Processing system and platform for reducing material roughness using irradiated etching solutions

By adjusting the reactivity to the liquid etching solution, the problem of controlling the surface roughness of polycrystalline materials in traditional wet etching process is solved, and the nano-scale etching uniformity and surface smoothness of polycrystalline materials are achieved, and the process is simplified. And reduce costs.

CN113302730BActive Publication Date: 2024-11-22TOKYO ELECTRON LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN201980089026.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-05-03
Filing Date
2019-12-10
Publication Date
2024-11-22
Estimated Expiration
2039-12-10

AI Technical Summary

Technical Problem

Traditional wet etching processes are difficult to achieve nanoscale etch uniformity control of polycrystalline material surfaces in microelectronic workpieces, especially in terms of surface roughness and smoothness, resulting in undesirable etching variability and roughness. change.

Method used

By irradiating the liquid etching solution, a highly reactive etchant is generated, and the etching behavior is controlled by using photosensitive compounds and actinic reactions to achieve controlled etching of polycrystalline materials, forming a uniform oxidized material layer and Remove to achieve a smooth surface.

Benefits of technology

The etching uniformity control of polycrystalline materials on microscopic and macroscopic scales is achieved, the surface roughness is reduced, the process chemistry is simplified, the wet etching process cost is reduced, and the device failure is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113302730B_ABST
    Figure CN113302730B_ABST
Patent Text Reader

Abstract

Irradiation of etching solutions is described to provide a processing system and platform embodiment for controlled etching of materials. These processing systems and platforms deposit liquid etching solutions on materials to be etched and irradiate the liquid etching solutions to adjust reactant levels. The liquid etching solution has a first reactant level, and the irradiation causes the liquid etching solution to have a second reactant level that is different from the first level. The material is modified with the irradiated etching solution, and the modified material is removed. The transport, exposure and removal can be repeated to provide cyclic etching. Further, oxidation and dissolution can occur simultaneously or in multiple steps. The etched material can be a polycrystalline material, a polycrystalline metal, and / or other materials. The liquid etching solution can include hydrogen peroxide that is irradiated to form perhydroxyl radicals.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] The present application also claims the benefit of priority to U.S. Provisional Patent Application Serial No. 62 / 779,604, filed on December 14, 2018, entitled “ROUGHNESS REDUCTION METHODS FOR WET ETCH OF POLYCRYSTALLINE MATERIALS”; and U.S. Provisional Patent Application Serial No. 62 / 726,603, filed on November 4, 2018, entitled “PHOTONICALLY TUNED ETCHANT REACTIVITY”; and U.S. Patent Application Serial No. 16 / 287,669, filed on February 27, 2019, entitled “ROUGHNESS REDUCTION METHODS FOR MATERIALS USING ILLUMINATED ETCH SOLUTIONS”; and U.S. Provisional Patent Application Serial No. 16 / 287,669, filed on February 27, 2019, entitled “PROCESSING SYSTEMS AND PLATFORMS FOR ROUGHNESS REDUCTION OF MATERIALS USING ILLUMINATED ETCH SOLUTIONS," each of which is incorporated herein by reference in its entirety. Background Art

[0003] The present disclosure relates to methods for the fabrication of microelectronic workpieces, including etching processes for material layers on the microelectronic workpieces.

[0004] The formation of devices within a microelectronic workpiece typically involves a series of manufacturing techniques associated with the formation, patterning, and removal of multiple material layers on a substrate of the microelectronic workpiece. Etching processes are typically used to remove material layers from the surface of a substrate. As the feature sizes of the materials to be etched for forming electronic devices on microelectronic workpieces continue to shrink, it is increasingly difficult to control etching uniformity on both a macro and micro scale. Conventional wet etching processes using liquid etching solutions typically lack precise nanoscale control over the etching behavior. This lack of control becomes a problem when there is a small amount of material to be removed and / or when a smooth surface finish is desired.

[0005] In particular, roughness control during etching processes for polycrystalline materials is a challenging task. Polycrystalline materials exhibit varying reactivity to etchants depending on the surface crystal orientation of the polycrystalline material. Polycrystalline materials also exhibit varying reactivity to etchants at grain boundaries and defect sites of the polycrystalline material. This varying reactivity leads to undesirable etch variability and surface roughness in conventional wet etching processes.

[0006] Figures 1A-1B (Prior Art) provide a simplified illustration of issues associated with such prior art etching solutions and related problems regarding varying reactivity and undesirable etching variability.

[0007] Turning first to FIG. 1A (Prior Art), an example embodiment 100 for a conventional etching method is provided. A liquid etching solution 106 is applied to a material 104 on a surface of a substrate 108 of a microelectronic workpiece. For the example embodiment 100, the material 104 being etched is cobalt (Co), and the material 104 has previously been formed on the surface of the substrate 108. For the example embodiment 100, the liquid etching solution 106 provides an oxidative dissolution etching mechanism. For the oxidative dissolution etching mechanism, the material 104 is oxidized by the liquid etching solution 106 and then dissolved by the liquid etching solution 106.

[0008] The conventional oxidative dissolution etching mechanism for cobalt results in significant roughening and pitting. For this conventional method, cobalt etching is driven by an oxidation / dissolution mechanism, in which an oxidant (e.g., hydrogen peroxide) oxidizes cobalt (Co) to form CoO x , whose oxidation rate constant is k ox (As indicated by arrow 110). Then CoO x The etchant dissolves in the solution by complexing with the etchant molecule (e.g., citrate anion) with a dissolution rate constant k d (As indicated by arrow 112). For this conventional method, k ox Less than k d (k ox <k d ), and this condition causes uneven etching at the grain boundaries of polycrystalline cobalt, resulting in pitting and roughening of the surface.

[0009] 1B (Prior Art) provides a representative surface image 150 for such pitting and roughening of the surface due to the undesirable etch variability associated with conventional oxidative dissolution methods. In contrast, an ideal wet etch process would provide a constant etch rate independent of the surface chemistry (e.g., grain boundaries) of the material being etched. Summary of the invention

[0010] Embodiments of controlled etching of materials using irradiation of etching solutions are described herein. The disclosed processing system and platform deposit liquid etching solutions on materials to be etched and irradiate these liquid etching solutions to adjust the level of reactants. The etched materials can be, for example, polycrystalline materials, polycrystalline metals and / or other materials to be etched. The disclosed embodiments use irradiation as a tool to control the reactivity of the etchant in the etching solution in contact with the material, thereby achieving modification of the etching behavior. Chemical compositions and other parameters can also be used to partially control the etching behavior and the surface morphology and chemical properties after etching. The disclosed embodiments thus control and / or reduce surface roughness during the etching of materials (such as polycrystalline materials) at microscopic and macroscopic levels. These results are achieved in the following manner: the etching solution applied to the surface of the material is irradiated, thereby generating highly reactive etchants at the point of use, and these highly reactive etchants are etched by the material independently of the surface chemical properties of the material. For one example embodiment, the liquid etching solution is an aqueous solution containing hydrogen peroxide, and hydroxyl radicals are generated by irradiation (such as ultraviolet light) to form a highly reactive etchant. Different or additional features, variations, and embodiments may also be implemented, and related systems and methods may also be utilized.

