Sulfide solid electrolyte, electrode mixture, solid battery and method for producing sulfide solid electrolyte
By adding specific elements and hydrates to the sulfide solid electrolyte to form a film, the problem of rising reaction resistance in solid batteries is solved, and the conductivity of lithium ions and the performance of the battery is improved.
Patent Information
- Application Number
- CN202080011188.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-11
- Filing Date
- 2020-09-03
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-09-03
AI Technical Summary
In a solid battery containing a sulfide solid electrolyte, the reaction of the electrode active substance with the sulfide solid electrolyte causes the reaction resistance to rise, limiting the movement of lithium ions.
The reaction resistance is reduced by adding lithium, phosphorus, sulfur, halogen and oxygen elements to the sulfide solid electrolyte and containing hydrates to form a coating. Specific methods include using lithium, phosphorus, sulfur and halogen elements, such as fluorine, chlorine, bromine, and iodine in the lithium-ion conductive sulfide solid electrolyte, and optimizing the content and volatilization temperature of the hydrate by thermogravimetric determination. range to reduce reaction resistance.
The reaction resistance between the electrode active substance and the sulfide solid electrolyte is significantly reduced, the discharge capacity and magnification characteristics of the solid battery are improved, and a high-performance solid battery is formed.
Smart Images

Figure BDA0003183438750000121 
Figure BDA0003183438750000131
Abstract
Description
Technical Field
[0001] The present invention relates to a sulfide solid electrolyte, an electrode mixture and a solid battery having the sulfide solid electrolyte, and a method for producing the sulfide solid electrolyte. Background Art
[0002] Currently, many lithium-ion secondary batteries use electrolytes containing flammable organic solvents. In contrast, solid batteries that use solid electrolytes instead of electrolytes and do not contain flammable organic solvents are expected to be put into practical use as batteries that have both safety and high energy density.
[0003] As one of the solid electrolytes for solid batteries, sulfide solid electrolytes have been studied. However, for solid batteries containing sulfide solid electrolytes, there is the following problem: if they are charged and discharged, the reaction resistance between the electrode active material and the sulfide solid electrolyte increases, and the movement of lithium ions is restricted. It is believed that the reason is that since the active material reacts with the sulfide solid electrolyte, a resistance layer is formed at their interface. For this problem, attempts have been made to suppress the increase in reaction resistance by coating the surface of the active material with a specific compound (Patent Documents 1 to 3).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: JP2012-99323A
[0007] Patent Document 2: US2014 / 072875A1
[0008] Patent Document 3: JP2015-201388A Summary of the invention
[0009] In the technologies described in the above-mentioned patent documents, a method is adopted to suppress the increase of the reaction resistance between the active material and the sulfide solid electrolyte by modifying the surface of the active material. However, these documents do not consider suppressing the increase of the reaction resistance by modifying the surface of the sulfide solid electrolyte.
[0010] Therefore, an object of the present invention is to provide a sulfide solid electrolyte capable of suppressing an increase in the reaction resistance with an active material.
[0011] The present invention provides a sulfide solid electrolyte having a weight reduction rate of 2.7% or more and 9.6% or less when heated from 25° C. to 400° C. in a thermogravimetric measurement performed at a heating rate of 10° C. / min. DETAILED DESCRIPTION
[0012] The present invention is described below based on the preferred embodiments of the present invention. The present invention relates to a solid electrolyte. The solid electrolyte of the present invention contains a sulfide solid electrolyte. The sulfide solid electrolyte (hereinafter also referred to as "solid electrolyte") has lithium ion conductivity. The degree of lithium ion conductivity of the solid electrolyte of the present invention will be described later.
[0013] The solid electrolyte of the present invention contains sulfur (S) element as its constituent element. The lithium ion conductivity of the solid electrolyte of the present invention is caused by the sulfide solid electrolyte. As for the sulfide solid electrolyte with lithium ion conductivity, various sulfide solid electrolytes are known in the technical field, and in the present invention, these various sulfide solid electrolytes can be used without particular restrictions. In particular, from the aspect of reducing the reaction resistance between the active material, it is advantageous for the sulfide solid electrolyte to contain lithium (Li) element, phosphorus (P) element, sulfur (S) element, halogen (X) element and oxygen (O) element. As the halogen (X) element, from the aspect of further reducing the reaction resistance with the active material, it is advantageous to use at least one of fluorine (F) element, chlorine (Cl) element, bromine (Br) element and iodine (I) element. The sulfide solid electrolyte may contain elements other than lithium element, phosphorus element, sulfur element and halogen element. For example, a part of the lithium element can be replaced by another alkali metal element, a part of the phosphorus element can be replaced by another pnictogen element, or a part of the sulfur element can be replaced by another chalcogen element.
