figure 4B It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a fourth embodiment of the present invention.
[0179] Figure 5A It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a fifth embodiment of the present invention.
[0180] Figure 5B It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a fifth embodiment of the present invention.
[0181] Figure 5C It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a fifth embodiment of the present invention.
[0182] Figure 5D It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a fifth embodiment of the present invention.
[0183] Figure 5E It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a fifth embodiment of the present invention.
[0184] Fig. 5F It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a fifth embodiment of the present invention.
[0185] Figure 6 It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a sixth embodiment of the present invention.
[0186] Figure 7 It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a seventh embodiment of the present invention.
[0187] Fig. 8A It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to an eighth embodiment of the present invention.
[0188] Figure 8B It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to an eighth embodiment of the present invention.
[0189] Figure 8C It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to an eighth embodiment of the present invention.
[0190] Fig.8D It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to an eighth embodiment of the present invention.
[0191] Fig. 8E It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to an eighth embodiment of the present invention.
[0192] Fig.9A It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a ninth embodiment of the present invention.
[0193] Fig. 9B It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a ninth embodiment of the present invention.
[0194] Fig. 9C It is a plan view and a cross-sectional structure view for explaining a method for manufacturing a pillar-shaped semiconductor device having SGT according to a ninth embodiment of the present invention.
[0195] Fig.10 FIG. 1 is a schematic structural diagram showing a well-known example of SGT. DETAILED DESCRIPTION
[0196] A method for manufacturing a pillar-shaped semiconductor device according to an embodiment of the present invention will be described below with reference to the drawings.
[0197] (First embodiment)
[0198] The following reference Figure 1A to Figure 1YY , a method for manufacturing a columnar semiconductor device having SGT according to the first embodiment of the present invention is described. Part (a) of these figures is a plan view, part (b) is a cross-sectional structure view along the line X-X' of part (a), and part (c) is a cross-sectional structure view along the line Y-Y' of part (a).
[0199] like Figure 1A As shown, an N layer 2 is formed on a P layer substrate 1 by an epitaxial growth method. Furthermore, an N+ layer 3 and P+ layers 4 and 5 are formed on the surface of the N layer 2 by an ion implantation method. Furthermore, an i layer (intrinsic Si layer) 6 is formed. Furthermore, a mask material layer 7 composed of a SiO2 layer, an aluminum oxide (Al2O3) layer, and a SiO2 layer is formed. In addition, the i layer 6 can also be formed using N-type or P-type Si containing a small amount of donor or acceptor impurities. Furthermore, a silicon nitride (SiN) layer 8 is stacked. Furthermore, a mask material layer 9 composed of a SiO2 layer is stacked. Furthermore, a mask material layer 10 composed of a SiN layer is stacked.
[0200] Then, if Figure 1BAs shown, a strip-shaped resist layer (not shown) extending in the Y direction when viewed from above formed by photolithography is used as a mask to etch the mask material layer 10. Thus, a strip-shaped mask material layer 10a extending in the Y direction when viewed from above is formed. In addition, the strip-shaped mask material layer 10a can be made thinner than the width of the resist layer by isotropic etching. Thus, a strip-shaped mask material layer 10a having a width smaller than the width of the smallest resist layer that can be formed by photolithography can be formed. Furthermore, the mask material layer 9 is etched by, for example, RIE (Reactive Ion Etching) using the strip-shaped mask material layer 10a as a mask to form a strip-shaped mask material layer 9a. The cross-section of the mask material layer 9a formed by isotropic etching is a trapezoidal shape in which the width at the bottom is larger than the width at the top, while the cross-section of the mask material layer 9a becomes a rectangle due to RIE etching. This rectangular cross section leads to an improved accuracy of the etching pattern using the strip-shaped mask material layer 9a as a mask.
[0201] Then, if Figure 1C As shown, the mask material layer 8 is etched by RIE method, using the mask material layer 9a as a mask to form the mask material layer 8a. The mask material layer 10a can be removed before etching the mask material layer 8, or can be left.
[0202] Then, if Figure 1D As shown, the SiGe layer 12 and the SiO2 layer 13 are formed by the ALD (Atomic Layered Deposition) method to cover the mask material layer 7 (first material layer), the strip-shaped mask material layer 8a (second strip-shaped material layer), and the 9a (first strip-shaped material layer) as a whole. At this time, the cross section of the SiGe layer 12 (second material layer) generates a circular arc portion R1 at the top. This circular arc portion R1 is preferably formed above the strip-shaped mask material layer 8a.
[0203] Then, if Figure 1E As shown, the entire surface is covered with a SiO2 layer (not shown) formed by, for example, a flow CVD (Flow Chemical Vapor Deposition) method, and the SiO2 layer 13 (third material layer) and the SiGe layer 12 are polished by CMP (Chemical Mechanical Polishing) until the upper surface position becomes the upper surface position of the strip-shaped mask material layer 9a, thereby forming the SiO2 layer 13a, SiGe layers 12a, 12b. At this time, it is desired that the top side surfaces of the SiGe layers 12a, 12b can be vertical. Therefore, in the polishing step of the SiO2 layer 13 and the SiGe layer 12, it is preferred to remove Figure 1D The arc portion R1 at the top of the SiGe layer 12 in FIG.
[0204] Then, if Figure 1F As shown in FIG. 1 , the top of the SiGe layers 12a and 12b is etched using the SiO2 layer and the strip-shaped mask material layer 9a as masks to form recesses 14a and 14b (first recesses). It is preferred to etch the arc portion R1 at the top of the SiGe layers 12a and 12b and the bottom of the recesses 14a and 14b is located below the strip-shaped mask material layer 9a. The SiO2 layer 13 and the SiGe layer 12 are removed in the grinding step. Figure 1D The arc portion R1 at the top of the SiGe layer 12 can form recessed portions 14a and 14b whose outer peripheral side surfaces are vertical.
[0205] Then, if Figure 1G As shown, a SiN layer (not shown) is fully coated, and the SiN layer is polished by CMP to the upper surface position to form the upper surface position of the strip-shaped mask material layer 9a. Accordingly, SiN layers 15a and 15b (third strip-shaped material layer) having the same shape as the top shape of the SiGe layers 12a and 12b in a plan view are formed on both sides of the strip-shaped mask material layers 8a and 9a.
[0206] And, if Figure 1H As shown, the SiO2 layer 13 is removed.
[0207] Then, if Fig. 1I As shown, the SiGe layers 12a and 12b are etched using the strip-shaped mask material layers 9a, 15a, and 15b as masks to form strip-shaped SiGe layers 12aa and 12ab (fourth strip-shaped material layers). At this time, the strip-shaped SiGe layers 12aa and 12ab have the same width in a plan view.
[0208] Then, if Figure 1J As shown in FIG. 1 , a SiN layer 16 formed by the ALD method and a SiO2 layer 13b formed by the FCVD method are formed in a manner that covers the entire surface. Figure 1D Likewise, the arc portion R2 formed on the top of the SiN layer 16 (fourth material layer) is preferably located above the strip-shaped mask material layer 9a.
[0209] Next, polishing is performed until the upper surface positions of the SiO2 layer 13b (fifth material layer) and the SiN layer 16 become the same as the upper surface position of the strip-shaped mask material layer 9a. Figure 1E , Figure 1F The same steps, but Figure 1KAs shown, recessed portions 14A and 14B (second recessed portions) are formed on the strip-shaped SiN layers 16A and 16B and sandwiched between the strip-shaped mask material layers 15a and 15b and the SiO2 layer 13ba.
[0210] like Figure 1L As shown, strip-shaped SiN layers 16a and 16b are formed on both sides of the strip-shaped SiGe layers 12aa and 12ab, and strip-shaped mask material layers 17a and 17b (fifth strip-shaped material layers) are formed on both sides of the strip-shaped mask material layers 15a and 15b.
[0211] Next, a SiGe layer (not shown) is formed to cover the entire surface by ALD. Also, a SiO2 layer (not shown) is formed to cover the entire surface. Also, polishing is performed until the upper surface positions of the SiO2 layer and the SiGe layer become the same as the upper surface position of the strip-shaped mask material layer 9a. Also, polishing is performed with FIG. 1E to FIG. 1I The same steps, such as Figure 1M As shown, strip-shaped SiGe layers 18a and 18b are formed on both sides of the strip-shaped mask material layers 16a and 16b (sixth strip-shaped material layers), and strip-shaped mask material layers 19a and 19b are formed on both sides of the strip-shaped mask material layers 17a and 17b.
[0212] Next, a SiN layer (not shown) is formed to cover the entire surface by ALD. Also, a SiO2 layer (not shown) is formed to cover the entire surface. Also, polishing is performed until the upper surface positions of the SiO2 layer and the SiN layer become the same as the upper surface position of the strip-shaped mask material layer 9a. Also, polishing is performed with FIG. 1E to FIG. 1I The same steps, such as Figure 1N As shown, strip-shaped mask material layers 20a and 20b are formed to connect to both side surfaces of the strip-shaped mask material layers 18a and 18b, and strip-shaped mask material layers 21a and 21b are formed to connect to both side surfaces of the strip-shaped mask material layers 19a and 19b.
[0213] Next, the strip-shaped mask material layers 15a, 15b, 19a, 19b and the strip-shaped SiGe layers 12aa, 12ab, 18a, 18b are removed by etching. Fig.1O As shown, strip-shaped mask material layers 8a, 16a, 16b, 20a, 20b are formed on the mask material layer 7, and strip-shaped mask material layers 9a, 17a, 17b, 21a, 21b are formed on the strip-shaped mask material layers 8a, 16a, 16b, 20a, 20b.
[0214] Then, the entire surface is covered with a SiO2 layer (not shown). Figure 1PAs shown, the SiO2 layer 22 is formed by grinding by CMP until the upper surface position of the SiO2 layer becomes the upper surface position of the strip-shaped mask material layer 9a. In addition, a SiN layer 24 and a SiGe layer (not shown) are formed on the entire surface. In addition, a strip-shaped mask material layer 26 (eighth strip-shaped material layer) composed of a SiN layer extending in the X direction is formed. In addition, the SiGe layer is etched using the strip-shaped mask material layer 26 formed by photolithography and RIE as a mask to form a strip-shaped SiGe layer 25 (ninth strip-shaped material layer) extending in the X direction.
[0215] Next, by conducting Figure 1C to Figure 1I The same steps (perform Figure 1C to Figure 1I The same steps are followed to form the sixth strip material layer, the seventh strip material layer, the third recess, the tenth strip material layer and the eleventh strip material layer. Figure 1Q As shown, strip-shaped mask material layers 28a, 28b (seventh strip-shaped material layer) composed of SiN layers connected to the two side surfaces of the strip-shaped SiGe layer 25, and SiO2 layers, aluminum oxide layers, and strip-shaped mask material layers 27a, 27b (seventh strip-shaped material layer) composed of SiO2 layers connected to the two side surfaces of the strip-shaped mask material layer 26 are formed.
[0216] Then, if Figure 1R As shown, the strip mask material layer 26 and the strip SiGe layer 25 are removed, and strip mask material layers 28a and 28b extending along the X direction in a plan view and strip mask material layers 27a and 27b on the strip mask material layers 28a and 28b are formed on the SiN layer 24.