[0011] For one embodiment, a processing system for performing a wet etching process on a substrate is disclosed, the processing system comprising: a wet processing chamber, the wet processing chamber being configured to perform a wet etching process; a substrate holder located within the wet processing chamber, the substrate holder being configured to support a substrate; a delivery system, the delivery system being arranged to supply a liquid etching solution to the substrate, the liquid etching solution having a first reactant level with respect to a material on a surface of the substrate; an illumination system, the illumination system being arranged to illuminate the liquid etching solution so that the etching solution has a second reactant level with respect to the material different from the first level; and a controller, the controller being coupled to the delivery system to control the delivery of the liquid etching solution, and being coupled to the illumination system to control illumination output by the illumination system.

[0012] In additional embodiments, the controller is configured to control the illumination system and the delivery system to etch the material in a cyclic manner.

[0013] In additional embodiments, the liquid etching solution oxidizes the surface of the material when irradiated to form an oxidized material as a modified layer. In further embodiments, a uniform layer of oxidized material is formed as the modified layer, and the liquid etching solution further dissolves the oxidized material. In still further embodiments, the liquid etching solution comprises an aqueous solution comprising hydrogen peroxide and citrate. In further embodiments, the delivery system is further configured to deliver an aqueous solution comprising a complexing agent to dissolve the oxidized material. In still further embodiments, the complexing agent comprises at least one of citrate, ethylenediamine, ethylenediaminetetraacetic acid (EDTA), malic acid, oxalic acid, glycine, alanine, or iminodiacetic acid.

[0014] In additional embodiments, the material to be etched comprises a polycrystalline material. In further embodiments, the polycrystalline material comprises at least one of polycrystalline metal, polycrystalline cobalt, ruthenium, tungsten, titanium, tantalum, titanium nitride, or tantalum nitride.

[0015] In additional embodiments, the illumination system is configured to selectively illuminate the liquid etching solution. In further embodiments, the illumination system is configured to selectively illuminate the liquid etching solution with ultraviolet (UV) light in one or more on / off modes. In further embodiments, the illumination system is configured to selectively illuminate with two or more different colors of light.

[0016] In an additional embodiment, the controller is configured to control the illumination system to cause different exposures to different regions of the liquid etching solution, thereby providing different amounts of etching for the material in these different regions. In a further embodiment, the different exposures are based on a measurement of at least one of the topology of the surface of the material or the thickness of the material.

[0017] For one embodiment, a platform for etching a substrate is disclosed, which includes: a dry etching processing system for etching a polycrystalline material on a substrate using dry etching chemistry; a wet etching processing system for etching the polycrystalline material to reduce the roughness of the polycrystalline material caused by the dry etching chemistry; a transfer module, which is connected to move the substrate between the dry etching processing system and the wet etching processing system; and an isolation pass-through module connected between the transfer module and the wet etching processing tool, wherein the isolation pass-through module separates the surrounding environment of the transfer module from the surrounding environment of the wet etching processing system. For the platform, the wet etching processing system includes: a wet process chamber, which is configured to perform a wet etching process; a substrate holder located in the wet process chamber, which is configured to support a substrate; a delivery system, which is arranged to supply a liquid etching solution to the substrate, the liquid etching solution having a first reactant level with respect to the polycrystalline material; an illumination system, which is arranged to illuminate the liquid etching solution so that the etching solution has a second reactant level with respect to the polycrystalline material different from the first level; and a controller, which is coupled to the delivery system to control the delivery of the liquid etching solution, and is coupled to the illumination system to control the illumination output by the illumination system.

[0018] In additional embodiments, the controller is configured to control the illumination system and the delivery system to etch the polycrystalline material in a cyclic manner.

[0019] In additional embodiments, the liquid etching solution when irradiated oxidizes the surface of the polycrystalline material to form an oxidized material as a modified layer. In further additional embodiments, the liquid etching solution comprises an aqueous solution containing hydrogen peroxide, and the irradiation comprises ultraviolet (UV) light.

[0020] In additional embodiments, the dry etching processing system implements one or more dry etching processes. In further embodiments, the one or more dry etching processes include at least one of a plasma etching process, a reactive ion etching (RIE) process, a chemical vapor etching (CVE) process, or an atomic layer etching (ALE) process.

[0021] In an additional embodiment, the dry etch processing system is configured to etch the polycrystalline material to produce a first surface roughness, and the wet etch process chamber is configured to adjust the first surface roughness to a second surface roughness less than the first surface roughness. In a further embodiment, the controller is configured to control the illumination system to cause different exposures to different areas of the liquid etching solution based on a measurement of at least one of a topology of a surface of the material or a thickness of the material, thereby providing different etching amounts for the polycrystalline material.

[0022] Different or additional features, variations, and embodiments may also be implemented, and related systems and methods may also be utilized. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] A more thorough understanding of the present invention and its advantages may be obtained by referring to the following description in conjunction with the accompanying drawings, wherein like reference numerals indicate like features. It should be noted, however, that these drawings only illustrate exemplary embodiments of the disclosed concept and are therefore not to be considered limiting of the scope, as the disclosed concept may admit to other equally effective embodiments.

[0024] FIG. 1A (Prior Art) provides a simplified diagram associated with prior art etching solutions having problems associated with varying reactivity and undesirable etching variability.

[0025] FIG. 1B (PRIOR ART) provides a representative surface image of pitting and roughness of the surface due to the undesirable etch variability associated with the conventional oxidative dissolution method of FIG. 1A (PRIOR ART).

[0026] Figure 2A Example embodiments are provided in which irradiation of a liquid etching solution is used to facilitate controlling, preferably in real time, the etch rate and uniformity of etching of material on a surface of a substrate of a microelectronic workpiece.

[0027] Figure 2B Provided due to Figure 2A Representative surface images of the smoother surfaces achieved with improved etch uniformity associated with the illumination methods.

[0028] Figure 3A Representative surface images of the roughness before the cyclic process mode with separate oxidation and dissolution reactions are provided.

[0029] Figure 3B Provides the following information after etching using the cyclic process mode: Figure 3A Representative surface images showing reduced roughness compared to .

[0030] Figure 3C Provides the Figure 3A and Figure 3B The surface image in FIG. 1 is a representative schematic diagram of an AFM (atomic force microscopy) surface roughness curve.

[0031] Figure 4A An example embodiment 400 of a scanner solution is provided in which light emitting diodes (LEDs) are used to illuminate a liquid etching solution applied to a surface of a substrate of a microelectronic workpiece.