[0014] In the case of the solid electrolyte of the present invention, a weight reduction was observed when a thermogravimetric measurement was performed on it. Specifically, a weight reduction was observed when the solid electrolyte of the present invention was heated from 25°C to 400°C. In the case of the solid electrolyte in which the weight reduction was observed, the reaction resistance with the active material was reduced compared to the existing sulfide solid electrolyte. Thus, the solid battery including the solid electrolyte of the present invention becomes a solid battery with a high discharge capacity and a solid battery with good discharge rate characteristics (i.e., rate characteristics).
[0015] The detailed reason why the solid electrolyte of the present invention can reduce the reaction resistance with the active material is not clear, for example, it is considered as follows. First, when the weight reduction is observed under the prescribed conditions, the sulfide solid electrolyte contains a substance that can reduce the weight under the prescribed conditions. As such a substance, for example, a hydrate can be listed. Here, the case where the weight reduction observed in the above-mentioned temperature range is from a hydrate is described.
[0016] When the weight reduction of the solid electrolyte of the present invention is determined by thermogravimetric measurement under prescribed conditions, it is possible to reduce the reaction resistance with the active material when the solid electrolyte of the present invention contains a hydrate. It is believed that the reason is that a film is formed on the surface of the sulfide solid electrolyte by contacting the hydrate or a portion of the hydrate with the sulfide solid electrolyte, and the contact state between the sulfide solid electrolyte and the active material becomes good through the formation of the film. It should be noted that although the hydrate is used as an example here, the inventors believe that the above-mentioned effects can be expected even for other substances.
[0017] In the present invention, in a thermogravimetric measurement performed at a heating rate of 10°C / min, the weight loss rate when heated from 25°C to 400°C is 2.7% or more and 9.6% or less. When the weight loss during thermogravimetric measurement of the solid electrolyte of the present invention under specified conditions comes from a hydrate, it is preferred that the weight loss rate when heated in a specified temperature range is 2.7% or more and 9.6% or less. Among them, the so-called "prescribed temperature range" is preferably a temperature range in which the hydrate volatilizes, for example, it can be above 50°C or above 100°C. On the other hand, the "prescribed temperature range" can be, for example, below 300°C, below 250°C, below 200°C, or below 170°C. Furthermore, the weight loss of the hydrate becomes significant particularly when heated from 100°C to 170°C.
[0018] The solid electrolyte of the present invention preferably has a weight reduction rate of 1.0% or more and 4.7% or less when heated from 100°C to 170°C in a thermogravimetric measurement performed at a heating rate of 10°C / min. The above-mentioned weight reduction rate is preferably 1.5% or more, and more preferably 1.8% or more. On the other hand, the above-mentioned weight reduction rate is more preferably 4.6% or less. By making the weight reduction rate under the prescribed conditions within the above range, the effect of the present invention can be made more significant.
[0019] From the viewpoint of making the above advantageous effects more significant, the weight reduction rate (unit: "weight %) of the solid electrolyte of the present invention when heated from 25°C to 400°C in thermogravimetric measurement is 2.7% or more and 9.6% or less. The above weight reduction rate is, for example, preferably 3.0% or more, more preferably 4.0% or more, particularly preferably 5.0% or more, and particularly preferably 6.0% or more. On the other hand, the above weight reduction rate is, for example, preferably 9.0% or less, more preferably 8.5% or less, and particularly preferably 8.0% or less. By having the above weight reduction rate within the above range, the reaction resistance between the sulfide solid electrolyte and the active material is further reduced, so it is preferred.
[0020] The weight reduction rate was calculated by the following formula (1).
[0021] Weight reduction rate (wt%) = (W 25 -W 400 ) / W 25 ×100 (1)
[0022] Where W 25 Indicates the weight of the sample at 25°C (g), W 400 It shows the weight (g) of the sample at 400°C.