[0217] Then, if Figure 1SAs shown, the strip-shaped mask material layers 27a, 27b, 28a, 28b are used as masks to etch the SiN layer 24, the strip-shaped mask material layers 9a, 17a, 17b, 21a, 21b, 8a, 16a, 16b, 20a, 20b, and the SiO2 layer 22. Accordingly, a strip-shaped SiN layer 24a, square mask material layers 21aa, 21ab, 17aa, 17ab, 9aa in a plan view, and square mask material layers 20aa, 20ab, 16aa, 16ab, 8aa located under the square mask material layers 21aa, 21ab, 17aa, 17ab, 9aa are formed under the strip-shaped mask material layers 27a, 28a. Similarly, a strip-shaped SiN layer 24b, square-shaped mask material layers 21ba, 21bb, 17ba, 17bb, 9ab in a plan view, and square-shaped mask material layers 20ba (not shown), 20bb (not shown), 16ba (not shown), 16bb (not shown), 8ab located under the square-shaped mask material layers 21ba, 21bb, 17ba, 17bb, 9ab are formed under the strip-shaped mask material layers 27b and 28b. Furthermore, a SiO2 layer 22a is formed under the strip-shaped SiN layer 24a and between the square-shaped mask material layers 21aa, 21ab, 17aa, 17ab, 9aa, 20aa, 20ab, 16aa, 16ab, 8aa. Similarly, a SiO2 layer 22b is formed under the square-shaped SiN layer 24b and between the strip-shaped mask material layers 21ba, 21bb, 17ba, 17bb, 9ab, 20ba, 20bb, 16ba, 16bb, and 8ab.
[0218] Then, if Figure 1T As shown, the strip-shaped mask material layers 27a, 27b, 28a, 28b, the strip-shaped SiN layers 24a, 24b, and the SiO2 layers 22a, 22b are removed. Accordingly, square mask material layers 21aa, 21ab, 21ba, 21bb, 17aa, 17ab, 17ba, 17bb, 9aa, 9ab and square mask material layers 20aa, 20ab, 20ba, 20bb, 16aa, 16ab, 16ba, 16bb, 8aa, 8ab are formed on the mask material layer 7 when viewed from above.
[0219] Next, the mask material layer 7 is etched by RIE method using the mask material layers 21aa, 21ab, 21ba, 21bb, 17aa, 17ab, 17ba, 17bb, 9aa, 9ab and the mask material layers 20aa, 20ab, 20ba, 20bb, 16aa, 16ab, 16ba, 17bb, 8aa, 8ab as masks. Then, the mask material layers 21aa, 21ab, 21ba, 21bb, 17aa, 17ab, 17ba, 17bb, 9aa, 9ab and the mask material layers 20aa, 20ab, 20ba, 20bb, 16aa, 16ba, 16bb, 16ab, 8aa, 8ab are removed. Figure 1U As shown, mask material layers 7a, 7b, 7c, 7d, 7e, 7f, 7g, 7h, 7i, 7j (first mask material layers) are formed on the i layer 6. For example, before etching the mask material layer 7 by RIE, one or both of the square mask material layers 21aa, 21ab, 21ba, 21bb, 17aa, 17ab, 17ba, 17bb, 9aa, 9ab and the square mask material layers 20aa, 20ab, 20ba, 20bb, 16aa, 16ab, 16ba, 16bb, 8aa, 8ab are slightly isotropically etched. Thus, the mask material layers 7a to 7j are circular in shape when viewed from above.
[0220] Then, if Figure 1V As shown, the i layer 6 is etched using mask material layers 7a to 7j as masks to form Si pillars 6a, 6b, 6c, 6d, 6e, 6f, 6g, 6h, 6i, and 6j (three-dimensional semiconductor layers) on the N+ layer 3 and the P+ layer 4.
[0221] Next, a SiO2 layer (not shown) is coated by FCVD, and then polished by CMP until the surface position becomes the top position of the mask material layers 7a to 7j. Then, the mask material layers 7b, 7i, and Si pillars 6b, 6i are removed by photolithography and RIE etching. Then, the SiO2 layer formed by FCVD is removed. Figure 1W As shown, Si pillars 6a, 6c, 6d, 6e, 6f, 6g, 6h, and 6j are formed on the N+ layer 3 and the P+ layers 4 and 5i.
[0222] Then, if Figure 1XAs shown, mask material layers 30a, 30b, 30c, 30d are formed to surround the side surfaces of mask material layers 7a to 7j (without mask material layers 7b and 7i), and mask material layers 31a, 31b, 31c, 31d (not shown) are formed to surround the side surfaces of Si pillars 6a to 6j (without Si pillars 6b and 6i). Furthermore, a SiO2 layer (not shown) is coated on the entire surface by FCVD method, and then polished by CMP method until the surface position becomes the top position of mask material layers 7a to 7j (without mask material layers 7b and 7i). Furthermore, a strip-shaped mask material layer 33a, for example, composed of a SiO2 layer, which connects Si pillars 6a, 6c, 6d, and 6e in a top view, and a strip-shaped mask material layer 33b, for example, composed of a SiO2 layer, which connects Si pillars 6f, 6g, 6h, and 6j, are formed on this smooth surface. Furthermore, the SiO2 layer, N+ layer 3, P+ layer 4, 5, N layer 2, and P layer 1 are etched by RIE method using mask material layers 30a, 30b, 30c, 30d, 7a to 7j, 33a, and 33b as masks. Accordingly, N layer 2a, N+ layer 3a, and P+ layer 4a are formed below Si pillars 6a, 6c, 6d, and 6e and on P layer 1. Similarly, N layer 2b, N+ layer 3c (not shown), 3d (not shown), and P+ layer 5a are formed below Si pillars 6f, 6g, 6h, and 6j and on P layer 1. Furthermore, SiO2 layer 32a is formed below mask material layer 33a and between Si pillars 6a and 6c. Similarly, SiO2 layer 32b (not shown) is formed below mask material layer 33b and between Si pillars 6h and 6j.
[0223] Then, if Figure 1Y As shown, the mask material layers 33a, 33b, the SiO2 layers 32a, 32b, and the mask material layers 30a, 30b, 30c, 30d, 31a, 31b, 31c, and 31d are removed.
[0224] Then, if Figure 1ZAs shown, a SiO2 layer 34 is formed on the periphery of the N+ layer 3a, 3b, 3c, 3d, the P+ layer 4a, 5a, the N layer 2a, 2b and the P layer substrate 1. Furthermore, by the ALD method, a HfO2 layer (not shown), a TiN layer (not shown), and a SiO2 layer (not shown) are formed to cover the entirety. At this time, the TiN layer between the Si pillars 6c, 6c, 6e is preferably in contact with each other on the side. Similarly, the TiN layer between the Si pillars 6f, 6g, 6h is preferably in contact with each other on the side. Furthermore, the CMP method is used to grind until the upper surface position of the HfO2 layer, the TiN layer, and the SiO2 layer becomes the upper surface position of the mask material layers 7a to 7j. Furthermore, the SiO2 layer is etched back by the RIE method. Furthermore, the TiN layer and the HfO2 layer are etched using this SiO2 layer as a mask until the upper surface position becomes the upper position of the Si pillars 6a to 6j. Then, a SiN layer (not shown) is formed to cover the entire structure by CVD. Then, the SiN layer is polished by CMP until the upper surface position becomes the upper surface position of the mask material layers 7a to 7j. Thus, SiN layers 37a, 37b, 37c, and 37d (not shown) with the same width when viewed from above are formed on the outer periphery of the top of the Si pillars 6a to 6j.
[0225] Next, mask material layers 38a, 38b, 38c, and 38d are formed on the upper surfaces of the mask material layers 7a to 7j so as to be connected to the Si pillars 6a, 6d, 6g, and 6j when viewed from above. Furthermore, the SiO2 layer and the TiN layer located at the periphery of the mask material layers 37a, 37b, 37c, 37d, 38a, 38b, 38c, and 38d when viewed from above are etched using the mask material layers 7a to 7j, 37a, 37b, 37c, 37d, 38a, 38b, 38c, and 38d as masks. Thus, a TiN layer 40a connected to the periphery of the Si pillar 6a, a TiN layer 40b connected to the periphery of the Si pillars 6c, 6d, and 6e, a TiN layer 40c connected to the periphery of the Si pillars 6f, 6g, and 6h, and a TiN layer 40d connected to the periphery of the Si pillar 6j are formed (not shown). Also, the mask material layers 38a to 38d, 37a to 37d, 7a to 7j are removed.
[0226] Then, if Figure 1XX As shown, the entire structure is covered with a SiO2 layer (not shown), and then polished by CMP until the upper surface position of the SiO2 layer becomes the upper surface position of the top of the Si pillars 6a to 6j. In addition, the upper part of the SiO2 layer is etched by RIE until its upper surface position becomes the top position of the TiN layer 40a to 40d. In addition, a SiN layer 42 is formed on the outer periphery of the top of the Si pillars 6a to 6j.
[0227] Next, after the tops of the Si pillars 6c and 6h are covered with a SiO2 layer (not shown), an N+ layer 43a containing donor impurities is formed to surround the top of the Si pillar 6a by a selective epitaxial growth method. At the same time, an N+ layer 43c covering the top of the Si pillar 6d, an N+ layer 43d (not shown) covering the top of the Si pillar 6e, an N+ layer 43e (not shown) covering the top of the Si pillar 6f, and an N+ layer 43h (not shown) covering the top of the Si pillar 6j are formed. Furthermore, the SiO2 layer covering the tops of the Si pillars 6c and 6h is removed. Furthermore, a SiO2 layer (not shown) is formed to cover the Si pillars 6a, 6d, 6e, 6f, 6g, and 6j. Furthermore, by a selective epitaxial growth method, P+ layers 43b and 43g containing acceptor impurities are formed to surround the tops of the Si pillars 6c and 6h. Furthermore, by heat treatment, donor impurities of the N+ layers 43a, 43c, 43d, 43e, 43f, and 43g are diffused to the tops of the Si pillars 6a, 6d, 6e, 6f, 6g, and 6j to form N+ layers 44a, 44c, 44d, 44e (not shown), 44f (not shown), and 44h (not shown). At the same time, acceptor impurities are diffused from the P+ layers 43b and 43g to form P+ layers 44b and 44g.
[0228] Then, if Figure 1YY As shown, a SiO2 layer 46 with a flat upper surface is formed by covering the entirety. Furthermore, a connection wiring metal layer C1 is formed through a connection hole 47a formed on the interface between the N+ layer 3a and the P+ layer 4a and on the TiN layer 40b. At the same time, a connection wiring metal layer C2 (not shown) is formed through a connection hole 47b formed on the interface between the N+ layer 3d and the P+ layer 5a and on the TiN layer 40b. A SiO2 layer 48 with a flat upper surface is formed by covering the entirety. Furthermore, a character wiring metal layer WL is formed through connection holes 49a and 49b formed on the TiN layers 40a and 40d. A SiO2 layer 50 with a flat upper surface is formed by covering the entirety. Furthermore, a ground wiring metal layer Vss1 is formed through connection holes 51a and 51b formed on the N+ layers 43c and 43d. At the same time, a ground wiring metal layer Vss2 is formed through the connection holes 51c and 51d formed on the N+ layer 43e and 43f. And, a SiO2 layer 52 with a flat upper surface is formed by covering the entirety. And, a power supply metal wiring layer Vdd is formed through the connection holes 53a and 53b formed on the P+ layer 43b and 43g. And, a SiO2 layer 54 with a flat upper surface is formed by covering the entirety. And, a bit output metal wiring layer BL and an inversion bit wiring metal layer RBL are formed through the connection holes 55a and 55b formed on the N+ layer 43a and 43h. In this way, an SRAM unit circuit is formed on the P layer substrate 1.