[0032] Figure 4B Example embodiments are provided for delivering illumination by one or more laser sources to a liquid etching solution dispensed onto a surface of a substrate of a microelectronic workpiece.

[0033] Figure 5A is a process flow diagram of an example embodiment of using illumination to adjust reactants within a liquid etching solution to improve etch uniformity in etching material on a surface of a substrate of a microelectronic workpiece.

[0034] Figure 5B is a process flow diagram of an example embodiment of using irradiation to form hydroxyl radicals within a liquid etching solution having hydrogen peroxide to improve etch uniformity of etching polycrystalline metal on a surface of a substrate of a microelectronic workpiece.

[0035] Figure 6 is a process flow diagram of an example embodiment of using radiation to adjust reactants within an etching solution (eg, at least one of a gaseous etching solution, a liquid etching solution, or a combination thereof) to improve etch uniformity of etching material on a surface of a substrate of a microelectronic workpiece.

[0036] Figure 7 is a process flow diagram of an example embodiment of polishing a material using irradiation of an etching solution (eg, at least one of a gaseous etching solution, a liquid etching solution, or a combination thereof).

[0037] Fig. 8A is a block diagram of an example embodiment for a wet etch processing system that may be used in conjunction with the disclosed techniques, the wet etch processing system including a delivery system for a liquid etching solution and an illumination system.

[0038] Figure 8B is a block diagram of an example embodiment for a processing platform including a wet etch processing system and a dry etch processing system that may be used in conjunction with the disclosed techniques. DETAILED DESCRIPTION

[0039] As described herein, various methods and related processing systems and platforms are disclosed to provide controlled etching of materials (such as polycrystalline materials or metals) using radiation to modulate etchant reactivity and promote etching that is independent of the surface chemistry of the material. Other advantages and embodiments may also be realized while still utilizing the process techniques described herein.

[0040] Controlling nanoscale etching uniformity helps minimize device failures of microelectronic devices and circuits formed on microelectronic workpieces. Typically, conventional wet etching chemistries cannot provide precise etching control for materials such as polycrystalline materials and metals. For example, varying etching rates at grain boundaries and / or different crystal facets of polycrystalline materials may cause surface roughening during etching. The disclosed embodiments provide a method for achieving etching uniformity on a microscale and macroscale by generating a highly reactive etchant at the point of use through controlled irradiation. For one embodiment, the disclosed embodiments provide these beneficial results when used to etch metal polycrystalline structures (such as polycrystalline metal cobalt). Other polycrystalline materials and polycrystalline metals and other materials may also be etched using the irradiation techniques described herein.

[0041] For one embodiment, highly reactive hydroxyl radicals (HO*) are generated as an etchant for polycrystalline materials by irradiating a liquid etching solution applied to the surface of the polycrystalline material. Hydroxyl radicals are strong oxidants and etch polycrystalline materials at room temperature. For one embodiment, hydroxyl radicals are generated using hydrogen peroxide (H2O2) in contact with the material to be etched. 2 O 2 ) aqueous solution by ultraviolet (UV) light irradiation. The irradiation can also be selectively provided at the point of use to better control the etching process and rate.

[0042] For this point-of-use solution, one or more regions of a liquid etching solution (e.g., an aqueous hydrogen peroxide solution) are selectively irradiated where the surface is desired to be etched, while other regions that are not desired to be etched are not irradiated. For example, irradiation of hydrogen peroxide causes the formation of hydroxyl radicals that cause the level of reactants to increase. However, once the irradiation is removed, the lifetime of the hydroxyl radicals is very short and is quickly absorbed back into the aqueous solution. For example, the lifetime of the hydroxyl radicals after the irradiation is removed is less than 2 to 5 microseconds. Therefore, selective UV irradiation can be used to adjust the etchant reactivity, thereby modifying the thermodynamics and kinetics of the etching reaction of the selected region of the liquid etching solution. The high reactivity combined with the microsecond lifetime of the hydroxyl radicals achieves rapid and / or nearly instantaneous oxidation of the material surface layer that is independent of the local surface reactivity. The oxide layer is subsequently removed, presenting a smooth etched surface. Additionally, large-scale etching uniformity can be achieved by spatially adjusting the UV light intensity in a feed-forward process during the irradiation process. While still utilizing the technology described herein, other variations may also be implemented.

[0043] A significant advantage of the disclosed embodiments is the ability to tune nearly instantaneous etchant reactivity in situ using controlled irradiation. This tuning capability allows a wider parameter space to be obtained on the potential-pH diagram (i.e., the Pourbaix diagram) of the photosensitive etchant without mixing additional reactants and chemicals. This simplifies the process chemistry and reduces the cost of the wet etch process.

[0044] As described herein, the disclosed embodiments provide one or more of the following: (1) adjust etchant reactivity in real time and at the point of use, thereby adjusting etching behavior without the need for additional chemical mixtures or erosion conditions; (2) exploit the short lifetime of reactive transient excited states by generating reactive transient excited states at the surface of a microelectronic workpiece (e.g., a semiconductor wafer) and then using them to etch the surface; (3) control surface roughness during etching of polycrystalline materials; (4) achieve temporal and spatial control of the etch rate on the surface of a microelectronic workpiece; and / or (5) provide feed-forward control to compensate for non-uniform layer thickness across the microelectronic workpiece. Additional and / or different advantages and features may also be provided according to the techniques described herein.

[0045] FIG. 2A to FIG. 2B and FIG. 3A to FIG. 3C A simplified diagram is provided in connection with a disclosed embodiment in which illumination is used to modulate the etch rate of a liquid etching solution of etched polycrystalline material applied to a surface of a microelectronic workpiece. Additional and / or different embodiments may be implemented while utilizing the techniques described herein.

[0046] It should be noted that the irradiation described herein can be selective irradiation applied in real time to provide point-of-use control. Liquid etching solutions typically have set reactivity and etch rates for a given material based on the composition and temperature of the solution. The disclosed embodiments adjust the etching behavior of a liquid etching solution of a given composition at a given temperature in real time. In addition, the disclosed embodiments allow the etch rate to be adjusted with respect to the location and / or positioning of the material on the surface of the microelectronic workpiece, and feed-forward control can be used to achieve better uniformity across the microelectronic workpiece.

[0047] Note further that conventional etching solutions have a set solution potential and a set pH. The set solution potential and the set pH of the solution place the solution at a single point on the Bourbaix diagram. The parameters are set by the solution composition. The solution composition uniquely sets the type of thermodynamic equilibrium that will occur when the solution is brought into contact with the surface to be etched, and also sets the solubility of the etched products. Thus, the etching behavior of the system is determined.