[0023] Thermogravimetric measurement is performed at a heating rate of 10°C / min. The atmosphere is preferably an Ar atmosphere. For example, TG-DTA2000SA (trade name) manufactured by MAC Science Co., Ltd. can be used for the measurement. In order to suppress an increase in weight loss, the sulfide solid electrolyte before the measurement is stored in an environment with a dew point of -50°C or less.
[0024] As mentioned above, the solid electrolyte of the present invention preferably comprises Li element, P element, S element and halogen (X) element. When the solid electrolyte of the present invention comprises a hydrate of lithium halide, the type of X element as a constituent element of the sulfide solid electrolyte and the type of X element as a constituent element of the hydrate of lithium halide may be the same, or may be different. The X element as a constituent element of the hydrate of lithium halide is, for example, preferably one or more of F element, Cl element, Br element and I element. In addition, the number of hydrated water contained in the hydrate of lithium halide may be, for example, 1, or may be more than 2. The research results of the inventors confirmed that satisfactory results were obtained by using a monohydrate.
[0025] As a method for obtaining the solid electrolyte of the present invention, for example, as long as it is a method for obtaining a sulfide solid electrolyte that can reduce weight under the specified conditions specified in the present invention, there is no particular limitation. For example, a method for obtaining a sulfide solid electrolyte containing a compound that volatilizes by heating under specified conditions can be cited. Specifically, a method for obtaining a sulfide solid electrolyte containing a compound having water of crystallization can be cited. In the present invention, after adding the above-mentioned compound to obtain the solid electrolyte of the present invention, a crushing step can be performed as needed. There is no particular limitation on the crushing means, and the crushing can be carried out by known crushing means such as a ball mill and a bead mill.
[0026] There are no particular restrictions on compounds having water of crystallization, and various compounds can be used as long as the properties of the sulfide solid electrolyte are not impaired. The hydrated salt of an organic compound is not particularly limited as long as it is a hydrated salt of a general organic compound. For example, hydrated salts of carboxylic acids can be cited. As hydrated salts of carboxylic acids, for example, hydrated salts of formic acid, hydrated salts of acetic acid, hydrated salts of propionic acid, hydrated salts of butyric acid, hydrated salts of valeric acid, hydrated salts of caproic acid, hydrated salts of heptanoic acid, hydrated salts of capric acid, hydrated salts of nonanoic acid, hydrated salts of lauric acid, hydrated salts of myristic acid, hydrated salts of palmitic acid, hydrated salts of stearic acid, hydrated salts of eicosanoic acid, hydrated salts of behenic acid, hydrated salts of montanic acid, hydrated salts of triacontanic acid, etc.; fatty acid derivatives such as hydrated salts of 1,2-hydroxystearic acid; hydrated salts of oxalic acid, hydrated salts of fumaric acid, hydrated salts of maleic acid, hydrated salts of succinic acid, hydrated salts of glutaric acid, hydrated salts of adipic acid, etc. can be cited. aliphatic dicarboxylic acids such as hydroxylated acid, hydroxylated acid, hydroxybutyric acid, hydroxylated acid, hydroxylated acid; and hydroxylated acid such as hydroxylated acid.
[0027] On the other hand, the hydrated salt of the inorganic compound is not particularly limited as long as it is a hydrated salt of a general inorganic compound. For example, hydrates of halides, hydrates of oxides, hydrates of nitrides, hydrates of carbides, hydrates of borides, etc. can be listed, wherein it is preferred that these hydrates contain alkali metals, and it is particularly preferred that the hydrates of halides contain alkali metals. These compounds can be used alone or in combination of two or more. When the solid electrolyte of the present invention contains a compound having water of crystallization, the content ratio of the compound having water of crystallization is preferably a ratio that can effectively reduce the reaction resistance. The above-mentioned content ratio is, for example, preferably greater than 0 mass%, more preferably 5 mass% or more, and particularly preferably 10 mass% or more. On the other hand, the above-mentioned content ratio is, for example, preferably less than 50 mass%, more preferably less than 45 mass%, and particularly preferably less than 40 mass%.