[0229] According to the manufacturing method of the first embodiment, the following features can be obtained.
[0230] 1. This embodiment is as follows Figure 1V As shown, ten Si pillars 6a to 6j are formed in one SRAM cell region. Among them, photolithography is used only when forming the strip-shaped SiN layer 8a for forming one row of Si pillars (6c, 6h) in the X direction. The other eight Si pillars (6a to 6j except 6c and 6h) are formed by strip-shaped SiGe layers 12aa, 12ab, 18a, 18b, and strip-shaped SiN layers 16a, 16b, 20a, 20b formed by the ALD method. The strip-shaped SiGe layers 12a and 12b are formed by the ALD method, and strip-shaped mask material layers 15a and 15b having a shape that allows the top shape of the strip-shaped SiGe layers 12a and 12b to remain intact are formed on the strip-shaped SiGe layers 12a and 12b. Using the ALD method, material layers can be carefully controlled to be stacked in atomic or molecular layers. According to this, the thickness of the strip SiGe layers 12a and 12b can be made high-precision and narrow-pitch in a top view in response to design requirements. According to this, the distance between the Si pillars 7a to 7j can be made high-precision and narrow-pitch without being limited by photolithography. According to this, the high integration of SRAM units can be sought. In addition, when the distance between the Si pillars 6c, 6h, Si pillars 6b, 6d, 6g, and 6i is to be formed with high precision and the narrowest pitch only in the X direction, the strip SiGe layers 12aa and 12ab and the strip mask material layers 15a and 15b can be formed by the manufacturing method provided by the present invention.
[0231] 2. Similarly, the strip-shaped SiN layers 16A and 16B formed by the ALD method, and the strip-shaped mask material layers 17a and 17b on the strip-shaped SiN layers 16A and 16B have a shape that allows the top shape of the strip-shaped SiN layers 16A and 16B to remain intact. According to this, the diameter of the Si pillars 7a to 7j in a top view can be made high-precision and small without being restricted by photolithography. According to this, the restrictions on high integration caused by photolithography can be eliminated to carry out unit design. According to this, the high precision and high integration of SRAM units can be sought.
[0232] 3. If the unit is to be highly integrated, there is a need for both high precision and high density of the diameter of the Si pillars 6a to 6j when viewed from above and the distance between the Si pillars 6a to 6j. FIG. 1D to FIG. 1OAs shown, the strip SiGe layers 12aa, 12ab, 18a, 18b formed on both sides of the strip SiN layer 8a in the X-direction section, and the strip SiN layers 16a, 16b, 20a, 20b can be formed with high precision and narrow pitch. The high precision of the thickness of the strip SiN layers 16a, 16b, 20a, 20b is associated with the high precision of the diameter of the Si pillars 6a to 6j. In addition, the high precision of the thickness of the strip SiGe layers 12aa, 12ab, 18a, 18b is associated with the high precision of the distance between the Si pillars 6a to 6j. Based on this, the high precision and high integration of the SRAM unit can be achieved.
[0233] 4. When etching the SiGe layers 12a, 12b and the SiN layers 16A, 16B by RIE, the portions of the strip-shaped mask material layers 15a, 15b, 17a, 17b that are hit by etching ions have a lower etching rate, but will still be etched. When the strip-shaped mask material layers 15a, 15b, 17a, 17b are, for example, trapezoidal in shape with a longer bottom side than a top side, the bottom side portions of the strip-shaped mask material layers 15a, 15b, 17a, 17b will be etched during etching. Accordingly, the mask layer ends of the strip-shaped mask material layers 15a, 15b, 17a, 17b viewed from above will change with the etching time. In this way, it is difficult for the strip-shaped SiGe layers 12aa, 12ab and the strip-shaped SiN layers 16a, 16b to be formed into a rectangular shape when viewed in cross section. In contrast, in this embodiment, SiGe layers 12a, 12b, and SiN layers 16A, 16B having the same thickness in the vertical direction are formed on both sides of the strip-shaped SiN layer 8a and the strip-shaped mask material layer 9a. In addition, strip-shaped mask material layers 15a, 15b, 17a, 17b are formed so that the top shapes of the SiGe layers 12a, 12b, and SiN layers 16A, 16B remain intact. Thus, strip-shaped mask material layers 15a, 15b, 17a, 17b having a rectangular cross section are formed. Furthermore, the SiGe layers 12a, 12b, and SiN layers 16A, 16B are etched using the strip-shaped mask material layers 15a, 15b, 17a, 17b having a rectangular cross section as a mask, thereby forming strip-shaped SiGe layers 12aa, 12ab, and strip-shaped SiN layers 16a, 16b having a rectangular cross section. This makes it possible to achieve higher precision and higher integration of the SRAM cell.
[0234] 5. As FIG. 1E to FIG. 1IAs shown, for example, the strip-shaped SiN layer 8a and the strip-shaped mask material layer 9a are covered with the strip-shaped mask material layers 15a and 15b as etching masks for the strip-shaped SiGe layers 12aa and 12ab, and the SiGe layer 12 is stacked by the ALD method. In addition, the SiO2 layer (not shown) is stacked. In addition, the SiO2 layer and the SiGe layer 12 are polished by the CMP method until their upper surface positions become the upper surface positions of the strip-shaped mask material layer 9a. The arc portion R1 of the upper part of the SiGe layer 12 is removed by this polishing. By removing the arc portion R1 of the upper part, the shapes of the recesses 14a and 14b are formed along the side shapes of the strip-shaped mask material layer 9a and the SiO2 layer 13 on both sides of the SiGe layers 12a and 12b, and along the shapes of the strip-shaped SiGe layers 12a and 12b of equal width in the vertical direction. Therefore, the cross-sectional shape of the recesses 14a and 14b is formed into a substantially rectangular shape. According to this, the cross-sectional shape of the strip-shaped mask material layers 15a and 15b maintains a shape with equal width in the vertical direction, and is generally rectangular in overall view. This means that the strip-shaped SiGe layers 12a and 12b formed by etching the SiGe layer 12a by the RIE method using the strip-shaped mask material layers 15a and 15b as masks can be formed with high precision both in a top view and in a cross-sectional view. In the same way, the strip-shaped SiN layers 16a, 16b, 20a, 20b and the strip-shaped SiGe layers 18a and 18b can be formed with high precision.
[0235] 6. This embodiment is as follows Figure 1Z As shown, the gate TiN layers 40b and 40c connecting the outer peripheries of the Si pillars 7c, 7d, 7e, and the Si pillars 7f, 7g, and 7h are in contact with the sides between the Si pillars 7c, 7d, and 7e, and between the Si pillars 7f, 7g, and 7h. On the other hand, in the Si pillars 6a and 6j, the gate TiN layers 40a and 40d are independently formed. The gate TiN layers 40b and 40c connecting the outer peripheries of the Si pillars 7c, 7d, 7e, and the Si pillars 7f, 7g, and 7h are in contact with the sides between the Si pillars 7c, 7d, 7e, and between the Si pillars 7f, 7g, and 7h, which means that the distance between the Si pillars 7c, 7d, 7e, and between the Si pillars 7f, 7g, and 7h can be shortened to twice the thickness of the gate HfO2 layer 35 and the gate TiN layers 40b and 40c added together. And, as Figure 1W As shown, by removing the Si pillars 7b and 7i, the gate TiN layers 40a and 40c can be separated from the gate TiN layers 40b and 40d. Figure 1WAs shown, after Si pillars 6a to 6j are formed at a high density in a plan view, Si pillars 7b and 7i are removed, thereby forming an area without Si pillars in a plan view. Accordingly, connection holes 47a and 47b can be formed in the area where Si pillars 7b and 7i are removed in a plan view. Accordingly, high density of SRAM cells can be sought. This embodiment can be applied not only to SRAM cells, but also to circuits having multiple Si pillars connecting gate conductor layers to each other, and one or more Si pillars adjacent to these multiple Si pillars and having separated gate conductor layers.
[0236] 7. This embodiment is as follows Figure 1P to Figure 1S As shown, the strip-shaped mask material layers 27a, 27b, 28a, 28b extending in the X direction orthogonal to the strip-shaped mask material layers 8a, 16a, 16b, 20a, 20b extending in the Y direction are formed in the same manner as the strip-shaped mask material layers 8a, 16a, 16b, 20a, 20b are formed. Thus, the Si pillars 6a to 6j can be formed with high precision and high density in both the X direction and the Y direction. In addition, the description of this embodiment forms the strip-shaped mask material layers 28a, 28b after the strip-shaped mask material layers 8a, 16a, 16b, 28a, 28b are formed. In contrast, even in the step of forming the strip-shaped mask material layers 8a, 16a, 16b, 28a, 28b after the strip-shaped mask material layers 28a, 28b are formed, the Si pillars 6a to 6j can be formed with high precision and high density. In addition, when there is sufficient space in the Y direction, the present method may not be used, and after the mask material layer is fully formed, the strip-shaped mask material layers 27a, 27b, 28a, 28b may be directly formed by photolithography and RIE etching. In addition, when there is sufficient space in the X direction, the present method may not be used, and after the mask material layer is fully formed, the strip-shaped mask material layers 8a, 16a, 16b, 20a, 20b or the strip-shaped mask material layers 9a, 17a, 17b, 21a, 21b may be directly formed by photolithography and RIE etching.
[0237] 8. This embodiment is as follows Fig.1OAs shown, five strip-shaped SiN layers 8a, 16a, 16b, 20a, and 20b extending in the Y direction when viewed from above are formed. In contrast, when the material of the strip-shaped SiN layer 8a is replaced from SiN to SiGe, and the material of the strip-shaped SiGe layers 12a and 12b is replaced with SiN, two strip-shaped SiN layers extending in parallel in the Y direction when viewed from above can be formed. Accordingly, Si pillars can be formed at high density at the positions of these two strip-shaped SiN layers when viewed from above. When viewed from above, the formation of the first formed strip-shaped SiN layer 8a, the formation of the material of the strip-shaped material layer composed of the strip-shaped mask material layer 9a, the formation of the strip-shaped SiN layer formed in parallel on both sides of the strip-shaped material layer, the formation of the material of the strip-shaped mask material layer, and the formation of the strip-shaped SiN layer or the strip-shaped SiGe layer are repeatedly performed, thereby forming three, four, five or more strip-shaped SiN layers extending in the Y direction when viewed from above. According to this, Si pillars can be formed at a high density at the position of the strip-shaped SiN layer in a plan view.
[0238] (Second embodiment)
[0239] Below, refer to FIG. 2A to FIG. 2D , a method for manufacturing a columnar semiconductor device having SGT according to a second embodiment of the present invention is described. Part (a) of these figures is a plan view, part (b) is a cross-sectional structure view along line X-X' of part (a), and part (c) is a cross-sectional structure view along line Y-Y' of part (a).
[0240] Conduct with Figures 1A to 1L Same steps. In this step, Figure 1A The configurations of the N+ layer 3 and the P+ layer 4 in the top view are different, such as Figure 2A As shown, strip-shaped N+ layers 3A and 3B are formed on both sides of the strip-shaped P+ layer 4A. Furthermore, SiGe layers 12Aa and 12Ab are formed on both sides of the strip-shaped SiN layer 8a having a strip-shaped mask material layer 9a on the top, and the width is wider than the strip-shaped SiGe layers 12aa and 12ab when viewed from above. Furthermore, strip-shaped mask material layers 15A and 15B are formed on the top of the strip-shaped SiGe layers 12Aa and 12Ab. Furthermore, strip-shaped mask material layers 16A and 16B having the same width as the strip-shaped SiN layer 8a and having strip-shaped mask material layers 17A and 17B on the top are formed on both sides of the strip-shaped SiGe layers 12Aa and 12Ab.