[0048] In contrast, the disclosed embodiments provide a wet etching process that uses irradiation to adjust the etchant reactivity and / or the potential of the etching solution and thereby achieve the desired etching behavior. For the embodiments herein, the etching solution includes a photosensitive compound that undergoes a photochemical reaction upon irradiation to generate a reactive etchant (e.g., free radicals or radical ions). The liquid etching solution may also include additional components for dissolving or volatilizing the etching products.

[0049] For one embodiment, hydroxyl radicals (HO*) are used as transient excited state species and are generated by photolysis of hydrogen peroxide. Other examples include, but are not limited to, singlet oxygen, excited state molecules, free radicals, dimers, complexes, and / or other materials having properties that generate and / or modulate reactive etchants by irradiation. For example, similar reactive species can be generated by photolysis of ozone or aqueous hypochlorous acid solutions. Other variations can also be implemented.

[0050] For one example implementation, the disclosed embodiments are used to reduce roughening in etching of polycrystalline metal materials. In a further example embodiment, the polycrystalline metal material is cobalt.

[0051] Wet etching of polycrystalline materials is typically accomplished by an oxidative dissolution mechanism. The etchant solution contains an oxidant and reactants that promote the dissolution of the etched products. The etching behavior (e.g., etching rate, etching uniformity) and therefore the final surface morphology depends on the chemical reactions that occur on the surface of the material to be etched. Variable etch rates on polycrystalline materials are a common problem with conventional wet etching processes, where such variability typically results in undesirable surface morphologies such as roughening and pitting. As described herein, adjusting the oxidation reaction rate and the dissolution reaction rate by irradiation (preferably in real time) allows the etching behavior to be modified and uniform etching to be achieved.

[0052] Hydrogen peroxide is a commonly used etchant in wet etching processes. As recognized in the current embodiment, irradiating hydrogen peroxide with light having a wavelength (λ) less than 560 nanometers (nm) (i.e., λ<560nm) can result in quantitative photolysis of hydroxyl radicals. For example, UV light with a wavelength of 10nm to 400nm (e.g., 10nm≤λ≤400nm) can be used for such irradiation. Hydroxyl radicals have a very high oxidation potential (e.g., 2.8 volts) and have a microsecond lifespan (e.g., lifespan≤2 to 5 microseconds). The combination of high reactivity and short lifespan results in a uniform surface layer being nearly oxidized instantaneously, and then the oxidized surface layer can be removed.

[0053] Cobalt may be considered as an example polycrystalline material that may be etched using the disclosed embodiments.

[0054] First Look Figure 2AAccording to the disclosed technology, an example embodiment 200 is provided, wherein irradiation of a liquid etching solution is used to facilitate control and preferably real-time control of etching rate and uniformity, as described herein. A liquid etching solution 206 is applied to a material 204 on a surface of a substrate 208 of a microelectronic workpiece. For the example embodiment 200, the etched material 204 is cobalt (Co), and the material 204 has previously been formed on the surface of the substrate 208. For the example embodiment 200, the liquid etching solution 206 provides an oxidative dissolution etching mechanism. For the oxidative dissolution etching mechanism, the material 204 is oxidized by the liquid etching solution 206 and then dissolved by the liquid etching solution 206. In contrast to existing solutions and according to the technology described herein, irradiation 205 is used to cause the liquid etching solution 206 to transition from a first reactant level with respect to the material 204 on the surface of the substrate 208 to a second reactant level with respect to the material 204. Further, the second reactant level is greater than the first reactant level.

[0055] For one embodiment, a method comprising using hydrogen peroxide (H 2 O 2 ) liquid etching solution. When irradiated with UV light, hydrogen peroxide cleaves to form two hydroxyl radicals (OH*). This formation of hydroxyl radicals increases the oxidation potential of the solution from about 1.8 volts (V) to about 2.8 V. The reactive hydroxyl radicals accelerate the oxidation reaction and result in an oxidation rate constant k ox (as indicated by arrow 210) is much greater than the dissolution rate constant k d (As indicated by arrow 212). This significantly increased oxidation rate (k ox >>k d ) promotes the formation of a thin and uniform layer of oxide material 214 on the surface of the material at a constant rate. The oxide material 214 is then slowly removed, thereby presenting a smooth surface. In the case of cobalt as the material 108, cobalt oxide (CoO x ) is an oxidized material 214.

[0056] Figure 2B A representative surface image 250 of such a smooth surface achieved due to the improved etch uniformity associated with the illumination methods of the disclosed embodiments described herein is provided. For the representative surface image 250, scale is provided by a bar 252 representing a length of 500 nm.

[0057] It should be noted that the rapid formation of the surface oxide layer additionally prevents the diffusion of the etchant through the grain boundaries and defect sites of the polycrystalline material, thereby reducing or minimizing pitting. Based on surface morphology analysis, using the irradiation techniques described herein, corrosion associated with pitting also does not occur or is reduced. In addition, the surface roughness is significantly reduced from the initial value. Additional and / or different advantages can also be achieved.

[0058] Example process modes were also tested using the UV enhanced peroxide (UVP) wet etch methods described herein for etching of polycrystalline materials. For these example process modes, polycrystalline cobalt was etched using two example process modes that applied the UVP wet etch method: a continuous UVP process and a cyclic oxidative dissolution process.

[0059] For the continuous UVP process example, hydrogen peroxide (H2O2) adjusted to pH 10 (pH=10) was used. 2 O 2 ) and citric acid (e.g., in the form of a citrate salt). In this mode, the oxidation reaction and the dissolution reaction are carried out simultaneously. The results of this process using irradiation are Figure 2B 1B (Prior Art) with respect to representative image 250. The results of this process without the use of illumination are shown with respect to representative surface image 150 in FIG.

[0060] As described above, FIG. 1A (prior art) provides a graph showing the reaction of cobalt with hydrogen peroxide (H2O2) without UV irradiation. 2 O 2 ) and an aqueous citrate solution. FIG. 1B (Prior Art) corresponds to an example surface image 150 of the post-etch morphology for the process represented by FIG. 1A (Prior Art) without UV irradiation.

[0061] In contrast to what is described above, Figure 2A Provides the reaction of cobalt and H under UV irradiation 2 O 2 Example embodiment 200 of oxidation and dissolution reaction rates in contact with an aqueous citrate solution. Figure 2B With regard to Figure 2A An example surface image 250 of the post-etch morphology of a process with UV irradiation is shown. UV irradiation generates transient hydroxyl radicals to achieve a higher oxidation rate, which can lead to surface roughness reduction even at very low etch amounts.

[0062] For one embodiment, a cyclic process mode is used. For this cyclic process mode example, the oxidation reaction and the dissolution reaction are separated. In the first step, the cobalt is oxidized for a given time using an irradiation process (e.g., a UVP process) without citrate (e.g., dissolution removal). Then an aqueous solution of citric acid (e.g., in the form of citrate) is used to remove the oxidized material layer (e.g., cobalt oxide). Carefully controlling the UVP oxidation time and the dissolution time allows the cobalt to be etched uniformly.