[0028] From the viewpoint of further reducing the reaction resistance with the active material, the particularly preferred sulfide solid electrolyte used in the present invention is a material containing a crystal phase having an argyrodite-type crystal structure. The so-called argyrodite-type crystal structure is a crystal structure possessed by a compound group derived from a mineral represented by the chemical formula: Ag8GeS6. From the viewpoint of further reducing the reaction resistance with the active material, it is particularly preferred that the sulfide solid electrolyte having an argyrodite-type crystal structure has a crystal structure belonging to a cubic crystal.
[0029] In the sulfide solid electrolyte including a crystal phase having an argyrodite-type crystal structure, as the halogen element contained therein, for example, one or more elements selected from the group consisting of F element, Cl element, Br element and I element can be used. From the viewpoint of improving ion conductivity, it is particularly preferable to use the Cl element and the Br element in combination as the halogen element.
[0030] From the viewpoint of further improving ion conductivity, a sulfide solid electrolyte containing a crystal phase having an argyrodite-type crystal structure is particularly preferred, for example, a sulfide solid electrolyte having a composition formula (I): Li a PS b X c A compound represented by (X is at least one of fluorine (F) element, chlorine (Cl) element, bromine (Br) element, and iodine (I) element). X is preferably one or two of chlorine (Cl) element and bromine (Br) element.
[0031] In the above composition formula (I), a, which represents the molar ratio of the lithium element, is preferably 3.0 or more and 6.5 or less, more preferably 3.5 or more and 6.3 or less, and further preferably 4.0 or more and 6.0 or less. As long as a is within this range, the cubic argyrodite-type crystal structure near room temperature (25° C.) is stable, and the conductivity of lithium ions can be improved.
[0032] In the above composition formula (I), b is a value indicating how much less the Li2S component is relative to the stoichiometric composition. From the viewpoint of stabilizing the argyrodite-type crystal structure near room temperature (25°C) and improving the conductivity of lithium ions, b is preferably 3.5 or more and 5.5 or less, more preferably 4.0 or more and 5.3 or less, and further preferably 4.2 or more and 5.0 or less.
[0033] In the above composition formula (I), c is preferably 0.1 or more and 3.0 or less, more preferably 0.5 or more and 2.5 or less, and further preferably 1.0 or more and 1.8 or less.
[0034] In addition, the sulfide solid electrolyte including a crystal phase having an argyrodite-type crystal structure may be, for example, a sulfide solid electrolyte having a composition formula (II): Li 7-d PS 6-d X d The composition represented by the composition formula (II) is the stoichiometric composition of the argyrodite type crystal phase. In the composition formula (II), X has the same meaning as in the composition formula (I).
[0035] In the above composition formula (II), d is preferably 0.4 or more and 2.2 or less, more preferably 0.8 or more and 2.0 or less, and further preferably 1.2 or more and 1.8 or less.
[0036] Furthermore, the sulfide solid electrolyte including a crystal phase having an argyrodite-type crystal structure may be, for example, a sulfide solid electrolyte having a composition formula (III): Li 7-d-2e PS 6-d-e X d The argyrodite-type crystal phase having a composition represented by formula (III) is generated, for example, by the reaction of the argyrodite-type crystal phase having a composition represented by formula (II) with P2S5 (phosphorus pentasulfide). The reaction formula is shown below.
[0037] Li 7-d PS 6-d X d +y / 3P2S5→Li 7-d-2e PS 6-d-e X d +2y / 3Li3PS4
[0038] As shown in the above reaction formula, Li3PS4 phase is generated together with the argyrodite-type crystal phase represented by the composition formula (III). In addition, a trace amount of LiX phase (X is at least one of fluorine (F) element, chlorine (Cl) element, bromine (Br) element, and iodine (I) element) is sometimes generated. In the composition formula (III), X and d have the same meaning as in the composition formula (II).
[0039] In the composition formula (III), e is a value indicating the deviation of the Li2S component from the stoichiometric composition represented by the composition formula (II). e is preferably greater than -0.9 and less than (-d+2), more preferably greater than -0.6 and less than (-d+1.6), and further preferably greater than -0.3 and less than (-d+1.0).