[0241] Next, proceed with Figures 1N to 1T The same steps. Figure 2B As shown, square SiN layers 8Aa, 8Ab, 16Aa, 16Ab (not shown), 16Ba, 16Bb (not shown) are formed on the mask material layer 7, and the tops of the mask material layers 9Aa, 9Ab, 17Aa, 17Ab, 17Ba, 17Bb have square shapes when viewed from above.
[0242] Next, proceed with Figure 1U , Figure 1V The same steps. Figure 2C As shown, Si pillars 61a, 61c, 61d, and 61f are formed on the N+ layers 3A and 3B, and Si pillars 61b and 61e are formed on the P+ layer 4A.
[0243] Next, proceed with Figure 1X to Figure 1YY The same steps. Figure 2D As shown, N layer 2A, N+ layer 3Aa, 3Ba, and P+ layer 4Aa are formed under Si pillars 61a, 61b, and 61c. Similarly, N layer 2B, N+ layer 3Ba (not shown), 3Bb (not shown), and P+ layer 4Ba are formed under Si pillars 61d, 61e, and 61f. In addition, SiO2 layer 33 is formed in a manner surrounding the lower portion of Si pillars 61a to 61f. In addition, HfO2 layer 63 of the gate insulating layer is formed in a manner surrounding Si pillars 61a to 61f. In addition, gate TiN layers 65a, 65b, 65c, 65d (not shown), and SiO2 layer 41 are formed in a manner surrounding HfO2 layer 63. In addition, SiN layer 42 is formed on the top periphery of Si pillars 61a to 61f. Furthermore, N+ layers 67a, 67c, 67d, 67f, and P+ layers 67b, 67e are formed on the tops of the Si pillars 61a to 61f by a selective epitaxial growth method. Next, heat treatment is performed to form N+ layers 66a, 66c, 66d (not shown), 66f (not shown), and P+ layers 66b, 66e on the tops of the Si pillars 61a to 61f.
[0244] Next, after the SiO2 layer 46 is formed on the entire surface, the N+ layer 3Aa, the P+ layer 4Aa, and the gate TiN layer 65c are connected via a metal layer (not shown) formed by a connection hole 69a formed on the boundary between the N+ layer 3Aa and the P+ layer 4Aa, and on the gate TiN layer 65c. At the same time, the N+ layer 3Bb, the P+ layer 4Ba, and the gate TiN layer 65b are connected via a metal layer (not shown) formed by a connection hole 69b formed on the boundary between the N+ layer 3Bb and the P+ layer 4Ba, and on the gate TiN layer 65b. Next, after the SiO2 layer 48 is formed on the entire surface, the gate TiN layers 65a and 65d are connected to the character wiring metal layer WL via a connection hole 70a formed on the gate TiN layer 65a, and a connection hole 70b formed on the gate TiN layer 65d. Next, after the SiO2 layer 50 is fully formed, the P+ layer 67b, 67e is connected to the power wiring metal layer Vdd through the connection holes 71a, 71b formed on the P+ layer 67b, 67e. Next, after the SiO2 layer 52 is fully formed, the N+ layer 67a is connected to the ground wiring metal layer Vss1 through the connection hole 73a. At the same time, the N+ layer 67f is connected to the ground wiring metal layer Vss2 through the connection hole 73b. Next, after the SiO2 layer 54 is fully formed, the N+ layer 67c is connected to the bit wiring metal layer BL through the connection hole 74a. At the same time, the N+ layer 67d is connected to the reverse bit wiring metal layer RBL through the connection hole 74b. In this way, an SRAM cell is formed on the P layer substrate 1.
[0245] According to the manufacturing method of this embodiment, the following features can be obtained.
[0246] 1. The first embodiment Figure 1N As shown in FIG. 1 , five strip-shaped SiN layers 8a, 16a, 16b, 20a, and 20b are formed on the mask material layer 7. Figure 2A As shown in FIG. 1 , three strip-shaped SiN layers 8a, 16A, and 16B are formed to form an SRAM cell. This simplifies the process.
[0247] 2. The first embodiment Figure 1V As shown in FIG. 1 , a step of removing the Si pillars 6 b and 6 i formed in the SRAM region is required. In contrast, the present embodiment does not require such a step of removing the Si pillars, thereby simplifying the steps.
[0248] (Third embodiment)
[0249] Below, refer to FIG. 3A to FIG. 3F, a method for manufacturing a columnar semiconductor device having SGT according to a third embodiment of the present invention is described. Part (a) of these figures is a plan view, part (b) is a cross-sectional structure view along line X-X' of part (a), and part (c) is a cross-sectional structure view along line Y-Y' of part (a).
[0250] like Figure 3A As shown, first, a strip-shaped SiGe layer 80 (a second strip-shaped material layer) is formed by using a strip-shaped mask material layer 81 (a first strip-shaped material layer) as an etching mask, and then Figure 1C The strip-shaped SiN layer 8a and the mask material layer 9a are shown.
[0251] Next, proceed with Figures 1D to 1M The same steps are shown in Figure 2. Figure 3B As shown, on both sides of the strip-shaped SiGe layer 80 having a strip-shaped mask material layer 81 on the top, strip-shaped SiN layers 82a and 82b (fourth strip-shaped material layer) having strip-shaped mask material layers 83a and 83b (third strip-shaped material layer) on the top are formed with equal width. Furthermore, on both sides of the strip-shaped SiN layers 82a and 82b, strip-shaped SiGe layers 84a and 84b having strip-shaped mask material layers 85a and 85b on the top are formed with equal width. Furthermore, on both sides of the strip-shaped SiGe layers 84a and 84b, strip-shaped SiN layers 86a and 86b having strip-shaped mask material layers 87a and 87b on the top are formed.
[0252] Next, proceed with Figures 1N to 1T The same steps are shown in Figure 2. Figure 3C As shown, square SiN layers 90a, 90b, 90c, 90d, 90e (not shown), 90f (not shown), 90g, 90h (not shown) are formed on the mask material layer 7, and the mask material layers 91a, 91b, 91c, 91d, 91e, 91f, 91g, 91h (first mask material layer) have square shapes on the top when viewed from above.
[0253] Next, proceed with Figure 1U , Figure 1V The same steps are shown in Figure 2. Figure 3D As shown, Si pillars 93a, 93b, 93c, 93d, 93e, 93f, 93g, 93h (three-dimensional shaped semiconductor layer) with mask material layers 92a, 92b, 92c, 92d, 92e, 92f, 92g, 92h on the top are formed on the N+ layer 3c, the P+ layer 4c, 4d.
[0254] Then, if Figure 3E As shown, the mask material layers 92b, 92g and Si pillars 93b, 93g are removed.
[0255] Next, proceed with Figure 1Z to Figure 1YY The same steps. Figure 3F As shown, N layer 2ca, N+ layer 3ca, 3cb, and P+ layer 4ca are formed under Si pillars 93a, 93c, and 93d. Similarly, N layer 2cb, N+ layer 3da (not shown), 3db (not shown), and P+ layer 4cb are formed under Si pillars 93e, 93f, and 93g. In addition, HfO2 layer 95 of the gate insulating layer is formed in a manner surrounding Si pillars 93a to 93h. In addition, gate TiN layers 96a, 96b, 96c, and 96d (not shown) are formed in a manner surrounding HfO2 layer 95. Furthermore, N+ layers 98a, 98c, 98d (not shown), 98f (not shown) are formed on the top of Si pillars 93a, 93d, 93e, 93h, and N+ layers 97a, 97c, 97d (not shown), 97e (not shown) are formed on the top of Si pillars 93a, 93d, 93e, 93h. Similarly, P+ layers 98b, 98e are formed on the top of Si pillars 93c, 93f, and P+ layers 97b, 97e are formed on the top. Next, the N+ layer 3ca, the P+ layer 4ca and the gate TiN layer 96c are connected through a metal layer (not shown) formed by a connection hole 99a formed on the boundary between the N+ layer 3ca and the P+ layer 4ca and on the gate TiN layer 96c. At the same time, the N+ layer 3db, the P+ layer 4cb and the gate TiN layer 96b are connected through a metal layer (not shown) formed at the boundary between the N+ layer 3db and the P+ layer 4cb and through a connection hole 99b formed on the gate TiN layer 96b. Furthermore, the gate TiN layers 96a and 96d are connected to the character wiring metal layer WL through a connection hole 101a formed on the gate TiN layer 96a and a connection hole 101b formed on the gate TiN layer 96d. The P+ layers 98b and 98e are connected to the power wiring metal layer Vdd through connection holes 102a and 102b formed on the P+ layers 98b and 98e. The N+ layer 98c is connected to the ground wiring metal layer Vss1 through a connection hole 103a. At the same time, the N+ layer 98d is connected to the ground wiring metal layer Vss2 through a connection hole 103b. The N+ layer 98a is connected to the inverted bit wiring metal layer RBL through the connection hole 104A, and the N+ layer 98f is connected to the bit wiring metal layer BL through the connection hole 104B. Thus, an SRAM cell is formed on the P layer substrate 1.
[0256] According to the manufacturing method of this embodiment, the following features can be obtained.
[0257] 3. The first embodiment Figure 1N As shown in FIG. 1 , five strip-shaped SiN layers 8a, 16a, 16b, 20a, and 20b are formed on the mask material layer 7. Figure 3BAs shown in the figure, four strip-shaped SiN layers 82a, 82b, 86a, and 86b are formed to form an SRAM cell. This can simplify the process.
[0258] 4. In this embodiment, similarly to the first embodiment, the gate TiN layers 96b and 96c connected to the outer periphery of the Si pillars 93c and 93d and the Si pillars 93e and 93f are in contact with each other at the sides between the Si pillars 93c and 93d and between the Si pillars 93e and 93f. On the other hand, the gate TiN layers 96a and 96d are independently formed at the Si pillars 93a and 93h. In this way, the gate TiN layers 96b and 96c are in contact with each other at the sides between the Si pillars 93c and 93d and between the Si pillars 93e and 93f, which means that the distance between the Si pillars 93c and 93d and between the Si pillars 93e and 93f can be shortened to twice the thickness of the gate HfO2 layer 95 and the gate TiN layers 96b and 96c added together. Based on this, the high integration of the SRAM unit can be achieved.
[0259] (Fourth embodiment)
[0260] Below, refer to Figure 4A , Figure 4B , a method for manufacturing a columnar semiconductor device having SGT according to a fourth embodiment of the present invention is described. Part (a) of these figures is a plan view, part (b) is a cross-sectional structure view along line X-X' of part (a), and part (c) is a cross-sectional structure view along line Y-Y' of part (a).
[0261] Conduct 1A to Figure 1R And, if Figure 4A As shown, by photolithography and RIE etching, the top view is removed. Figure 1R The strip-shaped mask material layers 27a and 28a in the area on the SiN layer 16a are removed to form strip-shaped mask material layers 28A and 28B having strip-shaped mask material layers 27A and 27B on the top. At the same time, the strip-shaped mask material layers 27b and 28b on the SiN layer 16b are removed to form strip-shaped mask material layers 28C and 28D having strip-shaped mask material layers 27C and 27D on the top (not shown).