[0063] It should be noted that the complexing agent is not limited to citrate, and different complexing agents can also be used for this purpose. For example, the complexing agent can include ligands from the family of carboxylic acids, amines, amino acids, alcohols, etc. Examples include, but are not limited to: ethylenediamine, ethylenediaminetetraacetic acid (EDTA), malic acid, oxalic acid, glycine, alanine, and iminodiacetic acid. It should be further noted that the removal rate depends on the type of complexing agent.

[0064] FIG. 3A to FIG. 3C Representative results for this cyclic process mode are provided.

[0065] Figure 3A A representative surface image 300 of the roughness before the cycling process is provided. This diagram represents the material on the surface of the substrate as received. For this example, the thickness of the material layer is 30nm and the RMS (root mean square) roughness is 1.76nm.

[0066] Figure 3B The cyclic UVP process is used to etch polycrystalline cobalt and Figure 3A 350. Etching has removed 4nm, so the thickness of the material layer is now 26nm. The RMS roughness has improved to 0.86nm, and the reduction in roughness can be seen in the surface image. For the representative surface image 350, scale is provided by bars 352 representing 200nm lengths.

[0067] Figure 3C Provides the Figure 3A and Figure 3B370 of a representative diagram of an AFM (atomic force microscopy) surface roughness curve 374 / 376 represented by a surface image in FIG. The roughness curve 374 / 376 shows the smoothness effect of the etching process, for example, after etching 4nm from the surface of polycrystalline cobalt. The vertical axis represents the normalized height of the surface in nanometers, and the horizontal axis represents the length in one direction along the surface of the material in micrometers (μm). The top line is the roughness curve 374 representing the surface of the material as received, and the surface change as received is represented by bar 378. The bottom line is the roughness curve 376 representing the surface of the material after 4nm etching, and the surface change after etching is represented by bar 380. For the representative diagram 370 and roughness curves 374 / 376, the scale is provided by the bar 372 representing the length of 4nm. As can be seen, the cyclic process significantly reduces the surface roughness.

[0068] For additional embodiments, the etch rate over a relatively large surface area of ​​a substrate of a microelectronic workpiece can be controlled by spatial and / or temporal control of the intensity of UV light delivered to the liquid etching solution. For example, for spatial control, different areas of the liquid etching solution can be irradiated with UV light while keeping other areas of the liquid etching solution from being exposed to the UV light. For temporal control, UV light can be applied to different areas of the surface for different amounts of time. Thus, by adjusting the spatial and / or temporal irradiation of the surface of the microelectronic workpiece, different etch rates are achieved.

[0069] Various irradiation systems can be used to irradiate the liquid etching solution applied to the surface of the substrate of the microelectronic workpiece, including a rotator solution and a laser / scanner solution. When implemented on a rotator, the irradiation light source can be optionally synchronized with the movement of the substrate, so that each area of ​​the wafer can be irradiated with a non-time-varying intensity. For example, a light emitting diode (LED) array can be used to achieve spatially resolved irradiation. When low spatial resolution is acceptable, the LED array works well. The LED array can rotate synchronously with the substrate in a rotating chamber, or the spatial intensity of the array can be synchronized with the movement of the wafer. When higher spatial resolution is desired, a laser source and a scanner can be used to provide irradiation. The laser source can move / scan on the entire wafer surface with such a movement: provide a higher light intensity for the wafer area that requires a higher etching rate. Both of these example embodiments can be used to irradiate the wafer with a single wavelength or multiple wavelengths, thereby adjusting the reactants in the wet etching solution. It should be noted that other light sources can also be used. Further, light sources can be combined, for example, the whole-piece exposure of the area enhanced by precise laser scanning can be used as an irradiation system. Other variations and implementations may be used while still utilizing the techniques described herein.

[0070] FIG. 4A to FIG. 4B Example embodiments are provided for scanner solutions and laser / scanner solutions with respect to illumination of a surface of a microelectronic workpiece.

[0071] First Look Figure 4A , an example embodiment 400 for a scanner solution is provided in which an LED array 402 is used to irradiate a liquid etching solution applied to the surface of a substrate of a microelectronic workpiece, such as a semiconductor wafer 404. Prior to irradiation, the liquid etching solution is dispensed onto the surface of the wafer 404 in a rotating chamber using a delivery system 406. For the example embodiment 400, the LED array 402 can be a single wavelength or can be multiple wavelengths by interspersing different emitters within the array. The power of each emitter can be adjusted in real time to control the intensity of illumination across the wafer surface. For one embodiment, the LED array 402 is mechanically synchronized with the movement of the wafer 404, as indicated by arrows 403 and 405. For another embodiment, the LED array 402 remains stationary while the intensity of each emitter is synchronized with the movement of the wafer 404. Additional variations may also be implemented.

[0072] Figure 4B An example embodiment 450 of delivering irradiation of a liquid etching solution dispensed on the surface of a substrate of a microelectronic workpiece (such as a semiconductor wafer 404) by one or more laser sources 452 / 456 is provided. Prior to irradiation, the liquid etching solution is dispensed on the surface of the wafer 404 in a rotating chamber using a delivery system 406. Irradiation is then performed using a single laser or multiple laser sources 452 / 456. For example, multiple laser sources 452 / 456 may be used where it is desired to irradiate the wafer 404 with multiple wavelengths. The laser beam from the laser source 452 / 456 is rasterized across the wafer surface using a steering optical device 454 / 458. The dwell time of the laser spot on a single point on the surface of the wafer 404 controls the etching enhancement at that point. As indicated by arrows 405, 455, and 459, the movement of the laser beam may be synchronized with the movement of the wafer 404.

[0073] For further additional embodiments, the uniformity of etching over a relatively large surface area of ​​a substrate of a microelectronic workpiece can be improved by feedforward techniques. For example, the topology and / or layer thickness of the surface of the substrate can be measured over a selected surface area, and the amount of etching for different areas within the surface area can be determined based on these measurements and the desired results. For example, if a smooth surface is desired, spatial and / or temporal control of UV light irradiation can be used to adjust the local etch rate to make the peaks and valleys within the topology uniform, thereby achieving the desired target surface parameters. Therefore, feedforward control provides a technique for compensating for uneven layer thickness and / or other changes across the entire microelectronic workpiece.

[0074] Figure 5A 1 is a process flow diagram of an example embodiment 500 of using irradiation to adjust reactants in a liquid etching solution to improve the etch uniformity of etching a material on a surface of a substrate of a microelectronic workpiece. In box 502, a substrate of a microelectronic workpiece is received, and the substrate has a material to be etched from the surface of the substrate. In box 504, a liquid etching solution is applied to the surface of the substrate, and the liquid etching solution has a first reactant level with respect to the material. In box 506, the liquid etching solution is irradiated so that the liquid etching solution has a second reactant level with respect to the material, and the second level is greater than the first level. In box 508, the material is oxidized with the liquid etching solution to form an oxidized material. In box 510, the oxidized material is removed. It should be noted that additional and / or different steps may also be used while still utilizing the irradiation techniques described herein.