[0040] In the composition formula (I), (II) or (III), a part of P may be replaced by at least one or more elements selected from Si, Ge, Sn, Pb, B, Al, Ga, As, Sb and Bi. In this case, the composition formula (I) becomes Li a (P 1-y M y )S b X c , the composition formula (II) becomes Li 7-d (P 1-y M y )S 6-d X d , the composition formula (III) becomes Li 7-d-2e (P 1-y M y )S 6-d-e X dM is one or more elements selected from Si, Ge, Sn, Pb, B, Al, Ga, As, Sb and Bi. y is preferably 0.01 to 0.7, more preferably 0.02 to 0.4, and further preferably 0.05 to 0.2.
[0041] Whether the sulfide solid electrolyte includes a crystal phase having an argyrodite-type crystal structure can be confirmed by, for example, XRD measurement. That is, in an XRD measurement using an X-ray diffraction device (XRD) using CuKα1 rays, the crystal phase of the argyrodite-type structure has characteristic peaks at 2θ=15.34°±1.00°, 17.74°±1.00°, 25.19°±1.00°, 29.62°±1.00°, 30.97°±1.00°, 44.37°±1.00°, 47.22°±1.00°, and 51.70°±1.00°. In addition, for example, characteristic peaks are present at 2θ=54.26°±1.00°, 58.35°±1.00°, 60.72°±1.00°, 61.50°±1.00°, 70.46°±1.00°, and 72.61°±1.00°. On the other hand, the fact that the sulfide solid electrolyte does not contain a crystalline phase of an argyrodite structure can be confirmed by the fact that it does not have a peak characteristic of a crystalline phase of an argyrodite structure.
[0042] The so-called sulfide solid electrolyte has a argyrodite crystal structure, which means that the sulfide solid electrolyte has at least a crystalline phase of the argyrodite structure. In the present invention, it is preferred that the sulfide solid electrolyte has a crystalline phase of the argyrodite structure as the main phase. The so-called "main phase" refers to the phase that accounts for the largest proportion relative to the total amount of all crystalline phases constituting the sulfide solid electrolyte. Therefore, with respect to the content ratio of the crystalline phase of the argyrodite structure contained in the sulfide solid electrolyte, relative to all crystalline phases constituting the sulfide solid electrolyte, for example, it is preferably 60% by mass or more, more preferably 70% by mass or more, 80% by mass or more, and 90% by mass or more. The proportion of the crystalline phase can be confirmed, for example, by XRD.
[0043] The solid electrolyte of the present invention is made of a powder as a particle aggregate. From the viewpoint of improving ion conductivity, the solid electrolyte of the present invention preferably has a volume cumulative particle size D at a cumulative volume of 50% by volume obtained by a laser diffraction scattering particle size distribution measurement method. 50 For example, it is 0.1 μm or more, more preferably 0.3 μm or more, and even more preferably 0.5 μm or more. 50 For example, it is preferably 20 μm or less, more preferably 10 μm or less, and further preferably 5 μm or less. The volume cumulative particle size D of the sulfide solid electrolyte is 50By making the particle size D of the sulfide solid electrolyte larger than 0.1 μm, the surface area of the entire powder formed by the sulfide solid electrolyte can be prevented from excessively increasing, and the occurrence of disadvantages such as increased resistance and difficulty in mixing with the active material can be effectively prevented. 50 When the solid electrolyte of the present invention is used in combination with other solid electrolytes, for example, the solid electrolyte of the present invention becomes easy to enter the gap of the other solid electrolytes, etc. Therefore, the contact points between the solid electrolytes increase and the contact area increases, which can effectively improve the ion conductivity.
[0044] The lithium ion conductivity of the solid electrolyte of the present invention at room temperature (25°C) shows a high value of preferably 4.0 mS / cm or more, more preferably 4.5 mS / cm or more, and further preferably 5.0 mS / cm or more. The lithium ion conductivity is measured using the method described below. The sulfide solid electrolyte is uniaxially pressed in a glove box replaced with fully dry Ar gas (dew point below -60°C) and in a ceramic cylinder (diameter 10 mm). The upper and lower surfaces of the molded sulfide solid electrolyte are clamped as electrodes with a hard chrome-plated SUS punch with a diameter of 10 mm, and fixed at 4 points with M6-sized bolts and nuts with a tightening torque of 6 N·m to prepare a sample for measuring the ionic conductivity of the sulfide solid electrolyte with a thickness of 0.4 mm to 1.0 mm. The ionic conductivity of the sample is measured using a frequency response measuring device 1260A manufactured by Solartron. The measurement is performed using an AC impedance method at a temperature of 25°C and a frequency of 0.1 Hz to 1 MHz.