[0262] Next, by performing the steps shown in Figures 1S and 1T, as shown in Figures 1S and 1T, Figure 4B As shown, mask material layers 21aa, 21ab, 21ba, 21bb, 17ab, 17ba, 9aa, 9ab, and square mask material layers 20aa, 20ab, 20ba (not shown), 20bb, 16ab, 16ba (not shown), 8aa, 8ab are formed on the mask material layer 7 in a plan view. Figure 1SThe SiN layers 16aa, 16bb and the mask material layers 17aa, 17bb are formed. Figure 1X to Figure 1YY In the step of forming an SRAM cell having the same structure as that of the first embodiment on the P-layer substrate 1.
[0263] According to the manufacturing method of this embodiment, the following features can be obtained.
[0264] In the first embodiment, after forming Si columns 6b, 6i and mask material layers 7b, 7i, these Si columns 6b, 6i and mask material layers 7b, 7i are removed. At this time, for Si columns 6b, 6i having a height in the vertical direction, it is necessary to carefully control the etching and remove them so that the etching end point is the same as the bottom of other Si columns 6a, 6c, 6d, 6e, 6f, 6g, 6h, 6j. In contrast, the etching in the first embodiment is performed in this embodiment. Figure 1R The mask material layers 27a, 27b, 28a, and 28b shown as the uppermost ones are sufficient. In this case, the etching end point is the mask material layer 7 which serves as an etching stopper, and there is no problem regarding the controllability of the etching end point as in the first embodiment.
[0265] (Fifth embodiment)
[0266] Below, refer to FIG. 5A to FIG. 5F , a method for manufacturing a columnar semiconductor device having SGT according to a fifth embodiment of the present invention is described. Part (a) of these figures is a plan view, part (b) is a cross-sectional structure view along line X-X' of part (a), and part (c) is a cross-sectional structure view along line Y-Y' of part (a).
[0267] like Figure 5A As shown, on the mask material layer 7, a strip-shaped SiN layer 101a and a strip-shaped SiN layer 101b (the seventh strip-shaped material layer, the twelfth strip-shaped material layer, and the sixteenth strip-shaped material layer) are formed on the top of the mask material layer 7 extending in the Y direction. The strip-shaped SiN layer 101a is formed on the N+ layer 3A in a top view. In addition, the strip-shaped SiN layer 101b is formed on the N+ layer 3B in a top view. The N+ layer 3A and the N+ layer 3B are formed in a strip shape on both sides of the strip-shaped P+ layer 4A in a top view.
[0268] Next, proceed FIG. 1D to FIG. 1I According to this, Figure 5BAs shown, strip-shaped mask material layers 102aa, 102ab and strip-shaped SiGe layers 103aa, 103ab are formed on both sides of the strip-shaped mask material layer 100a and the strip-shaped SiN layer 101a. Similarly, strip-shaped mask material layers 102ba, 102bb (eighth strip-shaped material layer, thirteenth strip-shaped material layer, seventeenth strip-shaped material layer) and strip-shaped SiGe layers 103ba, 103bb (ninth strip-shaped material layer, fourteenth strip-shaped material layer, eighteenth strip-shaped material layer) are formed on both sides of the strip-shaped mask material layer 100b and the strip-shaped SiN layer 101b.
[0269] Then, a SiN layer (not shown) is applied to the entire surface. Figure 5C As shown, the SiN layer is polished by CMP until the upper surface position is the same as the mask material layers 100a and 100b, thereby forming strip-shaped SiN layers 104a, 104b, and 104c.
[0270] Then, if Figure 5D As shown in FIG. 1 , a resist layer 105 having an open end outside the SiN layer 104a is formed in a plan view. Furthermore, etching is performed in such a manner that the upper surface position of the SiN layer 104a becomes the bottom position of the strip-shaped mask material layers 102ab and 102ba, using the resist layer 105 and the strip-shaped mask material layers 102ab and 102ba as masks, thereby forming a recess 106.
[0271] Next, the resist layer 105 is removed. Then, the recess 106 is filled by using the CVD method and the CMP method to form a strip-shaped mask material layer 108 (the twentieth strip-shaped material layer) whose upper surface position is the same as that of the strip-shaped mask material layers 102ab and 102ba. Figure 5E As shown, the SiN layer 104 is removed by etching using the mask material layers 100a, 100b, 102aa, 102ab, 102ba, and 102bb as masks.
[0272] Then, if Fig. 5F As shown, the strip-shaped mask material layers 102aa, 102ab, 102ba, 102bb are removed. Also, the SiGe layers 103aa, 103ab, 103ba, 103bb are removed. Thus, strip-shaped SiN layers 101a, 101b, 104a having mask material layers 100a, 100b, 108 on top are formed on the mask material layer 7. Also, by performing FIG. 2B to FIG. 2D By performing the steps, an SRAM circuit composed of six Si pillars 61a to 61f is formed in one cell region in the same manner as in the second embodiment.
[0273] According to the manufacturing method of this embodiment, the following features can be obtained.
[0274] In the second embodiment, after the strip-shaped SiN layer 8a is first formed, two strip-shaped SiN layers 16A and 16B are formed outside the strip-shaped SiN layer 8a. At this time, the secondary ALD film deposition and RIE etching accuracy for forming the strip-shaped SiGe layers 12Aa and 12Ab and the strip-shaped SiN layers 16A and 16B affect the positional accuracy of the strip-shaped SiN layers 16A and 16B in the X direction relative to the strip-shaped SiN layer 8a. In contrast, in the present embodiment, the strip-shaped SiN layers 101a and 101b on both sides are first formed, and then the strip-shaped SiGe layers 103aa, 103ab, 103ba, and 103bb are formed, and then the central strip-shaped SiGe layer 104a is formed. At this time, the accuracy of ALD film deposition and RIE etching for forming the strip-shaped SiGe layers 103aa, 103ab, 103ba, and 103bb affects the positional accuracy of the strip-shaped SiN layers 101a and 101b relative to the strip-shaped SiN layer 104a in the X direction. This can improve the accuracy of the SRAM cell.
[0275] In the description of this embodiment, the strip-shaped mask material layers 102aa, 102ab, 102ba, 102bb and the strip-shaped SiGe layers 103aa, 103ab, 103ba, 103bb are removed, and the strip-shaped mask material layers 100a, 100b, 108 and the SiN layers 101a, 101b, 104a are left. On the other hand, the strip-shaped mask material layers 102aa, 102ab, 102ba, 102bb and the strip-shaped SiGe layers 103aa, 103ab, 103ba, 103bb may be left, and the strip-shaped mask material layers 100a, 100b, 108 and the SiN layers 101a, 101b, 104a may be removed. At this time, the stripe-shaped mask material layers 102aa, 102ab, 102ba, 102bb and the stripe-shaped SiGe layers 103aa, 103ab, 103ba, 103bb serve as mask material layers when forming Si pillars. This can also achieve higher precision of the SRAM cell.
[0276] This embodiment is as shown in Sections 5B to Figure 5E As shown in FIG. 1 , the example of forming a strip-shaped SiN layer 104a and a strip-shaped mask material layer 108 between the strip-shaped SiGe layers 103ab and 103ba is described. In contrast, if the strip-shaped SiGe layers 103aa, 103ab, 103ba, and 103bb are formed, Figure 1J to Figure 1L The steps shown in the figure are similarly formed to form a strip-shaped mask material layer (not shown) and a strip-shaped SiN layer (not shown), so that a Figure 1NSimilarly, five strip-shaped mask material layers (not shown) and a strip-shaped SiN layer (not shown) extending in the Y direction are formed. Thus, an SRAM cell composed of eight SGTs can be formed as in the first embodiment. This method can reduce the steps of forming the strip-shaped mask material layer and the strip-shaped SiN layer by one time compared to the first embodiment. Thus, the steps can be simplified.
[0277] (Sixth embodiment)
[0278] Below, refer to Figure 6 , a method for manufacturing a columnar semiconductor device having SGT according to a sixth embodiment of the present invention is described. Part (a) of the figure is a plan view, part (b) is a cross-sectional structure view along line X-X' of part (a), and part (c) is a cross-sectional structure view along line Y-Y' of part (a).
[0279] conduct Figures 1A to 1E In this step, Si layers 110a and 110b are formed to replace SiGe layers 12a and 12b. In addition, an amorphous SiOC layer 111 is formed. In addition, a heat treatment is performed in an oxygen-containing environment to oxidize the tops of the Si layers 110a and 110b to form SiO2 layers 112a and 112b as mask material layers. In this way, a strip-shaped mask material layer can be formed by oxidation treatment.
[0280] According to the manufacturing method of this embodiment, the following features can be obtained.
[0281] The first embodiment requires a step of polishing the SiN layer stacked on the entire surface by CMP after forming the recesses 14a and 14b. In contrast, the present embodiment can form the SiO2 layers 112a and 112b of the mask material layer only by oxidation treatment. This simplifies the steps.
[0282] (Seventh Implementation Method)
[0283] Below, refer to Figure 7 , a method for manufacturing a columnar semiconductor device having SGT according to a seventh embodiment of the present invention is described. Part (a) of the figure is a plan view, part (b) is a cross-sectional structure view along line X-X' of part (a), and part (c) is a cross-sectional structure view along line Y-Y' of part (a).
[0284] conduct Figures 1A to 1E In addition, strip-shaped nitrided SiGe layers 114a and 114b are formed on the top of the SiGe layer 12a by nitrogen ion implantation. The strip-shaped nitrided SiGe layers 114a and 114b are used as mask material layers.
[0285] According to the manufacturing method of this embodiment, the following features can be obtained.
[0286] The first embodiment requires a step of polishing the SiN layer stacked on the entire surface by CMP after forming the recesses 14a and 14b. In contrast, the present embodiment can form the strip-shaped nitrided SiGe layers 114a and 114b as mask material layers only by ion implantation of nitrogen ions. This can simplify the steps.
[0287] (Eighth Implementation Method)
[0288] Below, refer to FIG. 8A to FIG. 8E , a method for manufacturing a three-dimensional semiconductor device according to an eighth embodiment of the present invention is described. Part (a) of these figures is a plan view, part (b) is a cross-sectional structural view along line X-X' of part (a), and part (c) is a cross-sectional structural view along line Y-Y' of part (a).
[0289] like Fig. 8A As shown, for example, a SiGe layer 120a (fourth material layer) is formed on a SiO2 substrate 1a by an ALD method. Furthermore, a Si layer 121a (first semiconductor layer), a SiGe layer 120b (fourth material layer), a Si layer 121b (first semiconductor layer), and a SiGe layer 120c are formed in sequence from the bottom by an epitaxial growth method. A retaining material layer (not shown) is formed at both ends of the SiGe layer 120a (eighth material layer), 120b (eighth material layer), 120c, and the Si layers 121a, 121b, and 121c in the Y direction. Furthermore, a mask material layer 122 is formed on the SiGe layer 120c. Furthermore, the same as Figures 1A to 1L In the same steps, a strip-shaped SiN layer 124 having a strip-shaped mask material layer 125 on the top is formed on the mask material layer 122, and strip-shaped SiGe layers 126a and 126b having strip-shaped mask material layers 127a and 127b on the top are formed on both sides of the strip-shaped mask material layer 125 and the strip-shaped SiN layer 124, and strip-shaped SiN layers 128a and 128b having mask material layers 129a and 129b on the top are formed on both sides of the strip-shaped SiGe layers 126a, 126b and the strip-shaped mask material layers 127a and 127b.
[0290] Then, if Figure 8B As shown, a SiO2 layer (not shown) is fully covered and polished by CMP until the upper surface position becomes the upper surface position of the strip-shaped mask material layer 125, thereby forming a SiO2 layer 130. In addition, a mask material layer 131 is formed whose two ends in the Y direction when viewed from above are consistent with the ends of the retaining material layer.