[0075] Figure 5B 1 is a process flow diagram of an example embodiment 550 of using irradiation to form hydroxyl radicals in a liquid etching solution with hydrogen peroxide to improve the etch uniformity of etching polycrystalline metal on the surface of a substrate of a microelectronic workpiece. In box 552, a substrate of a microelectronic workpiece is received, and the substrate has polycrystalline metal to be etched from the surface of the substrate. In box 554, a liquid etching solution containing hydrogen peroxide is applied to the surface of the substrate, and the liquid etching solution has a first reactant level with respect to the polycrystalline metal. In box 556, the liquid etching solution is irradiated to cause hydroxyl radicals to be formed from hydrogen peroxide, and the formation of hydroxyl radicals at least partially causes the liquid etching solution to have a second reactant level with respect to the polycrystalline metal. Further, the second reactant level is greater than the first reactant level. In box 558, the polycrystalline metal is oxidized with the liquid etching solution to form an oxidized metal. In box 560, the oxidized metal is removed. It should be noted that additional and / or different steps may also be used while still utilizing the irradiation techniques described herein.

[0076] Figure 6The present invention is a process flow chart of an example embodiment 600 of using irradiation to adjust the reactants in an etching solution (e.g., at least one of a gaseous etching solution, a liquid etching solution, or a combination thereof) to improve the etch uniformity of etching a material on a surface of a substrate of a microelectronic workpiece. In frame 602, a substrate of a microelectronic workpiece is received, and the substrate has a material to be etched from the surface of the substrate. In frame 604, an etching solution is applied to the surface of the substrate, and the etching solution has a first reactant level with respect to the material. In frame 606, the etching solution and the surface of the material are exposed to irradiation to form a modified material layer on the surface of the material, and this exposure causes the etching solution to have a second reactant level with respect to the material greater than the first level. In frame 608, the modified material layer is removed. It should be noted that additional and / or different steps may also be used while still utilizing the irradiation techniques described herein.

[0077] Figure 7 1 is a process flow chart of an example embodiment 700 of polishing a material using irradiation of an etching solution (e.g., at least one of a gaseous etching solution, a liquid etching solution, or a combination thereof). In block 702, a material to be polished is received. In block 704, an etching solution is applied to a surface of the material, and the etching solution has a first reactant level with respect to the material. In block 706, the etching solution and the surface of the material are exposed to irradiation to form a modified material layer on the surface of the material, and such exposure causes the etching solution to have a second reactant level with respect to the material greater than the first level. In block 708, the modified material layer is removed so that the material has a polished surface. The polished surface is polished because it has less surface variation than the surface of the original material being etched. It should be noted that additional and / or different steps may also be used while still utilizing the irradiation techniques described herein.

[0078] It should be further noted that the techniques described herein can be used with a wide range of processing systems, equipment, and platforms. For example, these techniques can be used in Fig. 8A The wet etching process system shown in FIG. 1 is used in the wet etching process system, and the wet etching process system can be used in Figure 8B The dry etching processing system shown in the processing platform embodiment can be used in combination. Other variations can also be implemented.

[0079] Fig. 8A806. The wet etch processing system 800 may be used in conjunction with the disclosed techniques to etch material on the surface of a substrate 806. The wet etch processing system 800 includes a wet process chamber 810. The wet process chamber 810 may be a pressure controlled chamber. A substrate 806 (a semiconductor wafer in one example) is held on a substrate holder 808 (such as an electrostatic chuck). The substrate holder 808 may also be configured to rotate at a controlled speed.

[0080] A delivery system 802 for a liquid etching solution and an irradiation system 804 are used with a wet process chamber 810. The delivery system 802 may include a reservoir for containing the liquid etching solution and a liquid delivery tube having a dispensing nozzle located within the wet process chamber 810. The delivery system 802 may be used to dispense the liquid etching solution onto a surface of a substrate 806. As described herein and with reference to FIG. 4A to FIG. 4B As described, the liquid etching solution is illuminated using an illumination system 804, which can be an LED array or other illumination device that provides light of a single wavelength or multiple wavelengths. Further, such illumination can be selective, synchronized with the rotation of the substrate holder 808, and / or delivered in other ways to illuminate the liquid etching solution to adjust the reactant level within the liquid etching solution as described herein.

[0081] As described herein, the disclosed embodiments provide beneficial results when used to etch polycrystalline structures, such as polycrystalline metal cobalt. Other polycrystalline materials and polycrystalline metals, as well as other materials, may also be etched using the irradiation techniques described herein. For example, additional polycrystalline materials and compounds that may be etched include ruthenium, tungsten, titanium, tantalum, titanium nitride, tantalum nitride, and / or other materials.

[0082] The components of the wet etch processing system 800 can be coupled to and controlled by a controller 812, which in turn can be coupled to corresponding memory storage units and user interfaces (not shown). Various processing operations can be performed via the user interfaces, and various processing schemes and operations can be stored in the storage units. Accordingly, a given substrate 806 can be processed within the wet process chamber 810 by various techniques. It will be appreciated that the controller 812 can be coupled to various components of the wet etch processing system 800 to receive inputs from these components and provide outputs to these components.

[0083] The controller 812 can be implemented in a variety of ways. For example, the controller 812 can be a computer. In another example, the controller can include one or more programmable integrated circuits programmed to provide the functions described herein. For example, one or more processors (e.g., microprocessors, microcontrollers, central processing units, etc.), programmable logic devices (e.g., complex programmable logic devices (CPLDs)), field programmable gate arrays (FPGAs), etc.) and / or other programmable integrated circuits can be programmed using software or other programming instructions to implement the functions of the prohibited plasma process scheme. It is further noted that the software or other programming instructions can be stored in one or more non-transient computer-readable media (e.g., memory storage devices, flash memory, DRAM memory, reprogrammable storage devices, hard drives, floppy disks, DVDs, CD-ROMs, etc.), and the software or other programming instructions, when executed by the programmable integrated circuit, cause the programmable integrated circuit to perform the processes, functions, and / or capabilities described herein. Other variations can also be implemented.

[0084] Figure 8B 850 is a block diagram of an example embodiment for a platform 850 that includes a wet etch processing system 800 and a dry etch processing system 852. As described herein, the wet etch processing system 800 dispenses a liquid etch solution onto a material to be etched, and then irradiates the liquid etch solution to adjust the level of reactants within the liquid etch solution. The dry etch processing system 852 can implement any desired dry etch process that etches a substrate or removes material from a substrate being processed. In operation, the dry etch processing system 852 etches material on a substrate using a dry etch chemistry.