[0045] The solid electrolyte of the present invention can be used as a material constituting a solid electrolyte layer, an electrode mixture constituting a solid electrolyte layer containing an active substance. Specifically, it can be used as a positive electrode mixture constituting a positive electrode layer containing a positive electrode active substance, or a negative electrode mixture constituting a negative electrode layer containing a negative electrode active substance. Therefore, the solid electrolyte of the present invention can be used in a battery having a solid electrolyte layer, a so-called solid battery. More specifically, it can be used in a lithium solid battery. A lithium solid battery can be a primary battery or a secondary battery, and is preferably used in a lithium secondary battery. It should be noted that the so-called "solid battery", in addition to a solid battery that does not contain any liquid substance or gel-like substance as an electrolyte, also includes a form containing, for example, less than 50% by mass, less than 30% by mass, or less than 10% by mass of a liquid substance or gel-like substance as an electrolyte.
[0046] The solid electrolyte layer of the present invention can be manufactured by, for example, the following methods: a method of dropping a slurry containing a sulfide solid electrolyte, a binder and a solvent onto a substrate and flattening it with a scraper or the like; a method of cutting the substrate with an air knife after contacting the slurry; a method of forming a coating film by screen printing or the like, and then removing the solvent by heating and drying. Alternatively, it can also be manufactured by appropriately processing the powder of the solid electrolyte of the present invention after compression molding. In the solid electrolyte layer of the present invention, in addition to the solid electrolyte of the present invention, other solid electrolytes may also be included. The thickness of the solid electrolyte layer of the present invention is typically preferably 5 μm or more and 300 μm or less, and more preferably 10 μm or more and 100 μm or less.
[0047] The solid battery has a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer, and has the solid electrolyte of the present invention. Examples of the shape of the battery include a laminated body, a cylindrical shape, and a square shape.
[0048] As the active material contained in the above-mentioned positive electrode mixture, for example, an active material used as a positive electrode active material for a lithium secondary battery can be appropriately used. As the positive electrode active material, for example, spinel-type lithium transition metal compounds, lithium metal oxides having a layered structure, etc. can be listed. The particles of the positive electrode active material may have a coating layer on their surface that can reduce the reaction resistance between the sulfide solid electrolyte and the positive electrode active material. In particular, according to the present invention, even if a coating layer is not formed on the surface of the particles of the active material, the reaction resistance between the sulfide solid electrolyte and the active material can be reduced, so there is no need to actively form a coating layer on the surface of the particles of the active material. In addition to the positive electrode active material, the positive electrode mixture may also contain other materials headed by a conductive auxiliary agent.
[0049] As the active material contained in the above-mentioned negative electrode mixture, for example, an active material used as a negative electrode active material of a lithium secondary battery can be appropriately used. As the negative electrode active material, for example, carbon materials such as lithium metal, artificial graphite, natural graphite and difficult graphitization carbon (hard carbon), silicon, silicon compounds, tin and tin compounds can be listed. In addition to the negative electrode active material, the negative electrode mixture may also include other materials headed by a conductive auxiliary agent.
[0050] Example
[0051] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to the examples.
[0052] [Example 1]
[0053] (1) Manufacturing of solid electrolyte
[0054] To become Li 5.4 PS4.4 Cl 0.8 Br 0.8 Li2S powder, P2S5 powder, LiCl powder and LiBr powder were weighed in a manner of composition so that the total amount reached 75 g. These powders were crushed and mixed using a ball mill to obtain a mixed powder. The mixed powder was sintered to obtain a sintered product of the above-mentioned composition. The sintering was carried out using a tubular electric furnace. During the sintering, 100% pure hydrogen sulfide gas was circulated in the electric furnace at 1.0 L / min. The sintering temperature was set to 500°C and sintering was carried out for 4 hours. The sintered product was crushed using a mortar and pestle, and then pulverized using a wet bead mill to obtain a solid electrolyte. The results of the XRD measurement confirmed that the solid electrolyte had a crystalline phase of a argyrodite-type structure.