[0291] Next, the SiO2 layer 130, the strip-shaped mask material layers 125, 127a, 127b, 129a, 129b, the SiN layers 124, 128a, 128b, and the strip-shaped SiGe layers 126a, 126b are etched using the mask material layer 131 as a mask. Furthermore, the mask material layer 131 is removed. Furthermore, the remaining SiO2 layer 130, the mask material layers 127a, 127b, and the SiGe layers 126a, 126b are removed. Furthermore, as shown in FIG. Figure 8C As shown, the mask material layer 122, the SiGe layer 120a, 120b, 120c, and the Si layer 121a, 121b are etched using the strip-shaped mask material layer 125, 129a, 129b, and the SiN layer 124, 128a, 128b as masks, and the SiGe layer 120a, 120ba, 120ca, the Si layer 121aa, 121ba, and the mask material layer 122a are formed under the SiN layer 128a. At the same time, the SiGe layer 120ab, 120bb, 120cb, the Si layer 121ab, 121bb, and the mask material layer 122b are formed under the SiN layer 124. At the same time, the SiGe layer 120ac, 120bc, 120cc, the Si layer 121ac, 121bc, and the mask material layer 122c are formed under the SiN layer 128b.
[0292] Then, if Fig.8D As shown, the strip-shaped mask material layers 125, 129a, 129b, the SiN layers 124, 128a, 128b, and the SiGe layers 120aa, 120ab, 120ac, 120ba, 120bb, 129ba, 120ca, 120cb, and 120cc are etched, thereby forming strip-shaped Si layers 121aa, 121ab, 121ac, 121ba, 121bb, and 121bc supported by the holding material layers at both ends in the Y direction.
[0293] Then, if Fig. 8EAs shown, gate HfO2 layers 130aa, 130ab, 130ac, 130ba, 130bb, 129bc are formed so as to surround the strip-shaped Si layers 121aa, 121ab, 121ac, 121ba, 121bb, 121bc. In addition, a gate TiN layer 132 is formed so as to surround the gate HfO2 layers 130aa, 130ab, 130ac, 130ba, 130bb, 129bc. In addition, the retaining material layers at both ends of the strip-shaped Si layers 121aa, 121ab, 121ac, 121ba, 121bb, 121bc are removed. In addition, N+ layers (not shown) or P+ layers (not shown) serving as sources or drains are formed at both ends of the strip-shaped Si layers 121aa, 121ab, 121ac, 121ba, 121bb, 121bc. Thus, a circuit using GAA (Gate All Around) transistors (see Non-Patent Document 3) using the strip-shaped Si layers 121aa, 121ab, 121ac, 121ba, 121bb, and 121bc as channels is formed.
[0294] According to the manufacturing method of this embodiment, the following features can be obtained.
[0295] According to this embodiment, the interval between the strip-shaped Si layers 121ab and 121bb, the strip-shaped Si layers 121aa and 121ba, and the strip-shaped Si layers 121ac and 121bc in a plan view can be narrowed. For example, when the strip-shaped Si layers 121aa and 121ba are used as channels of an N-channel GAA transistor, and the strip-shaped Si layers 121ab and 121bb and the strip-shaped Si layers 121ac and 121bc are used as channels of a P-channel GAA transistor, a high-density inverter circuit can be formed.
[0296] Similarly, the lower band-shaped Si layers 121aa, 121ab, and 121ac are used as channels of N-channel GAA transistors, and the upper band-shaped Si layers 121ba, 121bb, and 121bc are used as channels of P-channel GAA transistors, so that a high-density inverter circuit can be formed. In addition, as in the present embodiment, in addition to forming the GAA transistors into two upper bands and three horizontal columns, even if the circuit is formed into one upper band, three or more bands, and two or four horizontal columns, the circuit density can be increased.
[0297] (Ninth Implementation Method)
[0298] Below, refer to 9A to 9C, a method for manufacturing a three-dimensional semiconductor device according to a ninth embodiment of the present invention is described. Part (a) of these figures is a plan view, part (b) is a cross-sectional structural view along line X-X' of part (a), and part (c) is a cross-sectional structural view along line Y-Y' of part (a).
[0299] Conducted Figure 1A After the steps shown, a SiGe layer (not shown) and a mask material layer (not shown) are formed on the mask material layer 7. Then, by photolithography and RIE etching, as shown in FIG. Fig.9A As shown, two strip-shaped mask material layers 133a and 133b extending in the Y direction in a plan view are formed. Next, the SiGe layer is RIE-etched using the strip-shaped mask material layers 133a and 133b as masks to form strip-shaped SiGe layers 134a and 134b extending in the Y direction.
[0300] Next, a SiN layer (not shown) is formed on the entire surface by ALD. FIG. 1D to FIG. 1I Steps such as Fig. 9B As shown, the strip-shaped mask material layers 135aa, 135ab, 135ba, 135bb formed on both sides of the strip-shaped mask material layers 133a, 133b, and the strip-shaped SiN layers 136aa, 136ab, 136ba, 136bb located under the strip-shaped mask material layers 135aa, 135ab, 135ba, 135bb and connected to both sides of the SiGe layers 134a, 134b. The strip-shaped mask material layer 135ab is formed separately from the strip-shaped mask material layer 135ba. Similarly, the strip-shaped SiN layer 136ab is formed separately from the strip-shaped SiN layer 136ba.
[0301] Then, if Fig. 9C As shown in FIG. 1 , the strip-shaped mask material layers 133a, 133b and the strip-shaped SiGe layers 134a, 134b are removed, thereby forming strip-shaped mask material layers 135aa, 135ab, 135ba, 135bb and strip-shaped SiN layers 136aa, 136ab, 136ba, 136bb extending in the Y direction when viewed from above on the mask material layer 7. FIG. 3C to FIG. 3F steps to form Figure 3F Same SRAM cell.
[0302] According to the manufacturing method of this embodiment, the following features can be obtained.
[0303] In the third embodiment, the strip material layer forming step is repeated three times on both sides of the strip SiGe layer 80 to form strip SiN layers 82a, 82b, 86a, 86b and strip SiGe layers 84a, 84b. In contrast, in the present embodiment, the strip material layer forming step is performed only once on both sides of the strip SiGe layers 134a, 134b formed simultaneously, that is, strip SiN layers 136aa, 136ab, 136ba, 136bb are formed. Thus, the steps can be simplified.
[0304] The distance between the two strip-shaped SiN layers 136a and 136b is Fig.9A shown more separately and through with Figure 1I to Figure 1L In the same manner, a strip SiGe layer is formed on both sides of the strip SiN layers 136aa, 136ab and the strip SiN layers 136ba, 136bb, and a strip mask material layer (with the same shape as the strip SiGe layer) is formed on the strip SiGe layer. Fig. 1I Next, use the same FIG. 5B to FIG. 5E In the same method as shown in the above, a strip-shaped SiN layer is formed between the strip-shaped SiGe layers, and a strip-shaped mask material layer is formed on the strip-shaped SiN layer. Thus, as in the first embodiment, five strip-shaped SiN layers extending in the Y direction when viewed from above can be formed, and a strip-shaped mask material layer is formed on the strip-shaped SiN layer. Thus, the same SRAM cell as in the first embodiment can be formed. In the first embodiment, the strip-shaped material layer forming step is repeated four times on both sides of the strip-shaped SiN layer 8a. In contrast, the present method forms the SRAM cell by repeating the step twice. Thus, the steps can be simplified.
[0305] Furthermore, in the first to seventh embodiments of the present invention, one SGT is formed in one semiconductor pillar, but the present invention is also applicable to the formation of two or more circuits.
[0306] In addition, in the first embodiment, the mask material layer 7 is formed of a SiO2 layer, an aluminum oxide (Al2O3) layer, and a SiO2 layer. In addition, a silicon nitride (SiN) layer 8 is stacked. In addition, a mask material layer 9 composed of a SiO2 layer is stacked. In addition, a mask material layer 10 composed of a SiN layer is stacked. If these mask material layers 7, 9, 10, and SiN layer 8 are materials that meet the purpose of the present invention, other material layers composed of a single layer or multiple layers containing organic materials or inorganic materials can also be used, and this is also the same in other embodiments of the present invention.
[0307] In addition, in the first embodiment, if Figure 1DAs shown, the SiGe layer 12 is formed by the ALD method to cover the entire strip-shaped mask material layer 7, 8a, 9a. As long as the SiGe layer 12 is a material that meets the purpose of the present invention, other material layers including organic materials or inorganic materials composed of a single layer or multiple layers can also be used. The same applies to the strip-shaped SiGe layers 18a and 18b. In addition, the material matrix of the strip-shaped SiGe layers 12aa and 12ab and the strip-shaped SiGe layers 18a and 18b can also be different. This is also the same in other embodiments of the present invention.
[0308] In addition, the strip mask material layers 15a, 15b, 17a, 17b, 19a, 19b, 21a, 21b and the strip mask material layers 16a, 16b, 20a, 20b in the first embodiment may be other material layers composed of a single layer or multiple layers containing organic materials or inorganic materials if they are materials that meet the purpose of the present invention. The same is true in other embodiments of the present invention.
[0309] In addition, in the first embodiment, the upper surfaces and bottoms of each of the strip mask material layers 9a, 15a, 15b, 17a, 17b, 19a, 19b, 21a, and 21b are formed at the same position. If the material is consistent with the purpose of the present invention, the positions of the upper surfaces and bottoms of each may also be different in the vertical direction. This is also the same in other embodiments of the present invention.
[0310] In the first embodiment, the thickness and shape of the strip-shaped mask material layers 9a, 15a, 15b, 17a, 17b, 19a, 19b, 21a, and 21b are changed due to CMP polishing, RIE etching, and cleaning. There is no problem if the change is within the range that meets the purpose of the present invention. This is also the same in other embodiments of the present invention.
[0311] In addition, in the first embodiment, Figure 1Q to Figure 1S The SiO2 layer 22, SiN layer 24, strip SiGe layer 25, strip mask material layer 26 composed of SiN layer, strip mask material layers 27a, 27b, 28a, 28b shown in the figure may be other material layers containing organic materials or inorganic materials composed of a single layer or multiple layers if they are materials that meet the purpose of the present invention. The same is true in other embodiments of the present invention.
[0312] In addition, the first embodiment removes the Si pillars 7b and 6i. In this way, any of the formed Si pillars 6a to 6j can be removed by photolithography and etching in accordance with the circuit design. Even for circuits other than SRAM unit circuits, the formed Si pillars can be removed in accordance with the circuit design. In addition, as in the fourth embodiment, any area of the strip mask material layers 27a, 27b, 28a, 28b in a top view can be removed without forming any of the Si pillars 6a to 6j. The method provided in this embodiment can be applied to the formation of circuits other than SRAM unit circuits. This is also the same in other embodiments of the present invention.
[0313] In addition, in the first embodiment, if Figure 1Z As shown, TiN layers 40a, 40b, 40c, and 40d are used as gate metal layers. If the TiN layers 40a, 40b, 40c, and 40d are materials that meet the purpose of the present invention, a material layer consisting of a single layer or multiple layers can be used. The TiN layers 40a, 40b, 40c, and 40d can be formed by at least a single layer or multiple layers of metal layers having a desired work function. For example, a W layer can be formed on the outside. In this case, the W layer plays the role of a metal wiring layer connecting the gate metal layer. A single layer or multiple layers of metal layers can also be used in addition to the W layer. This is also the same in other embodiments of the present invention.