[0085] It should be noted that the dry etching processing system 852 can implement any of a variety of dry etching processes, such as a plasma etching process, a reactive ion etching (RIE) process, a chemical vapor etching (CVE) process, an atomic layer etching (ALE) process, and / or other dry etching processes. Further, the dry etching process can be performed before or after the wet etching process. For example, a dry etching process can be performed in a dry etching process chamber of the dry etching processing system 852 to remove material from the substrate, thereby generating a first surface roughness. The substrate is then transferred (via the transfer module 854) to the wet etching process chamber of the wet etching processing system 800 to perform a wet etching process, thereby generating a second surface roughness, wherein the second surface roughness is less than the first surface roughness. It should be further noted that multiple dry etching processes and multiple wet etching processes can be performed by using the transfer module 854 to transfer the substrate as needed. Other variations can also be implemented.

[0086] To facilitate processing of substrates within the dry etch processing system 852 and the wet etch processing system 800, a transfer module 854 and an isolation pass-through module 856 may also be coupled between the two systems 800 / 852. The transfer module 854 is configured to move the substrate between the dry etch processing system 852 and the wet etch processing system 800, as indicated by arrow 858. The isolation pass-through module 856 is disposed between the transfer module 854 and the wet etch processing system 800 to separate the surrounding environment of the transfer module 854 from the surrounding environment of the wet etch processing system 800. The substrate may then be moved between the dry etch processing system 852 and the wet etch processing system 800 without exposing the substrate to potential contaminants present outside of the processing system 800 / 852. This movement may also be controlled by a controller (such as a controller in conjunction with a controller). Fig. 8A 812) described above.

[0087] Further example embodiments that can be used for the dry etch processing system 852, the wet etch processing system 800, the transfer module 854, and the isolation pass-through module 856 are described in the following applications: U.S. Provisional Patent Application Serial No. 62 / 794,315, filed on January 18, 2019, entitled "Platform and Method for Operating for Integrated End-to-End Gate Contact Process"; U.S. Provisional Patent Application Serial No. 62 / 787,607, filed on January 2, 2019, entitled "Self-Aware and Correcting Heterogeneous Platform incorporating Integrated Semiconductor Processing Modules and Method for using same"; and U.S. Provisional Patent Application Serial No. 62 / 787,607, filed on January 2, 2019, entitled "Self-Aware and Correcting Heterogeneous Platform incorporating Integrated Semiconductor Processing Modules and Method for using same No. 62 / 787,608, filed on January 4, 2019, entitled “Substrate Processing Tool with Integrated Metrology and Method of using”; No. 62 / 788,195, filed on January 4, 2019, entitled “Substrate Processing Tool with Integrated Metrology and Method of using”; and No. 16 / 356,451, filed on March 18, 2019, entitled “PLATFORM AND METHOD OF OPERATING FOR INTEGRATED END-TO-ENDGATE CONTACT PROCESS”, each of which is incorporated herein by reference in its entirety.

[0088] It should be noted that one or more deposition processes may be used to form the material layer described herein. For example, chemical vapor deposition (CVD), plasma enhanced CVD (PECVD), physical vapor deposition (PVD), atomic layer deposition (ALD) and / or other deposition processes may be used to implement one or more depositions. For plasma deposition processes, a precursor gas mixture (including but not limited to hydrocarbons, fluorocarbons or nitrogen-containing hydrocarbons) may be used in combination with one or more diluent gases (e.g., argon, nitrogen, etc.) under a variety of pressures, powers, flows and temperature conditions. Photolithography processes for photoresist (PR) layers may be implemented using optical lithography, extreme ultraviolet (EUV) lithography and / or other lithography processes. Etching processes may be implemented using plasma etching processes, discharge etching processes, atomic layer etching (ALE) and / or other desired etching processes. For example, plasma etching processes may be implemented using plasmas containing fluorocarbons, oxygen, nitrogen, hydrogen, argon and / or other gases. In addition, the operating variables used for the process steps may be controlled to ensure that the CD (critical dimension) target parameters of the through-holes are achieved during through-hole formation. The operating variables may include, for example, chamber temperature, chamber pressure, flow rate of gases, frequency and / or power applied to the electrode assembly when generating plasma, and / or other operating variables for the processing steps.Variations may also be implemented while still utilizing the techniques described herein.

[0089] Note that references throughout this specification to "one embodiment" or "an embodiment" mean that a particular feature, structure, material, or characteristic described in conjunction with the embodiment is included in at least one embodiment of the invention, but does not imply that they are present in every embodiment. Therefore, the phrases "in one embodiment" or "in an embodiment" that appear throughout this specification do not necessarily refer to the same embodiment of the invention. Furthermore, in one or more embodiments, particular features, structures, materials, or characteristics may be combined in any suitable manner. In other embodiments, various additional layers and / or structures may be included, and / or described features may be omitted.

[0090] As used herein, "microelectronic workpiece" generally refers to an object processed according to the present invention. A microelectronic workpiece may include any material portion or structure of a device (particularly a semiconductor or other electronic device), and may be, for example, a base substrate structure (such as a semiconductor substrate), or a layer (such as a thin film) on or overlying a base substrate structure. Therefore, the workpiece is not intended to be limited to any particular base structure, underlying layer or overlying layer, patterned or unpatterned, but is contemplated to include any such layer or base structure, and any combination of layers and / or base structures. The following description may refer to a specific type of substrate, but this is for illustrative purposes only and not for limiting purposes.

[0091] As used herein, the term "substrate" means and includes the base material or structure on which the material is formed. It should be understood that the substrate may include a single material, multiple layers of different materials, one or more layers with different material regions or different structural regions, etc. These materials may include semiconductors, insulators, conductors, or combinations thereof. For example, the substrate may be a semiconductor substrate, a base semiconductor layer on a support structure, a metal electrode or a semiconductor substrate having one or more layers, structures, or regions formed thereon. The substrate may be a conventional silicon substrate or other bulk substrates including a semiconductor material layer. As used herein, the term "bulk substrate" refers to a silicon wafer, and includes not only a silicon wafer, but also a silicon on insulator ("SOI") substrate (such as silicon on sapphire ("SOS") substrate and silicon on glass ("SOG") substrate), a silicon epitaxial layer on a base semiconductor substrate, and other semiconductor or optoelectronic materials (such as silicon germanium, germanium, gallium arsenide, gallium nitride, and indium phosphide). The substrate may be doped or non-doped.

[0092] Systems and methods for processing microelectronic workpieces are described in various embodiments. Those skilled in the relevant art will recognize that various embodiments may be practiced without one or more of the specific details or with other alternative and / or additional methods, materials or components. In other cases, well-known structures, materials, or operations are not shown or described in detail to avoid obscuring the aspects of the various embodiments of the present invention. Similarly, specific numbers, materials, and configurations are set forth for the purpose of explanation in order to provide a thorough understanding of the present invention. However, the present invention may be practiced without specific details. In addition, it should be understood that the various embodiments shown in the drawings are illustrative representations and are not necessarily drawn to scale.