[0055] The obtained solid electrolyte was mixed with LiBr·H2O in an Ar atmosphere to obtain the target solid electrolyte. The amount of LiBr·H2O added was 10 mass % relative to the total amount of the solid electrolyte and LiBr·H2O.
[0056] [Example 2]
[0057] A solid electrolyte was obtained in the same manner as in Example 1 except that the amount of LiBr·H 2 O added was 20 mass %.
[0058] [Example 3]
[0059] A solid electrolyte was obtained in the same manner as in Example 1 except that the amount of LiBr·H 2 O added was 30 mass %.
[0060] [Example 4]
[0061] A solid electrolyte was obtained in the same manner as in Example 1 except that the amount of LiBr·H 2 O added was 40 mass %.
[0062] [Comparative Example 1]
[0063] A solid electrolyte was obtained in the same manner as in Example 1 except that LiBr·H 2 O was not added.
[0064] [Comparative Example 2]
[0065] A solid electrolyte was obtained in the same manner as in Example 1 except that the amount of LiBr·H 2 O added was 50 mass %.
[0066] [evaluate]
[0067] For the solid electrolytes obtained in the examples and comparative examples, thermogravimetric measurement was performed using the above method, and the weight reduction rate when heated from 25°C to 400°C was measured. The weight reduction rate per 50°C is shown in Table 1. In addition, the weight reduction rate when heated from 100°C to 170°C by thermogravimetric measurement using the above method is shown in Table 2. Furthermore, using the solid electrolytes obtained in the examples and comparative examples, solid batteries were prepared using the following method, and the reaction resistance was measured. Their results are shown in Table 1.
[0068] [Measurement of reaction resistance]
[0069] The positive electrode was prepared by a conventional method using the solid electrolytes of the examples and comparative examples. Specifically, 60 parts of LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, 37 parts of solid electrolyte and 3 parts of conductive carbon material are mixed to make a positive electrode mixture, which is then made into a positive electrode layer.
[0070] 47.5 parts of Si powder, 47.5 parts of solid electrolyte, and 5 parts of conductive carbon material were mixed to prepare a negative electrode mixture, which was then used as a negative electrode layer.
[0071] Next, the positive electrode, the solid electrolyte of the embodiment and the comparative example, and the negative electrode were stacked in sequence and pressed to form a solid battery. For the solid battery, after the third cycle of charge and discharge, after charging to 3.7V, AC impedance measurement was performed. Specifically, for the battery cell after charge and discharge, an electrochemical measurement system consisting of a voltage regulator Solartron1280Z manufactured by Solartron Analytical and a frequency response device Solartron1260 was used to make the open circuit voltage of the battery cell a DC bias, an AC amplitude of 10mV was applied, and the frequency of 1.0×10 6 ~1.0×10 -1 The diameter of the arc of the complex impedance diagram obtained by measurement is taken as the reaction resistance (Ω).
[0072]
[0073] Table 2
[0074]
[0075] From the results shown in Table 1, it can be seen that the solid batteries produced using the solid electrolytes obtained in the examples have lower reaction resistance than the solid batteries produced using the solid electrolytes obtained in the comparative examples.
[0076] Industrial Applicability
[0077] According to the present invention, a sulfide solid electrolyte capable of reducing the reaction resistance with an active material is provided.
Claims
1. A sulfide solid electrolyte, wherein in a thermogravimetric measurement performed at a heating rate of 10°C / min, the weight loss rate from hydrate when heated from 25°C to 400°C is 2.7% or more and 9.6% or less, and the weight loss rate from hydrate when heated from 100°C to 170°C is 1.0% or more, The sulfide solid electrolyte contains lithium (Li) element, phosphorus (P) element, sulfur (S) element, halogen (X) element and oxygen (O) element.
2. The sulfide solid electrolyte according to claim 1, wherein The halogen (X) element is at least one of chlorine (Cl), bromine (Br) and iodine (I). 3 . An electrode mixture comprising the sulfide solid electrolyte according to claim 1 or 2 and an active material.
4. A solid battery comprising a positive electrode layer, a negative electrode layer and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer, wherein: The solid electrolyte layer contains the sulfide solid electrolyte according to claim 1 or 2.