[0314] In addition, the description of the embodiments of the present invention uses an example of forming an SRAM cell. For example, in a microprocessor circuit, an SRAM circuit and a logic circuit are formed on the same chip. In the formation of this logic circuit, Figure 1W , Figure 4A The method described above can be used to avoid forming unnecessary Si columns. In addition, SRAM circuits and logic circuits can be formed by the methods of the respective embodiments. The same is true for other circuit formations.
[0315] In the sixth embodiment, an amorphous SiOC layer 111 is formed instead of the SiO2 layer 13 in the first embodiment. Furthermore, a heat treatment is performed in an oxygen-containing atmosphere to oxidize the top of the Si layers 110a and 110b, thereby forming strip-shaped SiO2 layers 112a and 112b as mask material layers. The amorphous SiOC layer 111 and the Si layers 110a and 110b may be other material layers as long as they are suitable for the purpose of the present invention.
[0316] In the seventh embodiment, strip-shaped nitrided SiGe layers 114a and 114b are formed on the top of the SiGe layer 12a by nitrogen ion implantation. If the nitrogen ion implantation and SiGe layer 12a are used to form a mask material layer, other atomic ion implantation or a material layer replacing the SiGe layer may also be used.
[0317] In the first embodiment, the mask material layers 7a to 7j are formed to be circular in plan view. The mask material layers 7a to 7j may be elliptical in shape. This is also the case in other embodiments of the present invention.
[0318] In the first embodiment, the HfO2 layer 35 is used as the gate insulating layer, and the TiN layers 40a, 40b, 40c, and 40d are used as the gate material layers, but other material layers composed of a single layer or multiple layers may be used. This is also the case in other embodiments of the present invention.
[0319] In addition, in the first embodiment, if Figure 1XX As shown, N+ layers 43a, 43c, 43d, 43e, 43f, 43h, and P+ layers 43b, 43g are formed by selective epitaxial growth. Furthermore, N+ layers 44a, 44c, 44d, 44e, 44f, 44h, and P+ layers 44b, 44g are formed on the tops of Si pillars 6a to 6j by thermal diffusion. Since the N+ layers 43a, 43c, 43d, 43e, 43f, 43h, and P+ layers 43b, 43g formed by the selective epitaxial growth method are single crystal layers, even if the N+ layers 44a, 44c, 44d, 44e, 44f, 44h, and P+ layers 44b, 44g are not formed on the tops of Si pillars 6a to 6j by thermal diffusion, they will become the source or drain of SGT. Similarly, the N+ layer or P+ layer formed around the periphery of the Si pillars 6a to 6j by the selective epitaxial growth method can be used as a source or a drain, replacing the N+ layer 3a, 3b, 3c, 3d, and the P+ layer 4a, 5a at the bottom of the Si pillars 6a to 6j as the source or the drain. This is also the same in other embodiments of the present invention.
[0320] In addition, the first embodiment uses a selective epitaxial growth method to perform Figure 1XX The N+ layers 43a, 43c, 43d, 43e, 43f, 43h, and P+ layers 43b, 43g are formed. The N+ layers 43a, 43c, 43d, 43e, 43f, 43h, and P+ layers 43b, 43g can be formed by a conventional epitaxial growth method, and then by photolithography and etching. This is also the same in other embodiments of the present invention.
[0321] In addition, in the first embodiment, SGT is formed on the P-layer substrate 1, but an SOI (Silicon On Insulator) substrate may be used instead of the P-layer substrate 1. Alternatively, any other material substrate may be used as long as it can function as a substrate. This is also the case in other embodiments of the present invention.
[0322] In addition, the first embodiment describes the SGTs that form the source and drain using the N+ layers 44a, 44c, 44d, 44f, 44h, P+ layers 44b, 44g, N+ layers 3a, 3b, 3c, 3d, and P+ layers 4a, 5a having the same conductivity polarity above and below the Si pillars 6a to 6j, but the present invention can also be applied to channel-type SGTs having sources and drains of different polarities. This is also the case in other embodiments of the present invention.
[0323] In addition, the above-mentioned embodiments describe examples of using Si (silicon) as semiconductor regions such as channels, sources, drains, etc. However, the present invention is not limited thereto, and the technical concept of the present invention can also be applied to semiconductor materials containing Si such as SiGe, or three-dimensional semiconductor devices using semiconductor materials other than Si.
[0324] In the first embodiment, the Si pillars 6a to 6j are formed of a single Si layer, but the SGT channel may be formed by vertically stacking semiconductor layers made of different semiconductor matrices. This is also the case in other embodiments of the present invention.
[0325] In addition, in the vertical NAND flash memory circuit, a semiconductor column is used as a channel, and multiple memory cells consisting of a channel oxide layer, a charge storage layer stack, an interlayer insulating layer, and a control conductor layer surrounding the semiconductor column are formed in the vertical direction. The semiconductor columns at both ends of these memory cells have a source line impurity layer corresponding to the source and a bit line impurity layer corresponding to the drain. In addition, for a memory cell, if one side of the memory cells on both sides thereof is the source, the other side acts as the drain. In this way, the vertical NAND flash memory circuit is a type of SGT circuit. Therefore, the present invention can also be applied to NAND flash memory circuits.
[0326] The present invention can be implemented in various ways and variations without departing from the broad spirit and scope of the present invention. In addition, the above-mentioned embodiment is used to illustrate an embodiment of the present invention and is not used to limit the scope of the present invention. The above-mentioned embodiment and variations can be combined arbitrarily. Moreover, even if a part of the constituent elements of the above-mentioned embodiment is removed as needed, it is also included in the scope of the technical idea of the present invention.
[0327] [Explanation of Reference Numerals]
[0328] 1 P-layer substrate
[0329] 1a SiO2 substrate
[0330] 2,2a,2b N layers
[0331] 3,3a,3b,3c,3d,43a,43c,43d,43e,43f,43g,43h,44a,44c,44d,44e,44 f,44g,44h,66a,66c,66d,66f,97a,97c,97d,97e,97h,98a,98c,98d,98f N+layer
[0332] 3A,3B Strip N+ layer
[0333] 4A Strip P+ layer
[0334] 4,4a,4c,4d,5,5a,43b,43g,44b,44g,66b,66e,97b,97e,98b,98e P+ layer
[0335] 6i layer
[0336] 7,8,9,10,26,7a,7b,7c,7d,7e,7f,7g,7h,7i,7j,30a,30b,30c,30d,31a,31b,31c,31d,38a,38b,38c,38d,60a,60b,60c,60d,60e,60f,92a,92b,92c,92d,92e,92f,92g,92h,122,131 Mask Material Layer
[0337] 8a,9a,10a,15a,15b,16a,16b,17a,17b,19a,19b,20a,20b,21a,21b,26,27a,27b,27A,27B,27C,27D,28a,28b,33a,33b,15A,15B,17A,17B,81,83a,83b,85a,85b,87a,87b,100a,100b,102aa,102ab,102ba,102bb,108,125,127a,127b,129a,129b,133a,133b,135aa,135ab,135ba,135bb strip mask material layer
[0338] 9Aa,9Ab,17Aa,17Ab,17Ba,17Bb,91a,91b,91c,91d,91e,91f,91g,91h square mask material layer
[0339] 8,16,16A,16B,24,42 SiN layers
[0340] 16A,16B,24a,24b,82a,82b,86a,86b,101a,101b,104a,104b,104c,124,128a,128b,136aa,136ab,136ba,136bb Ribbon SiN layer
[0341] 8Aa,8Ab,16AA,16AB,16BA,16BB,90a,90b,90c,90d,90e,90f,90g,90h square SiN layer
[0342] 12,12a,12b,18a,18b,120a,120b,120c SiGe layer
[0343] 12aa,12ab,18a,18b,25,12Aa,12Ab,80,103aa,103ab,103ba,103bb ribbon SiGe layer
[0344] 13,13a,13b,13ba,22,22a,22b,32a,32b,34,46,48,50,52,54,130SiO2 layer
[0345] R1, R2 arc part
[0346] 14a,14b,14A,14B,106 concave part
[0347] 8aa,8ab,9aa,9ab,16aa,16ba,16bb,17aa,17ba,17bb,20aa,20ba,20bb,21aa,21ba,21bb square mask material layer
[0348] 6a,6b,6c,6d,6e,6f,6h,6i,6j,61a,61b,61c,61d,61e,61f,93a,93b,93c,93d,93e,93f,93g,93h Si column
[0349] 35,63 HfO2 layer
[0350] 40a, 40b, 40c, 40d, 65a, 65b, 65c, 65d TiN layer
[0351] 47a,47b,49a,49b,51a,51b,51c,51d,53a,53b,55a,55b,69a,69b,71a,71b,73a,73b,74a,74b,100a,100b,102a,102b,103a,103b,104a,104b connection hole
[0352] 105 Resist layer
[0353] 111 SiOC layer
[0354] 114a, 114b Strip-shaped nitrided SiGe layer
[0355] 112a, 112b Strip-shaped SiO2 layer
[0356] WL Character wiring metal layer
[0357] BL Bit Wiring Metal Layer
[0358] RBL Reverse Bit Line Metal Layer
[0359] Vss1, Vss2 Ground wiring metal layer
[0360] Vdd power wiring metal layer
[0361] C1, C2 connect the wiring metal layer.
Claims
1. A method for manufacturing a three-dimensional semiconductor device, comprising: A step of forming a first material layer on a second substrate located on the first substrate and at least a portion of the second substrate or the entire second substrate is formed of a semiconductor layer; A step of forming a second strip material layer extending in one direction in a plan view on the first material layer, wherein the second strip material layer has the first strip material layer on top, and the first strip material layer has the same shape in a plan view as the second strip material layer; The step of forming a second material layer and a third material layer from the bottom in a manner of covering the entire first material layer, the first strip-shaped material layer and the second strip-shaped material layer; A step of smoothing so that the upper surface positions of the second material layer and the third material layer become the upper surface position of the first strip-shaped material layer; forming a third strip material layer on top of the smoothed second material layer and sandwiched between the smoothed third material layer and the side surfaces of the first strip material layer; a step of removing the smoothed third material layer; The step of etching the second material layer using the first strip material layer and the third strip material layer as masks to form a fourth strip material layer connected to both sides of the second strip material layer; The step of forming a fourth material layer and a fifth material layer from the bottom in a manner of covering the entire first material layer, the first strip material layer, the second strip material layer, the third strip material layer and the fourth strip material layer; A step of smoothing so that the upper surface positions of the fourth material layer and the fifth material layer become the upper surface position of the first strip-shaped material layer; forming a fifth strip-shaped material layer on top of the smoothed fourth material layer and sandwiched between the smoothed fifth material layer and the side surfaces of the third strip-shaped material layer; a step of removing the fifth material layer; Using the first strip material layer, the third strip material layer and the fifth strip material layer as masks, etching the fourth material layer to form a sixth strip material layer connected to a side surface of the fourth strip material layer; The step of removing the third strip material layer and the fourth strip material layer; A step of forming a seventh strip-shaped material layer composed of a single layer or multiple layers above or below the first strip-shaped material layer and perpendicular to the first strip-shaped material layer in a plan view; A step of forming a first mask material layer which is rectangular or circular in a plan view and is located in a first overlapping region of the seventh strip material layer, the second strip material layer, and the sixth strip material layer in a plan view by at least the first strip material layer and the fifth strip material layer, or the second strip material layer and the sixth strip material layer; as well as Using the first mask material layer as a mask, etching the second substrate to form a three-dimensional semiconductor layer composed of the semiconductor layer on the first substrate; And the aforementioned three-dimensional semiconductor layer is used as a channel.