[0093] In view of this description, further modifications and alternative embodiments of the described systems and methods will be apparent to those skilled in the art. Therefore, it will be appreciated that the described systems and methods are not limited by these example arrangements. It should be understood that the forms of the systems and methods shown and described herein will be considered as example embodiments. Various changes can be made in the embodiments. Therefore, although the present invention is described herein with reference to specific embodiments, various modifications and changes can be made without departing from the scope of the present invention. Therefore, the description and the accompanying drawings should be considered illustrative and not restrictive, and such modifications are intended to be included within the scope of the present invention. Further, any benefits, advantages, or solutions to problems described herein for specific embodiments are not intended to be interpreted as key, essential, or necessary features or elements of any or all claims.

Claims

1. A processing system for performing a wet etching process on a substrate, the processing system comprising: a wet process chamber configured to perform a wet etching process; a substrate holder located within the wet processing chamber, the substrate holder configured to support a substrate; a delivery system arranged to supply a liquid etching solution to the substrate, the liquid etching solution having a first reactant level with respect to a material on a surface of the substrate, an irradiation system arranged to irradiate the liquid etching solution so that the etching solution has a second reactant level with respect to the material different from the first reactant level and such that an oxidation rate constant k with respect to the material ox Greater than the dissolution rate constant k for the material d ; and, the liquid etching solution comprises a photosensitive compound that undergoes a photochemical reaction upon irradiation to generate a reactive etchant; as well as a controller coupled to the delivery system to control the delivery of the liquid etching solution and coupled to the illumination system to control the illumination output by the illumination system, and The controller is configured to control the irradiation system and the conveying system so as to etch the material in a cyclic manner, and in the cyclic manner, an oxidation reaction generated by the irradiation system and a dissolution reaction of the material are separated from each other.

2. The processing system according to claim 1, wherein: The liquid etching solution, when irradiated, oxidizes the surface of the material to form an oxidized material as a modified layer.

3. The processing system according to claim 2, wherein: A uniform oxide material layer is formed as the modified layer, and wherein the liquid etching solution further dissolves the oxide material.

4. The processing system according to claim 3, wherein: The liquid etching solution includes an aqueous solution containing hydrogen peroxide and citrate.

5. The processing system according to claim 2, wherein: The delivery system is further configured to deliver an aqueous solution including a complexing agent to dissolve the oxidizing material.

6. The processing system according to claim 5, wherein: The complexing agent includes at least one of citrate, ethylenediamine, ethylenediaminetetraacetic acid, malic acid, oxalic acid, glycine, alanine or iminodiacetic acid.

7. The processing system according to claim 1, wherein: The material to be etched includes polycrystalline material.

8. The processing system according to claim 7, wherein: The polycrystalline material includes at least one of polycrystalline metal, polycrystalline cobalt, ruthenium, tungsten, titanium, tantalum, titanium nitride, or tantalum nitride.

9. The processing system according to claim 1, wherein: The illumination system is configured to selectively illuminate the liquid etching solution.

10. The processing system according to claim 9, wherein: The irradiation system is configured to selectively irradiate the liquid etching solution with ultraviolet light in one or more on / off modes.

11. The processing system according to claim 9, wherein: The illumination system is configured to selectively illuminate with two or more different colors of light.

12. The processing system according to claim 1, wherein: The controller is configured to control the illumination system to cause different exposures to different regions of the liquid etching solution, thereby providing different amounts of etching of material in the different regions.

13. The processing system according to claim 12, wherein: The different exposures are based on measurements of at least one of a topology of a surface of the material or a thickness of the material.

14. A platform for etching a substrate, the platform comprising: A dry etch processing system for etching polycrystalline material on a substrate using dry etch chemistry; A wet etch processing system for etching the polycrystalline material to reduce the roughness of the polycrystalline material caused by the dry etch chemistry, the wet etch processing system comprising: a wet process chamber configured to perform a wet etching process; a substrate holder located within the wet processing chamber, the substrate holder configured to support a substrate; a delivery system arranged to supply a liquid etching solution to the substrate, the liquid etching solution having a first reactant level with respect to the polycrystalline material; an irradiation system arranged to irradiate the liquid etching solution so that the etching solution has a second reactant level with respect to the polycrystalline material different from the first reactant level and such that an oxidation rate constant k with respect to the material ox Greater than the dissolution rate constant k for the material d ; and the liquid etching solution contains a photosensitive compound that undergoes a photochemical reaction upon irradiation to generate a reactive etchant; and a controller coupled to the delivery system to control delivery of the liquid etching solution and coupled to the illumination system to control illumination output by the illumination system; a transfer module coupled to move the substrate between the dry etching process system and the wet etching process system; and an isolation pass-through module coupled between the transfer module and the wet etch processing tool, the isolation pass-through module separating an environment surrounding the transfer module from an environment surrounding the wet etch processing system; and The controller is configured to control the irradiation system and the conveying system so as to etch the material in a cyclic manner, wherein an oxidation reaction generated by the irradiation system and a dissolution reaction of the material are separated from each other.

15. The platform of claim 14, wherein: The liquid etching solution, when irradiated, oxidizes the surface of the polycrystalline material to form an oxidized material as a modified layer.

16. The platform of claim 14, wherein: The liquid etching solution comprises an aqueous solution including hydrogen peroxide, and wherein the irradiation comprises ultraviolet light.

17. The platform of claim 14, wherein: The dry etching processing system implements one or more dry etching processes.

18. The platform of claim 17, wherein: The one or more dry etching processes include at least one of a plasma etching process, a reactive ion etching process, a chemical vapor etching process, or an atomic layer etching process.

19. The platform of claim 14, wherein: The dry etching processing system is configured to etch the polycrystalline material to produce a first surface roughness, and wherein the wet etching process chamber is configured to adjust the first surface roughness to a second surface roughness that is less than the first surface roughness.

20. The platform of claim 19, wherein: The controller is configured to control the illumination system to cause different exposures to different regions of the liquid etching solution based on a measurement of at least one of a topology of a surface of the material or a thickness of the material to provide different etching amounts for the polycrystalline material.

Citation Information

Patent Citations

  • Platform and method of operating for integrated end-to-end gate contact process

    US20190295905A1

  • Processing systems and platforms for roughness reduction of materials using illuminated ETCH solutions

    US20200075351A1

  • Roughness reduction methods for materials using illuminated ETCH solutions

    US20200194278A1

  • Compositions and methods for selectively etching titanium nitride

    CN105683336A

  • Method for etching surface material with induced chemical reaction by focused electron beam on surface

    CN1479175A