2. The method for manufacturing a three-dimensional semiconductor device according to claim 1, wherein: The step of forming the third strip material layer comprises: Using the first strip material layer and the smoothed third material layer as masks, etching the top of the second material layer to form a first concave portion; as well as The step of filling the first recess to form the third strip-shaped material layer having an upper surface position identical to that of the first strip-shaped material layer.
3. The method for manufacturing a three-dimensional semiconductor device according to claim 1, wherein: The step of forming the fifth strip material layer comprises: Using the first strip material layer, the third strip material layer and the fifth material layer as masks, etching the top of the fourth material layer to form a second recess; as well as The step of filling the second recess to form the fifth strip-shaped material layer having an upper surface position identical to that of the first strip-shaped material layer.
4. The method for manufacturing a three-dimensional semiconductor device according to claim 1, wherein: In the vertical direction, a ninth strip material layer is formed above or below the first strip material layer, the ninth strip material layer having an eighth strip material layer extending in one direction when viewed from above and having the same shape as the seventh strip material layer when viewed from above, The seventh strip material layer is formed by the following steps: The step of forming a sixth material layer and a seventh material layer from the bottom in a manner of covering the entirety of the eighth strip-shaped material layer and the ninth strip-shaped material layer; A step of smoothing so that the upper surface positions of the sixth material layer and the seventh material layer become the upper surface position of the eighth strip-shaped material layer; Using the eighth strip material layer and the smoothed seventh material layer as masks, etching the top of the smoothed sixth material layer to form a third recess; The step of filling the third recess to form a tenth strip material layer having an upper surface position identical to that of the eighth strip material layer; a step of removing the seventh material layer; Using the eighth strip material layer and the tenth strip material layer as masks, etching the sixth material layer to form an eleventh strip material layer connected to both sides of the ninth strip material layer; as well as The eighth strip material layer and the ninth strip material layer are removed or the tenth strip material layer and the eleventh strip material layer are removed, and the lower layer or the upper and lower layers of the remaining strip material layer are used as the seventh strip material layer.
5. The method for manufacturing a three-dimensional semiconductor device according to claim 1, wherein: In a plan view, the width of one of the second strip-shaped material layer and the fourth strip-shaped material layer is formed to be larger than the width of the other.
6. The method for manufacturing a three-dimensional semiconductor device according to claim 1, wherein: In a plan view, the width of one of the second strip-shaped material layer and the sixth strip-shaped material layer is formed to be larger than the width of the other.
7. The method for manufacturing a three-dimensional semiconductor device according to claim 1, wherein: The three-dimensional semiconductor layer is a semiconductor column vertically erected on the first substrate.
8. The method for manufacturing a three-dimensional semiconductor device according to claim 7, wherein: The semiconductor column is composed of at least a first semiconductor column, a second semiconductor column and a third semiconductor column arranged adjacently along the one direction or a direction perpendicular to the one direction. The method for manufacturing the three-dimensional semiconductor device includes: A step of forming a first gate insulating layer surrounding the side surfaces of the first semiconductor column, the second semiconductor column and the third semiconductor column; and A step of forming a first gate conductor layer surrounding the first gate insulating layer; The first gate conductor layer is formed by filling a space between at least two of the first semiconductor pillar, the second semiconductor pillar, and the third semiconductor pillar. 9 . The method for manufacturing a three-dimensional semiconductor device according to claim 7 , comprising the step of removing any one of the plurality of semiconductor pillars formed on the substrate.
10. The method for manufacturing a three-dimensional semiconductor device according to claim 7, comprising the step of not forming a portion of the seventh strip material layer in a plan view before forming the plurality of semiconductor pillars. Furthermore, in a plan view, none of the plurality of semiconductor pillars is formed under the portion of the seventh strip material layer.
11. The method for manufacturing a three-dimensional semiconductor device according to claim 1, comprising: In parallel with the step of forming the second strip material layer having the first strip material layer on top, a step of extending a thirteenth strip material layer having a twelfth strip material layer on top along the same one direction on the first material layer, wherein the twelfth strip material layer has the same top view shape; In parallel with the step of forming a fourth strip material layer having the third strip material layer on top, a step of extending a fifteenth strip material layer having a fourteenth strip material layer on top along the same one direction on the first material layer, wherein the fourteenth strip material layer has the same top view shape; The step of forming a sixteenth strip material layer which is located between the fourth strip material layer and the fifteenth strip material layer and connected to the sides of the fourth strip material layer and the fifteenth strip material layer and has the same shape as the sixth strip material layer; as well as The step of removing the third strip-shaped material layer, the fourth strip-shaped material layer, the fourteenth strip-shaped material layer and the fifteenth strip-shaped material layer.
12. The method for manufacturing a three-dimensional semiconductor device according to claim 1, wherein: The top of the smoothed second material layer is oxidized to form the third strip-shaped material layer.
13. The method for manufacturing a three-dimensional semiconductor device according to claim 1, wherein: Atomic ions are ion-implanted into the top of the smoothed second material layer to form the third strip-shaped material layer.
14. The method for manufacturing a three-dimensional semiconductor device according to claim 1, comprising: In a top view, the steps of forming the second substrate by connecting two ends of one direction to the holding material layer and stacking a plurality of structures upwards with the first semiconductor layer and the eighth material layer as a group in a vertical direction; After forming the aforementioned three-dimensional semiconductor layer, removing the aforementioned eighth material layer; The step of forming a second gate insulating layer surrounding the first semiconductor layer mentioned above in the three-dimensional semiconductor layer; The step of forming a second gate conductor layer surrounding the second gate insulating layer; a step of removing the aforementioned retaining material layer; as well as The step of forming an impurity layer which is connected to both ends of the first semiconductor layer in the one direction in a plan view and contains donor or acceptor impurities.
15. A method for manufacturing a three-dimensional semiconductor device, comprising: A step of forming a first material layer on a second substrate located on the first substrate and at least a portion of the second substrate or the entire second substrate is formed of a semiconductor layer; A step of forming a second strip material layer extending in one direction in a top view on the first material layer, wherein the second strip material layer has the first strip material layer on top, and the first strip material layer has the same top view shape as the second strip material layer; The step of forming a second material layer and a third material layer from the bottom in a manner of covering the entire first material layer, the first strip-shaped material layer and the second strip-shaped material layer; A step of smoothing so that the upper surface positions of the second material layer and the third material layer become the upper surface position of the first strip-shaped material layer; forming a third strip material layer on top of the smoothed second material layer and sandwiched between the smoothed third material layer and the side surfaces of the first strip material layer; a step of removing the smoothed third material layer; Using the first strip material layer and the third strip material layer as masks, etching the second material layer to form a fourth strip material layer having the third strip material layer on top; The step of removing the third strip material layer and the fourth strip material layer; A step of forming a fifth strip-shaped material layer composed of a single layer or multiple layers above or below the first strip-shaped material layer and perpendicular to the first strip-shaped material layer in a plan view; A step of forming a first mask material layer which is rectangular or circular in a plan view and located in a first overlapping region of the first strip material layer and the fifth strip material layer in a plan view by at least the first strip material layer and the second strip material layer; as well as Using the first strip material layer as a mask, etching the second substrate to form a three-dimensional semiconductor layer composed of the semiconductor layer on the substrate; And the aforementioned three-dimensional semiconductor layer is used as a channel.
16. The method for manufacturing a three-dimensional semiconductor device according to claim 15, wherein: The step of forming the third strip material layer comprises: Using the first strip material layer and the third material layer as masks, etching the top of the second material layer to form a first concave portion; as well as The step of forming the third strip-shaped material layer which fills the first recess and has an upper surface position which is the same as that of the first strip-shaped material layer.
17. The method for manufacturing a three-dimensional semiconductor device according to claim 15, wherein: In a plan view, the width of the fourth strip-shaped material layer is formed to be larger than the width of the second strip-shaped material layer.
18. The method for manufacturing a three-dimensional semiconductor device according to claim 15, wherein: The three-dimensional semiconductor layer is a semiconductor column vertically erected on the first substrate.
19. The method for manufacturing a three-dimensional semiconductor device according to claim 18, wherein: The semiconductor column is composed of at least a first semiconductor column and a second semiconductor column arranged adjacent to each other along the one direction or a direction perpendicular to the one direction. The method for manufacturing the three-dimensional semiconductor device includes: A step of forming a first gate insulating layer surrounding the side surfaces of the first semiconductor column and the second semiconductor column; and A step of forming a first gate conductor layer surrounding the first gate insulating layer; The first gate conductor layer is formed to fill the space between the first semiconductor column and the second semiconductor column.
20. The method for manufacturing a three-dimensional semiconductor device according to claim 18, comprising the step of removing any one of the plurality of semiconductor pillars formed on the substrate.
21. The method for manufacturing a three-dimensional semiconductor device according to claim 18, comprising the step of not forming a part of the fifth strip material layer in a plan view before forming the plurality of semiconductor pillars. Furthermore, in a plan view, none of the plurality of semiconductor pillars is formed under the portion of the fifth strip material layer.
22. The method for manufacturing a three-dimensional semiconductor device according to claim 15, comprising: Simultaneously with the formation of the first and second strip material layers, a step of forming a seventh strip material layer which is parallel to the first and second strip material layers in plan view and has a sixth strip material layer on top; Simultaneously with the formation of the third and fourth strip material layers, a ninth strip material layer is formed which is connected to both sides of the sixth and seventh strip material layers and has the eighth strip material layer on the top; as well as In parallel with the step of removing the first strip-shaped material layer and the second strip-shaped material layer, the step of removing the sixth strip-shaped material layer and the seventh strip-shaped material layer is performed.
23. The method for manufacturing a three-dimensional semiconductor device according to claim 22, wherein: The interval between the ninth strip-shaped material layer and the fourth strip-shaped material layer in a plan view is formed to be the same as that of one of the second strip-shaped material layer and the seventh strip-shaped material layer, or both.
24. The method for manufacturing a three-dimensional semiconductor device according to claim 15, wherein: The smoothed top of the second material layer is oxidized to form the third strip-shaped material layer.
25. The method for manufacturing a three-dimensional semiconductor device according to claim 15, wherein: Atomic ions are ion-implanted into the top of the smoothed second material layer to form the third strip-shaped material layer.
26. The method for manufacturing a three-dimensional semiconductor device according to claim 15, comprising: In a top view, the step of forming the second substrate by connecting two ends of one direction to the holding material layer and stacking a plurality of structures upwards with the semiconductor layer and the fourth material layer as a group in a vertical direction; After forming the three-dimensional semiconductor layer, removing the fourth material layer; A step of forming a second gate insulating layer surrounding the semiconductor layer of the three-dimensional shape semiconductor layer; The step of forming a second gate conductor layer surrounding the second gate insulating layer; a step of removing the aforementioned retaining material layer; as well as The step of forming an impurity layer which is connected to both ends of the semiconductor layer in the one direction in the plan view and contains donor or acceptor impurities.
Citation Information
Patent Citations
MOS semiconductor device
JP1990188966A
Method for producing semiconductor device, and semiconductor device
CN103119720A
Vertical channel transistor and method for fabricating the same
KR1020090069135A
Semiconductor device and method for manufacturing semiconductor device
WO2015129021A1
Method for manufacturing columnar semiconductor device
WO2018070034A1